Magnetic disk and substrate for magnetic disk

By measuring concentric circle TIR in a specific area of ​​thin-walled disk and grinding the substrate, the physical errors caused by vibration and impact during rotation of thin-walled disks are solved, and a high-capacity and large-scale disk design is achieved, reducing the Head collision and read and write errors occur.

CN118946931AActive Publication Date: 2024-11-12FURUKAWA ELECTRIC CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380030321.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-06
Publication Date
2024-11-12
Estimated Expiration
2043-03-06

AI Technical Summary

Technical Problem

During the thin-walling and large-scale process of existing disks, vibration and impact during rotation lead to an increase in the frequency of physical errors, and read and write errors are inevitable, especially in thin-walled disks with a thickness of less than 0.60mm, the traditional peripheral ends. The TIR regulations are not sufficient to ensure disk flatness.

Method used

By measuring the TIR of multiple concentric circles in a specific area of ​​the disk, and setting the radial change amount to 0.50 μm/mm or less, combining the grinding and grinding process of aluminum alloy or glass substrate, the flatness and radial changes of the disk are ensured. The quantity is within the specified range to reduce the occurrence of physical errors.

Benefits of technology

It is realized that disks with a thickness of less than 0.60mm are not prone to physical errors in HDD devices, adapt to the high capacity requirements of hard disks, and maintain the stability of the data area when the outer diameter size is expanded to more than 95mm, reducing head collisions and operation errors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946931A_ABST
    Figure CN118946931A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a thin-walled and flat magnetic disk which is not susceptible to physical errors. The present invention is a magnetic disk having a hole in the center portion thereof and having a thickness dimension of 0.60 mm or less, where R (mm) is the radius of the disk, r (mm) is the distance in the radial direction measured from the center of the disk, and TIR1 ([mu] m) and TIR2 ([mu] m) are TIR1 ([mu] m) and TIR2 ([mu] m) when TIR1 ([mu] m) and TIR2 ([mu] m) are measured on the circumferences of different distances r1 (mm) and r2 (mm) in the outer peripheral region of the magnetic disk in which r / R is 0.70-0.99. The amount of change in the radial direction of TIR [Delta] TIR, which is represented by (TIR1-TIR2) / (r1-r2) of the absolute value of the ratio of the difference (TIR1-TIR2) between TIR1 and TIR2 to the difference (r1-r2) between the radial direction distance r1 and the radial direction distance r2 of the magnetic disk, is 0.50 [mu] m / mm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a magnetic disk and a substrate for the magnetic disk. Specifically, it relates to a magnetic disk that is thin-walled, has a small radial variation of TIR, is flat, and has reduced occurrence of physical errors, and in particular to a magnetic disk such as a hard disk installed in a data center or a computer, and a substrate for the magnetic disk such as an aluminum alloy substrate and a glass substrate. Background Art

[0002] Hard disk drives (hereinafter sometimes referred to as "HDD (Hard Disk Drive)") are often used as storage devices for data centers or computers. In recent years, the amount of data to be recorded has increased dramatically due to the popularity of smartphones and smart home appliances, the advancement of the Internet of Things (IoT), and the rapid popularization of cloud computing. These huge amounts of data are read and written to HDD devices in data centers via the Internet. In order to record huge amounts of data, HDD devices need to have larger capacities.

[0003] HDD devices use magnetic disks for recording data. One of the technologies for achieving a larger capacity of HDD devices is to reduce the thickness of the magnetic disks and increase the number of disks installed in the HDD device. Another technology trend is to increase the diameter of the magnetic disks and bring the data area on the disk surface as close to the outer diameter end as possible, thereby expanding the data area of ​​each magnetic disk.

[0004] If the thickness of the disk is simply reduced, the rigidity will decrease, so there is a tendency for the disk to deform more when vibration (flutter) and impact are applied when the disk rotates. Therefore, for example, in an HDD device equipped with multiple thin-walled disks using aluminum alloy substrates and glass substrates, the spacing between the disks and even between the disks and components such as the magnetic head becomes narrower, making it easy for the disks to contact each other or the disks and the magnetic head. As a result, errors are likely to occur during reading and writing. In order to reduce physical errors in such HDD devices, several discussions related to the flattening of the disks have been conducted.

[0005] For example, Patent Document 1 discloses a technique for regulating the height deviation and TIR at the peripheral end of a disk substrate in order to suppress a head crash of an HDD. Here, TIR is an index indicating the flatness of a surface. The so-called TIR at the peripheral end refers to the difference (PV value) between the highest point (P) located above and the lowest point (V) located below the aforementioned plane when the height of the peripheral end of the substrate is measured circumferentially by using the least squares method to obtain the plane of the main surface that best fits the peripheral end of the substrate. Patent Document 2 discloses a technique for precisely grinding a glass substrate of a specific composition in such a way that the TIR at the radius of two specified points is below a specified value.

[0006] [Prior Technical Literature]

[0007] (Patent Document)

[0008] Patent Document 1: Japanese Patent Application Publication No. 2013-16214

[0009] Patent Document 2: Japanese Patent Application Publication No. 2011-225436 Summary of the invention

[0010] [Problems to be solved by the invention]

[0011] In the past, the flatness of the disk was regulated by the flatness of the entire surface of the substrate, the undulation, the TIR value on the circumference at any position, etc. For example, in Patent Documents 1 and 2, the flatness is also evaluated by the TIR when measured along the circumferential direction. However, with the thinning and enlargement of disks in recent years, unprecedented new problems have emerged. When the thickness of the plate is simply reduced, for example, to less than 0.60 mm, the deformation of the disk will increase when vibration (flutter) or impact is applied during the rotation of the disk, thereby increasing the frequency of physical errors of the disk. In addition, when evaluating the disk, it is sometimes impossible to clearly determine whether the read and write errors are within the allowable range. The size of the substrate used as the subject of discussion in Patent Documents 1 and 2 is: the outer diameter is relatively small, for example, less than 2.5 inches (about 65 mm), and the thickness is also more than 0.635 mm. Therefore, physical errors can be avoided by only regulating the TIR of the outer peripheral end, but this alone is not enough as a countermeasure to avoid errors in thin-walled large disks.

[0012] In addition, in recent HDD devices, the distance between the disk and the magnetic head during HDD operation has been getting shorter and shorter. For example, in the case of a thin disk with a thickness of about 0.60 mm or less, sometimes the magnetic head that is floating / moving on the main surface for reading and writing becomes unstable due to the change in the shape of the main surface, resulting in operational errors such as read and write errors. Therefore, in a substrate for HDD with a short distance between the substrate and the magnetic head, the shape of the main surface must also be considered, not just the peripheral end. In particular, if the area from the radial center of the main surface to the outermost periphery is uneven, errors are likely to occur during HDD operation.

[0013] An object of the present invention is to provide a magnetic disk and a magnetic disk substrate which are thin-walled and flat, are less prone to physical errors, and can cope with the increase in the capacity of hard disks.

[0014] [Technical means to solve the problem]

[0015] The inventors of the present invention have conducted active research and found that by measuring the TIRs of respective disks on multiple concentric circles within a specific area of ​​the disk and setting the radial variation of these TIRs to be below a specified value, physical errors are less likely to occur even for thin disks with a thickness of less than 0.60 mm, thereby being able to cope with the increase in the capacity of hard disks; thus, the present invention was completed.

[0016] In order to achieve the above-mentioned object, the gist of the present invention is as follows.

[0017] (1) A magnetic disk having a hole in the center portion, and

[0018] The thickness is less than 0.60mm.

[0019] Let the radius of the disk be R (mm),

[0020] The radial distance of the magnetic disk measured from the center of the magnetic disk is defined as r (mm).

[0021] In the outer peripheral area of ​​the magnetic disk where r / R is 0.70 or more and 0.99 or less,

[0022] When the TIR measured on the circumference of the magnetic disk at different radial distances r1 (mm) and r2 (mm) is TIR1 (μm) and TIR2 (μm),

[0023] The radial change ΔTIR of TIR represented by the absolute value of the ratio of the difference (TIR1-TIR2) between TIR1 and TIR2 to the difference (r1-r2) between the radial distance r1 and r2 of the disk |(TIR1-TIR2) / (r1-r2)| is less than 0.50 μm / mm.

[0024] (2) The magnetic disk according to (1) above, wherein the flatness PV is 20.0 μm or less.

[0025] (3) The magnetic disk according to (1) or (2) above, wherein the outer diameter is 95 mm or more.

[0026] (4) A substrate used for the magnetic disk described in any one of (1) to (3) above.

[0027] (5) A method for manufacturing a magnetic disk, which is the method for manufacturing a magnetic disk according to any one of (1) to (3) above, characterized in that:

[0028] The aforementioned disk is made of an aluminum alloy substrate.

[0029] The method for manufacturing the magnetic disk comprises a grinding process step of grinding the aluminum alloy substrate.

[0030] The grinding process is carried out at a pressure of 50 g / cm 2 Above and 120g / cm 2 The test was performed under the following conditions: the platform rotation speed was 10 rpm to 35 rpm, and the coolant flow rate was 1 L / min to 10 L / min.

[0031] (6) A method for manufacturing a magnetic disk, which is the method for manufacturing a magnetic disk according to any one of (1) to (3) above, characterized in that:

[0032] The aforementioned disk is made of a glass substrate.

[0033] The method for manufacturing the magnetic disk comprises a grinding process step of grinding the glass substrate.

[0034] The grinding process is carried out at a pressure of 100 g / cm 2 Above and 200g / cm 2 The test was performed under the following conditions: the platform rotation speed was 10 rpm to 35 rpm, and the coolant flow rate was 1 L / min to 10 L / min.

[0035] (7) The method for manufacturing a magnetic disk according to (5) or (6) above, wherein in the grinding step, a grinding amount is 2.5 μm or more and 25 μm or less.

[0036] (8) A method for manufacturing a magnetic disk according to any one of (5) to (7) above, wherein in the grinding process, at least once the front and back sides of the aluminum alloy substrate or the glass substrate are reversed and then grinding is continued.

[0037] (9) A method for manufacturing a magnetic disk according to any one of (5) to (8) above, wherein, after the aforementioned grinding process, a grinding process is also performed for grinding the aforementioned aluminum alloy substrate or the aforementioned glass substrate, and in the aforementioned grinding process, at least once the front and back sides of the aforementioned aluminum alloy substrate or the aforementioned glass substrate are reversed and then the grinding is continued.

[0038] (Effects of the Invention)

[0039] According to the present invention, a magnetic disk can be provided, which has a thin wall with a thickness dimension of less than 0.60 mm, and a ΔTIR of less than 0.50 μm / mm and is extremely flat, so it is not easy to collide with an adjacent disk. Therefore, the magnetic disk of the present invention can be mounted in multiple pieces in an HDD device, so that the high capacity of the hard disk can be coped with. In addition, the magnetic disk of the present invention can be enlarged, for example, the outer diameter dimension can be set to more than 95 mm. Moreover, up to the limit of the outer peripheral end of the disk, it can be used as a data area, and in this respect, it can also contribute to the high capacity of the hard disk. Furthermore, even if the magnetic disk of the present invention is mounted on an HDD device with a short distance between the magnetic disk and the magnetic head, it is not easy to cause a collision with the magnetic head, and it is not easy to cause errors during the operation of the HDD device. Therefore, the magnetic disk of the present invention is particularly suitable as a magnetic disk for hard disks mounted in data centers or computers. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a conceptual diagram for explaining the measurement position and the outer peripheral area of ​​the radial variation of TIR in the magnetic disk of the present invention.

[0041] Figure 2 Is the drawing to be Figure 1 A conceptual diagram of an example of a graph in which the height measured along the circumferential direction on the concentric circles Ca or Cb in FIG. 1 is plotted against the angle at the measurement location.

[0042] Figure 3 This is a flow chart showing an example of a process for producing the aluminum alloy substrate for a magnetic disk according to the present invention.

[0043] Figure 4 This is a flow chart showing an example of the process for producing the magnetic disk glass substrate of the present invention. DETAILED DESCRIPTION

[0044] Hereinafter, the magnetic disk of the present invention will be described in detail.

[0045] "disk"

[0046] The magnetic disk of the present invention has a hole in the center portion and a thickness dimension of less than 0.60 mm. The radius of the magnetic disk is set to R (mm), the radial distance of the magnetic disk measured from the center of the magnetic disk is set to r (mm), and the TIR measured on the circumference of different radial distances r1 (mm) and r2 (mm) of the magnetic disk in the outer peripheral area of ​​the magnetic disk where r / R is greater than 0.70 and less than 0.99 is set to TIR1 (μm) and TIR2 (μm). The radial change ΔTIR of TIR represented by the absolute value of the ratio of the difference (TIR1-TIR2) between TIR1 and TIR2 to the difference (r1-r2) between the radial distance r1 of the magnetic disk and the radial distance r2 of the magnetic disk |(TIR1-TIR2) / (r1-r2)| is less than 0.50 μm / mm.

[0047] As described above, in the magnetic disk of the present invention, an important condition is that the radial variation ΔTIR of TIR in the outer peripheral region is 0.50 μm / mm or less. In the case where the plate thickness of the magnetic disk is thin, especially 0.60 mm or less, if ΔTIR in the outer peripheral region is greater than 0.50 μm / mm, physical errors are likely to occur. On the other hand, in the magnetic disk of the present invention having ΔTIR of 0.50 μm / mm or less, physical errors are unlikely to occur even if the thickness dimension is 0.60 mm or less.

[0048] Here, the “outer peripheral region” refers to a region where the ratio r / R of the radial distance r of the magnetic disk measured from the center of the magnetic disk to the radius R of the magnetic disk is 0.70 or more and 0.99 or less, as described above. Figure 1 1 is a conceptual diagram for explaining the measurement position and the outer peripheral area of ​​the radial variation of TIR in the magnetic disk of the present invention. Figure 1 Taking the disk 1 shown in the figure as an example, the area divided by the two concentric circles shown by the dotted lines, namely the outer circle Ca at the position where the aforementioned ratio r / R is 0.99 and the inner circle Cb at the position where the aforementioned ratio r / R is 0.70, is the outer peripheral side area.

[0049] <Radial variation of TIR>

[0050] The radial variation of TIR is the amount by which the TIR will vary due to the difference in radial distance when the TIR is measured on the circumference of two concentric circles with different radial distances on the disk surface. Figure 1Taking the magnetic disk 1 shown in FIG. 1 as an example, TIR is measured on the circumferences of concentric circles C1 and C2 at different radial distances r1 (mm) and r2 (mm) in the outer peripheral area of ​​the main surface of the magnetic disk 1, respectively, to obtain TIR1 (μm) and TIR2 (μm). Next, as shown in the following (Formula 1), the difference between TIR1 and TIR2 is divided by the difference between r1 and r2, and the absolute value is taken as the radial variation ΔTIR of TIR.

[0051] ΔTIR=|(TIR1-TIR2) / (r1-r2)|···(Formula 1)

[0052] (TIR)

[0053] TIR is the abbreviation of Total Indicated Reading, which is an indicator of the flatness of the surface. Figure 1 Taking the disk of as an example, first, the plane that best fits the main surface of the disk is obtained by the least square method. Then, the height (concavity and convexity) of the main surface of the disk in the concentric circle Ca or Cb portion is measured along the circumferential direction. Figure 2 This is a conceptual diagram showing an example of a graph in which the height measured along the circumferential direction is plotted against the angle at the measurement location. Here, the difference (PV value) between the highest point (P) located above the plane and the lowest point (V) located below the plane is the TIR on the circumference. Regarding TIR, it is also possible to measure on the circumference of the same radius on both main surfaces, and take the higher value as the TIR on the circumference.

[0054] (ΔTIR)

[0055] The TIR measurement on the circumference as described above is performed on multiple concentric circles with different radial distances, and the value calculated according to the above (Formula 1) is the radial change ΔTIR for how much the TIR changes at each radial distance. Therefore, ΔTIR is a numerical value that includes not only the change in height on a specific circumference (such as the outer circumference) of the disk, but also the change in height in the radial direction. That is, ΔTIR is an indicator that represents the change in height (thickness, undulation, concavity, etc.) in both the circumferential and radial directions of the disk. It can be said that the closer ΔTIR is to 0, that is, the smaller the absolute value of ΔTIR is, the flatter the disk is, and the less likely it is to cause physical errors caused by collisions, etc.

[0056] In the magnetic disk of the present invention, as the radial variation ΔTIR, the value in the outer peripheral region of the magnetic disk, i.e., the region where r / R is greater than 0.70 and less than 0.99, is used as described above. According to the findings of the inventors, the magnetic disk surface tends to be particularly rough in this region. In the manufacture of magnetic disks, a glass or metal substrate is ground / polished, and in the grinding / polishing process, the outer peripheral region is a portion where the roughness is particularly prone to change. Therefore, if the magnetic disk has a small radial variation ΔTIR in the outer peripheral region, it can be evaluated as a flatter magnetic disk with excellent grinding / polishing accuracy.

[0057] The magnetic disk of the present invention has a very small ΔTIR of 0.50 μm / mm or less in the outer peripheral area, so it has a thin wall thickness of 0.60 mm or less, and is not likely to cause collision with adjacent magnetic disks or magnetic heads in the HDD device, and is not likely to cause physical errors. From the viewpoint of further reducing physical errors, the ΔTIR in the magnetic disk of the present invention is preferably 0.40 μm / mm or less, further 0.30 μm / mm or less, and particularly 0.20 μm / mm or less.

[0058] (Disk shape evaluation method)

[0059] The surface shape of the magnetic disk such as TIR can be evaluated, for example, by a general optical inspection device. There is no particular limitation on the evaluation method and the inspection device, and for example, FT-17 (trade name) manufactured by Nidec, mesa (trade name) manufactured by Zygo, FM-200 manufactured by Tropel, etc. can be suitably used.

[0060] In order to make the magnetic disk of the present invention less likely to cause physical errors, it is preferred to evaluate it by using multiple ΔTIRs. For example, in a magnetic disk with an outer diameter of 95 mm (radius R of 47.5 mm), three radial variations ΔTIR are calculated based on TIRs on concentric circles with distances r from the center of 40 mm (r / R=84%), 45 mm (r / R=95%), 46 mm (r / R=97%), and 47 mm (r / R=99%). If the absolute values ​​of all three ΔTIRs are less than 0.50 μm / mm, a HDD device with further reduced operational errors and higher reliability can be provided.

[0061] <Disk flatness>

[0062] In addition, the disk of the present invention preferably has a small flatness PV value. If the PV is small, specifically, if the disk is less than 20.0μm, the risk of collision is low even if multiple disks are loaded in the HDD device, and physical errors are not likely to occur. In addition, from the perspective of shape evaluation, it is also preferred that the PV is as small as possible. If the flatness PV is large, when the surface shape of the disk is measured by an optical inspection device, in the optical system where the measurement light emitted by the inspection device is reflected on the disk surface and returned to the sensor of the inspection device, sometimes a part of the reflected measurement light cannot be returned to the sensor of the inspection device, and the surface shape of the desired area cannot be evaluated. On the other hand, if the PV is small, for example, a disk less than 20.0μm, the surface shape can be evaluated without problems using an optical inspection device.

[0063] Here, the so-called flatness PV is first obtained by the least square method in the same way as the TIR on the circumference mentioned above, and then the difference between the highest point (P) and the lowest point (V) when the height (roughness) of the main surface of the disk is measured on the entire surface. The flatness PV is used to represent the flatness of the entire surface of the disk, including not only the surface roughness of the disk, but also the undulations and concavities of the disk body. If the disk has a ΔTIR of less than 0.50 μm / mm and a small flatness PV, such as less than 20.0 μm, even if multiple disks are loaded in the HDD device, the risk of collision is low and it is not easy to cause action errors. From the viewpoint of reducing physical errors, the flatness PV of the disk of the present invention is preferably less than 15.0 μm, especially less than 10.0 μm. Here, the flatness can also be set to be the flatness of the substrate measured on the two main surfaces and a higher value is measured.

[0064] <Disk size>

[0065] As described above, since the surface of the magnetic disk of the present invention is extremely flat, it has the effect of not being easy to collide even if multiple magnetic disks are loaded in the HDD device. The effect of the present invention is remarkable in thin-walled magnetic disks with a thickness of less than 0.60 mm, especially less than 0.50 mm, less than 0.48 mm, and further less than 0.38 mm. This is because, in such a thin-walled substrate, the rigidity is low compared to a thicker magnetic disk, so the flatness will greatly affect the reliability of the hard disk. For the same reason, the effect of the present invention is remarkable in magnetic disks with an outer diameter (diameter) of, for example, more than 65 mm, especially more than 95 mm.

[0066] The magnetic disk of the present invention is not only flat in the circumferential direction, but also flat in the radial direction. Therefore, the risk of the undulation or concavity in the outer peripheral area increasing with the size of the disk (increase in radius) and causing collision is also reduced. Therefore, the magnetic disk of the present invention is suitable as a large hard disk with a diameter of 95 mm or more, further 96 mm or more, and especially 97 mm or more. In addition, the present invention also includes magnetic disks with an outer diameter of 95 mm or more. The outer peripheral side of the magnetic disk is particularly helpful in expanding the area of ​​the data area. Therefore, such a large and flat magnetic disk of the present invention is useful for realizing large capacity. In addition, the magnetic disk of the present invention has a flatness of ΔTIR of less than 0.50 μm / mm in the area less than 0.99 times the outer radius, so it can be used as a data area up to the limit of the outer peripheral end of the disk. In this respect, the magnetic disk of the present invention is also particularly useful in realizing large capacity of HDD devices.

[0067] In addition, the magnetic disk of the present invention can be used as a magnetic disk for any recording method. For example, as a large-capacity magnetic disk for a data center, a magnetic disk of a perpendicular magnetic recording method (PMR) or a shingled magnetic recording method (SMR) can be suitably used. In order to achieve further large capacity, energy-assisted magnetic recording technologies such as heat-assisted magnetic recording (HAMR) and microwave-assisted magnetic recording (MAMR) have also been developed, and research on the use of bit pattern media is also being conducted, and the bit pattern media is used to further increase the recording density of the surface. The magnetic disk of the present invention is suitable for such use.

[0068] The magnetic disk of the present invention may be any type of magnetic disk, and its material is not particularly limited, as long as the thickness dimension is less than 0.60 mm and the ΔTIR is less than 0.50 μm / mm as described above. Generally speaking, magnetic disks are manufactured by forming a magnetic film on a substrate such as metal, glass, or resin. In the magnetic disk of the present invention, there is no particular limitation on the material and film forming method of the magnetic film.

[0069] 《Substrate》

[0070] In addition, the present invention also includes a substrate for the above-mentioned magnetic disk (disk substrate). There is no particular restriction on the material of the substrate, and it can be a substrate of any material as described above. The substrate is usually ground before film formation, and the substrate of the present invention can be ground by any method / condition. However, in order to make the magnetic disk of the present invention have the flatness as described above, it is preferred to use a substrate composed of a metal substrate, especially an aluminum alloy or glass (sometimes referred to as "aluminum alloy substrate" and "glass substrate" in the present case specification). Aluminum alloy substrates and glass substrates are not prone to defects, and have good mechanical properties and processability, so they are suitable as the magnetic disk substrate of the present invention. In particular, as the magnetic disk substrate for the above-mentioned HAMR, a glass substrate with excellent heat resistance is preferred. As a magnetic disk substrate for MAMR, any of a glass substrate and an aluminum alloy substrate can be used.

[0071] In addition, in terms of flattening the disk substrate, it is preferred to grind with a method / condition corresponding to the material of the substrate. Below, for aluminum alloy substrates and glass substrates, particularly preferred materials are exemplified, and these substrates are used as examples to describe preferred grinding methods and conditions. In addition, the material and manufacturing method of the substrate are not limited to the following description.

[0072] <Aluminum alloy substrate>

[0073] There is no particular restriction on the material of the aluminum alloy substrate, and various known substances can be used. For example, alloys containing elements such as magnesium (Mg), copper (Cu), zinc (Zn) or chromium (Cr) used in the past can be cited, but are not limited to these. From the perspective of improving rigidity, alloys containing elements such as iron (Fe), manganese (Mn) or nickel (Ni) are preferably used. More preferably, alloys of A5000 series or A8000 series, especially A5086, are used. If it is such an alloy, it is not easy to produce defects in the substrate, and sufficient mechanical properties can be given in addition.

[0074] If we list examples of the specific composition of the above aluminum alloy, for example, in A5086, it contains Mg: 3.5-4.5%, Fe: 0.50% or less, Si: 0.40% or less, Mn: 0.20-0.7%, Cr: 0.05-0.25%, Cu: 0.10% or less, Ti: 0.15% or less, and Zn: 0.25% or less, and the remainder is composed of Al and inevitable impurities. In addition, as an example of other specific compositions of the aluminum alloy, it can be listed that it contains Mg: 1.0-6.5%, Cu: 0-0.070%, Zn: 0-0.60%, Fe: 0-0.50%, Si: 0-0.50%, Cr: 0-0.20%, Mn: 0-0.50%, Zr: 0-0.20%, Be: 0-0.0020%, and the remainder is composed of aluminum and inevitable impurities. In addition, regarding the components other than the above, for example, each element may be contained at 0.1% or less, and the total may be contained at 0.3% or less. In the above composition, "%" means "mass %".

[0075] As the magnetic disk substrate of the present invention, a substrate of an aluminum-iron alloy can also be used. Generally speaking, an aluminum-iron alloy is an alloy containing Fe as an essential element and one or two of Mn and Ni as optional elements. It is further preferred that the total content of these Fe, Mn and Ni is 1.00-7.00 mass %, and it is particularly preferred that it also contains one or more of Si: 14.0 mass % or less, Zn: 0.7 mass % or less, Cu: 1.0 mass % or less, Mg: 3.5 mass % or less, Cr: 0.30 mass % or less, and Zr: 0.20 mass % or less, and the remainder is an aluminum alloy composed of aluminum and inevitable impurities and other trace elements. These aluminum-iron alloys have high rigidity and are not easily deformed, so they are particularly useful as magnetic disk substrates of the present invention.

[0076] <Glass substrate>

[0077] Glass substrate has the characteristics of not easy to produce defects, good mechanical properties and processability, and also has the advantage of not easy to plastic deformation, so it is suitable as a disk substrate. There is no special restriction on the material of the glass substrate, and glass ceramics such as amorphous glass or crystallized glass can be used. In addition, from the perspective of the flatness, formability and processability of the substrate, it is preferred to use amorphous glass. There is no special restriction on the material, and examples include aluminosilicate glass (aluminosilicate glass), soda-lime glass, sodium aluminosilicate glass, borosilicate glass (borosilicate glass), and physical strengthened glass or chemical strengthened glass that has been treated with air cooling or liquid cooling, but are not limited to these. Among them, aluminosilicate glass, especially amorphous aluminosilicate glass, is preferred. The substrate of this material is excellent in terms of flatness and strength, and long-term reliability can also become good.

[0078] As aluminosilicate glass, for example, a material having SiO2: 55-75% as the main component, Al2O3: 0.7-25%, Li2O: 0.01-12%, Na2O: 0.7-12%, K2O: 0-8%, MgO: 0-7%, CaO: 0-10%, ZrO2: 0-10%, and TiO2: 0-1% is known, and a substrate of such a material can also be used in the present invention. In addition, in the above and following compositions, "%" means "mass %".

[0079] In the above glass composition, SiO2 is the main component forming the skeleton of the glass. If its content is 55% or more, it is easy to show high chemical durability, and if it is 75% or less, there is a tendency that the melting temperature will not be too high and molding will become easy.

[0080] Al2O3 is a component that has the effect of improving ion exchangeability and chemical durability. In order to exert the above effects, it is preferred that the Al2O3 content is 0.7% or more. In addition, if the Al2O3 content is 25% or less, the solubility and resistance to devitrification will not decrease. Therefore, it is preferred that the Al2O3 content is set to 0.7% to 25%.

[0081] Li2O is a component that chemically strengthens the glass by exchanging with Na ions, and improves the meltability, formability, and Young's modulus. In order to exert the above effects, the content of Li2O is preferably set to 0.01% or more. In addition, if the content of Li2O is 12% or less, especially 6% or less, the resistance to devitrification and chemical durability will not decrease. Therefore, it is preferred that the content of Li2O is set to 0.01% to 6%.

[0082] Na2O is a component that chemically strengthens glass by exchanging with K ions, reduces high temperature viscosity, improves solubility and formability, and improves resistance to devitrification. In order to exert the above effects, the content of Na2O is preferably set to 0.7% or more. In addition, if the content of Na2O is 12% or less, chemical durability and Knoop hardness will not decrease, so it is preferred.

[0083] Furthermore, K2O, MgO, CaO, ZrO2, and TiO2 are optional additives that can be included as needed. K2O is a component that has the following effects: reducing high-temperature viscosity, improving meltability, improving formability, and improving devitrification resistance; however, if the content of K2O exceeds 8%, there is a tendency that low-temperature viscosity decreases, the thermal expansion coefficient increases, and impact resistance decreases. Therefore, it is preferred that the content of K2O is set to 0% to 8%.

[0084] MgO and CaO are components that have the effects of reducing high temperature viscosity, improving solubility, clarity, and formability, and improving Young's modulus. In particular, CaO is contained as an essential component in soda-lime glass. Here, MgO and CaO can reduce high temperature viscosity, improve solubility, clarity, and formability, and can also be expected to improve Young's modulus. However, if the content of MgO exceeds 7% and / or the content of CaO exceeds 10%, there is a tendency to reduce ion exchange performance and devitrification resistance. Therefore, it is preferred that the content of MgO is set to 7% or less, and the content of CaO is set to 10% or less.

[0085] ZrO2 is a component that increases Knoop hardness, improves chemical durability and heat resistance, but if the content of ZrO2 exceeds 10%, there is a tendency for the meltability and resistance to devitrification to decrease. Therefore, it is preferred to set the content of ZrO2 to 0 to 10%.

[0086] TiO2 is a component that has the effects of reducing high temperature viscosity, improving melting properties, and increasing structural stability and durability. However, if the content of TiO2 exceeds 1%, there is a tendency to reduce ion exchange performance and resistance to devitrification. Therefore, it is preferred that the content of TiO2 is set to 0 to 1%.

[0087] In addition, the glass of the above composition contains: B2O3 which has the effect of reducing viscosity, improving solubility and clarity; SrO or BaO which has the effect of reducing high temperature viscosity, improving solubility and clarity, formability, and improving Young's modulus; ZnO which can reduce high temperature viscosity without reducing low temperature viscosity while improving ion exchange performance; SnO2 which has the effect of improving clarity and ion exchange performance; Fe2O3 which can function as a colorant; and As2O3 and Sb2O3 as clarifiers. In addition, as trace elements, oxides such as lanthanum (La), phosphorus (P), cerium (Ce), antimony (Sb), hafnium (Hf), rubidium (Rb), and yttrium (Y) may also be contained. In addition, B2O3 is contained as an essential component in aluminoborosilicate glass or borosilicate glass. In addition, the above-mentioned glass can also be a composition containing SiO2: 45~60%, Al2O3: 7~20%, B2O3: 1~8%, P2O5: 0.5~7%, CaO: 0~3%, TiO2: 1~15%, BaO: 0~4%, and other oxides such as MgO: 5~35%.

[0088] If the aluminum alloy substrate or glass substrate has the above composition, it will show a high degree of flatness and is not easily deformed by heat, so a magnetic disk with a thickness of less than 0.60 mm and a ΔTIR of less than 0.50 μm / mm can be manufactured. First, a method for manufacturing such a flat aluminum alloy substrate from the above aluminum alloy will be described below, taking a representative embodiment as an example.

[0089] <Method for manufacturing aluminum alloy substrate>

[0090] Figure 3 FIG. 1 is a flow chart showing an example of a manufacturing process of an aluminum alloy substrate for a magnetic disk of the present invention. Figure 3Among them, the preparation process of aluminum alloy components (step S101), the casting process of aluminum alloy (step S102), the homogenization process (step S103), the hot rolling process (step S104), and the cold rolling (step S105) are processes for manufacturing aluminum alloy raw materials by melting and casting, and making them into aluminum alloy plates. Secondly, by using a stamping process (step S106) using a press machine, a disk (hereinafter sometimes referred to as a "blank") of the desired inner diameter and outer diameter dimensions composed of an aluminum alloy is manufactured (blanking), and it is preferably delivered to a pressurized flattening process (step S107). Then, the manufactured blank is pre-treated by cutting / grinding processes (steps S108 to S109) to produce a circular aluminum alloy plate (hereinafter also referred to as a "bottom plate" or simply "bottom") with adjusted dimensions. The base plate is subjected to a zincate treatment process (step S110) and an electroless Ni-P plating process (step S111) to manufacture an aluminum alloy substrate for a magnetic disk. The manufactured aluminum alloy substrate for a magnetic disk is subjected to a rough grinding process (step S112) and a precision grinding process (step S113), and becomes a magnetic disk by a magnetic body attachment process (step S114). Figure 3 The content of each process is described in detail.

[0091] First, a molten metal of an aluminum alloy raw material having the above-mentioned composition is prepared by heating / melting according to a conventional method (step S101). Next, the prepared molten metal of the aluminum alloy raw material is cast by a semi-continuous casting (DC (direct chill casting) casting) method or a continuous casting (CC (continuous casting) casting) method, etc., to cast the aluminum alloy raw material (step S102). Vertical semi-continuous casting is particularly preferred. The manufacturing conditions of the aluminum alloy raw material in the DC casting method and the CC casting method are as follows.

[0092] In the DC casting method, the molten metal injected through the nozzle absorbs heat from the lower foot, the wall of the water-cooled mold, and the cooling water directly sprayed onto the outer periphery of the ingot (block), solidifies, and is led out downward as an ingot of aluminum alloy.

[0093] On the other hand, in the CC casting method, molten metal is supplied between a pair of rolls (or a belt caster or a block caster) through a casting nozzle, and a thin plate of an aluminum alloy is directly cast using heat dissipated from the rolls.

[0094] The major difference between the DC casting method and the CC casting method is the cooling rate during casting. The CC casting method having a high cooling rate is characterized in that the size of the second phase particles is smaller than that of the DC casting method.

[0095] For the aluminum alloy ingot cast by DC casting, a homogenization treatment is performed as needed (step S103). When performing the homogenization treatment, it is preferably heated at 280 to 620°C for 0.5 to 30 hours, and more preferably heated at 300 to 620°C for 1 to 24 hours. When the heating temperature during the homogenization treatment is less than 280°C or the heating time is less than 0.5 hours, the loss coefficient of each aluminum alloy plate may become uneven due to insufficient homogenization. If the heating temperature during the homogenization treatment exceeds 620°C, melting may occur in the aluminum alloy ingot. Even if the heating time during the homogenization treatment exceeds 30 hours, the effect is saturated and no additional significant improvement can be obtained.

[0096] Next, the aluminum alloy ingot (DC casting) that has been subjected to homogenization treatment as required or has not been subjected to homogenization treatment is hot rolled to form a plate (step S104). The conditions for hot rolling are not particularly limited, and the hot rolling start temperature is preferably set to 250 to 600°C, and the hot rolling end temperature is preferably set to 230 to 450°C.

[0097] Next, the hot rolled rolled sheet or the cast sheet cast by CC casting is cold rolled to form an aluminum alloy sheet of, for example, about 0.30 to 0.60 mm (step S105). The cold rolling conditions are not particularly limited and can be determined according to the required product sheet strength or sheet thickness, and the rolling rate is preferably set to 10 to 95%.

[0098] In addition, it is preferred to perform annealing treatment before or during cold rolling to ensure cold rolling workability. The temperature during annealing treatment is preferably set to 250-500°C, especially 300-450°C. By performing annealing treatment under such conditions, deformation is not easily caused during long-term use, and good flatness can be maintained. As more specific annealing conditions, for example, if it is batch heating, it can be carried out under the condition of maintaining at 300-450°C for 0.1-10 hours, and if it is continuous heating, it can be carried out under the condition of maintaining at 400-500°C for 0-60 seconds. Here, the so-called holding time of 0 seconds means cooling immediately after reaching the desired holding temperature.

[0099] Then, the aluminum alloy plate obtained by cold rolling is punched into a ring shape by a press machine or the like to make a ring-shaped aluminum alloy plate (blank) (step S106). The ring-shaped aluminum alloy plate is preferably made into a disk blank by punching / pressing flattening treatment (step S107). The punching / pressing flattening treatment (also called "pressure annealing") is preferably performed at a temperature above the recrystallization temperature of the aluminum alloy, applying 30 to 60 kg / cm 2For example, the blanks are stacked one on another and pressed at a temperature of 250 to 500° C., especially 300 to 400° C. in the atmosphere for about 0.5 to 10 hours, especially 1 to 5 hours, to produce a flattened blank.

[0100] Next, the blank is cut to produce a disk having a desired inner diameter, outer diameter and chamfered portion (hereinafter sometimes referred to as a "T-bottom") (step S108). Here, both surfaces of the blank may be cut to produce a T-bottom with an adjusted thickness. Furthermore, the T-bottom may be subjected to a heat treatment, for example, at 150 to 350°C for 0.1 to 10.0 hours, for the purpose of removing the machining strain generated inside the material due to the cutting process.

[0101] The obtained T-bottom is submitted to a grinding process (grinding process) in which the main surfaces on both sides are ground by a grinding machine, etc., to produce a disk of the desired thickness (hereinafter sometimes referred to as "G-bottom") (step S109). After this process, the G-bottom may also be subjected to a heat treatment under conditions such as 150 to 350°C × 0.1 to 10.0 hours for the purpose of removing the processing strain generated inside the material due to the cutting process. Here, the problem of the increase in the radial ΔTIR of the disk, which is a problem of the present invention, is mainly caused by the grinding process. Therefore, the grinding process will be described in detail below together with the polishing process.

[0102] Next, a disc (hereinafter sometimes referred to as "M bottom") is prepared with a desired thickness of plating formed on all surfaces including the surface, side surfaces, and chamfered surfaces of the G bottom. Prior to this, the G bottom is pre-treated for the purpose of improving the adhesion of the plating layer.

[0103] There is no particular restriction on the pretreatment method of the G bottom. For example, the surface of the G bottom is degreased, etched, and subjected to zincate treatment (Zn replacement treatment) (step S110). Degreasing can be performed using, for example, a commercially available AD-68F (manufactured by Uemura Industry Co., Ltd.) degreasing solution, under conditions of a concentration of 200 to 800 mL / L, a temperature of 40 to 70°C, and a treatment time of 3 to 10 min. Etching can also be performed by acid etching using, for example, a commercially available AD-107F (manufactured by Uemura Industry Co., Ltd.) etching solution, under conditions of a concentration of 20 to 100 mL / L, a temperature of 50 to 75°C, and a treatment time of 0.5 to 5 min. In the zincate treatment, a zincate film is formed on the surface of the bottom plate. The zincate treatment can be performed using a commercially available zincate treatment solution, preferably under conditions of a concentration of 100 to 500 mL / L, a temperature of 10 to 35°C, and a treatment time of 0.1 to 5 minutes. The zincate treatment is performed at least once, and may be performed twice or more. By performing zincate treatment multiple times, fine Zn can be precipitated to form a uniform zincate film. In the case of performing zincate treatment twice, a Zn stripping treatment can also be performed in between. The Zn stripping treatment is preferably performed using an HNO3 solution at a concentration of 10 to 60%, a temperature of 15 to 45°C, and a treatment time of 10 to 120 seconds (therefore, it is also called "nitric acid stripping treatment"). In addition, the second and subsequent zincate treatments are preferably performed under the same conditions as the initial zincate treatment.

[0104] Furthermore, the surface of the bottom plate treated with zincate is plated as a base treatment for the magnetic body to be attached to produce an M bottom (step S111). As a plating treatment, a non-electrolytic Ni-P plating treatment is preferred. The non-electrolytic Ni-P plating process preferably uses a commercially available plating solution, such as NIMUDEN (registered trademark) HDX manufactured by Uemura Industries Co., Ltd., under the conditions of Ni concentration: 3 to 10 g / L, temperature: 80 to 95°C, and treatment time: 30 to 180 minutes. It is also possible to heat the M bottom, for example, at 280 to 295°C × 15 to 60 minutes, for the purpose of removing the internal stress during plating. Since crystallization will occur and impart magnetism when it exceeds 300°C, the heating temperature must be less than 300°C.

[0105] The main surfaces of both sides of the M bottom thus obtained are subjected to a grinding process (steps S112 to S113) as described later to form a disk substrate. A magnetic body is attached to the substrate (step S114) and stacked as required to manufacture a disk such as a hard disk. The method and conditions of the grinding process will be described in detail below together with the grinding process (grinding process).

[0106] <Method for producing glass substrate>

[0107] Figure 4 This is a flowchart illustrating an example of a manufacturing process of a glass substrate for a magnetic disk of the present invention. First, a glass plate of a specified thickness is prepared (steps S201 to S202). Next, the prepared glass plate is cored, and the inner and outer circumferential end surfaces are ground, thereby forming / processing a circular ring-shaped glass substrate (steps S203 to S205). Next, it is ideal that the formed glass substrate is delivered to a grinding process (lapping) process using diamond particles or the like (step S206). Then, or depending on the state of the glass substrate, after step S205, a rough grinding process is performed in which the glass substrates are clamped from top to bottom using a grinding pad, and a plurality of glass substrates are simultaneously ground using, for example, cerium oxide abrasives (step S207), and chemical strengthening treatment is performed as required (step S208), and then a precision grinding process, for example, based on colloidal silica abrasives is performed (step S209). Next, a magnetic disk is manufactured by a magnetic body attachment process (step S210). Below, according to the Figure 4 The content of each process is described in detail.

[0108] First, a molten liquid of a glass raw material having the above-mentioned composition is prepared by heating / melting according to a conventional method (step S201). Next, the prepared molten liquid of the glass raw material is formed into a glass plate by a known manufacturing method such as a float method, a down-draw method, a direct pressing method, a re-draw method, a melting method, etc. (step S202). Here, if a re-draw method is used, that is, a re-draw method in which a base glass plate manufactured by a float method or the like is heated, softened, and stretched to a desired thickness, a glass plate with a small thickness difference can be manufactured relatively easily, so it is preferred. However, the forming method of the glass plate is not limited to the re-draw method, and for example, it can also be formed by a direct pressing method, in which a molten block is pressed and formed from both sides to produce a glass plate with a desired thickness.

[0109] Next, a circular ring-shaped glass substrate is formed from the glass plate obtained in step S202 by a core removal process (step S203). The inner and outer peripheral end surfaces may also be ground by cutting / end surface grinding (steps S204 to S205). The formed glass substrate (glass blank) becomes a circular ring-shaped plate having two main surfaces and a circular hole formed in the center.

[0110] The obtained glass blank may also be subjected to annealing treatment (annealing treatment). Annealing treatment can be performed, for example, by keeping the glass blank at a temperature near the strain point for more than about 15 minutes and slowly cooling it for about 3 to 12 hours. The temperature during annealing treatment also depends on the glass material, and is preferably set to 250 to 750°C, especially 500 to 700°C. By performing annealing treatment under such conditions, deformation is not easily caused during long-term use, and good flatness can be maintained. As a more specific annealing condition, for example, if it is batch heating, it can be carried out under the condition of keeping it at 500 to 650°C for 0.1 to 10 hours, and if it is continuous heating, it can be carried out under the condition of keeping it at 500 to 750°C for 0 to 60 seconds. Here, the so-called holding time of 0 seconds means cooling immediately after reaching the desired holding temperature. In addition, the glass substrate of the present invention can also be manufactured by, for example, forming a commercially available glass substrate having the above-mentioned composition into a ring shape and performing annealing treatment.

[0111] Next, in step S206, the formed annular plate is delivered to a grinding process (polishing) in which the main surfaces on both sides are ground by a grinding machine, etc., to adjust the plate thickness. In addition, according to the plate thickness of the glass substrate obtained in the process up to step S205, the grinding process S206 can also be omitted and transferred to the following grinding process. For example, the glass plate manufactured by the re-drawing method generally has a small thickness unevenness, so the grinding process S206 can sometimes be omitted, but in order to flatten the substrate, it is ideal to perform grinding. In addition, in the case of manufacturing a glass plate by a floating method or a direct pressing method, it is highly necessary to perform the grinding process S206. The grinding process can be implemented, for example, by a batch-type double-sided grinder using diamond particles. Here, the problem of the disc radial ΔTIR becoming larger, which is a problem of the present invention, is mainly caused by the grinding process in the glass substrate. Therefore, the grinding process will be described in detail below.

[0112] The surface of the glass substrate (blank substrate) obtained as mentioned above is subjected to grinding treatment (steps S207 to S209) as described later to make a disk substrate. On this substrate, a magnetic body (step S210) is attached and laminated as required to manufacture a disk such as a hard disk.

[0113] The above-mentioned grinding process, as described later, is roughly divided into a rough grinding process (step S207) and a precision grinding process (step S209). Preferably, between the rough grinding process and the precision grinding process, the glass substrate is subjected to chemical strengthening treatment (step S208). By chemical strengthening, the lithium ions and sodium ions on the surface of the glass substrate are replaced by sodium ions and potassium ions with relatively large ion radii in the chemical strengthening solution, respectively. As a result, a compressive stress layer is formed on the surface part, thereby strengthening the glass substrate. There is no particular restriction on the chemical strengthening treatment method, for example, it can be carried out by immersing the glass substrate in a chemical strengthening solution heated to 300 to 400 ° C for about 3 to 4 hours. Here, there is no particular restriction on the chemical strengthening solution, for example, potassium nitrate solution or sodium sulfate solution, their mixed solutions, especially a mixed solution of 60% by weight of potassium nitrate and 40% by weight of sodium sulfate, etc. can be used. In addition, the glass substrate is preferably cleaned before the chemical strengthening treatment and preheated to about 200 to 300 ° C. In addition, it is preferred that the glass substrate treated with chemical strengthening is delivered to the cleaning process. For example, after cleaning with an acid such as sulfuric acid, it is sufficient to further clean with pure water or the like.

[0114] <Grinding / polishing>

[0115] In the process of making the base plate, as mentioned above, in the manufacture of aluminum alloy substrates, grinding (grinding) is usually performed, and in the manufacture of glass substrates, it is ideal to perform polishing. In addition, the disk substrate is generally, no matter what kind of material the substrate is, before the magnetic body is attached, it must be delivered to the grinding process for flattening. In this grinding process, it is preferred to perform multiple stages of grinding with the diameter of the grinding abrasive adjusted. These grinding (grinding, polishing), rough grinding and precision grinding are generally preferably performed using a double-sided simultaneous grinding machine. The disk substrate of the present invention can also be ground or polished using a commercially available batch-type double-sided simultaneous grinding machine. In addition, it is preferred that before grinding / grinding, especially rough grinding, simulation (dummy) grinding is performed to manage the surface of the polishing pad.

[0116] (Double-sided grinding machine)

[0117] The double-sided simultaneous grinding machine usually has an upper platform and a lower platform made of cast iron, a carrier for holding multiple substrates between the upper platform and the lower platform, and a grinding pad or a grindstone installed on the contact surface of the substrates of the upper platform and the lower platform. During the grinding process, usually, multiple substrates are held between the upper platform and the lower platform by the carrier, and each substrate is clamped by the upper platform and the lower platform with a specified processing pressure. Then, each substrate is clamped from the top and the bottom by the grinding pad or the grindstone. Next, a grinding liquid or a cooling liquid is supplied between the grinding pad and each substrate in a specified supply amount, so that the upper platform and the lower platform rotate in different directions. At this time, since the carrier also rotates by the sun gear, the substrate performs a planetary motion. As a result, the substrate slides on the surface of the grinding pad or the grindstone, and both surfaces are ground at the same time.

[0118] (Carrier)

[0119] There is no particular restriction on the material and size of the carrier used in double-sided grinding, and a general-purpose carrier can be used. From the perspective of the strength of the carrier, a carrier made of resins such as aramid resin or epoxy resin can be used appropriately. It is also possible to contain fibrous reinforcing materials such as carbon fiber or glass fiber for the purpose of improving strength. The thickness of the carrier can be arbitrarily selected according to the thickness of the disc as the object to be processed. Among them, if the carrier is too thin, it will be insufficient in strength and may be damaged during grinding. Therefore, the carrier thickness is preferably more than about 0.3mm, more preferably more than about 0.4mm.

[0120] [Grinding of aluminum alloy substrates]

[0121] In the grinding process (grinding process, step S109) of the aluminum alloy substrate, a double-sided grinder as described above is used to rotationally press fixed abrasive grains called grindstones against the substrate held on a carrier from top and bottom, thereby grinding the main surfaces on both sides of the substrate.

[0122] [Grinding (polishing) of glass substrates]

[0123] In the grinding process (polishing process, step S206) of the glass substrate, the double-sided grinder as described above is also used to rotationally press the grindstone against the substrate held on the carrier from top and bottom, thereby grinding the main surfaces on both sides of the substrate.

[0124] [Grinding processing conditions]

[0125] (Speed ​​of grinding platform, etc.)

[0126] In the grinding process and the polishing process, coolant flows to the substrate, the carrier, and the grindstone during the grinding process. The rotation speed of the grinding platform (grindstone) is set in the range of 10 to 35 rpm, especially 15 to 30 rpm, which is preferred in terms of obtaining a smooth substrate. If the rotation speed is too fast, the grindstone may be unstable and the shape may deteriorate. In addition, if the rotation speed is too fast, a difference in the amount of coolant will occur between the inner and outer peripheries of the substrate, or between the inner and outer peripheries of the platform. In detail, the coolant is discharged by the centrifugal force generated by the rotation of the platform, but the coolant that assists in grinding is discharged on the outer side, so that the desired TIR cannot be achieved, resulting in a deterioration of ΔTIR. In addition, productivity deteriorates when the rotation speed is slow, so it is not preferred.

[0127] There is no particular restriction on the rotation speed of the sun gear, and it can be set to 5 to 15 rpm, for example. In addition, it is preferred that the grinding process is performed for about 1 to 10 minutes, especially about 2 to 5 minutes, and the grinding amount is set to about 2.5 to 25 μm, for example, about 5 to 20 μm. In addition, face cutting can also be performed before grinding.

[0128] (millstone)

[0129] The grindstone is composed of abrasive grains and a binder for bonding the abrasive grains. In the grinding process of aluminum alloy substrates, Si-C particles can be suitably used as abrasive grains, and porous sponge-like elastomers such as polyvinyl alcohol (PVA) can be suitably used as a binder. As grindstones used in the grinding of glass substrates, for example, grindstones formed by bonding abrasive grains such as diamond particles with a binder can be cited. In the grinding process, in the polishing process, grooves can be dug on the grindstone for the purpose of improving the discharge of grinding chips generated in the grinding process.

[0130] As mentioned above, the non-flattening of the substrate, i.e., the deterioration of the shape, is mainly caused by the grinding process (grinding, polishing process). According to the findings of the present inventors, the main reason for the deterioration of the substrate shape is the uneven clogging of the grindstone. This occurs because the grinding chips generated during grinding accumulate on the surface of the grindstone. When the uneven clogging of the grindstone occurs, the grinding of the substrate surface becomes uneven, resulting in the deterioration of the surface shape. During grinding, the grinding fluid is discharged from the peripheral part on the main surface, but the area of ​​the peripheral side area is relatively large, so it is greatly affected by the unevenness of the grinding. Therefore, suppressing the clogging of the grindstone can suppress the deterioration of the shape, and can also reduce the operation errors of the HDD device equipped with a magnetic disk. As a method for preventing the grindstone from clogging, the addition of the above-mentioned grooves and the method of regularly shaving (trimming) the surface of the grindstone before the grindstone is clogged are effective.

[0131] (Pressure of grinding stone)

[0132] As a method other than the above to suppress grinding stone clogging, for example, it is effective to appropriately apply external pressure to the substrate of the double-sided grinding device (grinding device, polishing device) platform in order to improve the discharge of grinding chips. If the pressure is too high, not only will the processing strain be applied to deteriorate the shape of the substrate, but the grinding stone surface will be pressed against the substrate surface, resulting in the flow path of the coolant being restricted. In particular, when the coolant flow rate is small, the discharge of grinding chips will be blocked, so that grinding is performed in a state where grinding chips remain on the grinding stone surface and the substrate surface.

[0133] Regarding the pressurization pressure (external pressure), in the case of an aluminum alloy substrate, specifically, it is preferably 50 to 120 g / cm 2 If the applied pressure exceeds 120g / cm 2 , there is a possibility that part of the grinding stone is elastically deformed and the parallelism between the substrate and the grinding stone is broken. As a result, a difference is generated in the pressure applied to the inner and outer peripheries of the aluminum alloy substrate, and TIR is deteriorated, resulting in a possible increase in ΔTIR. In addition, if the applied pressure exceeds 120 g / cm 2 If the flow path of the cooling liquid is restricted as described above, the friction coefficient between the aluminum alloy substrate and the grindstone will increase, causing the substrate to become stuck during rotation, making it difficult to perform uniform grinding, and the flatness will become greater than 20 μm. Furthermore, the applied pressure is preferably set to 70 to 110 g / cm 2 , especially 75-100g / cm 2 .

[0134] In the case of a glass substrate, the pressure (external pressure) is preferably 100 to 200 g / cm 2 Generally speaking, the Vickers hardness of glass substrates is higher than that of aluminum alloy substrates, so the applied pressure can be set high. However, if the applied pressure exceeds 200g / cm 2 , the disadvantage of increasing ΔTIR as in the case of the aluminum alloy substrate mentioned above may occur. Furthermore, if the applied pressure exceeds 200 g / cm in the case of the glass substrate, 2 , there is a possibility that the abrasive grains bite into the substrate, resulting in cuts and scratches, which requires increasing the removal margin of the grinding process in S206 and the grinding process as a post-process. Therefore, the upper limit is preferably set to 200g / cm 2 The external pressure on the glass substrate is more preferably 130 to 200 g / cm 2 .

[0135] (Coolant)

[0136] In terms of suppressing grindstone clogging, supplying coolant at an appropriate flow rate is also effective. In addition to cooling the heat generated by grinding, the coolant is also used for purposes such as improving lubricity and improving the discharge of grinding chips. The coolant flow rate is preferably about 1 to 10 L / minute, and more preferably about 3 to 5 L / minute. If the coolant flow rate is insufficient, there is a situation where the grinding chips cannot be fully discharged, and the shape of the substrate deteriorates. In more detail, if the coolant flow rate is small, sometimes there will be parts on the substrate that can be well removed by contact with fresh coolant, and parts that are reduced in cutting amount by contact with degraded coolant. In particular, in the peripheral part where the coolant is discharged, the coolant is insufficient, the grinding amount becomes uneven, and therefore the TIR deteriorates and ΔTIR tends to increase. In addition, since the ability to cut the entire substrate evenly is impaired, the flatness sometimes deteriorates.

[0137] The coolant is discharged to the outside of the table by the centrifugal force generated by the rotation of the table. However, if the coolant flow rate is large, the amount of coolant that is useless for grinding may increase, resulting in a decrease in productivity. Therefore, the upper limit is preferably set to 10 L / min.

[0138] The material of the coolant is not particularly limited, and a general-purpose product such as mechano aquacut ECO#408 (trade name) manufactured by Dayou Chemical Industry Co., Ltd. can be used. Here, by adding a surfactant or a lubricant to the coolant, a substrate with better flatness can be produced.

[0139] Regarding the rotation speed of the platform and the coolant flow rate mentioned above, by increasing them to a certain value, the amount of cutting per unit time (this is called cutting capacity) can be increased, but above this, there is a situation where the cutting capacity decreases in terms of the rotation speed of the platform and reaches the limit in terms of the coolant flow rate. Moreover, the desired values ​​of these two parameters are determined with the pressurization pressure as the center. In the manufacturing method of the present invention, it is found that the following is suitable for achieving the desired ΔTIR: for aluminum alloy substrates, the pressurization pressure is 100g / cm 2 Above and 200g / cm 2 The platform speed is 10 rpm or more and 35 rpm or less, the cooling liquid flow rate is 1 L / min or more and 10 L / min or less; for the glass substrate, the pressure is 50 g / cm 2 Above and 120g / cm 2 Below, the platform rotation speed is 10 rpm or more and 35 rpm or less, and the coolant flow rate is 1 L / min or more and 10 L / min or less.

[0140] That is, the present invention includes a method for manufacturing a magnetic disk, which is the method for manufacturing the magnetic disk, characterized in that the magnetic disk is manufactured from an aluminum alloy substrate, and the method for manufacturing the magnetic disk includes a grinding process for grinding the aluminum alloy substrate, and the grinding process is performed at a pressure of 50 g / cm 2 Above and 120g / cm 2 The test was performed under the following conditions: the platform rotation speed was 10 rpm to 35 rpm, and the coolant flow rate was 1 L / min to 10 L / min.

[0141] In addition, the present invention includes a method for manufacturing a magnetic disk, which is the method for manufacturing the magnetic disk, characterized in that the magnetic disk is manufactured from a glass substrate, and the method for manufacturing the magnetic disk includes a grinding process of grinding the glass substrate, wherein the grinding process is performed at a pressure of 100 g / cm 2 Above and 200g / cm 2 The test was performed under the following conditions: the platform rotation speed was 10 rpm to 35 rpm, and the coolant flow rate was 1 L / min to 10 L / min.

[0142] [Coarse grinding]

[0143] There is no particular restriction on the method of rough grinding, and it can be performed under any conditions corresponding to the material of the substrate. For example, the rough grinding of an aluminum alloy substrate can be performed using a grinding liquid containing aluminum oxide with a particle size of 0.1 to 1.0 μm and a grinding pad composed of hard or soft polyurethane, etc. In addition, the rough grinding of a glass substrate can be performed using a grinding liquid containing cerium oxide with a particle size of 0.1 to 1.0 μm and a grinding pad composed of hard polyurethane, etc. Abrasive grains of silica, zirconium oxide, SiC, diamond, etc. of the desired particle size can also be used instead of aluminum oxide and cerium oxide. In addition, the so-called hard refers to a substance with a hardness (ASKER C) of 85 or more measured by the measurement method specified in the standard specification of the Japan Rubber Association (benchmark specification: SRIS0101), and the so-called soft refers to a substance with a hardness of 60 to 80.

[0144] The specific rough grinding conditions are also affected by the material of the substrate used and the process until rough grinding (for example, steps S101 to S111 in the manufacture of aluminum alloy substrates, and steps S201 to S206 in the manufacture of glass substrates), and are difficult to determine fundamentally. In addition, it is not limited to specific conditions. For example, the rough grinding conditions of aluminum alloy substrates can be set to a grinding time of 2 to 5 minutes, a rotation speed of the grinding platform: 10 to 35 rpm, a rotation speed of the sun gear: 5 to 15 rpm, a grinding liquid supply rate: 1 to 5 L / min, and a processing pressure of 20 to 250 g / cm 2 , preferably 30 to 120 g / cm 2, Grinding amount (removing excess): 2.5~3.5μm.

[0145] The conditions for rough grinding of the glass substrate are not particularly limited. For example, it is preferred to use a hard grinding pad with a hardness of 86 to 88, and set the rotation speed of the grinding platform to 10 to 35 rpm, especially 15 to 30 rpm; the rotation speed of the sun gear to 5 to 15 rpm; the grinding liquid supply rate to 1 to 5 L / min, especially 2 to 4 L / min; the processing pressure to 20 to 250 g / cm 2 , especially 30-120g / cm 2 The grinding time is 2 to 10 minutes. There is no particular limitation on the grinding amount (removal of excess), but it is preferably about 2 to 50 μm, for example, about 5 to 25 μm.

[0146] (Simulation grinding)

[0147] During the grinding process, simulated grinding can also be performed to manage the surface of the grinding pad before the rough grinding as described above. Generally speaking, the simulated grinding process uses a simulated substrate, and is preferably carried out under the same conditions as the rough grinding process. There is no special limitation on the simulated substrate used. For example, an aluminum alloy substrate can be used for simulated grinding before the rough grinding of a glass substrate, but it is preferred to use a blank substrate of the same type as the blank substrate of the product, especially a blank substrate manufactured under the same conditions as the blank substrate of the product. The simulated grinding process, for example, is preferably performed until the ΔTIR of at least one surface of the simulated substrate becomes less than 0.50μm / mm or the flatness PV becomes less than 20.0μm.

[0148] By means of the above-mentioned simulation grinding, the surface of the grinding pad used in the above-mentioned rough grinding process can be adjusted to a suitable state. In addition, the simulation grinding is an arbitrary process, and as long as the grinding pad surface is adjusted / managed, it can also be omitted. For example, before the rough grinding batch begins, simulation grinding can be performed, and the rough grinding of the product blank substrate can be repeatedly performed in multiple batches using the adjusted grinding pad.

[0149] [Precision grinding]

[0150] There is no particular restriction on the method of precision grinding (polishing), and various known methods can be used for it. For example, the precision grinding of aluminum alloy substrates can be carried out using a grinding liquid containing colloidal silica with a particle size of about 0.01 to 0.10 μm and a soft grinding pad. In addition, the precision grinding of glass substrates can be carried out using a grinding liquid containing colloidal silica with a particle size of about 0.01 to 0.10 μm, especially about 10 to 50 nm, and a softer grinding pad composed of foamed urethane. Of course, the conditions for precision grinding are not limited to these. Abrasive grains of cerium oxide, zirconium oxide, SiC, diamond, etc. with the desired particle size can also be used. In addition, by this treatment, the main surface of the substrate is polished into a mirror surface, thereby manufacturing a disk substrate. The disk substrate of the present invention that has undergone the above-mentioned polishing process also has good flatness after the thermal shock test and presents a specified PV value. In addition, the polished substrate is preferably cleaned with a neutral detergent, pure water, isopropyl alcohol (IPA), etc.

[0151] The specific conditions for precision grinding are also affected by the material of the substrate used and the process until rough grinding, so it is difficult to determine fundamentally, and it is not limited to specific conditions. For example, in the precision grinding of aluminum alloy substrates, the grinding time can be set to 2 to 5 minutes, the rotation speed of the grinding platform: 10 to 35 rpm, the rotation speed of the sun gear: 5 to 15 rpm, the grinding liquid supply rate: 1000 to 5000 mL / min, and the processing pressure: for example, 10 to 200 g / cm 2 , especially 20-100g / cm 2 , Grinding amount: 1.0~1.5μm.

[0152] The conditions for precision grinding of the glass substrate are not particularly limited. For example, it is preferred to use a soft grinding pad with a hardness of 75 to 77, and set the rotation speed of the grinding platform to 10 to 35 rpm, the rotation speed of the sun gear to 5 to 15 rpm, the grinding liquid supply rate to 1000 to 5000 mL / min, and the processing pressure to, for example, 10 to 200 g / cm 2 , especially 20-100g / cm 2 The grinding time is 2 to 12 minutes. The grinding amount can be set to about 2 to 50 μm, especially about 5 to 25 μm, for example.

[0153] (Flip)

[0154] Here, when manufacturing the magnetic disk substrate of the present invention, the front and back sides of the substrate can also be reversed (turned over) in the middle of the grinding process (grinding process or polishing process) and / or the grinding process. That is, in the grinding process, at least once the front and back sides of the aluminum alloy substrate or the glass substrate are reversed and then the grinding is continued. Alternatively, after the grinding process, a grinding process is also performed to grind the aluminum alloy substrate or the glass substrate, and in the grinding process, at least once the front and back sides of the aluminum alloy substrate or the glass substrate are reversed and then the grinding is continued. Thus, it is easy to process the substrate after grinding / grinding into a flatter substrate. Preferably, the substrate is turned over in the middle of the rough grinding process, especially in the middle of the grinding process and the rough grinding process.

[0155] In double-sided grinding, the thickness of the layer removed by grinding is also likely to be different on the upper platform side and the lower platform side of the substrate. This tendency is particularly high in rough grinding. If a disk is made using a substrate ground in this way, the flatness may deteriorate. By flipping in the middle of the grinding / polishing process, especially the rough grinding process, the risk of disk deformation can be reduced. In addition, flipping can be performed once in the grinding or polishing process, but it can also be performed twice or more. In addition, it is preferred to flip the substrate in such a way that the two surfaces of the substrate contact the polishing pads on the upper platform side and the lower platform side under the same conditions. For example, in the case of one flip, the grinding / polishing speed and the polishing time are made the same before and after the flip, and in the case of multiple flips, the total time of each surface being on the upper side is consistent with the total time of each surface being on the lower side for grinding.

[0156] <Evaluation methods for magnetic disks and substrates>

[0157] By going through the grinding / polishing process as described above, especially the grinding (grinding, polishing) process, a disk substrate having a thickness of less than 0.60 mm and a ΔTIR of less than 0.50 μm / mm can be manufactured. Since the disk of the present invention is thin-walled and flat, it is not easy to cause collision in the HDD device, which can reduce operation errors. In addition, the disk can be evaluated by, for example, making the head float on the rotating disk and using the head to detect the signal from the disk. The disk that passed the evaluation test is put into the next HDD process, but when the thickness of the disk is less than about 0.60 mm, the pass rate will generally decrease. According to the discovery of the inventors, the result of this evaluation test is related to the radial change rate ΔTIR of TIR. Since the disk of the present invention has a flat and good surface shape because the ΔTIR is less than 0.50 μm / mm, it can pass the evaluation test as described above even if the thickness is less than 0.60 mm.

[0158] In addition, according to the findings of the present inventors, the surface shapes of the substrate and the magnetic disk have almost no change before and after the production of the magnetic film. Therefore, it is preferred to measure ΔTIR for the ground aluminum alloy substrate and glass substrate before the production of the magnetic film. That is, the evaluation of ΔTIR and PV as described above is preferably performed as a substrate inspection process after the substrate is manufactured. In addition, as mentioned above, the surface shape of the magnetic disk is mainly caused by the grinding process in the case of the aluminum alloy substrate and the polishing process in the case of the glass substrate. In any substrate, it is affected by multiple factors such as the plate thickness distribution in the substrate and the internal stress generated during processing. Therefore, if the evaluation of the substrate is performed after the grinding process or the polishing process is completed, the substrate quality of each processing batch can be immediately confirmed, which is more preferred.

[0159] Although the embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, but includes all aspects included in the concept of the present invention and the claims, and various modifications can be made within the scope of the present invention.

[0160] Example

[0161] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these.

[0162] [Example 1]

[0163] An aluminum alloy magnetic disk substrate having a thickness of 0.50 mm and an outer diameter of 97 mm was produced as follows. In Example 1, an Al-Mg alloy was used.

[0164] First, a semi-continuous casting method was used to produce an ingot, which was then hot-rolled and cold-rolled to produce a plate with a thickness of 0.52 mm. The plate was punched using a press to produce a billet with an inner diameter of 24 mm and an outer diameter of 98 mm. The billets were then stacked on top of each other and heated at 30 kg / cm 2 The blank was subjected to pressure annealing treatment at 320°C for 3 hours under pressure. Secondly, the inner diameter and outer diameter parts of the blank were cut and chamfered by a lathe processing machine to produce a T bottom with an inner diameter of 25mm and an outer diameter of 97mm, which was then subjected to a heat treatment at 300°C×30 minutes. Next, the surfaces of both sides of the T bottom were ground (grinded) by a grinding machine to produce a G bottom with a thickness of 0.48mm. After the G bottom was pre-treated, a non-electrolytic Ni-P plating treatment was performed, and a Ni-P plating layer with a thickness of 10μm was attached to each single side to produce an M bottom. Secondly, after a heat treatment at 250°C×30 minutes, the surfaces of both sides of the M bottom were ground by a grinding machine to produce an aluminum alloy disk substrate.

[0165] In addition, the pretreatment of the G bottom and the electroless Ni-P plating treatment are performed as follows.

[0166] (Preprocessing)

[0167] Degreasing treatment of G bottom: AD-68F degreasing liquid manufactured by Uemura Industry Co., Ltd. was used under the conditions of concentration: 500 mL / L, temperature: 45° C., and treatment time: 3 minutes.

[0168] Acid etching treatment: Acid etching treatment was performed using an etching solution AD-107F manufactured by Uemura Industry Co., Ltd. under the conditions of a concentration of 50 mL / L, a temperature of 60° C., and a treatment time of 2 minutes.

[0169] Zincate treatment: The zincate treatment was performed twice with a nitric acid stripping treatment interposed therebetween. Specifically, the zincate treatment was performed in the order of a first zincate treatment, pure water washing, nitric acid stripping treatment, pure water washing, and a second zincate treatment.

[0170] The first zincate treatment was performed using a zincate treatment solution AD-301F-3X manufactured by Uemura Industries Co., Ltd. under the conditions of concentration: 200 mL / L, temperature: 20° C., and treatment time: 1 minute. The nitric acid stripping treatment was performed under the conditions of nitric acid concentration: 30 volume %, temperature: 25° C., and treatment time: 1 minute. The second zincate treatment was performed under the same conditions as the first zincate treatment.

[0171] (Non-electrolytic Ni-P plating treatment)

[0172] The electroless plating solution was NIMUDEN (registered trademark) HDX manufactured by Uemura Industry Co., Ltd., and the conditions were Ni concentration: 6 g / L, temperature: 88° C., and treatment time: 130 minutes.

[0173] In addition, the above-mentioned grinding process was performed under the following conditions.

[0174] (grinding)

[0175] Grinding stone: #4000 silicon carbide (SiC) grinding stone

[0176] Processing pressure: 100g / cm 2

[0177] · Grinding platform speed: 30rpm

[0178] Coolant flow rate: 3.5L / min

[0179] Grinding time: 5 minutes

[0180] The above-mentioned grinding is performed by double-sided grinding under the following conditions.

[0181] (Coarse grinding)

[0182] Abrasive: Alumina abrasive with a particle size of 0.4 μm

[0183] Polishing pad: 87 hardness hard urethane polishing pad

[0184] Processing pressure: 100g / cm 2

[0185] · Grinding platform speed: 30rpm

[0186] Sun gear speed: 10rpm

[0187] ·Grinding liquid supply speed: 3.5L / min

[0188] Grinding time: 5 minutes

[0189] (Precision grinding)

[0190] Abrasive: Colloidal silica abrasive with a particle size of 0.08 μm

[0191] Polishing pad: 76 hardness foamed urethane polishing pad

[0192] Processing pressure: 100g / cm 2

[0193] · Grinding platform speed: 30rpm

[0194] Sun gear speed: 10rpm

[0195] ·Grinding liquid supply speed: 3.5L / min

[0196] Grinding time: 3 minutes

[0197] For the disk substrate, the optical inspection device Mesa manufactured by Zygo Corporation was used to measure the TIR on the circumference of the radial distance r = 40mm, 45mm, 46mm, and 47mm from the center, and the ΔTIR was calculated according to the above (Formula 1) for the adjacent radial distances. When all the three calculated ΔTIRs are within 0.5μm, the comprehensive evaluation is regarded as ○, and when one of the three calculated ΔTIRs exceeds 0.5μm, the comprehensive evaluation is regarded as ×. In addition, the flatness PV was measured using the optical inspection device Mesa also manufactured by Zygo Corporation. These results are shown in Table 1 described later together with the grinding processing conditions.

[0198] [Examples 2 to 4, Comparative Examples 1 to 3]

[0199] In the same manner as in Example 1, the following aluminum alloy magnetic disk substrate was produced.

[0200] ·Examples 2, 4, Comparative Examples 1 to 3: Al-Fe alloys

[0201] Example 3: Al-Mg alloy.

[0202] The same operation as in Example 1 was performed except that the coolant flow rate during grinding was increased to 10.0 L / min (Example 2). In addition, except that the thickness of the aluminum alloy substrate was set to 0.60 mm (Example 3), or the processing pressure was set to 70 g / cm 2 The same operation as in Example 1 was performed except that the grinding pressure was changed to 150 g / cm 2 (Comparative Example 1) The same operation as in Example 1 was performed except that the rotation speed of the grinding plate was changed to 40 rpm (Comparative Example 2) or the flow rate of the coolant was changed to 0.1 L / min (Comparative Example 3). The evaluation results of each of the obtained magnetic disk substrates are shown in Table 1 described later, together with the material of the substrate and the grinding processing conditions.

[0203] [Example 5]

[0204] An aluminosilicate glass magnetic disk substrate having a thickness of 0.60 mm and an outer diameter of 97 mm was produced as follows.

[0205] The glass raw materials were heated at 1600-1700°C to form a melt, and then redrawn to form an aluminosilicate glass plate of 100 mm and 10 m in length. After that, a glass plate with a thickness of approximately 0.6 mm was selected for core removal and end surface grinding of the inner and outer peripheries (cutting, sizing, chamfering, and grinding of the chamfered portion of the inner and outer diameters of the glass plate) to produce a circular glass plate with an outer diameter of 97 mm and an inner diameter of a circular hole of 25 mm. The glass plate was ground (polished), roughly ground, and precisely ground using a double-sided grinder to produce a glass substrate.

[0206] The above-mentioned grinding is carried out under the following conditions.

[0207] (Polishing)

[0208] Grinding stone: Diamond grain

[0209] Processing pressure: 150g / cm 2

[0210] · Grinding platform speed: 30rpm

[0211] Coolant flow rate: 3.5L / min

[0212] Grinding time: 5 minutes

[0213] The above-mentioned rough grinding and precision grinding processes are performed by double-sided grinding under the following conditions.

[0214] (Coarse grinding)

[0215] ·Abrasive: Cerium oxide abrasive with a particle size of 0.1 to 0.4 μm and an average particle size of 0.19 μm

[0216] Polishing pad: 87 hardness hard urethane polishing pad

[0217] Processing pressure: 160g / cm 2

[0218] Grinding platform speed: 15rpm

[0219] Sun gear speed: 10rpm

[0220] ·Grinding liquid supply speed: 2.0L / min

[0221] Grinding time: 5 minutes

[0222] (Precision grinding)

[0223] Abrasive: Colloidal silica abrasive with a particle size of 10 to 100 nm and an average particle size of 80 nm

[0224] Polishing pad: 76 hardness foamed urethane polishing pad

[0225] Processing pressure: 100g / cm 2

[0226] · Grinding platform speed: 30rpm

[0227] Sun gear speed: 10rpm

[0228] ·Grinding liquid supply speed: 3.5L / min

[0229] Grinding time: 5 minutes

[0230] About the obtained aluminosilicate glass magnetic disk substrate, ΔTIR and flatness PV were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1 together with the grinding (polishing) conditions.

[0231] [Table 1]

[0232] [Table 1 Material / grinding conditions and evaluation results of each sample]

[0233]

[0234] 1)mm 2)g / cm 2 3) rpm 4) L / min 5) μm

[0235] 6) The radial change rate of TIR on each circumference at radial distances r1 and r2 shown in the row directly below (μm / mm)

[0236] 6a) ΔTIR for rl = 40 mm, r2 = 45 mm (rl / R = 0.82, r2 / R = 0.93)

[0237] 6b) ΔTTR for rl = 45 mm, r2 = 46 mm (rl / R = 0.93, r2 / R = 0.95)

[0238] 6c) ΔTIR when rl = 46 mm, r2 = 47 mm (rl / R = 0.95, r2 / R = 0.97)

[0239] According to the present invention, a disk substrate is provided, which has a thin wall with a thickness of less than 0.60 mm and is extremely flat with a ΔTIR of less than 0.50 μm / mm. These substrates can be mounted in multiple pieces in an HDD device due to their flatness, and since they are large in outer diameter of 97 mm, the data area on the surface can be expanded. In addition, the flatness PV of the disk substrates of Examples 1 to 3 is also less than 20.0 μm, showing a good surface shape. Therefore, it can be seen that the disks based on these substrates can reduce physical errors even when assembled into HDD devices, and can also cope with the high capacity of hard disks.

[0240] On the other hand, in Comparative Example 1, since the pressure applied to the aluminum alloy substrate was high, a difference occurred in the applied pressure depending on the position in the aluminum alloy substrate, and TIR deteriorated, resulting in deterioration of ΔTIR.

[0241] In Comparative Example 2, the rotation speed of the platen was too high, so the grindstone was unstable, and the coolant that should assist grinding was discharged on the outer peripheral side. As a result, TIR varied depending on the measurement position, and ΔTIR deteriorated.

[0242] In Comparative Example 3, since the coolant flow rate was small, the grinding chips were not sufficiently discharged, and TIR deteriorated as a whole, and ΔTIR deteriorated.

[0243] Example 5 Since the glass substrate is used, even if the pressure is 150g / cm 2 , TIR is also good, and as a result, an extremely flat magnetic disk substrate with a ΔTIR of 0.50 μm / mm or less is provided.

[0244] Reference numerals

[0245] 1 Disk

[0246] 2 Center of Disk 1

[0247] C1 A circle for measuring TIR1 with a radius of r1 measured from the center 2 of disk 1

[0248] C2 A circle for measuring TIR2 with a radius of r2 measured from the center 2 of disk 1

[0249] Ca represents the outer circumference of the outer circumference area of ​​the magnetic disk 1.

[0250] Cb represents the inner circumference of the outer circumference area of ​​the disk 1.

Claims

1. A magnetic disk having a hole in the center, and The thickness is less than 0.60mm. Let the radius of the disk be R (mm), The radial distance of the magnetic disk measured from the center of the magnetic disk is defined as r (mm). In the outer peripheral area of ​​the magnetic disk where r / R is 0.70 or more and 0.99 or less, When the TIR measured on the circumference of the magnetic disk at different radial distances r1 (mm) and r2 (mm) is TIR1 (μm) and TIR2 (μm), The radial change ΔTIR of TIR represented by the absolute value of the ratio of the difference (TIR1-TIR2) between TIR1 and TIR2 to the difference (r1-r2) between the radial distance r1 and r2 of the disk |(TIR1-TIR2) / (r1-r2)| is less than 0.50 μm / mm.

2. The magnetic disk according to claim 1, wherein The flatness PV is 20.0 μm or less.

3. The magnetic disk according to claim 1 or 2, wherein: The outer diameter is 95mm or more. 4 . A substrate used for the magnetic disk according to claim 1 .

5. A method for manufacturing a magnetic disk, which is the method for manufacturing a magnetic disk according to any one of claims 1 to 3, characterized in that: The aforementioned disk is made of an aluminum alloy substrate. The method for manufacturing the magnetic disk comprises a grinding process step of grinding the aluminum alloy substrate. The grinding process is carried out at a pressure of 50 g / cm 2 Above and 120g / cm 2 The test was performed under the following conditions: the platform rotation speed was 10 rpm to 35 rpm, and the coolant flow rate was 1 L / min to 10 L / min.

6. A method for manufacturing a magnetic disk, which is the method for manufacturing a magnetic disk according to any one of claims 1 to 3, characterized in that: The aforementioned disk is made of a glass substrate. The method for manufacturing the magnetic disk comprises a grinding process step of grinding the glass substrate. The grinding process is carried out at a pressure of 100 g / cm 2 Above and 200g / cm 2 The test was performed under the following conditions: the platform rotation speed was 10 rpm to 35 rpm, and the coolant flow rate was 1 L / min to 10 L / min.

7. The method for manufacturing a magnetic disk according to claim 5 or 6, wherein: In the grinding process, the grinding amount is 2.5 μm or more and 25 μm or less.

8. The method for manufacturing a magnetic disk according to any one of claims 5 to 7, wherein: In the grinding process, at least once the front and back surfaces of the aluminum alloy substrate or the glass substrate are turned over and then the grinding is continued.

9. The method for manufacturing a magnetic disk according to any one of claims 5 to 8, wherein: After the grinding process, a grinding process is performed to grind the aluminum alloy substrate or the glass substrate. In the grinding process, at least once the front and back sides of the aluminum alloy substrate or the glass substrate are reversed and then the grinding is continued.

Citation Information

Patent Citations

  • Aluminum alloy sheet for magnetic disk and production method therefor, and magnetic disk using said aluminum alloy sheet for magnetic disk

    CN112470221A

  • Substrate for magnetic disks, and magnetic disk

    CN112513985A

  • Glass substrate for HDD, process for producing glass substrate for HDD, and magnetic recording medium for HDD

    JP2013016214A

  • Glass substrate for information recording medium, method for producing glass substrate for information recording medium, and information recording medium

    WO2011096310A1

  • Process for producing glass substrate for information-recording medium