Multilayer system consisting of thin layers for temporary bonding
By optimizing the layer thickness and structure of the multi-layer system, using the interference effect to improve laser absorption, the problems of substrate damage and polymer bonding agent transparency during laser debonding are solved, and damage-free substrate bonding and debonding are achieved, simplifying the The process flow is completed.
Patent Information
- Application Number
- CN202280094391.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-03
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the substrate is prone to damage during laser debonding, and the polymer-based bonding agent is opaque in the ultraviolet region, resulting in the need for additional layers for protection and bonding, and the silicon carrier substrate is opaque in the UV region, Limits the effect of laser de-engaging.
By optimizing the layer thickness and structure of the multi-layer system, the interference effect is used to improve the absorption degree of laser light at a specific wavelength, and the jointing and de-joining of no additional layers are required. The multi-layer system is used as the intermediate layer of the substrate stack, and laser radiation is used to make it impossible to avoid any additional layers. Damaged separation.
It is possible to efficiently bond and debond the substrate without the need for additional protective layer and adhesive, reducing material use and processing damage, and improving the efficiency and stability of laser debond.
Smart Images

Figure CN118946961A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for providing a multilayer system, a substrate stack and a method for bonding and debonding a multilayer system. Background Art
[0002] In the prior art, various methods are known for loosening or disjoining two temporarily joined substrates. The substrates are in particular a product substrate and a carrier substrate, wherein the carrier substrate enables handling, further processing and transport of the product substrate. After processing, the carrier substrate is separated from the product substrate.
[0003] The use of bonding agents is very extensive, so that two substrates can be temporarily and relatively easily releasably bonded. Such temporary adhesive layers are used in particular as intermediate layers in substrate stacks. Bonding agents are usually polymers, in particular thermoplastics. The debonding of the two substrates is carried out, for example, by a shearing process at elevated temperatures. Debonding can also be carried out by additional mechanical action or chemical treatment of the bonding agent.
[0004] One of the newest and most important methods for separating substrate stacks is laser debonding. In the case of laser debonding, the laser light is coupled in on the substrate side through a substrate that is as transparent as possible and is absorbed by the adjacent coating (release layer) on the back side. The laser light is preferably coupled in through a largely transparent carrier substrate. The transparency of the carrier substrate for certain electromagnetic radiation allows the photons to reach the release layer unhindered to the greatest extent possible.
[0005] A method for separating two substrates from each other consists in using a special release layer in combination with a bonding agent and applying it to a carrier substrate, which is in particular transparent. The transparency of the carrier substrate for certain electromagnetic radiation allows the photons to reach the release layer without hindrance. The release layer is accordingly changed by the photons and reduces the adhesion to the bonding agent. The publication US 10,468,286 B2 describes such a method. Depending on where the bonding agent is applied - whether directly on the carrier substrate or after the release layer, the bonding agent must also be substantially transparent to the selected electromagnetic radiation.
[0006] In the case of laser bonding, polymers, especially those based on polyimide, can be used as release layers, because the release layers can be selectively removed with an ultraviolet laser beam source. Separation occurs at the carrier substrate-bonding agent interface. The ultraviolet laser beam source used for this purpose requires a carrier substrate made of glass, which has the necessary transparency for specific electromagnetic radiation in the ultraviolet region. US9,827,740B2 shows a system consisting of a bonding agent and a release layer made of polyimide, which is directly applied to a carrier substrate made of glass. In US10,703,945B2, the bonding agent contains a light-absorbing material, so only the polymer layer is used for simultaneous connection and release.
[0007] The release layer can also be a metal layer in particular. In WO 2011 / 159456 A2, for example, an adhesive layer with a metal layer is used for laser debonding. Due to the strong absorption of laser radiation by the metal coating, separation of the product substrate and the carrier substrate is possible. However, in WO 2011 / 159456 A2, the connection of the two substrates is not possible without a bonding agent. Publication US 9,269,561 B2 also shows a release layer consisting of a metal coating and a bonding agent between a silicon carrier substrate and a product substrate.
[0008] Publication US10,112,377B2 discloses different materials, they can be used for the release layer of laser debonding, and are made up of a single layer.Here, except the release layer, also need a bonding agent to temporarily connect substrates.
[0009] The use of polymer adhesives has the disadvantage that the surface needs to be cleaned after UV laser debonding to remove adhesive residues. In addition, the demand for 3D stacking and CMOS-compatible processes leads to the need for high-quality silicon carrier substrates, which are not transparent in the UV region. In addition, polymer-based adhesives are not heat-resistant at higher temperatures.
[0010] If a metal layer is applied to the product substrate and / or the carrier substrate and used as a bonding layer, then in the prior art, additional layers are first required in order to enable a careful and essentially non-destructive laser debonding, since the surface of the coating is destructively removed. The at least one additional layer serves as protection for the product substrate and is in particular an antireflection coating (AR coating). Other protective layers are, for example, relaxation layers. In WO 2015 / 014265 A1, in addition to a metal layer used as a release layer, such AR coatings and relaxation layers are also disclosed.
[0011] One problem in the prior art is that damage to the substrate, in particular to expensive functional components of the substrate, may occur due to exposure to the laser beam. Therefore, in addition to the release layer, further layers are required, in particular polymer-based adhesive layers. In addition, the bonding agents for laser debonding that are curable in the UV region are not compatible with carrier substrates made of silicon. Therefore, additional layers are necessary in the prior art and serve to protect the substrate and / or to connect the substrate as an adhesive layer.
[0012] Many products in the semiconductor industry, such as electronic and optoelectronic components, consist partly of layer sequences of different materials. Many multilayer systems are used in the bonding process, but are also required for many production processes where bonding and debonding take place. Especially in laser debonding, only lasers with specific wavelengths work effectively. Summary of the invention
[0013] The object of the present invention is therefore to at least partially eliminate, in particular completely eliminate, the disadvantages listed in the prior art. In particular, the object of the present invention is to specify an improved method for providing and using a multilayer system for joining and de-joining.
[0014] This object is achieved with the features of the parallel independent claims. Advantageous developments of the invention are described in the dependent claims. All combinations of at least two features described in the specification, the claims and / or the drawings also fall within the scope of the invention. In the case of specified value ranges, the values within the ranges are also to be considered disclosed as limit values and can be claimed in any combination.
[0015] The invention therefore relates to a method for providing a multilayer system consisting of at least two layers, in particular for temporarily joining substrates to form a substrate stack, the method having the following steps in the following order:
[0016] i) Provide a multi-layer system,
[0017] ii) determine the degree of absorption of laser radiation of a specific wavelength by the multilayer system,
[0018] iii) changing at least one parameter of the multilayer system,
[0019] iv) determining the degree of absorption of laser radiation of a specific wavelength by a multilayer system having at least one parameter varied according to step iii),
[0020] v) Repeating steps i) to iv) until the absorption level is maximum, wherein in step i) a multilayer system having a maximum absorption level is provided in each case.
[0021] The multilayer system consists of at least two layers. The layers preferably have a uniform layer thickness and are arranged flat on top of one another, wherein the layers can also be applied in a structured manner instead of flat. In this case, the same material is located in the layers of the multilayer system. The layers are so-called thin films, particularly preferably with a layer thickness in the nanometer range. In this case, it is advantageously possible to use multilayer systems that are known in terms of the structure and arrangement of the layers.
[0022] The provision in step i) also includes the provision of material data of the multilayer system, so that during the determination a computer-aided calculation or simulation can also be performed for the corresponding parameters. In other words, the parameters of the multilayer system with regard to the degree of absorption are determined in different combinations, and the maximum parameter is selected in each case. In the repetition, a technically suitable value is selected for the parameter in the case of a new change or adaptation of the multilayer system. The wavelength of the laser radiation, based on which the corresponding degree of absorption or degree of absorption comparison is performed, is kept constant.
[0023] Parameters may be, for example, the sequence or structure of the layers of the multilayer system and the layer thicknesses. When determining the degree of absorption, the degree of absorption for the respective case may be measured or calculated. Preferably, the simulation of the multilayer system is performed with respect to the respective parameters.
[0024] While searching for solutions to the disadvantages described in the prior art, it was surprisingly found that, given certain parameters, the respectively provided multilayer systems can be significantly improved in their absorption behavior, especially in the case of established multilayer systems. In this way, the multilayer systems or material combinations can be used in other fields of application. In addition, thinner layers can be used for debonding and multilayer systems can be used without additional polymer adhesive / bonding layers and without antireflection layers for bonding and simultaneous debonding. In addition, due to the greater degree of absorption, the energy input and therefore the heat input in the substrate arranged behind the multilayer system is minimized. Advantageously, therefore, damage during laser debonding can be prevented.
[0025] In a preferred embodiment of the method for providing a multilayer system, it is provided that at least one parameter of the multilayer system is the layer thickness of a layer of the multilayer system. In other words, the layer thickness of a specific layer of the multilayer system is changed, i.e. increased or reduced, in order to achieve the greatest possible absorption. It was surprisingly found that a greater degree of absorption can be achieved by changing the layer thickness in a multilayer system consisting of thin layers by interference effects. Thus, by means of this method, the degree of absorption can advantageously be significantly increased by changing the thickness of the layer. In this case, other unnoticed influences associated with the absorption behavior remain undetected by the systematic change. Thus, advantageously, a layer structure for the multilayer system, in particular interference-optimized, is determined by means of this method. Here, the wavelength of the laser radiation, for which the degree of absorption should be greatest, remains unchanged.
[0026] In laser debonding, one is limited to laser radiation of specific wavelengths, since only these can be efficiently generated. In this regard, it has therefore also surprisingly been found that, for specific wavelengths, a greater degree of absorption can be achieved by varying the layer thickness. By systematically varying the layer thickness of the individual layers of the coating in the multilayer system, a greater absorption can surprisingly be achieved, whereby the multilayer system can be used not only as a bonding layer but also simultaneously as a release layer in laser debonding.
[0027] The provision of the multilayer system can advantageously be carried out without changing or replacing the material, and thus enables existing systems (i.e. coatings or multilayer systems known to those skilled in the art in the semiconductor industry) to be used. Existing multilayer systems or materials can also be partially changed in terms of the arrangement of the materials. However, in particular, the layer thickness is adjusted with respect to the absorption behavior, in particular the absorptivity and reflectivity of the entire multilayer system, because it has been surprisingly found that the same or greater degree of absorption can be achieved with the same or smaller total thickness of the multilayer system. In this way, a multilayer system with optimized layer thickness can advantageously be used not only for bonding, but also for debonding. Here, the energy input into other materials can advantageously be kept small. In addition, material can be saved and the thickness of the multilayer system can be reduced. The multilayer system can also advantageously be used as a debonding layer by irradiating with laser radiation of a specific wavelength to specifically reduce the holding force of the multilayer system of the substrate stack to be debonded.
[0028] In a preferred embodiment of the method for providing a multilayer system, it is provided that at least one parameter of the multilayer system is the layer thickness of another layer of the multilayer system. Thus, in addition to the layer thickness of one layer, the layer thickness of another layer of the multilayer system is also varied simultaneously. Advantageously, therefore, by varying the thickness, it is possible to efficiently and quickly provide a multilayer system which has the greatest possible degree of absorption with respect to the laser radiation of a specific wavelength and the layer structure. If the multilayer system has three layers, preferably one layer thickness is kept constant and the simulation or test series of two adjacent layers are determined.
[0029] In a preferred embodiment of the method for providing a multilayer system, it is provided that the wavelength in the determination in steps ii) and iv) is between 1100 nm and 10,000 nm, preferably between 1100 nm and 5000 nm, more preferably between 1500 nm and 2500 nm. In studies of multilayer systems, it has also been found that for laser debonding of multilayer systems consisting of thin, in particular polymer-free layers, the absorption behavior can be influenced in particular in a specific wavelength range by varying the parameters. The laser debonding of the multilayer system according to the invention is preferably carried out in the infrared range.
[0030] Furthermore, the invention relates to a substrate stack having at least one multilayer system provided according to a method for providing a multilayer system, the multilayer system having at least two layers consisting of different materials. The multilayer system is preferably configured as an intermediate layer and connects two substrates to form a substrate stack. The multilayer system has a layer structure with optimized layer thickness, wherein the layer thickness is selected so that the multilayer system has a maximum degree of absorption for a specific wavelength, wherein the layers can be kept as thin as possible at the same time. The multilayer system is thus optimally adapted to the highest possible absorption of electromagnetic radiation of a specific wavelength in terms of layer thickness or another parameter. The multilayer system can therefore advantageously be used as a bonding layer and a debonding layer in a substrate stack.
[0031] Thus, the substrate stack can be separated damage-free, effectively and simply by means of laser radiation or in particular the product substrate is detachable. The multilayer system is advantageously produced on a substrate and then connected to another substrate, so that the multilayer system can be used as a bonding layer and simultaneously as a debonding layer.
[0032] In a preferred embodiment of the substrate stack, it is provided that the total thickness of the multilayer system is between 1 nm and 10 μm, more preferably between 5 nm and 2 μm, most preferably between 10 nm and 1 μm, most preferably between 10 nm and 500 nm. In this way, the substrate stack is stable and small. Furthermore, debonding along the multilayer system or in regions of the multilayer system can advantageously be carried out easily and efficiently.
[0033] In a preferred embodiment of the substrate stack, it is provided that the respective layers of the multilayer system each have a layer thickness of between 1 nm and 1 μm, preferably between 1 nm and 500 nm, more preferably between 1 nm and 250 nm. It has surprisingly been found that even for very thin layers, a high degree of absorption can be achieved by optimizing the layer thickness. Thus, in the multilayer system, interference can be generated particularly well for thin layers with a layer thickness in the subwavelength range with respect to the laser radiation. In particular, a highly constructive interference of the laser radiation in the multilayer system can advantageously be achieved by the combination of layer thicknesses.
[0034] In a preferred embodiment of the substrate stack, it is provided that the multilayer system has at least one layer with a layer thickness of between 10 nm and 100 nm, preferably between 20 nm and 100 nm, more preferably between 25 nm and 75 nm, most preferably between 35 nm and 65 nm. In the course of developing a method for providing a multilayer system and a substrate stack having a multilayer system, it has been found that a particularly high increase in the degree of absorption can be achieved if at least one layer has a corresponding layer thickness.
[0035] In a preferred embodiment of the substrate stack, it is provided that at least one layer of the multilayer system comprises, preferably consists of, titanium (Ti), aluminum (Al), aluminum nitride (AlN), tantalum nitride (TaN), germanium (Ge), (tin)TiN or copper (Cu). In this case, the layer thickness is particularly preferably between 25 and 75 nm.
[0036] In a preferred embodiment of the substrate stack, it is provided that at least one layer of the multilayer system consists of amorphous silicon dioxide (SiO2). The layer thickness of this layer of the multilayer system is preferably greater than the other layers or the other layer. The layer thickness is preferably greater than 100 nm, more preferably greater than 200 nm.
[0037] In a preferred embodiment of the substrate stack, it is provided that the substrate stack has at least a carrier substrate and a product substrate, wherein the carrier substrate is connected to the product substrate via a multilayer system. The multilayer system is thus arranged as an intermediate layer and simultaneously as a bonding layer between the carrier substrate and the product substrate. In this way, the substrate stack can be debonded particularly quickly and efficiently.
[0038] In a preferred embodiment of the substrate stack, it is provided that the multilayer system, preferably the substrate stack, does not have any polymer-based binders. In other words, due to the high degree of absorption of the multilayer system, additional bonding layers or auxiliary layers can be omitted. The substrate stack is particularly preferably free of polymer-based materials, so that the substrate stack can be processed at particularly high temperatures. In addition, an adhesive layer and therefore a subsequent and laborious residue removal can be omitted.
[0039] In a preferred embodiment of the substrate stack, it is provided that the multilayer system, preferably the substrate stack, does not comprise an antireflection layer. Due to the high degree of absorption of an optimally designed multilayer system, an antireflection layer which is usually arranged on the side of the multilayer system facing away from the laser beam or on the side of the intermediate layer where the bonding layer is arranged during laser debonding can be omitted. Furthermore, even without an antireflection layer, damage can advantageously be prevented by the multilayer system.
[0040] In a preferred embodiment of the substrate stack, it is provided that at least one substrate arranged on the multilayer system, in particular a carrier substrate, consists of silicon. In this way, the multilayer system can advantageously be irradiated through the substrate with laser radiation having a wavelength greater than 1300 nm. Laser debonding can therefore advantageously be performed from the back side of the substrate stack.
[0041] In a preferred embodiment of the substrate stack, it is provided that the degree of absorption of the multilayer system with respect to laser radiation of a specific wavelength is greater than 0.5, preferably greater than 0.65, more preferably greater than 0.75, even more preferably greater than 0.85, most preferably greater than 0.9. In this way, it can be ensured that a further substrate, in particular a product substrate, which is arranged downstream of the multilayer system is prevented from being damaged during debonding of the substrate stack.
[0042] In a preferred embodiment of the substrate stack, it is provided that the multilayer system has exactly three layers, two of which consist of the same material and are separated from one another by the remaining layer. The layers adjacent to the substrate in the multilayer system are therefore made of the same material and preferably include a smaller layer, which is preferably a metal layer.
[0043] In a preferred embodiment of the substrate stack, it is provided that the substrate stack can be debonded by irradiating the multilayer system with laser radiation of a specific wavelength.
[0044] Furthermore, the invention relates to a method for bonding substrates to form a substrate stack according to the invention, having the following steps,
[0045] 1) providing a first substrate, in particular a carrier substrate,
[0046] 2) Joining a second substrate, in particular a product substrate, to the first substrate.
[0047] The substrate provided in step 1) serves in particular as a bonding layer. Bonding can be carried out particularly easily and effectively with multilayer systems.
[0048] The layers of the multilayer system can be arranged on the first substrate and / or on the second substrate.
[0049] Furthermore, the invention relates to a method for debonding a substrate stack, having the following steps,
[0050] a) providing a substrate stack according to at least one of claims 5 to 13,
[0051] b) irradiating the multilayer system with laser radiation of a specific wavelength through at least one substrate of the substrate stack, and then
[0052] c) Separation of the substrate stack in the region of the multilayer system.
[0053] Debonding or laser debonding can be performed particularly easily, reliably and quickly with a substrate stack or a substrate stack with a thickness-optimized multilayer system.
[0054] Since the arrangement of the layers is usually predetermined for process or intended use reasons and by the respective substrate used, the optimization of the layer thickness with respect to the degree of absorption is an unexpected and extremely useful effect. This is especially so because it offers a previously unrecognized possibility for adjusting the absorption behavior of thin layers for laser bonding. In this case, the order of the materials in the multilayer system is usually retained for purpose reasons.
[0055] In an exemplary embodiment of a method for providing a multilayer system, an optimization of the layer thickness is first performed for each individual layer L1 to Ln of a given multilayer system, the given multilayer system consisting of layers L1 to Ln, preferably having three layers (L1 to L3), particularly preferably having two layers (L1, L2), wherein the absorption of the entire multilayer system is determined numerically and also measured experimentally.
[0056] Parameters such as the carrier substrate (preferably Si), the wavelength (preferably in the IR range suitable for Si carrier substrates) and the laser incidence angle (e.g. 0° in the main beam, i.e. perpendicular to the surface) are constant. With a constant laser wavelength, the layer thickness can be varied simultaneously in the simulation. Thus, the thickness distribution of the multilayer system with the maximum absorption is determined in the simulation. In the test, the substrate stack with the multilayer system is tested with respect to the residual bond strength, ablation form, homogeneity and stability of production and processing parameters with a defined layer thickness.
[0057] In a preferred embodiment of the method, it is also provided that in the arrangement of the materials the material layers of the multilayer system are first determined and then their layer thicknesses are optimized in such a way that maximum light absorption is achieved and reflection losses are minimized. Thus, the substrate stack produced by bonding and optimized for laser debonding with the multilayer system (in particular as an intermediate layer) can be separated again by laser debonding in a subsequent process step.
[0058] The separation of the substrates is carried out by means of laser irradiation by debonding or delamination along the interface. In a preferred embodiment, the debonding is carried out by laser irradiation through the carrier substrate with light of a selected wavelength, intensity and pulse duration (ΔT in the μs to fs range). The pulses are particularly preferably in the picosecond range.
[0059] The product substrate is released from the carrier substrate in a method for debonding a substrate stack by focusing laser radiation of a specific wavelength through the carrier substrate onto the multilayer system optimized by interference or thickness. As a result, at least one layer of the multilayer system is destroyed or its adhesive properties are significantly reduced by melting, evaporation and / or sublimation and photo- or thermo-chemical conversion of the multilayer temporary bonding layer.
[0060] An important aspect of the method for providing a multilayer system is to determine and provide a multilayer system with the highest possible absorption, preferably at the same or lower total thickness. The absorption of the multilayer system with a layer structure optimized by interference layer thickness distribution is thus as great as possible or close to 1 (100%). Higher absorption can be achieved by adjusting the layer thickness of the individual layers in the multilayer system, which makes it possible to use the existing multilayer system as a bonding layer and at the same time as a release layer during laser debonding.
[0061] The arrangement of the individual layers is generally given by the bonding method and the bonded substrate stack known to the technician in the semiconductor industry. Therefore, the optimization of the multilayer system preferably occurs without changing the materials and enables the use of existing systems. Existing materials are optimized with respect to the absorptivity and reflectivity of the entire multilayer system in terms of layer thickness. For example, if the optimal layer thickness is exceeded or fallen below, the interference changes and the absorption of the multilayer system is therefore reduced. The layer thickness of the individual layers is in the nm range and can therefore interact highly with electromagnetic waves. In addition, a simplified laser debonding can be achieved by the interference-optimized layer structure, because the product substrate does not have to be protected with an additional antireflection coating (AR). Because the multilayer system is used for bonding and laser debonding, no additional bonding agent is preferably required for bonding.
[0062] The layer thicknesses of the individual bonding layers and laser debonding layers depend in particular on the process (CVD, PVD, MBE, surface oxidation, etc.) They are in particular between 10 nm and 500 nm, preferably between 20 nm and 100 nm.
[0063] The optimization of the multilayer system is in particular a pattern optimization, with preferably two optimized parameters. Multidimensional (i.e. more than two parameters) optimization is possible, but less preferred. The layer thickness is determined in the optimization, in particular by simulation. In tests, further criteria of laser debonding, in particular process efficiency and stability as well as residual bonding force, ablation form and homogeneity, are checked with the layer thickness selected from the simulation.
[0064] The layer thickness d of the individual layers of the multilayer system is most easily controlled and varied if the layers, substrate and carrier substrate from a given substrate stack are known. Therefore, the layer thickness d of the individual layers of the multilayer system is mainly changed or varied. In particular, the laser wavelength and the laser angle (English: angle of incidence) remain unchanged. If the multilayer system consists of two layers, the two layer thicknesses d1 and d2 can be varied simultaneously. Here, the multilayer system consists of a plurality of layers L1 to Ln, preferably L1 to L3. The selected parameters, in particular, for example, the two layer thicknesses d1 and d2 are varied, and the degree of absorption in the debonded structure is calculated and represented graphically. The degree of absorption in the debonded structure should be as high as possible. Preferably, a maximum of three layers are used to maximize the absorption. In the represented graph, the area with high absorption must be large enough so as not to be too sensitive to changes. The layer thicknesses d1 and d2 from the area with high absorption are selected for the thicknesses of the layers L1 and L2.
[0065] In this context, a method for providing a multilayer system, a multilayer system and a method for joining and dejoining are particularly advantageous because:
[0066] -For the first time, laser debonding of some bonded layers is possible with optimized multilayer systems,
[0067] - the combination of several very thin layers enables high absorption to be achieved through the interference of the layers of the multilayer system,
[0068] - reduction of the layer thickness (nm region) by optimizing the individual layer thicknesses of the multilayer system, whereby less material has to be applied,
[0069] - in the case of shorter pulses, the available pulse energy is several orders of magnitude smaller (in the J range for high-power lasers compared to μJ for “ultrafast” picosecond and femtosecond lasers), so that the total energy input into the material to be processed is reduced, which leads to smaller thermal damage zones due to the shorter action time and thus less thermal diffusion,
[0070] - Achieving higher efficiency separation by debonding or delamination along the interface by means of laser irradiation with ultrashort laser pulses,
[0071] - No additional layers are needed to protect the product substrate (anti-reflection (AR) layer), and
[0072] -Joint is not necessary.
[0073] The production of substrate stacks with multilayer systems is therefore suitable not only for bonding, but also for laser debonding of substrate stacks. In this case, in particular existing materials of the multilayer bonding layer (multilayer system) are used between the carrier substrate and the product substrate. Subsequently, a transparent carrier substrate is selected for substrate-side irradiation with laser radiation. For example, silicon as a carrier substrate is transparent at wavelengths λ>1300nm or λ>1900nm, so lasers in the near infrared (NIR) and mid-infrared (MIR) are selected here. Therefore, in the present case, silicon is preferred as a carrier substrate, and laser debonding in the infrared region is possible. The carrier substrate (Si) and the laser source with the laser wavelength (selected when used with a Si carrier substrate: for example 1940m, 1960μm or 2030μm) are thereby determined.
[0074] The optimum layer thickness or thicknesses of the individual layers of the multilayer system are then determined, which should not be exceeded or fallen below. The material layers are optimized with regard to their layer thickness, in particular in simulations, in such a way that maximum light absorption (absorptivity) is achieved and reflection losses are minimized. In this case, a plurality of layer thicknesses, preferably two, are varied simultaneously. The substrate stack with the multilayer system optimized with layer thicknesses can then be laser debonded by laser irradiation with a selected wavelength, intensity and pulse duration (ΔT in the μs to ps range). In the region of the multilayer system, complete loosening or separation of the product substrate by debonding or delamination along the interface by means of laser irradiation is carried out.
[0075] An exemplary method for providing a multilayer system, particularly for temporary bonding of substrates, the multilayer system comprising:
[0076] a first layer consisting of a first material having a first layer thickness, and
[0077] a second layer consisting of a second material having a second layer thickness,
[0078] The method comprises at least the following steps in the following order:
[0079] a) determining the degree of absorption of laser radiation of a specific wavelength by the multilayer system for different first layer thicknesses, wherein the second layer thickness is constant,
[0080] b) the thickness of the first layer is chosen so that the absorption of the multilayer system is maximized,
[0081] c) determining the degree of absorption of laser radiation of a specific wavelength by the multilayer system for different second layer thicknesses, wherein the first layer thickness is constant to the first layer thickness selected in step b),
[0082] d) the thickness of the second layer is chosen so that the absorption of the multilayer system is maximized,
[0083] e) Providing a multilayer system having a first layer thickness according to step b) and a second layer thickness according to step d).
[0084] In this regard, the exemplary method describes a way in which the corresponding optimal layer thickness for achieving the highest possible absorption degree of the multilayer system can be determined. It was surprisingly found that the thin layers of the multilayer system have a high absorption degree despite the small layer thickness, because the layer thickness is arranged or configured in an optimal manner for laser debonding. In this regard, the occurrence of interferences, especially in multilayer systems with thin layers having a specific layer thickness distribution, is the cause of the higher absorption degree. For example, if the optimal layer thickness is exceeded or fallen below, the interference changes and the absorption of the multilayer system decreases. The layer thickness of the individual layers is in the nm range and can therefore interact highly with electromagnetic waves. In addition, a simplified laser debonding can be achieved by the interference-optimized layer structure, because the product substrate does not have to be protected with an antireflection coating (AR). Since the multilayer system is used for bonding and laser debonding, preferably no additional bonding agent is required for the bonding.
[0085] Here, the (temporary) bonding layer consists of a multilayer system. The multilayer system is used as a connecting layer and a release layer at the same time during laser debonding. The temporary bonding layer is preferably a plurality of layers for bonding and debonding processes. Here, the materials of the multilayer system are known to those skilled in the art. The temporary bonding layer consists of a plurality of layers, the thickness of which is optimized so that the multilayer system causes maximum absorption of the laser radiation. Improved and simpler laser debonding can be achieved by an interference-optimized layer structure, wherein additional layers for protecting the substrate or bonding the substrate, such as anti-reflection (AR) protective layers and / or relaxation layers and / or bonding agents, are not required. The individual layers can be used, for example, as selective absorption layers or phase shifters.
[0086] In this case, during laser debonding, the product substrate is separated from the carrier substrate by an optimized multilayer system, wherein damage to the product substrate and / or to the carrier substrate is minimized to a large extent or eliminated as far as possible. A prerequisite is, in particular, a strong absorption of the laser light by the multilayer system optimized by interference. Due to the use of ultrashort laser pulses, the heat conduction during the removal is minimized or essentially negligible. The distribution of the absorbed laser energy is determined by the absorption in the multilayer material system, which is triggered by linear and nonlinear processes when the material system is irradiated with ultrashort laser pulses, preferably in the ps range. Due to the high photon density that can be generated when using very short pulses, rapid removal of the material occurs, so that no or only very little heat is input into the remaining adjacent substrate.
[0087] Separation by debonding or delamination along the interface by means of laser irradiation requires maximum radiation absorption by the release layer of the multilayer system by linear and / or nonlinear processes. Debonding occurs primarily thermally, in particular by forming gases, but also partially chemically. The intermediate layer is mostly an absorbing layer and absorbs the energy of the laser radiation. The auxiliary layer(s) react / interact with the absorbing layer.
[0088] The transparency of the carrier substrate to specific electromagnetic radiation allows photons to enter the multilayer system to a large extent without hindrance. Carrier materials are, for example, silicon (Si), glass, sapphire and silicon carbide. Although the use of a carrier substrate made of glass enables the use of ultraviolet lasers, it has many disadvantages, such as poor thermal conductivity and incompatibility with specific semiconductor processes and semiconductor processing equipment. Therefore, a carrier substrate made of silicon (Si) is preferred. Since the Si substrate is opaque to the ultraviolet spectrum, a laser in the infrared (IR) range, preferably in the mid-infrared and near-infrared (MIR and NIR), is used because the carrier wafer made of silicon is transparent to the selected wavelength in the mid-infrared and near-infrared. Lasers with high efficiency and high economy have only been used for specific wavelengths so far. In addition, due to other material properties, the wavelength range that can be reached is significantly limited. Therefore, the laser source and the laser wavelength are constant.
[0089] An exemplary method for temporarily bonding a product substrate to a carrier substrate made of silicon (Si) has at least the following steps:
[0090] - producing a multilayer system as a bonding and debonding layer for temporary bonding on a carrier substrate and / or product substrate,
[0091] - Bonding the product substrate to the carrier substrate.
[0092] In this case, no bonding agent is required for the temporary bonding. In particular, the connection is produced by means of a direct bonding method or other known bonding techniques, such as metal diffusion bonding or anodic bonding.
[0093] Furthermore, a substrate stack, in particular a substrate stack produced by a method comprising a product substrate and a carrier substrate, wherein the product substrate and the carrier substrate are connected via a multilayer system as a temporary bonding layer, can be separated in a simplified manner by laser debonding by means of laser irradiation of the multilayer system.
[0094] The substrate stack preferably comprises the following components:
[0095] -Product substrate,
[0096] - multilayer systems with a layer structure optimized by interference for temporary bonding and laser debonding in the IR range,
[0097] - A carrier wafer made of silicon, transparent for selected wavelengths in the mid-infrared and near-infrared.
[0098] In a preferred embodiment, the layers of the multilayer system are produced frontally. In a less preferred embodiment, at least one of the layers is structured.
[0099] An exemplary method for laser debonding a product substrate from a carrier substrate composed of silicon, wherein the product substrate and the carrier substrate are connected via a multilayer system and form a substrate stack, the method having in particular at least the following steps:
[0100] - receiving and fixing the substrate stack on the substrate holder,
[0101] - focusing the debonding radiation, in particular a laser beam of a laser source, through the carrier substrate onto the multilayer system optimized by interference and thereby melting, evaporating and / or sublimating the multilayer temporary bonding layer,
[0102] - Release the product substrate from the carrier substrate.
[0103] In this case, no antireflection layer is required as a protective layer on the product substrate. Through targeted energy input and energy conversion in the multilayer system of bonding layers, in particular thermal and / or photothermal loading of the substrate, in particular functional components of the substrate, is minimized.
[0104] Furthermore, an exemplary method for producing and processing a substrate stack has the following steps:
[0105] - providing a carrier substrate, in particular a silicon carrier wafer, which is substantially transparent to light of a predetermined wavelength,
[0106] - production of optimized multilayer systems as bonding and release layers for temporary bonding on carrier substrates and / or product substrates,
[0107] - bonding the product substrate to the carrier substrate,
[0108] -Process the product substrate,
[0109] The product substrate is released from the carrier substrate by focusing debonding radiation, in particular a laser beam of a laser source, through the carrier substrate onto the multilayer system optimized by interference and thereby melting, evaporating and / or sublimating the multilayer temporary bonding layer.
[0110] According to a preferred embodiment, the laser source is a pulsed laser source, in particular an ultrashort pulsed laser source.
[0111] According to another preferred embodiment, the ultrashort pulse laser source is a femtosecond laser source.
[0112] According to another preferred embodiment, the system is further equipped with a scanner for scanning the pulsed laser beam.
[0113] Depending on the effect of the laser radiation upon absorption by the multilayer system, the multilayer system is separated from the substrate by delamination / peeling and / or ablation. Debonding preferably takes place along the interface between carrier substrate and multilayer system (delamination).
[0114] In a preferred embodiment, the release device is a substrate holder, to which the product substrate and the carrier substrate are each fixed or can be fixed. The separation is carried out, for example, by parallel displacement of the substrate and the carrier substrate relative to each other or by raising the substrate or the carrier substrate. Both are known to the person skilled in the art and will not be described further. Further mechanical, physical and / or chemical aids can be used for the separation.
[0115] The laser acts on the multilayer system and reduces the adhesive strength between the silicon carrier substrate and the multilayer system. The adhesive strength is reduced in particular by more than 50%, preferably by more than 75%, and more preferably by more than 90%.
[0116] Substrates and carrier substrates
[0117] The substrate and the carrier substrate can have any desired shape, but are preferably circular. The diameter of the substrate is in particular standardized in the industry. For wafers, diameters commonly used in the industry are 1 inch, 2 inches, 3 inches, 4 inches, 5 inches, 6 inches, 8 inches, 12 inches and 18 inches. The size and shape of the carrier substrate are matched to the size and shape of the product substrate so that the processing technology used is as simple as possible. It is also conceivable here to fix and handle non-circular substrates, such as panels, and to release them from the carrier substrate.
[0118] The carrier substrate consists predominantly, preferably completely, of one or more of the following materials: glass, minerals (especially sapphire), semiconductor materials (especially silicon), polymers, compound materials (SiC). Carrier substrates made of glass are generally preferred for laser debonding, since here electromagnetic beams in the UV-VIS wavelength range can preferably be used in combination with UV-VIS transparent bonding agents in order to prevent heating as much as possible.
[0119] If a carrier substrate made of silicon is preferred, an electromagnetic beam in the infrared (IR) wavelength range, in particular in the near and mid-IR, is required, corresponding to the transparency of the Si carrier substrate.
[0120] In another particularly preferred embodiment, the carrier substrate is made of silicon. The Si carrier substrate is compatible with CMOS processes or front-end processes.
[0121] The transparency of a carrier substrate for electromagnetic radiation is described by the transmittance, which gives the ratio of transmitted and incident radiation. However, the transmittance depends on the thickness of the irradiated body and is therefore given in relation to a unit length of 1 cm.
[0122] With respect to a selected thickness of 1 cm and for a respectively selected wavelength, the carrier substrate has a transmittance of more than 60%, preferably more than 70%, more preferably more than 80%, most preferably more than 90%, most preferably more than 95%. The transparency is particularly preferably dependent on the wavelength of the debonding laser radiation.
[0123] The thermal conductivity of the carrier substrate is preferably between 0.1 W / (m*K) and 5000 W / (m*K), more preferably between 0.5 W / (m*K) and 2500 W / (m*K), still more preferably between 1 W / (m*K) and 1000 W / (m*K).
[0124] The thickness of the carrier substrate can vary depending on the diameter and the requirements for structural stability.
[0125] Laser radiation
[0126] In particular, the laser radiation is selected such that it passes through the substrate to the interface to be separated and is strongly absorbed there by the multilayer coating.
[0127] The laser energy is delivered in the form of very short light pulses. In a preferred embodiment, this is ultrashort pulse laser radiation.
[0128] According to a preferred embodiment, the separation is brought about by multiphoton excitation caused by laser radiation, in particular a femtosecond laser or a picosecond laser.
[0129] In the case of thin metal layers, laser radiation with picosecond (ps) pulses has been shown to be the best parameter combination for processing from silicon.
[0130] The multilayer coating is separated from the substrate by irradiation on the carrier substrate side with light, in particular laser radiation, which is strongly absorbed by the multilayer coating at or near the interface between the materials to be separated.
[0131] The preferred silicon carrier substrate is opaque below a wavelength of 1.3 μm. Particularly preferred lasers and their wavelengths suitable for irradiation through a silicon carrier substrate are:
[0132] -Nd: YAG (1.064μm; 1.320μm; 1.444μm)
[0133] -Ho: YLF (2.05μm)
[0134] -Ho: YAG (2.09 μm)
[0135] -Cr:ZnSe,Cr:ZnS(MIR)
[0136] In a particularly preferred embodiment, a pulsed solid-state laser is used, preferably a Nd:YAG laser or a Ho:YAG laser. The pulsed solid-state laser operating in the infrared region above 1.3 μm is doped with ions consisting of Er3+ (1.55 μm), Tm3+ (1.9 μm), Ho3+ (2.09 μm) or Cr3+ (2.4 μm).
[0137] For example, preferred laser wavelengths for use with Si carrier substrates are 1940 μm, 1960 μm or 2030 μm. The power of the laser providing the laser radiation, measured as optical power, in particular radiant power, which can be continuously output at the substrate, is at least 2 W.
[0138] The preferred wavelength range of the laser light is between >1100 nm and 10000 nm, preferably between >1100 nm and 5000 nm, more preferably between 1500 nm and 2500 nm.
[0139] Here, too, a laser beam having at least two wavelengths can be used. The layer thickness of the multilayer system is then optimized for both wavelengths.
[0140] The total energy of the laser radiation per substrate is set in particular between 1 mJ and 500 kJ, preferably between 100 mJ and 200 kJ, particularly preferably between 500 mJ and 100 kJ.
[0141] The laser beam can be operated in continuous mode or preferably in pulsed mode. The pulse frequency is set in particular between 0.1 Hz and 300 MHz, preferably between 100 Hz and 500 kHz, particularly preferably between 1 kHz and 400 kHz, very particularly preferably between 1 kHz and 100 kHz.
[0142] The energy with which each radiation pulse impinges on the substrate stack is set in particular between 0.1 nJ and 1 J, preferably between 1 nJ and 900 J, particularly preferably between 1 nJ and 10 μJ.
[0143] The beam spot size is especially 1μm 2 and 10mm 2 between 5 μm and 1 μm. 2 and 1mm 2 between 400 μm and 100 μm, preferably between 400 μm and 100 μm. 2 and 1502μm 2 Between (1 / e of the radiation intensity distribution of the laser spot at the substrate 2 measured in the case).
[0144] The spatial distance (pitch) of the laser pulses at the substrate is in particular between 0.1 μm and 1000 μm, preferably between 1 μm and 500 μm, particularly preferably between 10 μm and 200 μm, most preferably between 20 μm and 100 μm.
[0145] Depending on the required total energy, the number of pulses per substrate stack is in particular between 10 million pulses and 10 billion pulses, preferably between 10 million pulses and 1 billion pulses, particularly preferably between 20 million pulses and 100 million pulses.
[0146] The total energy of the laser radiation per substrate is set in particular between 1 mJ and 500 kJ, preferably between 100 mJ and 200 kJ, particularly preferably between 500 mJ and 100 kJ.
[0147] The pulses have a length in the microsecond to femtosecond range (μs-fs), preferably in the nanosecond to femtosecond range (ns-fs), in particular between 100 ns and 100 fs, preferably between 10 ps and 1 ps.
[0148] With short pulses, very high peak powers can be achieved without increasing the average laser power. Since the pulse energy available for shorter pulses is several orders of magnitude smaller (in the J range for high-power lasers compared to μJ for “ultrafast” picosecond and femtosecond lasers) at different pulse durations, the total energy input into the material to be processed is reduced, which generally leads to smaller thermal damage zones due to the shorter action time and the resulting lower thermal diffusion.
[0149] The high power density allows the material to be heated in the shortest possible time, thereby achieving removal or sublimation. The short action time thus results in less thermal energy input into the underlying material and thus minimal damage to the unprocessed area.
[0150] In case of pulse durations below a few picoseconds, direct ablation by laser radiation is assumed for most materials, whereas in case of longer pulse durations, thermally induced removal is facilitated by additional effects arising from the interaction of the laser, the laser-induced plasma, and the material in different states of aggregation.
[0151] At high radiation intensities, a plasma glow occurs when a material is ablated by laser radiation. After the plasma glow occurs, cumulative ionization and thermal ionization occur to such an extent that the material damage is no longer confined to the laser focus. It is known from the prior art that the energy threshold for the formation of a plasma glow decreases significantly with decreasing pulse duration.
[0152] In general, ultrashort pulses in the ps range are preferred so that linear and nonlinear absorption occurs in the multilayer system. 12 W / cm 2 Starting from laser intensities of 10,000 nm, in addition to single-photon absorption, interactions between photons and atoms also occur due to multiphoton absorption. Therefore, depending on the intensity, linear or nonlinear processes may dominate the absorption. 12 to 10 14 W / cm 2 The multiphoton effect plays a major role when the intensity is between 20 and 100 Å, which is achieved with ultrashort pulses.
[0153] Pulses with high intensity and pulse durations of less than 100 ps can induce a plasma glow, which advantageously leads to a significant increase in the local absorption at the multilayer system through the interaction of free electrons and ions with the residual electromagnetic field.
[0154] The pulse energy and / or the pulse duration and / or the length of the pulse train are preferably temporally modulated by a control unit of a laser beam source generating the pulsed laser beam, wherein the modulation is preferably controlled by an external signal transmitter. The energy coupled into the treatment region by the laser beam is preferably temporally modulated by modulation of the pulse duration of the laser pulses, wherein the pulse duration is preferably modulated between 0.1 ps and 20 ps.
[0155] Those skilled in the art know that the synonym of the irradiation area is the spot size or the beam spot (English: laserspot size).
[0156] The shape of the irradiated area is in particular circular, in other preferred embodiments oval or rectangular.
[0157] In the case of laser debonding, the laser light is coupled in on the substrate side via a substrate that is as transparent as possible and is absorbed in the adjacent release layer on the back side. The laser light is preferably coupled in via a substantially transparent carrier substrate made of silicon. Si carrier substrates, which are usually between 725 and 775 μm thick, are increasingly transparent for wavelengths starting from 1100 nm. Due to the absorption caused by nonlinear interactions in silicon in the range below 1300 nm, ultrashort pulses in the ps range are used, so that wavelengths greater than 1300 nm are preferred, more preferably greater than 1900 nm. Shorter pulse durations require higher wavelengths for the substantial transparency of the Si carrier substrate.
[0158] In the interaction of the laser beam with the material, optical and physical processes play a role. These are, for example, the numerical aperture (NA) of the lens and the energy of the laser beam or the laser power density when the laser beam is focused into the material.
[0159] The following parameters lead to different interactions of ultrashort laser pulses with materials:
[0160] - Pulse energy
[0161] -Numerical aperture NA
[0162] - Pulse duration
[0163] - Pulse train frequency
[0164] -Laser wavelength
[0165] -Beam profile
[0166] - Pulse form.
[0167] Here, the following criteria are evaluated for the multi-layer system depending on the parameter settings:
[0168] -Area of ablation per shot
[0169] - Debonding area or delamination area per bombardment
[0170] - Pulse energy per shot ablation threshold
[0171] -Energy of each pulse that hits the delamination threshold.
[0172] For example, the following parameters of a multi-layer system can be determined:
[0173] - With the help of simulations and in tests the thickness of the individual layers,
[0174] - the arrangement / order of the individual layers, if required,
[0175] - Additional layer(s) of material if further layers are required.
[0176] In this case, multilayer systems are known to the person skilled in the art, so that no material optimization takes place. The materials of the multilayer systems are coatings known to the person skilled in the art, which are used during joining and whose layer thicknesses are optimized with regard to interference in order to absorb the laser radiation as highly as possible. In many cases, laser dejoining is not possible until the layer thicknesses have been selected.
[0177] Multi-layer system and multi-layer design optimization
[0178] The basic idea of this patent is to provide a multilayer layer structure optimized by interference for bonding and laser debonding of substrates.
[0179] Many factors play a role in the absorption of radiation. This interaction is influenced both by the properties of the laser and by the properties of the material. In the case of lasers, the most important are the wavelength, polarization, angle of incidence and spatial and temporal properties of the radiation, while in the case of materials, the chemical composition and microscopic or macroscopic properties have a major influence.
[0180] For different coatings, the effects of scattering, reflection and absorption are used empirically in the prior art. The optimization of individual parameters is also common, but in the prior art it is not known to adjust the layer thickness in order to increase the absorption in an optimal way, minimizing the losses due to reflection or transmission and balancing the pulse duration with the layer thickness. In this case, factors such as the laser wavelength, the angle of incidence and the layer material are kept constant.
[0181] The multilayer design optimizes the use of existing materials and coatings known to a person skilled in the art in the semiconductor industry, which are optimized, in particular with regard to their layer thickness, in such a way that a maximum absorption is achieved by interference of the electromagnetic radiation in the multilayer system.
[0182] The layer thicknesses are in the subwavelength range, so that for incident waves the multilayer system has a different wave impedance than the individual materials used for the individual layers. The absorption of the multilayer system is thus significantly improved.
[0183] If electromagnetic radiation can be absorbed in a material, the intensity of the absorption is described by a material parameter, namely the degree of absorption, which usually depends on several parameters (temperature, wavelength, etc.). The absorption or degree of absorption is given between 0 and 1. Radiation that strikes the surface of an object is usually partially reflected, partially passes through the object, and the rest is absorbed. The absorbed energy increases the internal energy of the object. The degree of absorption (also called absorption coefficient or spectral absorption coefficient SAK) specifies the proportion of the incident radiation that is absorbed. This proportion can take values between 0 and 1. The degree of absorption depends on the direction of incidence and the frequency of the incident radiation.
[0184] If the absorption for different wavelengths and different layer thicknesses of selected layers from a multilayer system is represented graphically, a representation of different absorption ranges is possible. In general, the absorption is mainly a lossy interaction of the electromagnetic field in the material, which can (usually) be described by the electromagnetic susceptibility and thus by the complex-valued refractive index n+ik. Thus, even nonlinearities such as act precisely in the case of short pulses (for example when the response to an increase in the electric field increases in proportion to a higher potential) can be represented. Furthermore, simulations are used to show that, by the occurrence of multiple interferences at the interfaces between the individual layers of the multilayer system, an increase in the absorption of the entire multilayer system can be achieved by varying the layer thickness in the nm range.
[0185] The laser wavelength is preferably constant and two parameters, in particular the layer thicknesses d1 and d2 of the two layers in the multilayer system, are varied simultaneously and the absorption is calculated. By optimizing the layer thicknesses in the multilayer system, a higher absorption and a reduction in the losses due to scattering or reflection and thus a higher laser debonding efficiency can be achieved. It is also possible to make full use of scattering or diffraction effects to change the propagation direction of the light and thus increase the interaction duration. It is also possible to make full use of scattering or diffraction effects to protect the next layer located below or the product substrate located below.
[0186] The layer thickness of each individual layer L1 to Ln of the multilayer system consisting of layers L1 to Ln, preferably L1 to L3, is optimized, wherein the absorption of the entire multilayer system is determined numerically and also measured experimentally. The individual influences of the layers are investigated and optimized with regard to the efficiency and stability of the effect.
[0187] The separation of the multilayer system from the substrate is carried out by irradiation on the substrate side with light, in particular laser radiation, which is strongly absorbed by the multilayer coating at or near the interface between the materials to be separated. The following exemplary effects at adjacent layers are utilized: constructive interference, scattering, diffraction and phase shift.
[0188] The layers of the multilayer system can be applied by means of chemical or physical vapor deposition, sputtering, evaporation, epitaxy and / or by means of spin coating, as well as combinations thereof or other suitable techniques.
[0189] Antireflective coatings (AR) are advantageously not required to significantly reduce Fresnel reflections due to the increased, optimized local absorption of the coating.
[0190] An additional connecting layer, in particular a bonding agent, is also advantageously not necessary, since the multilayer system, which contains, in particular, a metallic or metal-containing light-to-heat multilayer conversion layer, is simultaneously the connecting layer. No additional sacrificial layer is required either.
[0191] The energy absorbed here causes the decomposition of the multilayer coating, wherein separation occurs at the interface between substrate and coating. The decomposition mechanism can be, for example, sublimation or a chemical reaction. The decomposition can be initiated thermally and photochemically. Separation is particularly facilitated if gaseous products are produced during the decomposition.
[0192] At least one layer of the multilayer system preferably consists of the following compounds or elements, alone or in combination:
[0193] -Metals, such as Ti, Au, Ag, Cu, Fe, Ni, Al, Cr, Pt, Sn
[0194] -alloy,
[0195] -Semiconductors (such as Ge)
[0196] - compounds, especially nitrides, especially TiN, TaN, AlN, GaN, InN, SiN, Si3N4
[0197] - compounds, especially oxides, especially SiO2, TiO2
[0198] - Compounds, especially dielectrics
[0199] - Ceramic materials, especially silicon carbide (SiC) and aluminum oxide (Al2O3)
[0200] - Highly absorbent non-metals, especially polymers with nanoparticles (polymers with Al or C particles).
[0201] In this case, the individual layers of the multilayer system may consist of a material or a combination of materials from one of the 3rd main group (boron group), the 4th main group (carbon group) and the 5th main group (nitrogen group) of the periodic table.
[0202] In a less preferred embodiment, the material is not applied over the entire surface, but rather as a 2D structure (eg pattern) or a 3D structure for individual layers of the multilayer system.
[0203] The multilayer system is applied as a layer sequence of different compounds or elements on the product substrate and / or the carrier substrate. In this case, any number n of coatings can be formed as a multilayer system (L1 to Ln). Preferably, up to three layers (L1 to L3) are used in the multilayer system.
[0204] In another embodiment, at least one compound or one element is applied alternately multiple times.
[0205] The individual layers can be used, for example, as selective absorber layers or phase shifters. Examples of absorbers are metals, such as aluminum (Al) or gold (Au). Silicon dioxide (SiO2) can be used, for example, as an auxiliary layer and / or phase shifter in order to position the field maximum of the wavelength within the selective absorber. The layer thicknesses are in the lower nm range. If desired, thicker (metal) coatings can be used as mirrors.
[0206] Preferably, further layers such as sacrificial layers and / or antireflection layers and / or relaxation layers and / or bonding agents are not required and are omitted.
[0207] The thickness of the individual layers of the multilayer coating is between 1 nm and 10 μm, preferably between 1 nm and 1 μm, more preferably between 5 nm and 500 nm. Due to the very thin layer sequence, a high degree of interaction with electromagnetic radiation is possible. This high degree of interaction in the case of very thin layers is used for simplified laser debonding. Due to the optimization of the thickness of the individual layers of the multilayer system, the layer thickness (nm range) is reduced, whereby advantageously less material must be applied.
[0208] Metals are strong absorbers and can block laser radiation already from a layer thickness of <100 nm. In contrast, organic absorbers generally require a layer thickness of >3 μm in order to absorb 67% of the incident light.
[0209] The thickness of the multilayer system is preferably between 1 nm and 10 μm, more preferably between 5 nm and 1 μm, most preferably between 10 nm and 1 μm.
[0210] Optimized laser debonding of substrate stacks with multilayer systems and silicon carrier substrates
[0211] The optimized process for separation by debonding or delamination along the interface by means of laser radiation comprises, for example, the following steps:
[0212] - Laser selection. Silicon as a carrier substrate is mainly transparent at wavelengths λ>1300nm or λ>1900nm, so lasers in the near infrared (NIR) and mid-infrared (MIR) are selected here, which show low linear and nonlinear absorption in Si carrier substrates;
[0213] - Use of existing materials for a multilayer bonding layer between the Si carrier substrate and the product substrate; the multilayer system enables an interference-controlled optimization of the absorption required for laser debonding. The individual layers of the multilayer system can be used, for example, depending on the layer thickness, as selective absorber layers or phase shifters or mirrors, and thereby maximize the absorption at the multilayer system as a whole. Examples of absorbers are metals, such as aluminum (Al) or gold (Au). For example, silicon dioxide (SiO2) and aluminum nitride (AlN) can be used as phase shift layers in order to position the field maximum of the wavelength within the selective absorber. Here, the layer thickness is in the lower nm range. If necessary, thicker coatings can be used as mirrors. The metal layer can, for example, be used, depending on the layer thickness, as a mirror layer (layer thickness > 100 nm) or a selective absorption layer (layer thickness < 10 μm).
[0214] - Laser throughput and laser quality optimization. In a preferred embodiment, ultrashort pulse laser radiation is involved. The laser source and the laser wavelength are fixed parameters. Here, for example, the following laser parameters are optimized: pulse duration, pulse train frequency, energy, shape of the irradiation area per pulse, multi-spot laser.
[0215] - Optimization of the material layers. The material layers are optimized with regard to their layer thicknesses in such a way that a maximum light absorption is achieved by interference and reflection losses are minimized. The absorption increase due to the optimization of the layer thickness is spatially localized and enhanced within the multilayer system. Exceeding or falling below the optimum layer thickness of the individual layers of the multilayer system will lead to a significant reduction in the absorption.
[0216] The optimization of the layer thickness is carried out in particular by simulations and / or laser debonding tests of substrate stacks with layer thicknesses selected from the simulations. The remaining bonding forces, the ablation pattern and the homogeneity during laser debonding are investigated in the tests. The produced system is also checked with regard to the stability of the production and processing parameters. BRIEF DESCRIPTION OF THE DRAWINGS
[0217] Further advantages, features and details of the invention are apparent from the following description of preferred embodiments with reference to the accompanying drawings. The accompanying drawings are schematically shown in:
[0218] Figure 1a : Cross-sectional view of a substrate stack consisting of a carrier substrate, a multilayer system with three layers and a product substrate with functional units.
[0219] Figure 1b : Cross-sectional view of a substrate stack consisting of a carrier substrate, a multilayer system with three layers and a product substrate with a structured portion.
[0220] Figure 1c : Cross-sectional view of a substrate stack consisting of a carrier substrate, a multilayer system with two layers and a product substrate.
[0221] Figure 2 : Cross-sectional view of a product substrate-carrier substrate stack with schematic representation of optical components for irradiating the multilayer system with laser radiation.
[0222] Figure 3a : Schematic representation of the absorption spectrum A of a multilayer system. The figure shows the absorption of a multilayer system consisting of three layers L1, L2 and L3, wherein the thickness d1 and the wavelength of layer L1 are varied, while the thicknesses of layers L2 and L3 remain unchanged.
[0223] Figure 3b : Schematic representation of the absorption spectrum A of a multilayer system. The figure shows the absorption of a multilayer system consisting of two layers L1 and L2, wherein the thickness d1 of layer L1 and the thickness d2 of layer L2 are varied, while the laser wavelength remains unchanged.
[0224] In these figures, the same components or components having the same function are denoted by the same reference numerals. DETAILED DESCRIPTION
[0225] according to Figure 1a , by way of example, three layers L1 (5), L2 (6) and L3 (7) are applied over the entire surface to a product substrate 2 and / or a carrier substrate 3. A structure 8 is located in and / or on the product substrate 2. In this case, the layer thicknesses d1, d2 and d3 of the respective coatings L1 (5), L2 (6) and L3 (7) are optimized. Thus, the multilayer system 4 consists of a plurality of layers 5, 6, 7, which are selected such that the multilayer system 4 leads to a maximum absorption of the laser radiation during the laser debonding process. The interference-optimized layer structure 4 enables improved and simpler laser debonding, wherein no additional layers are required to protect the substrate or to bond the substrate, such as antireflection coatings and / or relaxation layers and / or bonding agents.
[0226] The thickness of the individual layers 5, 6, 7 of the multilayer system 4 is between 1 nm and 1 μm, preferably between 1 nm and 500 nm, more preferably between 1 nm and 250 nm. Due to the very thin layer sequence, a high degree of interaction with the electromagnetic waves of the laser radiation is possible.
[0227] The thickness of the multilayer system 4 is preferably between 1 nm and 10 μm, more preferably between 5 nm and 2 μm, most preferably between 10 nm and 1 μm, most preferably between 10 nm and 500 nm.
[0228] according to Figure 1a After coating the multilayer system 4 on the product substrate 2 and / or the carrier substrate 3, the product substrate 2 is bonded to the carrier substrate 3 in a (temporary) bonding method by alignment, contacting and bonding. (Temporary) bonding techniques are known to those skilled in the art.
[0229] exist Figure 1a and 1b Three coating layers L1 to L3 (5, 5', 6, 6', 7, 7') are shown in FIG. 1 , but any other number n of coating layers may also be formed. Figure 1c The embodiment of a multilayer system with two coatings 5", 6" is shown, for example. In this case, the layer thickness of each individual layer L1 to Ln of the multilayer system consisting of layers L1 to Ln is optimized, wherein the absorption of the entire multilayer system is measured. Preferably, for example, the two layer thicknesses d1 and d2 are first varied simultaneously in a simulation while keeping the wavelength the same, and according to Figure 3b The resulting absorption is determined. The layer thicknesses d1max and d2max of the coatings 5 , 6 are selected which result in a maximum, effective and stable absorption. In particular, the other variable laser parameters are optimized by analyzing the laser debonding of substrate stacks in tests.
[0230] Figure 1b A further embodiment of a substrate stack 1 ′ is shown, which consists of a carrier substrate 3 ′, a multilayer system 4 ′ having three layers L1 to L3 ( 5 ′, 6 ′, 7 ′), and a product substrate 2 ′ having a structuring.
[0231] Figure 1c A further embodiment of a substrate stack 1 ″ is shown, which consists of a carrier substrate 3 ″, a multilayer system 4 ″ having two layers L1 ( 5 ″) and L2 ( 6 ″), and a product substrate 2 ″.
[0232] In the following section, based on Figures 1a to 1c A plurality of non-limiting examples of multilayer systems (e.g., layers L1-L2-L3 or layers L1-L2) are described with reference to the multilayer systems in FIG. 1 . Multilayer systems known to those skilled in the art and used in the semiconductor industry, in particular also for CMOS-compatible or front-end-compatible processes, consist, for example, of:
[0233] SiO2-metal-SiO2(L1-L2-L3),
[0234] SiO2-metal 1 (L1-L2),
[0235] Metal 1 (layer thickness d1) - oxide or nitride compound (e.g. SiO2) - metal 1 (layer thickness d2) (L1-L2-L3),
[0236] SiO2-nitride compound-SiO2(L1-L2-L3),
[0237] Nitride compounds - SiO2 (L1-L2),
[0238] Oxide or nitride compound (e.g. SiO2)-metal 1-metal 2 (L1-L2-L3),
[0239] Metal 1-Metal 2-Metal 3 (L1-L2-L3),
[0240] Metal 1-Metal 2 (L1-L2),
[0241] Metal 1-Metal 2-Metal 1 (L1-L2-L3).
[0242] In particular, the following multilayer system is described for laser debonding, which is applied on a 300 mm silicon carrier substrate (thickness 775 μm, both surfaces polished):
[0243]
[0244] The TEOS layer is a layer composed of amorphous silicon dioxide (SiO 2 ), and is preferably finely polished by chemical mechanical polishing (CMP).
[0245] In an alternative embodiment, a 300 mm silicon carrier substrate also has a thickness of 725 μm.
[0246] The bonded product substrate (also made of silicon) follows layer L2. During debonding, the laser first penetrates the 775 μm silicon carrier layer, then layer L1 and layer L2.
[0247] The laser wavelength is determined by the choice of carrier substrate and does not change. The laser angle of incidence also remains constant.
[0248] Other specific examples of the layer system:
[0249] SiN—SiO2(L1-L2)
[0250] TEOS(50-250nm)-TiN(20-100nm)-TEOS(50-400nm)(L1-L2-L3)
[0251] TiN(50nm)-TEOS(400nm)(L1-L2)
[0252] SiO2 (hot, 50-100nm)-TiN (50nm)-TEOS (400nm) (L1-L2-L3)
[0253] At least one layer of the multilayer system preferably consists of the following compounds or elements, alone or in combination:
[0254] -Metals, such as Ti, Au, Ag, Cu, Fe, Ni, Al, Cr, Pt, Sn
[0255] -alloy,
[0256] -Semiconductors (such as Ge)
[0257] - compounds, especially nitride compounds, especially TiN, TaN, AlN, GaN, InN, SiN, Si3N4
[0258] - compounds, especially oxide compounds, especially SiO2, TiO2
[0259] - Ceramic materials, especially silicon carbide (SiC) and aluminum oxide (Al2O3)
[0260] - Highly absorbent non-metals, especially polymers with nanoparticles (e.g. polymers with Al or C particles)
[0261] The individual layers of the multilayer system can be used, for example, depending on the layer thickness and the material, as a selective absorption layer, an auxiliary layer and / or a phase shift layer or a mirror layer and thus maximize the absorption at the multilayer system as a whole. For example, depending on the layer thickness, a metal layer can be used as a mirror layer (layer thickness>100 nm) or a selective absorption layer (layer thickness<10 μm). For example, silicon dioxide (SiO2) and aluminum nitride (AlN) can be used as phase shift layers.
[0262] In the case of three layers, the absorbing layer is usually the middle layer. In the case of two layers, the absorbing layer is usually the first layer. The absorbing layer absorbs the energy of the laser radiation.
[0263] In one example, the absorber layer is composed of SiN and the auxiliary layer is composed of SiO 2 Due to the interaction of the SiN and SiO 2 layers, NOx gas is generated, which causes the layers to split and thus cause debonding.
[0264] In a preferred embodiment, the layer thickness of the absorber layer is between 10 nm and 200 nm, and the thickness of the auxiliary layer(s) is between 1 and 1000 nm.
[0265] Figure 2 A cross section through a product substrate-carrier substrate stack 1 is shown during laser debonding by irradiating the multilayer system 4 with laser radiation 11. Suitable light sources are, for example, light sources which emit ultrashort light pulses with a duration of 10 ps to 50 ps and a repetition frequency of 1000 Hz.
[0266] The ultrashort pulse laser beam 11 is focused into a processing region 12 by an optical system 9. In this case, a relative movement (not shown) between the substrate stack 1 and the laser beam 11 occurs with the substrate stack positioning and / or beam positioning. Further optical elements include, for example, beam shaping elements, scanners, modulators, etc. and are known to those skilled in the art.
[0267] The relevant wavelength range for Si as a carrier substrate is between 1940 and 2140 nm, since Si has very strong nonlinearities and the nonlinear absorption / refraction reaches beyond 1700 nm, which leads to self-focusing. Also important here are the energy and power density required for ablation. The wavelength and laser selection are usually different from the case of other carrier materials (e.g. sapphire).
[0268] Figure 3a Describes the optimization method used to Figure 1a The method flow of an exemplary multilayer system 4 consisting of three layers L1, L2 and L3 (5, 6, 7) is to be used for temporary bonding and laser debonding of product substrate 2 and carrier substrate 3. It is conceivable that the product substrate 2, 2', 2" has no topography, either because there is no structure 8 or because the structure 8 has been produced directly in the product substrate 2, 2', 2". Alternatively, the structure can be, for example, a chip or a structured coating and form the topography.
[0269] according to Figure 3a The thickness d1 of the first layer L1 was varied between 0 and 100 nm in order to determine the maximum absorption of the multilayer system at different wavelengths. Figure 3a Region 1 in the graph shows the maximum absorption. Figure 3a The areas with increasing numbers in the figure show that the absorption of the multilayer system becomes less and less. The thicknesses d2 and d3 of the other two layers L2 and L3 are kept constant here. The individual thicknesses of the layers influence the interference pattern and thus the absorption of the multilayer system. By determining the optimum layer thicknesses d1, d2 and d3, the maximum absorption of the multilayer system is determined for improved and simplified laser debonding. Figure 3a The diagrams are presented using simulations and determined using measurement series. In this case, there is no need to optimize or change the materials of the individual layers, and in the case of existing multilayer systems, simplified laser debonding by maximum absorption is achieved by optimizing the layer thicknesses. The absorption can be increased from <10% to >90%.
[0270] The absorptivity is calculated primarily with known solution algorithms via the Fresnel equations for multilayer systems by means of linear estimates, based on the layer thicknesses and the (linear but complex-valued) refractive index. In addition, nonlinear properties can be used for more complex simulations, which also take into account the field intensity distribution.
[0271] exist Figure 3a In an alternative embodiment, according to Figure 3b , the absorption can be expressed, for example, for a system consisting of two layers L1 and L2 at a selected laser wavelength, according to two layer thicknesses d1 and d2. The layer thickness d of the individual layers of the multilayer system can be controlled and varied most easily if the layers from a given substrate stack, the substrate and the carrier substrate are known. The layer thickness d of the individual layers of the multilayer system is thus initially optimized. In particular, the laser wavelength and the laser angle (angle of incidence) remain constant. If the multilayer system consists of two layers, according to Figure 3b , the layer thicknesses d1 and d2 can be varied simultaneously. Selected parameters, in particular for example the two layer thicknesses d1 and d2, are varied and the degree of absorption in the debonded structure is calculated. The degree of absorption in the debonded structure must be as high as possible. In order to maximize the absorption, preferably a maximum of three layers are used. Similar to Figure 3a , Figure 3b The area 1 in the graph shows the maximum absorption. The areas with increasing numbers show that the absorption of the multilayer system becomes less and less. In the represented graph, the area 1 with high absorption must be large enough not to be too sensitive to changes.
[0272] Reference numerals list
[0273] 1 Substrate stacking
[0274] 2Product chip
[0275] 3 Carrier wafer
[0276] 4 Multi-layer system
[0277] 5-layer L1
[0278] 6-layer L2
[0279] 7th floor L 3
[0280] 8 Structure
[0281] 9. Optical System
[0282] 10 Optical Elements
[0283] 11 Laser beam
[0284] 12 processing areas.
Claims
1. A method for providing a multilayer system (4) consisting of at least two layers (5, 6, 7), in particular for temporarily joining substrates to form a substrate stack (1), the method comprising the following steps in the following order: i) providing a multi-layer system (4), ii) determining the degree of absorption of laser radiation (11) of a specific wavelength by the multilayer system (4), iii) changing at least one parameter of the multilayer system (4), iv) determining the degree of absorption of laser radiation (11) of a specific wavelength by a multilayer system (4), said multilayer system having at least one parameter varied according to step iii), v) Repeating steps i) to iv) until the absorption level is maximum, wherein in step i) a multilayer system (4) having a maximum absorption level is provided in each case.
2. The method according to claim 1, wherein at least one parameter of the multilayer system (4) is a layer thickness of a layer (5, 6, 7) of the multilayer system (4).
3. The method according to claim 2, wherein at least one parameter of the multilayer system (4) is additionally a layer thickness of a further layer (5, 6, 7) of the multilayer system (4).
4. The method according to claim 1, wherein the wavelength during the determination in steps ii) and iv) is between 1100 nm and 10000 nm, preferably between 1100 nm and 5000 nm, more preferably between 1500 nm and 2500 nm.
5. A substrate stack (1) having at least one multilayer system (4) according to at least one of claims 1 to 4, the multilayer system having at least two layers (5, 6, 7) composed of different materials.
6. A substrate stack (1) according to at least one of the preceding claims, wherein the multilayer system (4) has a total thickness between 1 nm and 10 μm, more preferably between 5 nm and 2 μm, most preferably between 10 nm and 1 μm, and most preferably between 10 nm and 500 nm.
7. A substrate stack (1) according to at least one of the preceding claims, wherein the corresponding layers (5, 6, 7) of the multilayer system (4) each have a layer thickness between 1 nm and 1 μm, preferably between 1 nm and 500 nm, more preferably between 1 nm and 250 nm.
8. The substrate stack (1) according to claim 1, wherein the multilayer system (4) comprises at least one layer (5, 6, 7) having a layer thickness of between 25 nm and 75 nm.
9. A substrate stack (1) according to at least one of the preceding claims, wherein at least one layer (5, 6, 7) of the multilayer system (4) comprises, preferably consists of, titanium (Ti), aluminum (Al), aluminum nitride (AlN), tantalum nitride (TaN), (germanium) Ge, (tin) Tin or copper (Cu).
10. The substrate stack (1) according to claim 1, wherein at least one layer (5, 6, 7) of the multilayer system (4) consists of amorphous silicon dioxide (SiO2).
11. The substrate stack (1) according to at least one of the preceding claims, wherein the substrate stack (1) comprises at least a carrier substrate (3) and a product substrate (2), wherein the carrier substrate (3) is connected to the product substrate (2) via a multilayer system (4). 12 . The substrate stack ( 1 ) according to claim 1 , wherein the multilayer system ( 4 ), preferably the substrate stack ( 1 ), has no polymer-based binder.
13. The substrate stack (1) according to at least one of the preceding claims, wherein the multilayer system (4), preferably the substrate stack (1), has no antireflection layer.
14. A method for bonding substrates to form a substrate stack (1) according to at least one of claims 5 to 13, the method comprising the following steps: 1) providing a first substrate, in particular a carrier substrate (3), 2) Joining a second substrate, in particular a product substrate (2), to the first substrate.
15. A method for debonding a substrate stack (1), the method comprising the following steps, a) providing a substrate stack (1) according to at least one of claims 5 to 13, b) irradiating the multilayer system (4) with laser radiation (11) of a specific wavelength through at least one substrate of the substrate stack (1), and then c) Separating the substrate stack ( 1 ) in the region of the multilayer system ( 4 ).