Biofouling resistant roofing coatings

By using acrylic polymer binder and non-toxic antifouling additives on the roof, the antifouling coating is formed, and the problem of bioscaling on the roof is solved, and the roof life is extended and the energy reflection is improved. Environmentally friendly and harmless.

CN118946642APending Publication Date: 2024-11-12DOW GLOBAL TECHNOLOGIES LLC +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029385.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-02
Filing Date
2023-04-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively and environmentally friendly to prevent roof bioscaling for a long time, especially on low slope and flat roofs. The commonly used biocide methods are labor-intensive, short-term and may damage the environment.

Method used

An antifouling coating is formed to inhibit the adhesion and growth of bioscaling organisms by spraying or brushing on the roof surface using an aqueous coating composition containing an acrylic polymer binder and a non-toxic antifouling additive.

Benefits of technology

Effectively extend the life of the roof, reduce bioscaling, improve the roof's reflective energy capacity, and do not use harmful biocides, which is environmentally friendly and long-term effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005054230740000141
    Figure BDA0005054230740000141
  • Figure BDA0005054230740000151
    Figure BDA0005054230740000151
  • Figure BDA0005054230740000161
    Figure BDA0005054230740000161
Patent Text Reader

Abstract

Biofouling of roof structures is reduced by applying to a roof a coating composition containing an acrylic binder and a non-toxic antifouling additive that interferes with the ability of biofouling to adhere to the coating. Examples of non-toxic antifouling additives include polysiloxanes and cross-linked silicone rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of roof systems. Background Art

[0002] Biofouling is a well-known problem in many situations. Bacteria, algae, mold, mildew and more complex organisms attach to and grow on ships, docks, homes and other structures. This growth can interfere with the function of the structure it is on and can damage the surface it is on.

[0003] Biofouling problems are widespread on roofs. Roof surfaces can include many different materials, such as shingles, tiles, metal roofs, polymer membranes, or composite roofs made of asphalt and reinforcement layers. Roof surfaces may also have different angles or "slopes" from the horizontal. Some roofs have a slope of 10 degrees or less (no more than 2 horizontal feet per 12 vertical feet) and are considered low-slope roofs. Some roofs are substantially horizontal and are considered flat roofs. Shingles and tiles are commonly used in roofs with a slope of more than 10 °, while metals and membranes are commonly used in low-slope or horizontal roofs. Composite roofs are only common in flat roofs. Examples of common membranes include ethylene propylene diene terpolymers (EPDM), thermoplastic polyolefins (TPO), and polyvinyl chloride.

[0004] Roofs, especially low-slope and flat roofs, are often coated with coating compositions to provide additional protection to the roof substrate. The coating compositions often contain white pigments to reflect sunlight so as to reduce heat and energy to the structure below the roof.

[0005] All roofs are susceptible to biofouling organisms, such as bacteria, algae, mold and mildew, and other organisms. Flat roofs are more susceptible because they collect water after heavy rains. Biofouling organisms can stain the light-colored surface of the roof and increase the amount of solar energy it absorbs. In addition, biofouling organisms can firmly attach to the roof and cause coating failure through repeated wet-dry cycles.

[0006] A common method of treating biofouling on roofs is to wash the roof with a biocide that kills the biofouling organisms. Sodium hypochlorite (bleach) solutions are often used for this purpose. This method is undesirable for several reasons. It is labor intensive. It requires cleaners to work on the roof, which can damage the roof and is dangerous on sloped roofs. It is a short-term solution and must be repeated regularly. It requires the use of large amounts of biocide on the roof; the biocide will eventually wash off the roof and may harm desirable plants around the structure or enter the ecosystem.

[0007] What is needed is a long-term, environmentally friendly solution to roof biofouling. Summary of the invention

[0008] Antifouling coatings are divided into two categories: toxic and non-toxic. Toxic antifouling coatings contain biocidal additives that are released over time and kill biofouling organisms that adhere to the coating. Examples of biocidal additives include 4,5-dichloro-2-octyl-4-isothiazolin-3-one (DCOIT), 2-n-octyl-4-isothiazolin-3-one (OIT), and zinc pyrithione (ZPT). Non-toxic antifouling coatings are formulated to prevent biofouling organisms from attaching to the coating. Biofouling organisms that cannot attach to solid surfaces generally cannot grow or reproduce adequately and do not create biofouling problems.

[0009] One aspect of the present invention is a method of protecting a roof of a structure having an exposed top surface, the method comprising the steps of:

[0010] a. applying an aqueous coating composition to the top surface of the roof, the aqueous coating composition comprising the following coating components dissolved or suspended in an aqueous solvent:

[0011] i. an acrylic polymer binder in a concentration suitable for forming a stable coating,

[0012] ii. a non-toxic antifouling additive in a concentration suitable for inhibiting scaling on the roof, and

[0013] iii. 0 wt % to 80 wt % of other coating components based on the weight of the coating components in the composition excluding the solvent; and

[0014] b. Drying the aqueous coating composition so that it forms a solid coating adhered to the top surface of the roof.

[0015] A second aspect of the present invention is an aqueous coating composition that can be used in the method of the present invention, the coating composition comprising the following coating components dissolved or suspended in an aqueous solvent:

[0016] a) an acrylic polymer binder having a glass transition temperature not exceeding 0° C. at a concentration suitable for forming a stable coating;

[0017] b) a non-toxic antifouling additive in a concentration suitable for inhibiting scaling on the roof; and

[0018] c) 0% to 80% by weight of other coating components, based on the weight of the coating components in the composition excluding the solvent.

[0019] A third aspect of the invention is a structure comprising a roof having an exposed top surface, wherein a solid coating is adhered to the top surface of the roof and the coating contains the following coating components: (a) an acrylic polymer binder having a glass transition temperature of no more than 0° C. and bonding the coating to the roof; (b) a nontoxic antifouling additive at a concentration suitable for inhibiting scaling on the roof; and (c) 0 wt % to 80 wt % of other coating components, based on the weight of the coating components in the composition excluding solvents.

[0020] Using the present invention, biofouling of a roof can be inhibited, extending the life of the roof and the ability of the roof to reflect energy without introducing unnecessary biocides into the environment. DETAILED DESCRIPTION

[0021] The present invention uses a waterborne coating composition comprising an acrylic binder and a non-toxic antifouling additive. In some embodiments, the waterborne coating composition may also contain other components such as pigments, thickeners, surfactants, hydrophobic additives, leveling agents and coalescing agents, antioxidants, UV stabilizers, fillers or other additives known for outdoor coatings.

[0022] Solvents

[0023] The coating composition contains an aqueous solvent. The term "solvent" does not mean that all coating components of the composition are soluble or dissolved in the solvent; some or all coating components may be suspended in the solvent as a suspension or emulsion, with or without an emulsifier. In some embodiments, the pH of the aqueous solvent is at least 5, or at least 5.5, or at least 6, or at least 6.5, or at least 6.75, or at least 6.9. In some embodiments, the pH of the aqueous solvent is at most 9.8, or at most 8.5, or at most 8, or at most 7.7, or at most 7.5, or at most 7.2.

[0024] Binder

[0025] The coating composition contains an acrylic polymer binder. Acrylic polymer binders and dispersions thereof are known and they are commercially available. They are described in publications such as "Paints" published by the Department of Chemistry at York University at https: / / www.essentialchemicalindustry.org / materials-and-applications / paints.html (March 18, 2013).

[0026] Acrylic polymers are polymers or copolymers containing repeating units derived from acrylic acid monomers. Acrylic acid monomers include acrylic acid, methacrylic acid, and their esters. Exemplary esters used in acrylic acid monomers include alkyl esters, such as alkyl groups containing 1 to 8 carbon atoms or 1 to 4 carbon atoms, or in some cases methyl groups or ethyl groups. Particularly useful acrylic acid monomers are acrylic acid, methacrylic acid, butyl acrylate, 2-ethylhexyl acrylate, methyl acrylate, ethyl acrylate, methyl methacrylate, and ethyl methacrylate.

[0027] Exemplary acrylic polymers may contain at least 70% by weight, or at least 80% by weight, or at least 90% by weight, or at least 95% by weight of repeating units derived from acrylic acid monomers. Exemplary acrylic polymers may contain up to 100% of repeating units derived from acrylic acid monomers. Some exemplary acrylic polymers are copolymers containing units derived from two or more acrylic acid monomers, such as copolymers of butyl acrylate with methyl methacrylate and / or methacrylic acid. Some exemplary acrylic polymers may also contain ethylenically unsaturated comonomers derived from non-acrylic acids, such as vinyl acetate and similar vinyl esters or styrene.

[0028] The choice of acrylic monomers and their proportions depends on the intended use of the acrylic polymer. Binders used in roof coatings may be subject to thermal expansion and contraction at low temperatures. Acrylic binders may be selected to have a low Tg, such as up to 0°C, or -10°C, or -15°C, or -20°C, or 30°C, or 40°C. There is no minimum desired Tg, but a Tg below -60°C is rarely necessary.

[0029] It is known that increasing the content of certain monomers (such as methyl methacrylate) will increase the Tg of the resulting polymer, and it is known that increasing the content of other monomers (such as butyl acrylate) will reduce the Tg of the resulting polymer. In some embodiments, the acrylic polymer binder comprises at least 7 weight % or at least 10 weight % or at least 12 weight % of units derived from methyl methacrylate. In some embodiments, the acrylic polymer binder comprises at most 50 weight % or at most 45 weight % or at most 40 weight % of units derived from methyl methacrylate. In some embodiments, the acrylic polymer binder comprises at least 50 weight % or at least 55 weight % or at least 60 weight % of units derived from butyl acrylate. In some embodiments, the acrylic polymer binder comprises at most 93 weight % or at most 90 weight % or at most 88 weight % of units derived from butyl acrylate.

[0030] In some embodiments, the particles of the acrylic polymer binder have an average diameter of at least 50 nm, or at least 100 nm, or at least 200 nm. In some embodiments, the particles of the acrylic polymer binder have an average diameter of at most 700 nm, or at most 500 nm, or at most 400 nm.

[0031] In coatings for roof applications, it is also useful for the acrylic polymer binder to remain non-melting at the temperatures to which the roof is typically exposed. In some embodiments, the melting temperature of the acrylic polymer binder is at least 60° C., or at least 75° C., or at least 80° C., or at least 95° C., or at least 110° C. There is no maximum desired melting temperature, but temperatures above 200° C. are rarely necessary.

[0032] In coatings for roofing applications, it is also useful for the acrylic binder to be stable under ultraviolet light.In some embodiments, the acrylic binder is substantially free of aromatic groups, such as avoiding phenyl esters of acrylic acid and methacrylic acid.

[0033] Binders are generally film-forming under the conditions under which they are applied to the intended substrate. "Film-forming" means that the substance is capable of forming a film when applied to a solid surface. The ability of polymers and their solutions or emulsions to form films is known and described in publications such as: P.A. Steward et al., "An Overview of Polymer Latex Film Formation and Properties", 1986. Advances in Colloid and Interface Science , 195-267 (2000) and J. Guerts et al., "New Waterborne Acrylic Binders for Zero VOC Paints", 5 J.CoatingTechnol.Res .57-63(2008). In general, the film-forming ability of a polymer increases with lower molecular weight and / or lower Tg, and decreases with higher molecular weight and / or higher Tg.

[0034] In coatings for structural and outdoor applications, a binder that is insoluble in water may be selected so that the coating remains stable in rain and humidity.

[0035] In the coating composition, the binder particles are suspended in an aqueous dispersion. In some embodiments, the binder particles contain surface modifications to prevent particle agglomeration, or the dispersion contains a dispersing agent (also referred to as a dispersant) to prevent particle agglomeration. For example, in some embodiments, the aggregation of charged parts on the surface of the binder particles can inhibit the agglomeration of the binder particles. The charge on the surface of the particles can be measured by zeta potential, as described in "Zeta Potential-An Introduction in 30 Minutes", which is published by Malvern Panalytical (2010) and can be obtained at https: / / www.malvernpanalytical.com / en / . In some embodiments, the zeta potential of the binder particles in the suspension is at least 30mV, or at least 40mV, or at least 50mV, or at least 60mV. It is known that the zeta potential of polymer particles is increased by incorporating polarized monomers that preferentially aggregate on the surface of polymer particles into polymers. In some embodiments, the dispersion contains a dispersing agent (such as a surfactant) to stabilize the particles and prevent agglomeration. In some embodiments, the surfactant is a nonionic surfactant.

[0036] Examples of commercially available binders include those sold under the trade names RHOPLEX TM 、PARALOID TM and MAINCOTE TM Acrylic polymers and polymer dispersions are available from the Dow Chemical Company under the trademark AUTOEXA®.

[0037] The concentration of the binder in the coating composition is suitable for adhering the coating components of the composition to the substrate to which the composition is applied. In some embodiments, the binder accounts for at least 20% by weight, or at least 25% by weight, or at least 35% by weight, or at least 45% by weight of the coating components in the composition (excluding the solvent). In some embodiments, the binder accounts for at most 80% by weight, or at most 70% by weight, or at most 60% by weight of the coating components in the composition (excluding the solvent).

[0038] (“Coating components” are the non-volatile components of the aqueous coating composition other than solvents that are expected to be deposited on the roof and become part of the roof coating. Binders, non-toxic antifouling additives, and other components listed below are coating components. In many cases, when they are not dissolved or suspended in a solvent, they are solid or glassy solids at room temperature, and they are often referred to as “solids”).

[0039] Non-toxic antifouling additives

[0040] The compositions useful in the present invention also contain non-toxic antifouling additives. Without wishing to be bound, we assume that non-toxic antifouling additives reduce the ability of biofouling organisms to attach to the coating surface. Examples of non-toxic antifouling additives include:

[0041] a. Polysiloxane

[0042] b. cross-linked silicone rubber particles, and

[0043] c. Fluorinated polymers.

[0044] In some embodiments, the antifouling additive is a silicon-containing material, such as a polysiloxane or a cross-linked silicone rubber.

[0045] Polysiloxanes are known and commercially available. Polysiloxanes are oligomers or polymers characterized by the repeating unit:

[0046] -(-SiR 1 R 2 -O-) n -

[0047] Where R 1 and R 2 Each R group is independently an organic moiety and n is the number of repeating units. In some embodiments, each R group is a relatively non-reactive organic group, such as an unsubstituted or halogenated alkyl, aryl or alkaryl group. For example,

[0048] • One or both R groups may independently be an alkyl or fluorinated alkyl group, and in some embodiments, the alkyl or fluorinated alkyl group may contain 1 up to 8, or up to 6, or up to 4 carbon atoms. In some embodiments, each R group is independently a methyl or trifluoromethyl group.

[0049] • One or both R groups may independently be phenyl or an alkyl-substituted phenyl group, such as dimethylphenyl or trimethylphenyl. In some embodiments, aryl groups may be avoided to improve the photostability of the siloxane.

[0050] In some embodiments, the polysiloxane forms a ring, such as a ring containing 3 or 4 of the above repeating units. In some embodiments, the polysiloxane forms a substantially linear chain terminated at the end with a -OH or -OR3 moiety, wherein R3 is an organic moiety as previously described.

[0051] In some embodiments, the average degree of polymerization (n) is at least 3, or at least 10, or at least 50, or at least 90. In some embodiments, the average degree of polymerization is at most 10,000, or at most 7000, or at most 5000, or at most 4000. In some embodiments, the weight average molecular weight of polysiloxane is at least 700Da, or at least 1500Da, or at least 3000Da, or at least 5000Da. In some embodiments, the weight average molecular weight of polysiloxane is at most 700,000Da, or at most 500,000Da, or at most 350,000Da, or at most 300,000Da, or at most 220,000Da. Many polysiloxanes are liquids at room temperature, and their degree of polymerization can be inferred from their viscosity. In some embodiments, the viscosity of polydimethylsiloxane can be at least 4cSt, or at least 10cSt, or at least 25cSt, or at least 80cSt. In some embodiments, the viscosity of the polydimethylsiloxane may be at most 3,000,000 cSt, or at most 1,500,000 cSt, or at most 1,000,000 cSt, or at most 500,000 cSt, or at most 350,000 cSt.

[0052] In some embodiments, the polysiloxane has a low glass transition temperature (Tg), such as no more than -50°C, or -75°C, or -100°C, or -125°C.

[0053] In some embodiments, the polysiloxane is hydrophobic.

[0054] In some embodiments, the polysiloxane has a low surface tension and is capable of wetting the surface. For example, the surface tension may be at most 40 mN / m, or at most 30 mN / m, or at most 25 mN / m, or at most 21 mN / m.

[0055] Suitable polysiloxanes can be prepared by condensing dichlorosilanes in the presence of excess water, such as Treatise onCoatings Vol 1, Part III (Film Forming Composition). Edited by Raymond R. Myers and JS Long, published by Marcel Dekker, Inc. New York 1972.

[0056] Many suitable polysiloxanes are insoluble in water; they can be maintained in a solvent as an emulsion with an emulsifier. An emulsifier keeps an insoluble liquid suspended in an aqueous solvent. Emulsifiers are typically surfactants, such as anionic surfactants and nonionic surfactants. For example, some commonly used emulsifiers are fatty alkyl sulfates (such as sodium lauryl sulfate), alcohol ether sulfates, aryl sulfonates (such as sodium branched dodecylbenzene sulfonate), alkyl diphenyl oxide disulfonates (such as disodium lauryl phenyl ether disulfonate), nonylphenol ether sulfates (such as ammonium nonylphenol ether sulfate), fatty alcohol ethoxylates, nonylphenol ethoxylates or alkyl phosphates (such as ammonium phosphate), polyoxyethylene tridecyl ether. Suitable emulsifiers can be found under the trademark DOWSIL TM TERGITOL TM TRITON TM , RHODAFAC TM 、RHODACAL TM 、DISPONIL TM , Lutensol and DOWFAX TM get.

[0057] Suitable silicones and silicone emulsions are commercially available, for example under the tradename: DOWSIL TM 8004、DOWSIL TM 84 Additives, DOWSIL TM 910H and DOWSIL TM 8005. One common polysiloxane that can be used is polydimethylsiloxane, which is often abbreviated as PDMS. PDMS is available under the trademark XIAMETER TM Commercially available.

[0058] Crosslinked silicone rubber particles and their emulsions are also known and commercially available. Crosslinked silicone rubber particles are typically prepared by emulsifying a liquid polysiloxane polymer and crosslinking it using a crosslinking agent. Such methods are described in publications such as the following U.S. Patents: 5,708,057; 6,433,041; and 6,710,124 B2.

[0059] The polysiloxane polymer may meet the broad description given above. In some embodiments, the polysiloxane polymer may have a relatively low viscosity and molecular weight within the specified ranges prior to crosslinking.

[0060] Different crosslinking agents and systems are also known.

[0061] In some embodiments, a peroxide catalyst (such as dichlorobenzoyl peroxide or dicumyl peroxide) causes direct free radical crosslinking of unsaturated organic moieties on different polysiloxane chains. An example of this reaction is described in U.S. Patent Publication No. 2022 / 0049097 A1. This reaction is typically carried out at elevated temperatures (such as 80° C. to 200° C.).

[0062] In some embodiments, the polysiloxane has a vinyl moiety that can be crosslinked in the presence of a platinum group catalyst such as platinum, rhodium, palladium, or their oxides. Examples of this polymerization are described in PCT Patent Publication WO 2021 / 262497, and useful catalysts are particularly described in paragraphs

[0033] to

[0037] of the publication. This reaction is typically carried out at room temperature.

[0063] In some embodiments, crosslinking is accomplished by condensing hydrolyzable groups on the polysiloxane using a hydrolyzable crosslinking agent such as methyltrimethoxysilane or methyltriacetoxysilane. The hydrolyzable groups on the polysiloxane and the crosslinked liner are hydrolyzed by water in the presence of a catalyst such as dibutyltin dilaurate, and when the emulsion dries, the hydrolyzable groups condense and crosslink the polymer. This reaction is typically performed at room temperature.

[0064] In some embodiments, the crosslinked silicone rubber particles have an average particle size of at least 0.1 μm, or at least 0.5 μm, or at least 1 μm. In some embodiments, the crosslinked silicone rubber particles have an average particle size of at most 5 μm, or at most 3 μm, or at most 1.5 μm.

[0065] In some embodiments, the glass transition temperature (Tg) of the rubber particles is similar to the Tg already described for siloxanes.

[0066] The rubber is typically suspended in the coating composition as a dispersion, which may use a dispersing agent as described above. Examples of suitable crosslinked rubber dispersions include DOWSIL TM Trademark commercially available.

[0067] Fluorinated polymers suitable for antifouling coatings are known and described in publications such as Nurioglu et al., Non-Toxic, Non-Biocide-Release Antifouling Coatings Based on Molecular Structure Design for Marine Applications, 3 J.Mater.Chem B6547 (2015) and Sun et al., Antifouling Surfaces Based on Fluorine-Containing Asymmetric Polymer Brushes: Effect of Chain Length of Fluorinated Side Chain, 35 Langmuir 1235(2019). In some embodiments, the fluoropolymer dispersion is added to the coating. In some cases, the fluoropolymer side chains are grafted onto another coating composition, such as a polyurethane binder.

[0068] Suitable fluorinated polymers can be prepared by polymerization of the corresponding fluorinated vinyl monomers as described in US Pat. No. 7,851,573 B2.

[0069] Suitable fluoropolymers are commercially available, such as under the trade names: Tedlar, Kynar and Teflon.

[0070] The non-toxic antifouling additive is present in a concentration suitable for reducing biofouling on the roof surface. In some embodiments, the non-toxic antifouling additive accounts for at least 2 weight % or at least 3 weight % or at least 4 weight % or at least 5 weight % of the coating component in the composition (excluding the solvent). In some embodiments, the non-toxic antifouling additive accounts for at most 35 weight % or at most 25 weight % or at most 20 weight % of the coating component in the composition (excluding the solvent). Antifouling additives with mid-range molecular weight or degree of polymerization may be highly effective at the lower limit of the concentration listed above (such as no more than 10 weight % or no more than 8 weight %). On the other hand, antifouling additives with very high or very low molecular weight or degree of polymerization may be more effective at the upper limit of the concentration listed above (such as at least 8 weight % or at least 10 weight % or at least 12 weight %).

[0071] Other components

[0072] The aqueous compositions of the present invention may optionally contain other coating components and additives suitable for roof coatings. Many such components are described in the publication Johan Bieleman (ed.), published by WILEY-VCH Verlag GmbH (2000), Additives for Coatings Some examples of commonly used additives are listed below. All additives listed below are commercially available.

[0073] The aqueous composition may optionally contain a pigment, such as titanium dioxide or carbon black. For roof applications, white or reflective pigments (such as titanium dioxide or metal flakes) may be selected to reflect solar energy and reduce solar heating of the building under the roof. Alternatively, in cold climates, black pigments (such as carbon black) may be selected to increase solar heating of the roof.

[0074] The aqueous composition may optionally contain a thickener to make it easier to handle and apply. Examples of thickeners include inorganic materials (such as certain clays) and polymeric thickeners (such as certain cellulose derivatives, starches, and acrylic acid polymers).

[0075] The aqueous composition may optionally contain a surfactant for a variety of purposes. Some surfactants are emulsifiers, wetting agents, and dispersants that help insoluble components enter and remain in an emulsion or dispersion in an aqueous solvent. Some surfactants are defoamers. Some surfactants can promote adhesion of the adhesive to the roof surface.

[0076] The aqueous composition may optionally contain a hydrophobic additive to increase its resistance to water penetration. Examples of hydrophobic components may include waxes and polymers such as polypropylene.

[0077] The waterborne composition may optionally contain leveling agents and coalescing agents to provide complete coverage and a smooth surface on the roof. Examples of leveling additives include certain polyacrylate polymers that have a low glass transition temperature, such as -20°C or less. Coalescing agents promote the interaction of binder molecules as the coating dries on the substrate to form a solid, uniform film that no longer dissolves when subjected to new water. Examples of coalescing agents include

[0078] Certain branched and cyclic alkanes,

[0079] Certain esters, such as 3-hydroxy-2,2,4-trimethylpentyl isobutyrate (TPiB), adipic acid diester (ADE), dimethyl phthalate (DMP), 2-hydroxypropyl ethylhexanoate (HPE), and benzyl benzoate, and

[0080] • Certain ether alcohols, such as ethylene glycol butyl ether, propylene glycol butyl ether, dipropylene glycol butyl ether (DPB), and propylene glycol and ethylene glycol phenyl ethers (PPH and EPH).

[0081] The aqueous composition may optionally contain an antioxidant. The antioxidant may include a primary antioxidant (such as certain amines or sterically hindered phenols) and / or a secondary antioxidant (such as certain organic phosphates or thioesters).

[0082] The aqueous composition may optionally contain light and ultraviolet (UV) stabilizers. Examples of light and ultraviolet (UV) stabilizers may include:

[0083] UV absorbers, such as benzotriazole and other compounds with coordinated double bonds; and

[0084] Sterically hindered amines, such as compounds containing a 2,2,6,6-tetramethylpiperidinyl group;

[0085] The aqueous composition may optionally contain a filler. Fillers are solid particles added to a coating to improve properties and / or reduce cost. Suitable fillers for coatings are known and commercially available. Examples of suitable fillers include clays (such as kaolin, diatomaceous earth, glass powder and microspheres), aluminum hydroxide and various powdered minerals (such as calcium carbonate, dolomite, feldspar, mica, quartz, silica and silicates), talc and metal carbonates. Fillers and their production and use are described in publications such as: Gysau, Fillers for Paints (3rd Edition), Vincentz Network GmbH & Co. (2017); and "Functional Silicate Fillers: Basic Principles", Painting&CoatingsIndustry (August 1, 2002) ( https: / / www.pcimag.com / articles / 84909-functional-silicate-fillers-basic-principles).

[0086] In some embodiments, the pigment and filler account for at least 20% by weight, or at least 30% by weight, or at least 40% by weight of the coating components in the composition (except the solvent). In some embodiments, the pigment and filler account for at most 80% by weight, or at most 75% by weight, or at most 65% by weight of the coating components in the composition (except the solvent).

[0087] The concentration of other additive components may optionally be lower than that of binder and pigment. In some embodiments, other additive components account for at least 0.2% by weight, or at least 0.5% by weight, or at least 1% by weight of the coating components in the composition (excluding solvent). In some embodiments, other additive components account for up to 20% by weight, or up to 10% by weight, or up to 5% by weight of the coating components in the composition (excluding solvent).

[0088] Aqueous compositions and methods of the present invention

[0089] In some embodiments, the aqueous composition of the present invention contains at least 20% by weight, or at least 30% by weight, or at least 40% by weight, or at least 50% by weight of the coating component. In some embodiments, the aqueous composition of the present invention contains at most 80% by weight, or at most 75% by weight, or at most 70% by weight of the coating component. In some embodiments, the aqueous composition of the present invention contains at least 20% by weight, or at least 25% by weight, or at least 30% by weight of the aqueous solvent. In some embodiments, the aqueous composition of the present invention contains at most 80% by weight, or at most 70% by weight, or at most 60% by weight, or at most 50% by weight of the aqueous solvent.

[0090] In the method of the present invention, the aqueous composition is applied to the roof surface and dried to form a solid coating adhered to the top surface of the roof. In some embodiments, the roof pitch is less than 15 degrees, or less than 10 degrees, or less than 5 degrees from the horizontal plane. In some embodiments, the entire roof pitch is substantially horizontal.

[0091] The roof surface may optionally comprise known materials such as shingles, tiles, metal roofing, polymer membranes, or tar and gravel. In some embodiments, the roof surface comprises a membrane such as ethylene propylene diene terpolymer (EPDM), thermoplastic polyolefin (TPO), or polyvinyl chloride.

[0092] The aqueous composition can be applied to the roof surface by known means, such as spraying, rolling or brushing. As with other aqueous outdoor coatings, it is usually applied during dry weather at a sufficiently high temperature to allow the aqueous solvent to evaporate quickly, leaving a dry coating. In some embodiments, the temperature will be at least 10°C, or 12°C, or at least 15°C, or at least 20°C, or at least 23°C.

[0093] The waterborne composition is allowed to dry, leaving a solid dry coating on top of the roof surface. As with other waterborne outdoor coatings, the waterborne composition can be applied as a single coating, or two or more coatings can be applied, wherein each coating is allowed to dry substantially before applying the next coating.

[0094] The content of dry coating is substantially the same as the coating component of aqueous composition. In some embodiments, dry coating comprises a solvent that is no more than 5 % by weight, or no more than 3 % by weight, or no more than 1 % by weight, or no more than 0.5 % by weight. There is no solvent of the desired content in the coating, but in some cases, it may be impractical to remove the solvent to a content lower than 0.01 % by weight. The coating does not have the necessary thickness, but in some embodiments, the average thickness of the coating is at least 100 μm, or at least 250 μm, or at least 400 μm, and in some embodiments, the average thickness is at most 1000 μm, or at most 800 μm, or at most 600 μm.

[0095] The non-toxic antifouling additives prevent mold, mildew and other organisms from anchoring to the coating. As a result, the organisms cannot grow well and scaling on the coated portion of the roof is reduced.

[0096] In some embodiments, the tensile strength of the dried coating (measured as described in the test methods) is at least 50 psi, or at least 60 psi, or at least 80 psi, or at least 100 psi. There is no maximum desired tensile strength, but tensile strengths above 500 psi are generally unnecessary.

[0097] In some embodiments, the elongation at break of the dried coating (measured as described in the test methods) is at least 120%, or at least 150% psi, or at least 180%, or at least 200%. There is no maximum desired elongation at break, but an elongation at break of greater than 400% is generally unnecessary.

[0098] In some embodiments, the dry adhesion of the dried coating to steel (measured as described in the Test Methods) is at least 2.5 p / li, or at least 3 p / li, or at least 3.5 p / li, or at least 4 p / li.There is no maximum desired adhesion.

[0099] In some embodiments, the 7-day water absorption of the dried coating (measured as described in the test methods) is at most 20 wt%, or at most 16 wt%, or at most 15 wt%. There is no maximum desired minimum water absorption, but water absorption below 5 wt% may be difficult to achieve.

[0100] The present invention is illustrated by the following examples, which do not limit the full scope of the invention.

[0101] Example

[0102] Test Method

[0103] ASTM D903 Test Method for Peel Strength of Adhesive Bonds - Used to measure the adhesion of coatings to roofing substrates

[0104] ASTM D1653 Test Method for Water Vapor Permeability of Organic Coating Films - For water permeability measurements

[0105] ASTM D471 Test Method for Rubber Properties - Effects of Liquids - for Water Absorption Measurements

[0106] ASTM D2370 Test Method for Tensile Properties of Organic Coatings - Tensile and Elongation Tests

[0107] ASTM D4283 Test Method for Viscosity of Silicone Fluids - For measuring the viscosity of silicone fluids emulsified in water

[0108] ASTM D3719 Test Method for Quantifying Dust Collection on Coated Exterior Panels Binder emulsion ("binder Binder Emulsion 1") :

[0109] An acrylic binder emulsion was prepared that simulated a typical roof coating binder except that the emulsion contained no biocide to prevent the biocide from interfering with further testing.

[0110] A reactor was prepared by adding deionized water (372.5 g) and Na2CO3 (0.5 g) to a 3000 mL 4-neck round bottom flask equipped with a condenser, overhead stirrer, and thermocouple. The contents of the reactor were stirred and heated to 83°C under a nitrogen atmosphere.

[0111] A monomer emulsion was prepared in a separate container. Deionized water (222.6 g), Polystep A-16-22 surfactant (5.8 g, 22.0% active in water), and butyl acrylate monomer (272.1 g) were mixed. Additional butyl acrylate (642.1 g), methyl methacrylate (132.1 g), methacrylic acid (17.7 g), and benzophenone (2.9 g) were added to the container with mixing. Aqueous sodium persulfate solution (3.0 g in 18.2 g deionized water), 30% ammonia (1.5 g in 2.5 g water), and 100 nm pre-emulsion polymer seeds (52 wt % methyl methacrylate, 46.7 wt % butyl acrylate, and 1.3 wt % methacrylic acid, 45% solids) (52.9 g) were added to the reactor, followed by rinsing the feed container with deionized water (13.6 g).

[0112] The monomer emulsion and sodium persulfate solution (1.7 g in 52.9 g water) were fed simultaneously to the reactor at a temperature of 79° C. to 83° C. over a period of 90 minutes. At about 36 minutes into the feed (about 40% of the monomer emulsion was added), a 21.4 g quantity of 2-ethyleneureaethyl methacrylate was added to the remaining monomer emulsion container with mixing and rinsed with deionized water (4.5 g). After the feed was complete, the temperature was maintained at 82° C. to 83° C. for an additional 30 minutes. Next, 30% aqueous ammonia (1.2 g diluted with 27.2 g water), VERSENE TMA chelating agent (0.27 g, 1% active in H2O) and an aqueous FeSO4 solution (2.7 g, 0.15% active in water) were added to the reactor in succession. Then, water containing 70% tert-butyl hydroperoxide (0.8 g, diluted in 25.1 g water) and sodium formaldehyde sulfoxylate (0.94 g, in 25.1 g water) were simultaneously fed to the reactor over 60 minutes. After the first 30 minutes, the reactor was cooled to 75°C. After all the feeds were added, the reactor was cooled to 45°C and 30% ammonia (4.0 g, diluted with 7.0 g water) was added dropwise. The reactor was cooled to room temperature and the aqueous dispersion was filtered. The final polymer dispersion had a solids content of 54.7% and a Z average particle size of 275.2 nm, as measured by dynamic light scattering using a Malvern Zetasizer. The dispersion is referred to as "Binder Latex 1".

[0113] Basic emulsion coating composition :

[0114] A base latex coating composition containing Binder Emulsion 1 was prepared in a 2L stainless steel grinding jar under stirring using a high speed mixer equipped with a 2 inch Cowles sawtooth blade. The ground ingredients of Table 1 below were added to the jar in the order listed, with the mixer set at 200 rpm. The mixer was set to 2000 rpm and the grind was mixed for 20 minutes. Agitation was reduced to 500 rpm and the remaining letdown ingredients were added in the order listed. The contents were mixed at 500 rpm for 20 minutes until the latex coating composition had a smooth, uniform consistency.

[0115] Table 1. Formulation ingredients for elastomeric roof coatings .

[0116]

[0117]

[0118] Example 1: Coating with PDMS emulsion

[0119] A series of polydimethylsiloxanes with different viscosities (corresponding to different molecular weights) were formulated into emulsions.

[0120] Emulsion containing PDMS fluid with a viscosity of 5 cSt

[0121] The following ingredients were added to a 600 gram stainless steel beaker: 75.0 grams of water, 11.7 grams of Lutensol XP-79 nonionic surfactant, and 2.76 grams of Hostapur SAS-30 anionic surfactant. This mixture was mixed at a low speed (150 RPM) using a Lightnin's mixer equipped with a propeller and Cowle blade to incorporate the surfactant without generating foam. A 207.5 gram portion of XIAMETER 5000 with a viscosity of 5 cSt was added to the mixture.TM PMX-200 silicone fluid. (PDMS) was added slowly with increasing mixing to minimize foaming. This mixture was then stirred at 500 RPM for 15 minutes. The resulting emulsion was placed in a Speedmixer cup with a small hole in the lid and spun at 3500 RPM to remove air. The resulting emulsion was 69% silicone by weight and had an average particle size of 1.24 μm.

[0122] Emulsions containing PDMS fluids having viscosities of 100 cSt and 350 cSt

[0123] The following ingredients were added to a 3.5 kg stainless steel beaker: 500.0 grams of water, 78.0 grams of Lutensol XP-79 nonionic surfactant, and 18.48 grams of Hostapur SAS-30 anionic surfactant. This mixture was mixed at a low speed (150 RPM) using a Lightnin's mixer equipped with a 45 degree pitch blade on the top and a 90 degree pitch blade on the bottom to incorporate the surfactant without creating foam. 1400 grams of XIAMETER TM PMX-200 silicone fluid (100 or 350 cSt). (PDMS) was then added slowly with increasing mixing to minimize foaming. This mixture was finally stirred at 500 RPM for 45 minutes. The resulting emulsion was sheared at 1700 PSI by a Sonolator homogenizer. The resulting emulsion was 70.1% silicone by weight and had an average particle size of approximately 0.4 μm.

[0124] Emulsions containing PDMS fluids with viscosities of 5000, 60000, 300000 and 2.5 MM cSt

[0125] Add the following ingredients to the DAC100 Speedmixer cup: 70.0 g XIAMETER TM PMX-200 silicone fluid (5000, 60000, 300000 and 2.5MM cSt viscosity) (PDMS), 3.90 grams of Lutensol XP-79 nonionic surfactant and 0.92 grams of Hostapur SAS-30 anionic surfactant and 0.91 grams of water. This mixture was blended with a DAC150 Speedmixer at maximum speed (3500RPM, 30 seconds). Subsequently, 4.20 grams, 9.80 grams and 10.10 grams of dilutions of water were added, rotating after each. The resulting emulsion was 70% to 78% silicone by weight and had an average particle size of 0.23 μm to 6.8 μm depending on the polymer viscosity.

[0126] Table 2 summarizes the different emulsions .

[0127] Table 2

[0128]

[0129] For each of the above emulsion samples, 500 g of the base latex coating composition was mixed using an overhead mixer at an rpm sufficient to create a small vortex in the coating. The PDMS emulsion was added dropwise in the amounts shown in Table 3, and the coating composition was then mixed for an additional 5 minutes. The composition of each coating and the properties of each coating formulation are shown in Table 3.

[0130] Additionally, a comparative example (CE1) was prepared without the addition of PDMS emulsion.

[0131] Samples (11 g to 15 g) of each freshly prepared roof coating (ERC) formulation were added to three different sterile polystyrene Petri dishes (Fisher Scientific (FB0875712)). As a comparison, three Petri dishes were coated with a roof coating formulation without PDMS emulsion. The coating was evenly distributed in each Petri dish by tapping the Petri dish on a flat surface. The Petri dishes were cured for 2 weeks at 75°F and 50% relative humidity. After curing, the coating was sterilized using isopropyl alcohol. The Petri dishes were dried overnight to ensure complete evaporation of the solvent.

[0132] Inoculation, growth experiments, and photography were performed in a biosafety level 2 (BSL-2) laboratory. Prepare the inoculum mixture. Dilute the stock solution of BG-11 broth (Sigma Aldrich) 100-fold using sterile deionized water. The diluted solution was sterilized by autoclaving, cooled to room temperature (RT), and then stored in a refrigerator at 4°C. Four environmental isolation samples of roof algae were obtained. Inside a biosafety cabinet, 500 μL of each of the four algae strains was added to a sterile vial. BG-11 solution (1%, 10 mL) was added to this vial at room temperature and the mixture was vortexed until well mixed.

[0133] A 200 μL sample of the inoculum mixture was added to each petri dish along with a 20 ml sample of 1% BG-11 broth solution. The petri dish was gently swirled to mix the contents and take photos of each dish. Photos were taken with a Nikon D80 digital SLR camera. The samples were illuminated with LED light to give a reading of 1270 lumens at the coating surface, as measured with a handheld photometer. The camera was set to: shutter speed = 1 / 1000 sec, F-Stop = 5.6, white balance = 5 (Daywhite fluorescence), ISO = 1600. The same lighting and camera settings were used for all pictures to allow comparison of photos taken at different time points. Each dish was stored in a timed light box (daylight spectrum lamp, 12 hours of illumination every 24 hours) at approximately 100% relative humidity for 8 weeks. The BG-11 growth medium was updated every 3 weeks. Once a week, new photos of each dish were taken.

[0134] After 8 weeks, algae growth in each petri dish was measured based on color change. Weekly images of the dish were compared to the 0 week images and analyzed using image analysis software to quantify the color change on the coating using the CIELAB system. Each dish was divided into nine areas and the average L, a, and b values ​​for each area were calculated using image analysis software. The color change for each area of ​​the coating is given by:

[0135] ΔEi=√((L i -L0) 2 +(a i -a0) 2 +(b i -b0) 2 )

[0136] Where L i 、a i and b i is the value obtained at a particular week after inoculation; and L0, a0, and b0 are the corresponding values ​​obtained at week 0. The average ΔE over all nine regions represents the average color change of the culture dish. The results are shown in Tables 4A (Examples of the present invention) and 4B (Comparative Examples). Larger ΔE values ​​indicate greater biofilm growth. ΔE values ​​less than 10 show minimal growth (growth is difficult to observe with the naked eye). Values ​​greater than 30 indicate significant biofilm colonization, and values ​​greater than 50 indicate total coverage of the coating.

[0137] In addition, samples of each coating were brushed on concrete, polyurethane, and metal (18-24 square inches of coating with 18-20 grams per square inch of coating) and dried. The following qualities of the coatings were measured: tensile strength, elongation at break, surface adhesion, water absorption, water penetration, and staining. The results are shown in Tables 5-9.

[0138]

[0139]

[0140] Table 4. ΔE values ​​from biofilm growth tests of inventive examples and comparative examples

[0141]

[0142]

[0143]

[0144] Testing showed that the inventive examples retained physical properties useful for roof coatings compared to coatings without PDMS. In particular, the elongation at break was not substantially altered by the additive.

[0145] Table 6. Adhesion Data for Elastomeric Roof Coatings (p / li = pounds force per linear inch)

[0146]

[0147]

[0148] C = Cohesive failure of the coating

[0149] A = Failure of adhesion of coating to substrate

[0150] Testing showed that the inventive examples maintained useful adhesion to the roofing substrate compared to coatings without PDMS.

[0151]

[0152] Table 8. Water Permeability Results for Elastomeric Roof Coatings

[0153]

[0154] Table 9. Stain Resistance of Elastomeric Roof Coatings

[0155]

[0156]

[0157] Tables 7, 8, and 9 show that the inventive examples retain useful properties for roof coatings compared to coatings without PDMS.

[0158] Example 2: Coating containing cross-linked silicone rubber

[0159] Commercially available silicone rubber dispersions were blended with the base emulsion coating compositions shown in Table 10 to prepare coating compositions of inventive Examples IE 15-26. The procedure for coating petri dishes, inoculated dishes, growing cultures, and test dishes was repeated as in Example 1. Comparative Example CE 11 without silicone rubber was also prepared and tested. The results are shown in Table 10.

[0160] Table 11

[0161]

[0162] A=AllGuard,3-2345

[0163] B=DOWSIL TM IE 2610,

[0164] C=DOWSIL TM 33.

Claims

1. A method of protecting a roof of a structure having an exposed top surface, the method comprising the steps of: a) applying an aqueous coating composition to the top surface of the roof, the aqueous coating composition comprising the following coating components dissolved or suspended in an aqueous solvent: i) an acrylic polymer binder in a concentration suitable for forming a stable coating, ii) a non-toxic antifouling additive at a concentration suitable to inhibit scaling on said roof, and iii) 0 wt % to 80 wt % of other coating components based on the weight of the coating components in the composition excluding solvent; as well as b) drying the aqueous coating composition so that it forms a solid coating adhered to the top surface of the roof.

2. The method according to claim 1, wherein the acrylic polymer binder has a glass transition temperature of not higher than 0°C, and at least one of the other coating components is selected from the group consisting of: pigments, fillers, thickeners, surfactants, hydrophobic additives, leveling agents and coalescing agents, antioxidants and UV stabilizers.

3. The method according to claim 2, wherein the acrylic polymer binder has a glass transition temperature of not higher than -20°C.

4. The method of claim 2, wherein the non-toxic antifouling additive comprises a silicon-containing material.

5. The method of claim 4, wherein the non-toxic antifouling additive comprises polysiloxane. The method according to claim 5 , wherein the polysiloxane is polydimethylsiloxane.

7. The method of claim 5, wherein the polysiloxane comprises 2 to 10 weight percent of the coating components in the composition excluding solvent.

8. The method of claim 7, wherein the polysiloxane comprises 8 to 20 weight percent of the coating components in the composition excluding solvent.

9. The method of claim 5, wherein the polysiloxane has a weight average molecular weight of at least 5000 Da and at most 350,000 Da.

10. The method of claim 4, wherein the non-toxic antifouling additive comprises cross-linked silicone rubber particles.

11. The method of claim 10, wherein the crosslinked silicone rubber particles comprise at least 2 weight percent of the coating components in the composition excluding solvent.

12. The method of claim 10, wherein the crosslinked silicone rubber particles comprise up to 20 weight percent of the coating components in the composition excluding solvent.

13. The method of claim 11, wherein the cross-linked silicone rubber particles have an average particle size of at least 0.5 mm and at most 5 mm.

14. An aqueous coating composition comprising the following coating components dissolved or suspended in an aqueous solvent: a) an acrylic polymer binder having a glass transition temperature not exceeding 0° C. at a concentration suitable for forming a stable coating; b) a non-toxic antifouling additive at a concentration suitable to inhibit scaling on said roof; and c) 0% to 80% by weight of other coating components based on the weight of the coating components in the composition excluding solvents.

15. A structure comprising a roof having an exposed top surface, wherein a solid coating is adhered to the top surface of the roof and the coating contains the following coating components: (a) an acrylic polymer binder having a glass transition temperature of no more than 0° C. and bonding the coating to the roof; (b) a nontoxic antifouling additive at a concentration suitable for inhibiting scaling on the roof; and (c) 0 wt % to 80 wt % of other coating components, based on the weight of the coating components in the composition excluding solvents.