Multilayer ceramic capacitor

By using alternate stacked dielectric layers and internal electrodes in the external electrodes of the laminated ceramic capacitor, combined with the design of metal layer, glass film and firing layer, the problem of insufficient moisture resistance and reliability of the external electrode is solved, and better moisture is achieved Suppression effect.

CN118946942APending Publication Date: 2024-11-12MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034083.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-02
Filing Date
2023-04-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The external electrodes of the existing stacked ceramic capacitors have insufficient moisture resistance and reliability, mainly because the external electrodes are prone to cracks, resulting in damage to the moisture intrusion suppression function.

Method used

A laminated body with alternately stacked dielectric layers and internal electrodes is adopted. The outer electrode provided on the surface has a metal layer, a glass film and a calcined layer. The calcined layer contains glass and metal and covers a plating film. The thickness of the metal layer is above 0.1 μm. The thickness of the calcined adhesion layer is 0.1 μm or more than 1.0 μm, and the calcined adhesion layer has a void, and there is a plating material inside it. The area of ​​the metal part of the plating film is 10 times larger than the area of ​​the glass part, and the glass film covers it. Around the metal layer, the metal layer partly exposed from the firing layer.

Benefits of technology

It effectively suppresses cracks from external electrodes, improves the moisture resistance and reliability of the stacked ceramic capacitors, and ensures the protection effect of moisture intrusion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946942A_ABST
    Figure CN118946942A_ABST
Patent Text Reader

Abstract

Provided is a multilayer ceramic capacitor capable of suppressing the occurrence of cracks in an external electrode and improving moisture resistance reliability. An external electrode of a multilayer ceramic capacitor (1) is provided with: metal layers (41a, 41b) disposed on a first end surface (E1) and a second end surface (E2) so as to cover an internal electrode led out to the first end surface (E1) and an internal electrode led out to the second end surface (E2); glass films (42a, 42b) which are disposed on the first end surface (E1) and the second end surface (E2) and are disposed around the metal layers (41a, 41b) so as to be adjacent to the metal layers (41a, 41b); a sintered layer (43a, 43b) that contains glass and a metal and is disposed so as to cover the metal layer (41a, 41b); and plating films (44a, 44b) disposed so as to cover the sintered layers (43a, 43b), the thickness of the metal layers (41a, 41b) being 0.1 [mu] m or more and 15.0 [mu] m or less, and the thickness of the sintered layers (43a, 43b) being 0.1 [mu] m or more and 1.0 [mu] m or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminated ceramic capacitor. Background Art

[0002] A multilayer ceramic capacitor is known that includes a multilayer body in which dielectric layers and internal electrodes are alternately stacked, and an external electrode that is electrically connected to the internal electrode and is provided on a surface of the multilayer body.

[0003] Patent Document 1 describes a method for forming external electrodes in a multilayer ceramic capacitor.

[0004] Prior Art Literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-266208 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] A multilayer ceramic capacitor having external electrodes has a problem of insufficient moisture resistance reliability. One of the main causes of insufficient moisture resistance reliability is the occurrence of cracks in the external electrodes.

[0009] An object of the present invention is to provide a multilayer ceramic capacitor that can suppress the occurrence of cracks in external electrodes and has improved moisture-resistant reliability.

[0010] Technical solutions to solve problems

[0011] The multilayer ceramic capacitor of the present invention comprises:

[0012] A laminated body in which a plurality of dielectric layers and internal electrodes are alternately laminated; and

[0013] a pair of external electrodes, provided on the surface of the stacked body and electrically connected to the internal electrodes led out to the surface of the stacked body;

[0014] The laminated body has:

[0015] The first main surface and the second main surface are opposite to each other in the thickness direction which is the lamination direction of the dielectric layer and the internal electrode;

[0016] The first end surface and the second end surface are opposed to each other in a longitudinal direction which is a direction in which the pair of external electrodes are opposed to each other, and the external electrodes are provided thereon; and

[0017] The first side surface and the second side surface are opposite to each other in a width direction perpendicular to the thickness direction and the length direction.

[0018] The external electrode comprises:

[0019] a metal layer disposed on the first end surface and the second end surface so as to cover the internal electrode led out to the first end surface and the internal electrode led out to the second end surface;

[0020] A glass film is disposed on the first end surface and the second end surface and is adjacent to the metal layer and disposed around the metal layer;

[0021] a sintered layer comprising glass and metal and configured to cover the metal layer; and

[0022] a coating film configured to cover the sintered layer,

[0023] The thickness of the metal layer is greater than or equal to 0.1 μm and less than or equal to 15.0 μm.

[0024] The thickness of the sintered layer is greater than or equal to 0.1 μm and less than or equal to 1.0 μm.

[0025] Effects of the Invention

[0026] According to the present invention, it is possible to provide a multilayer ceramic capacitor which can suppress the occurrence of cracks in external electrodes and has improved moisture-resistant reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a perspective view of a multilayer ceramic capacitor of the present invention.

[0028] Figure 2 yes Figure 1 Line II cross-sectional view.

[0029] Figure 3 yes Figure 1 Cross-sectional view along line III-III.

[0030] Figure 4 yes Figure 1 Sectional view along line IV-IV. DETAILED DESCRIPTION

[0031] Hereinafter, an example of an embodiment of the present invention will be described with reference to the accompanying drawings. In addition, in each figure, the same reference numerals are attached to the same or corresponding parts.

[0032] <Outline of Multilayer Ceramic Capacitors>

[0033] based on Figure 1 The outline of the appearance of the multilayer ceramic capacitor 1 will be described. Figure 1 1 is a perspective view showing a multilayer ceramic capacitor 1 according to the present embodiment.

[0034] like Figure 1As shown, the multilayer ceramic capacitor 1 includes a multilayer body 2 and external electrodes 4 (4a, 4b). The external electrodes 4 include a first external electrode 4a and a second external electrode 4b.

[0035] <Definition of direction>

[0036] exist Figures 1 to 4 , the L direction, the W direction, and the T direction are shown. The L direction is the length direction L of the multilayer ceramic capacitor 1. The W direction is the width direction W of the multilayer ceramic capacitor 1. The T direction is the stacking direction of the multilayer ceramic capacitor 1, that is, the thickness direction T.

[0037] thus, Figure 2 The section shown is called the LT section. Figure 3 as well as Figure 4 The section shown is called the WT section.

[0038] The length direction L, the width direction W, and the thickness direction T do not necessarily need to be orthogonal to each other. The length direction L, the width direction W, and the thickness direction T may be intersecting to each other.

[0039] <Outer Shape of Laminated Body>

[0040] like Figure 1 As shown, the shape of the stacked body 2 is a substantially rectangular parallelepiped shape.

[0041] The laminate has two end surfaces, two main surfaces, and two side surfaces.

[0042] The end faces are faces facing each other in the longitudinal direction L. The main faces are faces facing each other in the thickness direction T. The side faces are faces facing each other in the width direction W.

[0043] The two end faces are referred to as the first end face E1 and the second end face E2. The two principal faces are referred to as the first principal face M1 and the second principal face M2. The two side faces are referred to as the first side face S1 and the second side face S2.

[0044] The corners and ridges of the laminate 2 are preferably rounded. The corners are the portions where three surfaces of the laminate 2 intersect. The ridges are the portions where two surfaces of the laminate 2 intersect.

[0045] <Size of laminated body>

[0046] The size of the laminated body 2 can be set, for example, as follows.

[0047] The length L of the laminate 2 can be 200 μm to 2000 μm. The length in the thickness direction of the laminate 2 can be 100 μm to 1000 μm. The length in the width direction W of the laminate 2 can be 100 μm to 1000 μm.

[0048] The length of each portion of the laminate 2 can be measured using a micrometer or an optical microscope.

[0049] <Internal structure of laminate>

[0050] based on Figure 2 as well as Figure 3 , the internal structure of the stacked body 2 is described.

[0051] Figure 2 yes Figure 1 FIG. 1 is a cross-sectional view of the multilayer ceramic capacitor taken along line II shown in FIG. Figure 3 yes Figure 1 FIG. 1 is a cross-sectional view of the multilayer ceramic capacitor taken along line III-III shown in FIG.

[0052] like Figure 2 As shown, the laminate 2 includes a plurality of dielectric layers 7 ( 7 a , 7 b ) and a plurality of internal electrodes 8 ( 8 a , 8 b ). The plurality of dielectric layers 7 and the plurality of internal electrodes 8 are stacked in the thickness direction T on one another.

[0053] <Dielectric Layer>

[0054] like Figure 2 As shown, the dielectric layer 7 includes an outer dielectric layer 7a and an inner dielectric layer 7b.

[0055] <Outer Dielectric Layer>

[0056] The outer dielectric layers 7a are the dielectric layers 7 located on the first and second principal surfaces M1 and M2 of the laminate 2. That is, the outer dielectric layers 7a are the dielectric layers 7 located on both outer sides in the thickness direction T of the laminate 2.

[0057] Specifically, the outer dielectric layer 7 a is the dielectric layer 7 located between the first main surface M1 and the internal electrode 8 closest to the first main surface M1 , and between the second main surface M2 and the internal electrode 8 closest to the second main surface M2 .

[0058] <Inner Dielectric Layer>

[0059] The inner dielectric layer 7 b is the dielectric layer 7 located between the internal electrodes 8 .

[0060] Specifically, the inner dielectric layer 7b is the dielectric layer 7 located between a first inner electrode 8a and a second inner electrode 8b described below.

[0061] <Internal Electrode>

[0062] like Figure 2As shown, the internal electrode 8 includes a first internal electrode 8a and a second internal electrode 8b. The first internal electrode 8a is an internal electrode connected to the first external electrode 4a. The second internal electrode 8b is an internal electrode connected to the second external electrode 4b.

[0063] The first inner electrode 8a extends from the first end surface E1 toward the second end surface E2. The second inner electrode 8b extends from the second end surface E2 toward the first end surface E1.

[0064] <Opposing portion and lead portion>

[0065] The first internal electrode 8a and the second internal electrode 8b each have an opposing portion and a lead portion.

[0066] The opposing portion is a portion where the first internal electrode 8a and the second internal electrode 8b oppose each other.

[0067] The lead portion is a portion led out from the opposing portion to the end faces E1 and E2 of the laminate 2. Specifically, the lead portion of the first internal electrode 8a is a portion led out from the opposing portion to the first end face E1 of the laminate 2. The lead portion of the second internal electrode 8b is a portion led out from the opposing portion to the second end face E2 of the laminate 2.

[0068] The facing portion of the first internal electrode 8a and the facing portion of the second internal electrode 8b face each other via the inner dielectric layer 7b, thereby forming capacitance at the facing portions. Thus, the multilayer ceramic capacitor 1 functions as a capacitor.

[0069] <Lengthwise Gap>

[0070] like Figure 2 As shown, the region from the front end of the first inner electrode 8a on the second end face E2 side to the second end face E2 is defined as the longitudinal gap LG. Similarly, the region from the front end of the second inner electrode 8b on the first end face E1 side to the first end face E1 is defined as the longitudinal gap LG.

[0071] The length of the longitudinal direction L of the longitudinal gap LG can be set to, for example, 5 μm or more and 30 μm or less.

[0072] <Gap in Width Direction>

[0073] like Figure 3 As shown, the region from the end of the internal electrode 8 in the width direction W to the first side surface S1 is defined as the width direction gap WG. Similarly, the region from the end of the internal electrode 8 in the width direction W to the second side surface S2 is defined as the width direction gap WG.

[0074] The length of the width direction W of the width direction gap WG can be set to, for example, 5 μm or more and 30 μm or less.

[0075] <Number of Dielectric Layers>

[0076] The number of dielectric layers 7 stacked in the stacked body 2 can be, for example, 10 or more and 1000 or less. The number of dielectric layers 7 includes the number of outer dielectric layers 7a and the number of inner dielectric layers 7b.

[0077] <Thickness of Dielectric Layer>

[0078] The thickness of the outer dielectric layer 7 a among the dielectric layers 7 can be set to, for example, 10 μm or more and 100 μm or less. The thickness of the inner dielectric layer 7 b can be set to, for example, 0.3 μm or more and 5.0 μm or less.

[0079] <Material for Dielectric Layer>

[0080] The material of the dielectric layer 7 can be, for example, a dielectric ceramic including BaTiO 3 , CaTiO 3 , SrTiO 3 , or CaZrO 3 .

[0081] The material of the dielectric layer 7 may be a material obtained by adding a Mn compound, a Fe compound, a Cr compound, a Co compound, a Ni compound, or the like to the above-mentioned dielectric ceramic.

[0082] <Number of Internal Electrodes>

[0083] The number of the internal electrodes 8 can be set, for example, to not less than 10 and not more than 1000. The number of the internal electrodes 8 includes the number of the first internal electrodes 8a and the number of the second internal electrodes 8b.

[0084] <Thickness of Internal Electrode>

[0085] The thickness of the internal electrode 8 can be set to, for example, 0.3 μm or more and 5.0 μm or less. When the thickness of the internal electrode 8 is 0.5 μm or more, a plated film easily grows when a metal layer is formed by plating. The metal layer will be described later.

[0086] <Material of Internal Electrode>

[0087] The material of the internal electrode 8 can be, for example, metals such as Ni, Cu, Ag, Pd, and Au, alloys of Ni and Cu, alloys of Ag and Pd, etc. In addition, the material of the internal electrode 8 may include dielectric particles of the same composition as the ceramic included in the dielectric layer 7 .

[0088] <External Electrode>

[0089] As based on Figure 1 As described above, the external electrodes include the first external electrode 4 a and the second external electrode 4 b .

[0090] <First External Electrode>

[0091] like Figure 1 As shown, the first external electrode 4 a is an external electrode disposed on the first end surface E1 of the stacked body 2 .

[0092] The first external electrode 4 a extends from the first end surface E1 to a part of both main surfaces and a part of both side surfaces.

[0093] The portion of the first external electrode 4a disposed on the first end surface E1 of the stacked body 2 is referred to as the end surface external electrode 4Ea. The portion of the first external electrode 4a disposed on a portion of the first principal surface M1 or a portion of the second principal surface M2 is referred to as the principal surface external electrode 4Ma. The portion of the first external electrode 4a disposed on a portion of the first side surface S1 or a portion of the second side surface S2 is referred to as the side surface external electrode 4Sa.

[0094] like Figure 2 As shown, the first external electrode 4a is electrically connected to the first internal electrode 8a.

[0095] <Second External Electrode>

[0096] The second external electrode 4 b is an external electrode disposed on the second end surface E2 of the stacked body 2 .

[0097] The second external electrode 4b has the same structure as the first external electrode 4a.

[0098] That is, the second outer electrode 4 b extends from the second end surface E2 to a part of both main surfaces and a part of both side surfaces.

[0099] The portion of the second external electrode 4b disposed on the second end surface E2 of the stack 2 is referred to as the end surface external electrode 4Eb. The portion of the second external electrode 4b disposed on a portion of the first principal surface M1 or a portion of the second principal surface M2 is referred to as the principal surface external electrode 4Mb. The portion of the second external electrode 4b disposed on a portion of the first side surface S1 or a portion of the second side surface S2 is referred to as the side surface external electrode 4Sb.

[0100] like Figure 2 As shown, the second outer electrode 4b is electrically connected to the second inner electrode 8b.

[0101] <Layer Structure of External Electrode>

[0102] based on Figure 2 The layer structure of the external electrode 4 will be described.

[0103] like Figure 2As shown, the first external electrode 4a includes a metal layer 41a, a glass film 42a, a sintered layer 43a, and a plated film 44a. The second external electrode 4b includes a metal layer 41b, a glass film 42b, a sintered layer 43b, and a plated film 44b.

[0104] Each layer of the external electrode 4 will be described by taking the first external electrode 4 a as an example.

[0105] In addition, each layer of the second external electrode 4b has the same structure as each layer of the first external electrode 4. Therefore, the description about the first external electrode 4a is also applicable to the second external electrode 4b.

[0106] <Metal Layer>

[0107] The end portion of the first internal electrode 8a is exposed from the end surface E1. The metal layer 41a is a metal layer provided on the first end surface E1 so as to cover the exposed end portion of the first internal electrode 8a.

[0108] The metal layer 41a is formed of, for example, a material containing at least one metal selected from Cu, Ni, Ag, Pd, Au, etc. The metal layer 41a may be formed of, for example, an alloy such as an alloy of Cu and Ni or an alloy of Ag and Pd.

[0109] A part of the material forming the metal layer 41a may diffuse into the first internal electrode 8a which is in contact with the metal layer 41a. The material forming the metal layer 41a and the material forming the first internal electrode 8a are mixed together, thereby improving the bonding strength between the metal layer 41a and the first internal electrode 8a.

[0110] The metal layer 41 a can be formed by, for example, plating.

[0111] <Thickness of Metal Layer>

[0112] Figure 2 The thickness of the metal layer 41a is indicated by d1.

[0113] The thickness d1 of the metal layer 41 a can be set to, for example, 0.1 μm or more and 15.0 μm or less.

[0114] When the thickness d1 of the metal layer 41a is less than 0.1 μm, the continuity of the metal layer 41a tends to decrease. Therefore, the bonding strength between the metal layer 41a and the first internal electrode 8a may decrease. In addition, the conductivity of the metal layer 41a may decrease.

[0115] When the thickness d1 of the metal layer 41a exceeds 15.0 μm, the internal stress in the metal layer 41a tends to increase, so that the metal layer 41a may be separated from the first internal electrode 8a.

[0116] <Burn layer>

[0117] The sintered layer 43a is a layer arranged to cover at least a portion of the metal layer 41a. The sintered layer 43a includes glass and metal.

[0118] The sintered layer 43a is formed of a material including at least one metal selected from Cu, Ni, Ag, Pd, Au, etc. The sintered layer 43a may be a single layer or may include a plurality of layers.

[0119] The sintered layer 43a can be formed, for example, as follows. That is, first, a conductive paste is applied on the metal layer 41a. The conductive paste contains glass and metal. Next, the applied conductive paste is fired. In this way, the sintered layer 43a can be formed.

[0120] This firing or sintering can be performed simultaneously with the firing of the laminate 2. Alternatively, the sintering layer 43a can be fired after the laminate 2 is fired.

[0121] The sintered layer 43a will be described in more detail later.

[0122] <Glass Film>

[0123] The glass film 42a is a film mainly made of glass and is disposed around the metal layer 41a.

[0124] like Figure 2 As shown, the glass film 42a is disposed around the metal layer 41a so as to be adjacent to the metal layer 41a and surround the metal layer 41a. Specifically, the glass film 42a is in contact with the end 5 of the metal layer 41a.

[0125] The glass film 42a extends from a portion of the first end face E1 to a portion of the first main face M1 of the laminate 2. Similarly, the glass film 42a extends from a portion of the first end face E1 to a portion of the second main face M2 of the laminate 2.

[0126] In addition, although Figure 2 Although not shown, the glass film 42 a extends from a portion of the first end surface E1 of the stacked body 2 to a portion of the first side surface S1 and a portion of the second side surface S2 .

[0127] The glass film 42a is formed together with the sintered layer 43 in the process of forming the sintered layer 43a. In the process of forming the sintered layer 43a, a conductive paste is applied to the first end surface E1. The conductive paste contains glass.

[0128] The glass moves to the exposed portion of the dielectric layer 7 during the sintering process. The exposed portion of the dielectric layer 7 is a portion where the metal layer 41a is not arranged in the laminate 2. The glass moves to a portion of the first end face E1, a portion of the first main face M1, a portion of the second main face M2, a portion of the first side face S1, and a portion of the second side face S2. In this way, the glass moved to the exposed portion of the dielectric layer 7 forms a glass film 42a after the sintering is completed.

[0129] As described above, the glass contained in the conductive paste moves to the exposed portion of the dielectric layer 7 during sintering. Therefore, the glass content of the glass film 42a becomes higher than the glass content of the sintered layer 43a.

[0130] <Ratio of Metal to Glass in Sintered Layer>

[0131] In particular, it is preferred that the surface of the sintered layer 43a has a low glass content.

[0132] This is because the adhesion of the plating film 44a described later to the surface of the sintered layer 43a is improved. In addition, this is because the adhesion between the surface of the sintered layer 43a and the plating film 44a is improved.

[0133] Specifically, in the surface of the sintered layer 43a on the plated film 44a side, the area of ​​the portion including metal is preferably larger than 10 times the area of ​​the portion including glass.

[0134] Thereby, the adhesion of the plated film 44a to the sintered layer 43a can be sufficiently improved. In addition, the adhesion between the sintered layer 43a and the plated film 44a can be sufficiently improved.

[0135] The glass film 42a is not necessarily formed only of glass. The glass film 42a may contain other materials such as metal materials in addition to glass. However, the ratio of glass contained in the glass film 42a is preferably high. This is because the higher the ratio of glass, the higher the effect of suppressing the intrusion of moisture into the interior of the laminate 2, etc., which will be described later.

[0136] As described above, the glass film 42a is arranged to be in contact with the end 5 of the metal layer 41a and adjacent to the metal layer 41a so as to surround the periphery of the metal layer 41a. In other words, the end 5 of the metal layer 41a is buried and sealed by the glass film 42a.

[0137] This can suppress the intrusion of moisture from the periphery of the metal layer 41 a into the interface between the dielectric layer 7 and the internal electrode 8 .

[0138] From the viewpoint of suppressing moisture intrusion, it is preferred that the glass film 42a is in continuous contact with the end portion 5 around the entire periphery of the metal layer 41a, thereby covering the entire periphery of the metal layer 41a.

[0139] Whether the glass film 42 a is formed on the surface of the laminate 2 can be determined by appropriately polishing the laminate 2 and performing elemental analysis on the portion using a field emission wavelength dispersive X-ray spectrometer.

[0140] <Plating film>

[0141] The plated film 44a is a film containing metal formed by plating and is arranged to cover the sintered layer 43a.

[0142] The plated film 44a is formed of a material containing at least one metal selected from Cu, Ni, Ag, Pd, Au, etc. The plated film 44a may be formed of an alloy such as an alloy of Ag and Pd. In addition, the plated film 44a does not contain glass.

[0143] The plating film 44a includes a lower plating film and an upper plating film. The upper plating film is a plating film formed on the lower plating film.

[0144] The lower plating film is formed of a material containing at least one metal selected from the group consisting of Cu, Ni, Ag, Pd, an alloy of Ag and Pd, and Au, for example.

[0145] The upper plating film is formed using Sn as a material, for example.

[0146] By using Sn as the material of the upper plating film, the wettability of the solder to the first external electrode 4 a can be improved.

[0147] The thickness of the upper plating film can be set to, for example, 1 μm or more and 10 μm or less. In addition, the thickness of the plating films 44 a and 44 b can also be set to, for example, 1 μm or more and 10 μm or less.

[0148] The above description of the first external electrode 4a is also applicable to the second external electrode 4b because the first external electrode 4a and the second external electrode 4b are the same except that the first external electrode 4a and the second external electrode 4b are provided on different surfaces.

[0149] Therefore, the metal layer 41b, the glass film 42b, the sintered layer 43b, and the plated film 44b in the second external electrode 4b are the same as the components described in relation to the first external electrode 4a.

[0150] <Size of Multilayer Ceramic Capacitors>

[0151] The length L of the entire multilayer ceramic capacitor 1 including the laminate 2 and the external electrodes 4 can be set to, for example, 0.2 mm or more and 2.0 mm or less. The length T of the entire multilayer ceramic capacitor 1 in the thickness direction can be set to, for example, 0.1 mm or more and 1.2 mm or less. The length W of the entire multilayer ceramic capacitor 1 in the width direction can be set to, for example, 0.1 mm or more and 1.2 mm or less.

[0152] <Details of External Electrodes>

[0153] based on Figure 2 , the external electrode 4 is described in detail.

[0154] As mentioned earlier, Figure 2 yes Figure 1 Here, the II-line cross-sectional view is a LT cross-sectional view at the center position in the width direction W of the multilayer ceramic capacitor 1 .

[0155] exist Figure 3 The center position in the width direction W is shown in FIG. Figure 3 The position of the line I is the center position of the multilayer ceramic capacitor 1 in the width direction W. Figure 3 yes Figure 1 III-III section view. Figure 3 WT is a diagram showing a cross section of the multilayer ceramic capacitor 1 .

[0156] Will Figure 2 The LT cross section at the center position in the width direction W of the multilayer ceramic capacitor 1 shown is set to be a 1 / 2 LT cross section.

[0157] Hereinafter, the external electrode 4 will be described by taking the first external electrode 4a as an example. In addition, the second external electrode 4b has the same structure as the first external electrode 4a. Therefore, the following description is also appropriate for the second external electrode 4b.

[0158] <Metal layer and glass film>

[0159] At the first end face E1, Figure 2 As shown, the metal layer 41a is arranged on substantially the entire area of ​​the first end surface E1. However, a glass film 42a is arranged in the vicinity of the first main surface M1 and the vicinity of the second main surface M2 in the first end surface E1 instead of the metal layer 41a. The glass film 42a is in contact with the end 5 of the metal layer 41a.

[0160] In addition, although Figure 2 Although not shown, the glass film 42a is also disposed in the first end surface E1, in the vicinity of the first side surface S1 and in the vicinity of the second side surface S2. The glass film 42a is also in contact with the end portion 5 of the metal layer 41a.

[0161] As described above, the glass film 42 a is arranged to cover the periphery of the metal layer 41 a .

[0162] More specifically, the glass film 42 a on the first end surface E1 extends from the end 5 of the metal layer 41 a to a portion of the first main surface M1 and a portion of the second main surface M2 .

[0163] In addition, although Figure 2 Although not shown, the glass film 42a extends from the end 5 of the metal layer 41a to a portion of the first side surface S1 and a portion of the second side surface S2.

[0164] That is, the glass film 42 a is arranged so as to cover the ridgeline portion of the laminate 2 between the first end surface and the two main surfaces and the two side surfaces.

[0165] <Burn layer>

[0166] The sintered layer 43a is not disposed over the entire area of ​​the metal layer 41a. Figure 2 As shown in FIG. 1 , in the vicinity of the end portion of the first end surface E1 , the outer edge of the sintered layer 43 a is located inside the outer edge of the metal layer 41 a .

[0167] In other words, the sintered layer 43 a does not extend continuously from the first end surface E1 to a part of the first main surface M1 and a part of the second main surface M2 .

[0168] The sintered layer 43a is temporarily interrupted near the ridges between the first end surface E1 and the first main surface M1 and between the first end surface E1 and the second main surface M2. As described above, the ridges are portions where two surfaces of the laminate 2 intersect.

[0169] Thus, since the sintered layer 43a is interrupted near the ridgeline, the end 5 of the metal layer 41a is not covered by the sintered layer 43a. In other words, the end 5 of the metal layer 41a is exposed from the sintered layer 43a.

[0170] In addition, although Figure 2 Although not shown in the figure, the sintered layer 43a is also arranged on a part of the first side surface S1 and a part of the second side surface S2.

[0171] However, similar to the first main surface M1 and the second main surface M2 described above, the sintered layer 43 a does not extend continuously from the first end surface E1 to the first side surface S1 and the second side surface S2 .

[0172] The sintered layer 43 a is temporarily interrupted near the ridgeline between the first end face E1 and the first side face S1 , and between the first end face E1 and the second side face S2 .

[0173] Accordingly, the end portion 5 of the metal layer 41a is not covered by the fired layer 43a. In other words, the end portion 5 of the metal layer 41a is exposed from the fired layer 43a.

[0174] As described above, the entire periphery of the metal layer 41a is not covered by the fired layer 43a.

[0175] Precisely, the entire periphery of the metal layer 41a is exposed from the fired layer 43a. Regarding this, an explanation will be given later based on Figure 4 this.

[0176] <Plated film>

[0177] The plated film 44a is arranged to cover the entire fired layer 43a. That is, the plated film 44a is arranged over the range where the fired layer 43a is disposed and on a part of the first end face E1 and the two main faces. Further, although not shown in Figure 2 this figure, the plated film 44a is also arranged on a part of the two side faces in the same manner as the two main faces.

[0178] Hereinafter, the arrangement of the metal layer 41a and the fired layer 43a and the like will be described based on the WT cross-section of the multilayer ceramic capacitor 1.

[0179] <WT cross-section>

[0180] Figure 3 and Figure 4 are both WT cross-sectional views of the multilayer ceramic capacitor 1. However, in Figure 3 and Figure 4 the positions of the cross-sections are different.

[0181] As described above, Figure 3 is Figure 1 the III-III line cross-sectional view. Figure 3 is a view showing the WT cross-section at the line L1 of Figure 2 this figure.

[0182] As Figure 3 shown, outside the laminate 2, the glass film 42a is arranged to surround the entire periphery of the laminate 2.

[0183] Moreover, outside the glass film 42a, the fired layer 43a is arranged to surround the entire periphery of the glass film 42a.

[0184] And, outside the fired layer 43a, the plated film 44a is arranged to surround the entire periphery of the fired layer 43a.

[0185] Figure 4 is Figure 1 the IV-IV line cross-sectional view. Figure 4 is a view showing the WT cross-section at the line L2 of Figure 2 this figure.

[0186] like Figure 4 As shown in FIG. 1 , a plating film 44a is disposed around the metal layer 41a. No sintered layer 43a is disposed around the metal layer 41a.

[0187] Therefore, the entire periphery of the metal layer 41a is exposed from the sintered layer 43a.

[0188] <Thickness of the sintered layer>

[0189] based on Figure 2 The thickness d2 of the sintered layer 43a will be described. Figure 2 LT is a diagram showing a cross section of the multilayer ceramic capacitor 1 .

[0190] exist Figure 2 d2 indicates the thickness of the sintered layer 43a. In the present embodiment, the thickness of the sintered layer 43a is thin. Specifically, in the multilayer ceramic capacitor 1 of the present embodiment, the thickness d2 of the sintered layer 43a is 0.1 μm or more and 1.0 μm or less.

[0191] Here, as described above, the thickness d1 of the metal layer 41a is 0.1 μm or more and 15.0 μm or less. Therefore, in the ceramic capacitor 1 of the present embodiment, the thickness d2 of the sintered layer 43a is also much thinner than the thickness of the metal layer 41a.

[0192] <Voids in the Burnt Layer>

[0193] based on Figure 2 The voids 6 of the sintered layer 43a will be described.

[0194] In the multilayer ceramic capacitor 1 of the present embodiment, the voids 6 are formed in the sintered layer 43 a .

[0195] The voids 6 are portions of the sintered layer 43a that are not filled with the glass or metal material. Here, the glass or metal material refers to the glass or metal material contained in the conductive paste used to form the sintered layer 43a.

[0196] <Position of the gap>

[0197] like Figure 2 As shown, the void 6 is formed in the entire thickness direction of the sintered layer 43a. However, it is more preferable that the void 6 is formed at least in a portion close to the metal layer 41a.

[0198] <Filling of plating material>

[0199] The plating film 44a is formed outside the sintered layer 43a. Therefore, the plating material exists in at least a part of the gap 6. This is because the plating material enters the gap 6 when the plating film 44a is formed.

[0200] <1 / 2LT section and side LT section>

[0201] As mentioned earlier, Figure 2 The LT cross section shown is the LT cross section at the center position in the width direction W of the multilayer ceramic capacitor 1. That is, Figure 2 The LT section shown is a 1 / 2 LT section.

[0202] In the multilayer ceramic capacitor 1 of the present embodiment, the LT cross section at a position close to the side surface in the width direction W is identical to the LT cross section at a center position in the width direction W, that is, the 1 / 2 LT cross section.

[0203] The LT cross section at a position close to the side surface in the width direction W refers to, for example, Figure 1 The II-II line section. This section is, for example, the LT section at the position of the end surface on the first side surface S1 side of the internal electrode 8. Figure 3 The LT section at line II is shown. This section is referred to as the side end LT section.

[0204] In this embodiment, there is no significant difference between the 1 / 2LT cross section and the side end LT cross section. Figure 3 LT section at line I and Figure 3 There is no big difference in the LT profile at line II.

[0205] In the multilayer ceramic capacitor 1 of the present embodiment, although not shown in the drawings, there is no significant difference in the arrangement of the external electrodes 4 or the like in the LW cross-sections at different positions in the thickness direction T.

[0206] This means that the thickness of the external electrode 4, especially the sintered layer 43a, does not vary greatly within the plane.

[0207] Therefore, in the multilayer ceramic capacitor 1 of the present embodiment, as Figure 4 As shown in the WT cross section, it is easy to expose the entire periphery of the metal layer 41a from the sintered layer 43a.

[0208] When the thickness of the sintered layer 43a varies greatly within the plane, a portion of the sintered layer 43a is likely to be disposed beyond the outer edge of the metal layer 41a. This makes it difficult to expose the entire periphery of the metal layer 41a from the sintered layer 43a.

[0209] <Effect>

[0210] The multilayer ceramic capacitor 1 of the present embodiment can suppress the occurrence of cracks in the external electrodes 4. Furthermore, the multilayer ceramic capacitor 1 of the present embodiment is a multilayer ceramic capacitor 1 having improved moisture resistance reliability.

[0211] <Conventional Multilayer Ceramic Capacitors>

[0212] In the past, in a laminated ceramic capacitor having a metal layer disposed on the external electrode, cracks sometimes occurred in the metal layer. As a cause of cracks in the metal layer, stress applied from other components can be cited. As the other component, there is a sintered layer. The sintered layer is a layer disposed in contact with the metal layer.

[0213] Due to changes in ambient temperature or humidity, stress may be generated in the sintered layer. This stress is applied to the metal layer, causing cracks in the metal layer.

[0214] When cracks are generated in the metal layer, the function of the metal layer to suppress water intrusion is destroyed.

[0215] In addition, the suppression of moisture intrusion is not easily replaced by other layers such as the sintered layer because the film density of other layers is inferior to that of the metal layer.

[0216] Therefore, it is desired to suppress the occurrence of cracks.

[0217] <Thickness of Metal Layer>

[0218] In the multilayer ceramic capacitor 1 of the present embodiment, the thickness of the metal layer 41 a is 0.1 μm or more and 15.0 μm or less. Also, the thickness of the sintered layer 43 a is 0.1 μm or more and 1.0 μm or less.

[0219] In the multilayer ceramic capacitor 1 of the present embodiment, the thickness of the sintered layer 43 a is thin.

[0220] By reducing the thickness of the sintered layer 43a, the stress of the sintered layer 43a can be reduced. As a result, the occurrence of cracks in the metal layer 41a can be suppressed.

[0221] Furthermore, by making the thickness of the sintered layer 43a less than 1.0 μm, the continuity of the sintered layer 43a can be reduced. If the continuity is reduced, the bonding in the surface direction of the sintered layer 43a is weakened. If the bonding is weakened, the stress of the sintered layer 43a is reduced.

[0222] As a result, it is possible to suppress the occurrence of cracks in the metal layer 41 a.

[0223] Furthermore, by setting the thickness of the sintered layer 43a to 1.0 μm or less, the thickness of the external electrode 4 can be reduced. As a result, the outer dimensions of the multilayer ceramic capacitor 1 can be reduced.

[0224] In the multilayer ceramic capacitor 1 of the present embodiment, the area of ​​the portion including metal on the surface of the sintered layer 43a on the plated film 44a side is 10 times larger than the area of ​​the portion including glass.

[0225] Thereby, the plating adhesion of the plating film 44a to the sintered layer 43a can be ensured.

[0226] The plating adhesion refers to the ease of plating adhesion including, for example, the adhesion of the plating film 44a to the sintered layer 43a, the adhesion between the sintered layer 43a and the plating film 44a, and the like.

[0227] <Voids in the Burnt Layer>

[0228] In the multilayer ceramic capacitor 1 of the present embodiment, the sintered layer 43a has the voids 6. Since the sintered layer 43a has the voids 6, the stress of the sintered layer 43a can be reduced. As a result, the occurrence of cracks in the metal layer 41a can be suppressed.

[0229] <Exposure of Metal Layer>

[0230] In the multilayer ceramic capacitor 1 of the present embodiment, at least a portion of the metal layer 41 a is exposed from the sintered layer 43 a .

[0231] Specifically, when the metal layer 41a is viewed from the longitudinal direction L, the sintered layer 43a is not disposed around the metal layer 41a. As a result, the vicinity of the outer edge of the metal layer 41a is exposed from the sintered layer 43a over the entire periphery of the outer edge.

[0232] In the multilayer ceramic capacitor 1 of the present embodiment, at least a portion of the metal layer 41 a is exposed from the sintered layer 43 a , so that the occurrence of cracks in the metal layer 41 a can be further suppressed.

[0233] Since the metal layer 41a is exposed from the sintered layer 43a, the stress received by the exposed portion of the metal layer 41a from the sintered layer 43a is weakened. Therefore, it is possible to suppress the occurrence of cracks in the metal layer 41a.

[0234] In addition, the exposed portion of the metal layer 41a is the portion where the sintered layer 43a is interrupted. Since there is an interrupted portion in the sintered layer 43a, the bonding in the surface direction of the sintered layer 43a becomes weaker. As a result, the stress of the sintered layer 43a is reduced. As a result, it is possible to suppress the generation of cracks in the metal layer 41a.

[0235] <Method for Manufacturing Multilayer Ceramic Capacitor>

[0236] An overview of a general method for manufacturing the multilayer ceramic capacitor 1 will be described.

[0237] (1) Ceramic green sheets for dielectric layer 7 and conductive paste for internal electrode 8 are prepared.

[0238] (2) Forming an internal electrode pattern on a ceramic green sheet. The pattern can be formed by printing a conductive paste in a predetermined pattern on the ceramic green sheet. This printing can be performed by, for example, screen printing, gravure printing, or the like.

[0239] (3) Stacking a plurality of ceramic green sheets for outer dielectric layers on which no internal electrode pattern is formed. Stacking ceramic green sheets on which internal electrode patterns are printed in sequence. Stacking a plurality of ceramic green sheets for outer dielectric layers on top. In this way, a laminated sheet is produced.

[0240] (4) The laminated sheets are pressed in the thickness direction by isostatic pressing or the like. Thus, a laminated block is produced.

[0241] (5) Cut the laminated block into a given size. Thus, laminated chips are cut out.

[0242] (6) The corners and ridges of the stacked small pieces are rounded by barrel grinding or the like.

[0243] (7) The stacked small pieces are fired to obtain a fired stacked body.

[0244] (8) A metal layer is formed on the end surface of the fired laminate. Specifically, the metal layer is formed on the end surface so as to cover the internal electrode led out to the end surface of the laminate. The metal layer can be formed by plating, for example.

[0245] Plating can be performed by electrolytic plating or electroless plating. As a plating process, for example, barrel plating can be used.

[0246] (9) A conductive paste for a sintered layer is applied onto the metal layer.

[0247] (10) The conductive paste is dried and then sintered.

[0248] Thus, sintered layers 43a and 43b are formed. In addition, glass contained in the conductive paste for sintered layers 43a and 43b moves to the surface of dielectric layer 7. The moved glass moves to the surface of dielectric layer 7. The moved glass becomes glass films 42a and 42b.

[0249] (11) Forming a plated film on the sintered layers 43a and 43b. Specifically, first, Ni plating is performed so as to cover the sintered layers 43a and 43b. Thus, a lower plated film is formed. Sn plating is performed thereon. Thus, an upper plated film is formed.

[0250] <Characteristics of the manufacturing method>

[0251] The multilayer ceramic capacitor 1 of the present embodiment has the following features in the manufacturing method in addition to the above-described general multilayer ceramic capacitor manufacturing method.

[0252] The thickness of the sintered layer 43a of the multilayer ceramic capacitor 1 of this embodiment is thin. Therefore, when the conductive paste for the sintered layer 43a is applied on the metal layer 41a, the application amount is strictly adjusted. Thus, the sintered layer 43a having a thickness of 1.0 μm or less is formed.

[0253] The sintered layer 43 a of the multilayer ceramic capacitor 1 of the present embodiment has voids 6 .

[0254] In order to form the voids 6, the sintering temperature and sintering time are optimized. Specifically, the sintering is performed at a temperature of 600°C or more and 750°C or less for a period of 5 minutes or more and 15 minutes or less. The temperature is more preferably 650°C or more and 700°C or less. In addition, the time is more preferably less than 15 minutes. In addition, the sintering can be performed in an inert gas atmosphere such as nitrogen.

[0255] By such firing, the voids 6 can be formed in the sintered layer 43 a .

[0256] However, the glass film 42a is not formed in the above-mentioned firing.

[0257] As described above, the glass film 42 a is formed by the glass contained in the conductive paste for forming the sintered layer 43 a moving to the exposed portion of the dielectric layer 7 .

[0258] In the above-mentioned firing, since the glass does not move sufficiently, the glass film 42 a is not formed.

[0259] Therefore, in addition to the above-mentioned firing, firing in an air atmosphere is performed.

[0260] This sintering can be performed at 700° C. for 5 minutes in an air atmosphere, for example.

[0261] The sintered layer 43 a can be formed by the sintering in the air atmosphere.

[0262] By firing in the air atmosphere, the metal particles such as Cu contained in the sintered layer 43a are oxidized. Moreover, the glass wets and spreads on the surface of the oxidized metal particles. Thus, the movement of the glass is promoted. Moreover, the glass further wets and spreads on the surface of the dielectric layer 7 formed of BaTiO3 or the like as an oxide, thereby forming a glass film 42a.

[0263] Furthermore, in the multilayer ceramic capacitor 1 of the present embodiment, the thickness of the sintered layer 43a is 1.0 μm or less. Therefore, the continuity of the sintered layer 43a is easily suppressed. If the continuity is suppressed, the effect of squeezing the glass toward the surface of the dielectric layer 7 by the necking of the metal particles such as Cu contained in the sintered layer 43a is suppressed. That is, the formation of the glass film 42a becomes more difficult.

[0264] Therefore, it is more effective to simultaneously use the above-mentioned firing in the air atmosphere to promote the movement of the glass.

[0265] <Method for measuring length>

[0266] The length of each portion of the multilayer ceramic capacitor 1 can be measured by observing the cross section of the multilayer body exposed by grinding with a scanning electron microscope, for example. Each value can be an average value of measured values ​​at a plurality of locations corresponding to the locations to be measured.

[0267] <Moisture Resistance Reliability Test>

[0268] As a durability test, a moisture resistance reliability test was conducted. The samples, test conditions, etc. are as follows.

[0269] (Sample)

[0270] Length in the longitudinal direction L: 0.6 mm

[0271] Length in width direction W: 0.3mm

[0272] Length in thickness direction T: 0.3mm

[0273] Capacitance: 2.2μF

[0274] Thickness of inner dielectric layer 7b: 0.65 μm

[0275] Thickness of internal electrode 8: 0.43 μm

[0276] Number of internal electrodes 8: 280

[0277] Thickness of metal layers 41a, 141b: 5 μm

[0278] (Moisture resistance reliability test)

[0279] Temperature, humidity: 85℃, 85%RH

[0280] Voltage: 6.3V

[0281] Voltage application time: 120 hours

[0282] Judgment criteria: Based on the logarithmic value (log IR) of the insulation resistance (IR) immediately after the start of the moisture resistance reliability test, samples that are lower by two or more digits are judged to have IR deterioration.

[0283] A moisture resistance reliability test was performed using 72 samples according to the embodiment of the present invention and 72 conventional samples.

[0284] The sample of the embodiment has a sintered layer 43a with a thickness of 0.5 μm. On the other hand, the conventional sample has a sintered layer 43a with a thickness of 3.0 μm.

[0285] The results of the moisture resistance reliability test are as follows.

[0286] Among the samples of the embodiment, IR degradation was not observed in all 72 samples.

[0287] On the other hand, among the conventional samples, IR degradation was observed in 3 out of 72 samples.

[0288] In conventional samples, cracks may have occurred in the metal layer during the moisture resistance reliability test, resulting in IR degradation.

[0289] On the other hand, in the sample of the embodiment, it is considered that cracks did not occur in the metal layer in the moisture resistance reliability test, and as a result, IR degradation did not occur.

[0290] The above test results show that the multilayer ceramic capacitor of the present embodiment can suppress the occurrence of cracks in the external electrodes and has improved moisture-resistant reliability.

[0291] In addition, the description so far is mainly based on the first external electrode 4a. As mentioned above, the description of the first external electrode 4a is also appropriate for the second external electrode 4b. This is because the first external electrode 4a and the second external electrode 4b are the same only in that the surface on which they are provided is different.

[0292] Furthermore, although the embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various changes and modifications can be made.

[0293] <1> A multilayer ceramic capacitor, characterized by comprising:

[0294] A laminated body in which a plurality of dielectric layers and internal electrodes are alternately laminated; and

[0295] a pair of external electrodes provided on the surface of the stack and electrically connected to the internal electrodes led out to the surface of the stack;

[0296] The laminated body has:

[0297] The first main surface and the second main surface are opposite to each other in the thickness direction which is the lamination direction of the dielectric layer and the internal electrode;

[0298] The first end surface and the second end surface are opposed to each other in a longitudinal direction which is a direction in which the pair of external electrodes are opposed to each other, and the external electrodes are provided thereon; and

[0299] The first side surface and the second side surface are opposite to each other in a width direction perpendicular to the thickness direction and the length direction.

[0300] The external electrode comprises:

[0301] a metal layer disposed on the first end surface and the second end surface so as to cover the internal electrode led out to the first end surface and the internal electrode led out to the second end surface;

[0302] A glass film is disposed on the first end surface and the second end surface and is adjacent to the metal layer and disposed around the metal layer;

[0303] a sintered layer comprising glass and metal and configured to cover the metal layer; and

[0304] a coating film configured to cover the sintered layer,

[0305] The thickness of the metal layer is greater than or equal to 0.1 μm and less than or equal to 15.0 μm.

[0306] The thickness of the sintered layer is greater than or equal to 0.1 μm and less than or equal to 1.0 μm.

[0307] <2> according to <1> The multilayer ceramic capacitor is characterized in that:

[0308] The sintered layer has voids,

[0309] A plating material exists in at least a portion of the void.

[0310] <3> according to <1> or <2> The multilayer ceramic capacitor is characterized in that:

[0311] On the surface of the sintered layer on the plated film side, the area of ​​a portion including metal is 10 times larger than the area of ​​a portion including glass.

[0312] <4> according to <1> to <3> The multilayer ceramic capacitor according to any one of the preceding claims is characterized in that:

[0313] A glass film is disposed around the metal layer and in contact with an end portion of the metal layer.

[0314] Description of Reference Numerals

[0315] 1 Multilayer Ceramic Capacitors

[0316] 2 Laminated body

[0317] 4a 1st external electrode

[0318] 4b Second external electrode

[0319] 4Ma, 4Mb Main surface external electrode

[0320] 4Ea, 4Eb End surface external electrode

[0321] 4Sa, 4Sb Side external electrodes

[0322] 41a, 41b metal layer

[0323] 42a, 42b Glass film

[0324] 43a, 43b Sintered layer

[0325] 44a, 44b coating film

[0326] 5 End of the metal layer

[0327] 6. Voids in the burnt layer

[0328] 7a Outer dielectric layer

[0329] 7b Inner dielectric layer

[0330] 8a 1st internal electrode

[0331] 8b Second internal electrode

[0332] M1 1st main surface

[0333] M2 Second main surface

[0334] E1 1st end face

[0335] E2 2nd end face

[0336] S1 Side 1

[0337] S2 Side 2

[0338] L Length direction

[0339] T thickness direction

[0340] W Width direction.

Claims

1. A laminated ceramic capacitor, characterized in that: have: A laminated body in which a plurality of dielectric layers and internal electrodes are alternately laminated; and a pair of external electrodes, provided on the surface of the stacked body and electrically connected to the internal electrodes led out to the surface of the stacked body; The laminated body has: The first main surface and the second main surface are opposite to each other in the thickness direction which is the lamination direction of the dielectric layer and the internal electrode; The first end surface and the second end surface are opposed to each other in a length direction which is a direction in which the pair of external electrodes are opposed to each other, and the external electrodes are provided thereon; and The first side surface and the second side surface are opposite to each other in a width direction perpendicular to the thickness direction and the length direction. The external electrode comprises: a metal layer, arranged on the first end surface and the second end surface so as to cover the internal electrode led out to the first end surface and the internal electrode led out to the second end surface; A glass film is disposed on the first end surface and the second end surface and is adjacent to the metal layer and disposed around the metal layer; a sintered layer comprising glass and metal and configured to cover the metal layer; as well as a coating film configured to cover the sintered layer, The thickness of the metal layer is greater than or equal to 0.1 μm and less than or equal to 15.0 μm. The thickness of the sintered layer is greater than or equal to 0.1 μm and less than or equal to 1.0 μm.

2. The multilayer ceramic capacitor according to claim 1, wherein: The sintered layer has voids, A plating material exists in at least a portion of the void.

3. The multilayer ceramic capacitor according to claim 1 or 2, wherein: On the surface of the sintered layer on the plated film side, the area of ​​a portion including metal is 10 times larger than the area of ​​a portion including glass.