Positive electrode material and secondary battery using same

By placing sulfur positive electrode active material and lithium halide in porous carbon materials, the problem of high internal resistance of all-solid lithium secondary batteries is solved, and the charging and discharge rate characteristics and overall performance of the battery are improved.

CN118946984APending Publication Date: 2024-11-12NISSAN MOTOR CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030846.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing all-solid-state lithium secondary batteries are difficult to fully reduce internal resistance at high charge and discharge rates, which affects the charge and discharge characteristics of the battery.

Method used

The positive electrode active substance and lithium halide that contain both sulfur in the porous carbon material are used, and the conductivity of electrons and lithium ions is improved by placing these substances in the pores of the porous carbon material.

Benefits of technology

It effectively reduces the internal resistance of the battery, improves the charge and discharge rate characteristics, and enhances the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946984A_ABST
    Figure CN118946984A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a means for further reducing the internal resistance of a secondary battery using a sulfur-containing positive electrode active material. The present invention provides a positive electrode material characterized by containing a porous carbon material, a positive electrode active material containing sulfur, and a lithium halide, at least a portion of the positive electrode active material and at least a portion of the lithium halide being arranged in pores of the porous carbon material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode material and a secondary battery using the same. Background Art

[0002] In recent years, there is an urgent need to reduce carbon dioxide emissions in order to combat global warming. In the automotive industry, the introduction of electric vehicles (EVs) and hybrid electric vehicles (HEVs) is expected to reduce carbon dioxide emissions, and the development of non-aqueous electrolyte secondary batteries such as engine drive secondary batteries, which are the key to their practical application, is being actively pursued.

[0003] As secondary batteries for driving motors, they are required to have extremely high output characteristics and high energy compared to lithium secondary batteries for daily use used in mobile phones, notebook computers, etc. Therefore, lithium secondary batteries, which have the highest theoretical energy among all practical batteries, have attracted much attention and are currently being developed rapidly.

[0004] Here, the electrolyte of lithium secondary batteries, which are now widely used, uses a flammable organic electrolyte. In such liquid lithium secondary batteries, safety measures against leakage, short circuit, overcharge, etc. are required to be more stringent than other batteries.

[0005] Therefore, in recent years, research and development of all-solid-state lithium secondary batteries using oxide-based and sulfide-based solid electrolytes in the electrolyte has been actively conducted. A solid electrolyte is a material composed mainly of an ion conductor capable of ion conduction in a solid. Therefore, in principle, in all-solid-state lithium secondary batteries, various problems caused by flammable organic electrolytes will not occur as in the previous liquid-based lithium secondary batteries. In addition, in general, if high-potential / large-capacity positive electrode materials and large-capacity negative electrode materials are used, a significant increase in the output density and energy density of the battery can be achieved. For example, elemental sulfur (S 8 ) has a large theoretical capacity of about 1670mAh / g, and has the advantages of low cost and abundant resources.

[0006] On the other hand, elemental sulfur is a high resistance, and therefore, when used under a practical current as a positive electrode material, it is not easy to ensure sufficient charge and discharge capacity. In order to cope with such a problem, Japanese Patent Publication No. 2010-95390 proposes a technique for using a mesoporous carbon composite material containing at least mesoporous carbon and sulfur disposed in the mesopores of the mesoporous carbon as a positive electrode material for a solid-state battery. According to Japanese Patent Publication No. 2010-95390, by forming a positive electrode material having such a structure, the electronic conductivity is improved according to the micronization of sulfur and the composite with mesoporous carbon, and the battery performance can be improved. Summary of the invention

[0007] Here, according to the purpose of the secondary battery, it is required to take out sufficient capacity during charging and discharging at a high charge and discharge rate (that is, the so-called sufficient charge and discharge rate characteristics). For example, a secondary battery with insufficient charge and discharge rate characteristics cannot cope with rapid charging and discharging and use sufficient capacity. Moreover, in order to improve the charge and discharge rate characteristics of the secondary battery, it is necessary to reduce the internal resistance of the battery. However, according to the research of the inventors, it is known that even if the technology of the above-mentioned Japanese Patent Gazette No. 2010-95390 is adopted, it is difficult to fully reduce the internal resistance.

[0008] Therefore, an object of the present invention is to provide a means for further reducing the internal resistance of a secondary battery using a positive electrode active material containing sulfur.

[0009] The present inventors have conducted intensive studies to solve the above problems and have found that the above problems can be solved by using a positive electrode material containing both a positive electrode active material containing sulfur and a lithium halide in the pores of a porous carbon material, thereby completing the present invention.

[0010] One embodiment of the present invention is a positive electrode material, characterized in that it contains: a porous carbon material, a positive electrode active material containing sulfur, and a lithium halide, wherein at least a portion of the positive electrode active material and at least a portion of the lithium halide are arranged in pores of the porous carbon material. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a perspective view showing the appearance of a flat laminated all-solid lithium secondary battery as one embodiment of the present invention.

[0012] Figure 2 For along Figure 1 A cross-sectional view along line 2-2 is shown.

[0013] Figure 3 (a) is a schematic cross-sectional view of an existing positive electrode material. Figure 3 (b) is a schematic cross-sectional view of a positive electrode material according to one embodiment of the present invention.

[0014] Figure 4 This is the XRD spectrum of the positive electrode material prepared in Example 1.

[0015] Figure 5 This is the XRD spectrum of the positive electrode material prepared in Example 6.

[0016] Figure 6 : This is the XRD spectrum of the positive electrode material prepared in Comparative Example 1.

[0017] Figure 7 This is the XRD spectrum of the positive electrode material prepared in Comparative Example 2. DETAILED DESCRIPTION

[0018] Hereinafter, the above-mentioned embodiments of the present invention will be described with reference to the accompanying drawings, but the technical scope of the present invention should be determined according to the description of the claims, and is not limited to the following methods. It should be noted that, for the sake of convenience of explanation, the dimensional ratios of the accompanying drawings are exaggerated and sometimes different from the actual ratios. Hereinafter, the present invention will be described by taking a form of secondary battery, namely a stacked type (internal parallel type) all-solid-state lithium secondary battery as an example. As described above, the solid electrolyte constituting the all-solid-state lithium secondary battery is a material composed mainly of an ion conductor capable of ion conduction in a solid. Therefore, the all-solid-state lithium secondary battery has the following advantages: in principle, various problems caused by flammable organic electrolytes will not occur like the previous liquid-based lithium secondary batteries. In addition, in general, if a high-potential / large-capacity positive electrode material and a large-capacity negative electrode material are used, the following advantages are also provided: a significant improvement in the output density and energy density of the battery can be achieved.

[0019] One embodiment of the present invention is a positive electrode material, characterized in that it contains: a porous carbon material, a positive electrode active material containing sulfur, and a lithium halide, at least a portion of the positive electrode active material and at least a portion of the lithium halide are arranged in the pores of the porous carbon material. According to the positive electrode material of this embodiment, the internal resistance of the secondary battery can be further reduced.

[0020] According to the present invention, in a secondary battery using a positive electrode active material containing sulfur, the internal resistance of the secondary battery can be further reduced.

[0021] Figure 1 It is a perspective view showing the appearance of a flat laminated all-solid lithium secondary battery as one embodiment of the present invention. Figure 2 It is along Figure 1 The cross-sectional view of the line 2-2 is shown. By making the battery into a stacked type, the battery can be made compact and have a high capacity. It should be noted that in this specification, Figure 1 and Figure 2 The flat stacked non-bipolar lithium secondary battery (hereinafter also referred to as "stacked battery") is used as an example for detailed description. From the perspective of the internal electrical connection form (electrode structure) of the lithium secondary battery described in this embodiment, both non-bipolar (internal parallel type) batteries and bipolar (internal series type) batteries can be applied.

[0022] like Figure 1 As shown, the stacked battery 10a has a rectangular flat shape, and the negative electrode collector plate 25 and the positive electrode collector plate 27 for extracting electricity are led out from both sides thereof. The power generation element 21 is wrapped by the battery outer packaging material (laminated film 29) of the stacked battery 10a, and the surrounding is heat-welded, and the power generation element 21 is sealed in a state where the negative electrode collector plate 25 and the positive electrode collector plate 27 are led outward.

[0023] It should be noted that the lithium secondary battery described in this embodiment is not limited to a stacked flat shape. In a wound lithium secondary battery, it can be a cylindrical shape, or it can be a shape such as a rectangular flat shape that is deformed by deforming the cylindrical shape, etc., without particular limitation. In the above-mentioned cylindrical battery, its outer packaging material can use a laminated film, or a conventional cylindrical can (metal can), etc., without particular limitation. The power generation element is preferably housed inside the aluminum-containing laminated film. Lightweighting can be achieved through this form.

[0024] In addition, about Figure 1 The removal of the collector plates (25, 27) shown in the figure is not particularly limited. The negative collector plate 25 and the positive collector plate 27 can be led out from the same side, or the negative collector plate 25 and the positive collector plate 27 can be divided into multiple parts and taken out from each side, etc. Figure 1 In the case of a wound lithium battery, the terminal may be formed by replacing the tab with a cylindrical can (metal can), for example.

[0025] like Figure 2 As shown, the stacked battery 10a of the present embodiment actually has a structure in which a flat, roughly rectangular power generation element 21 that performs charge and discharge reactions is sealed inside a laminate film 29 that serves as the battery outer packaging material. Here, the power generation element 21 has a structure in which a positive electrode, a solid electrolyte layer 17, and a negative electrode are stacked. The positive electrode has a structure in which a positive electrode active material layer 15 containing a positive electrode active material is arranged on both sides of a positive electrode collector 11". The negative electrode has a structure in which a negative electrode active material layer 13 containing a negative electrode active material is arranged on both sides of a negative electrode collector 11'. Specifically, the positive electrode, the solid electrolyte layer, and the negative electrode are stacked in sequence in such a manner that one positive electrode active material layer 15 is opposite to the negative electrode active material layer 13 adjacent thereto via a solid electrolyte layer 17. Thus, the adjacent positive electrode, solid electrolyte layer, and negative electrode constitute a single battery layer 19. Therefore, it can also be said that Figure 2 The stacked battery 10 a shown has a structure in which a plurality of single cell layers 19 are stacked and electrically connected in parallel.

[0026] like Figure 2 As shown, the outermost negative electrode collectors located at the two outermost layers of the power generation element 21 are each provided with the negative electrode active material layer 13 only on one side, or the active material layer may be provided on both sides. That is, instead of making a collector dedicated to the outermost layer with the active material layer provided on only one side, the collector with the active material layer on both sides may be directly used as the outermost collector. In addition, depending on the situation, the negative electrode active material layer 13 and the positive electrode active material layer 15 may be used as the negative electrode and the positive electrode, respectively, without using the collector (11', 11").

[0027] The negative electrode collector 11' and the positive electrode collector 11" are respectively installed with a negative electrode collector plate (pole tab) 25 and a positive electrode collector plate (pole tab) 27 that are conductive to each electrode (positive electrode and negative electrode), and have a structure that is clamped by the end of a laminate film 29 that serves as the battery outer packaging material and is led out to the outside of the laminate film 29. The positive electrode collector plate 27 and the negative electrode collector plate 25 can be installed on the positive electrode collector 11" and the negative electrode collector 11' of each electrode respectively with the help of a positive electrode lead and a negative electrode lead (not shown) as needed and by ultrasonic welding, resistance welding, etc.

[0028] Hereinafter, main components of the lithium secondary battery according to this embodiment will be described.

[0029] [Current Collector]

[0030] The current collector has the function of mediating the movement of electrons from the electrode active material layer (positive electrode active material layer or negative electrode active material layer). The material constituting the current collector is not particularly limited. As the constituent material of the current collector, for example, metals and conductive resins can be used.

[0031] Specifically, as metals, aluminum, nickel, iron, stainless steel, titanium, copper, etc. can be listed. In addition to these, cladding materials of nickel and aluminum, cladding materials of copper and aluminum, etc. can be used. In addition, it can be a foil formed by covering aluminum on the metal surface. Among them, from the viewpoints of electronic conductivity, battery operating potential, and the adhesion of the negative electrode active material achieved by sputtering the collector, aluminum, stainless steel, copper, and nickel are preferred. In addition, as a resin with conductivity, a resin having a conductive filler added to a non-conductive polymer material can be listed.

[0032] It should be noted that the current collector can be a single-layer structure formed by a single material, or it can be a stacked structure obtained by appropriately combining layers formed by these materials. From the viewpoint of lightweighting the current collector, it is preferred to at least include a conductive resin layer formed by a conductive resin. In addition, from the viewpoint of blocking the movement of lithium ions between single cell layers, a metal layer can be provided on a portion of the current collector. Furthermore, as long as the negative electrode active material layer and the positive electrode active material layer described later are themselves conductive and can perform the current collection function, a current collector that is a component different from these electrode active material layers may not be used. In this way, the negative electrode active material layer described later directly constitutes the negative electrode, and the positive electrode active material layer described later directly constitutes the positive electrode.

[0033] [Negative electrode (negative electrode active material layer)]

[0034] exist Figure 1 and Figure 2In the stacked battery described in the embodiment shown, the negative electrode active material layer 13 contains a negative electrode active material. The type of the negative electrode active material is not particularly limited, and examples thereof include carbon materials, metal oxides, and metal active materials. Examples of carbon materials include natural graphite, artificial graphite, mesophase carbon microbeads (MCMB), highly oriented graphite (HOPG), hard carbon, and soft carbon. In addition, examples of metal oxides include Nb 2 O 5 , Li 4 Ti 5 O 12 Etc. Furthermore, metal active materials such as silicon-based negative electrode active materials and tin-based negative electrode active materials can be used. Here, it is known that silicon and tin belong to Group 14 elements, which are negative electrode active materials that can greatly increase the capacity of non-aqueous electrolyte secondary batteries. These simple substances can absorb and release multiple charge carriers (lithium ions, etc.) per unit volume (mass), and thus become high-capacity negative electrode active materials. Here, as a silicon-based negative electrode active material, Si simple substance is preferably used. In addition, similarly, it is also preferred to use silicon oxides such as SiOx (0.3≤x≤1.6) that are not homogenized into two phases, Si phase and silicon oxide phase. At this time, the range of x is more preferably 0.5≤x≤1.5, and further preferably 0.7≤x≤1.2. Furthermore, alloys containing silicon (silicon-containing alloy-based negative electrode active materials) can also be used. On the other hand, as the negative electrode active material containing tin element (tin-based negative electrode active material), Sn single substance, tin alloy (Cu-Sn alloy, Co-Sn alloy), amorphous tin oxide, tin silicon oxide, etc. can be listed. Among them, as amorphous tin oxide, SnB 0.4 P 0.6 O 3.1 In addition, SnSiO 3 . In addition, as the negative electrode active material, a metal containing lithium can be used. Such a negative electrode active material is not particularly limited as long as it is an active material containing lithium, and in addition to metallic lithium, lithium-containing alloys can also be listed. As lithium-containing alloys, for example, alloys formed by Li and at least one selected from In, Al, Si and Sn can be listed. Depending on the circumstances, two or more negative electrode active materials can be used in combination. It should be noted that it goes without saying that negative electrode active materials other than the above can be used. The negative electrode active material preferably contains metallic lithium, a silicon-based negative electrode active material or a tin-based negative electrode active material, and particularly preferably contains metallic lithium.

[0035] The content of the negative electrode active material in the negative electrode active material layer is not particularly limited, but is, for example, preferably in the range of 40 to 99 mass %, and more preferably in the range of 50 to 90 mass %.

[0036] The negative electrode active material layer preferably further includes a solid electrolyte. By making the negative electrode active material layer include a solid electrolyte, the ion conductivity of the negative electrode active material layer can be improved. Examples of solid electrolytes include sulfide solid electrolytes and oxide solid electrolytes, preferably sulfide solid electrolytes. In this specification, a solid electrolyte refers to a material composed mainly of an ion conductor capable of ion conduction in a solid, and in particular refers to a material having a lithium ion conductivity of 1×10 at room temperature (25°C). -5 Here, the value of ion conductivity can be measured by an alternating current impedance method.

[0037] Examples of sulfide solid electrolytes include LiI-Li 2 S-SiS 2 、LiI-Li 2 SP 2 O 5 、LiI-Li 3 PO 4 -P 2 S 5 , Li 2 SP 2 S 5 、LiI-Li 3 PS 4 、LiI-LiBr-Li 3 PS 4 , Li 3 PS 4 , Li 2 SP 2 S 5 -LiI, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-LiI、Li 2 S-SiS 2 , Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 -LiI, Li 2 S-SiS 2 -P2 S 5 -LiI, Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (wherein m and n are positive numbers, and Z is any one of Ge, Zn, and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (where x and y are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga, and In). 2 SP 2 S 5 "This record refers to the use of Li 2 S and P 2 S 5 The sulfide solid electrolyte formed by the raw material composition is the same as the other descriptions.

[0038] Sulfide solid electrolytes may have, for example, Li 3 PS 4 The skeleton can also have Li 4 P 2 S 7 The skeleton can also have Li 4 P 2 S 6 As a Li 3 PS 4 The sulfide solid electrolyte of the skeleton can be exemplified by LiI-Li 3 PS 4 、LiI-LiBr-Li 3 PS 4 , Li 3 PS 4 In addition, as a Li 4 P 2 S 7 The sulfide solid electrolyte of the skeleton includes, for example, Li-PS solid electrolytes called LPS (e.g., Li 7 P 3 S 11)。In addition, as the sulfide solid electrolyte, for example, Li can be used (4-x) Ge (1-x) P x S 4 such as LGPS represented by (where x satisfies 0 < x < 1). Among them, a sulfide solid electrolyte containing a P element is preferred, and more preferably a material having Li 2 S-P 2 S 5 as the main component. Furthermore, the sulfide solid electrolyte may contain a halogen (F, Cl, Br, I). In a preferred embodiment, the sulfide solid electrolyte contains Li 6 PS 5 X (here, X is Cl, Br, or I, preferably Cl).

[0039] In addition, when the sulfide solid electrolyte is of the Li 2 S-P 2 S 5 system, the ratio of Li 2 S and P 2 S 5 is preferably in the range of Li 2 S:P 2 S 5 = 50:50 to 100:0 in molar ratio, and preferably Li 2 S:P 2 S 5 = 70:30 to 80:20.

[0040] In addition, the sulfide solid electrolyte can be a sulfide glass, a crystallized sulfide glass, or a crystalline material obtained by a solid-phase method. It should be noted that the sulfide glass can be obtained, for example, by mechanically grinding a raw material composition (such as a ball mill). In addition, the crystallized sulfide glass can be obtained, for example, by heat-treating the sulfide glass at a temperature above the crystallization temperature. In addition, the ionic conductivity (e.g., Li ion conductivity) of the sulfide solid electrolyte at room temperature (25 °C) is preferably, for example, 1 × 10 -5 S / cm or more, and more preferably 1 × 10 -4 S / cm or more.

[0041] As the oxide solid electrolyte, for example, a compound having a NASICON-type structure can be cited. As an example of a compound having a NASICON-type structure, a compound represented by the general formula Li 1+x Al x Ge 2-x (PO 4 ) 3 (0 ≤ x ≤ 2) (LAGP), the general formula Li1+x Al x Ti 2-x (PO 4 ) 3 (0≤x≤2) represented by the compound (LATP) and the like. In addition, other examples of oxide solid electrolytes include LiLaTiO (e.g., Li 0.34 La 0.51 TiO 3 ), LiPON (such as Li 2.9 PO 3.3 N 0.46 ), LiLaZrO (e.g. Li 7 La 3 Zr 2 O 12 )wait.

[0042] The content of the solid electrolyte in the negative electrode active material layer is, for example, preferably in the range of 1 to 60 mass %, more preferably in the range of 10 to 50 mass %.

[0043] The negative electrode active material layer may contain at least one of a conductive aid and a binder in addition to the negative electrode active material and the solid electrolyte.

[0044] As the conductive aid, metals such as aluminum, stainless steel (SUS), silver, gold, copper, titanium, alloys containing these metals or metal oxides can be listed; carbon fibers (specifically, vapor grown carbon fibers (VGCF), polyacrylonitrile carbon fibers, pitch carbon fibers, rayon carbon fibers, activated carbon fibers, etc.), carbon nanotubes (CNTs), carbon black (specifically, acetylene black, Ketjen black (registered trademark), furnace black, channel carbon black, thermal lamp black, etc.) and other carbons, but not limited to them. In addition, the material obtained by coating the above-mentioned metal material around the granular ceramic material or resin material by plating can also be used as a conductive aid. Among these conductive aids, from the viewpoint of electrical stability, it is preferred to include at least one selected from the group consisting of aluminum, stainless steel, silver, gold, copper, titanium and carbon, preferably at least one selected from the group consisting of aluminum, stainless steel, silver, gold and carbon, and more preferably at least one carbon. These conductive aids can be used alone or in combination of two or more.

[0045] When the negative electrode active material layer includes a conductive auxiliary agent, the content of the conductive auxiliary agent in the negative electrode active material layer is not particularly limited, and is preferably 0 to 10% by mass, more preferably 2 to 8% by mass, and further preferably 4 to 7% by mass relative to the total mass of the negative electrode active material layer. If it is within this range, a more solid electron conduction path can be formed in the negative electrode active material layer, which can effectively contribute to improving battery characteristics.

[0046] On the other hand, the binder is not particularly limited, and the following materials can be cited, for example: thermoplastic polymers such as polybutylene terephthalate, polyethylene terephthalate, polyvinylidene fluoride (PVDF) (including compounds in which hydrogen atoms are replaced by other halogen elements), polyethylene, polypropylene, polymethylpentene, polybutene, polyether nitrile, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, ethylene-vinyl acetate copolymer, polyvinyl chloride, styrene-butadiene rubber (SBR), ethylene-propylene-diene copolymer, styrene-butadiene-styrene block copolymer and its hydrogenate, styrene-isoprene-styrene block copolymer and its hydrogenate; tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), ethylene-tetrafluoroethylene Fluorine resins such as ethylene-ethylene copolymer (ETFE), polytrifluoroethylene (PCTFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinyl fluoride (PVF), etc.; vinylidene fluoride-hexafluoropropylene fluororubber (VDF-HFP fluororubber), vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene fluororubber (VDF-HFP-TFE fluororubber), vinylidene fluoride-pentafluoropropylene fluororubber (VDF-PFP fluororubber), vinylidene fluoride-pentafluoropropylene-tetrafluoroethylene fluororubber (VDF-PFP-TFE fluororubber), vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene fluororubber (VDF-PFMVE-TFE fluororubber), vinylidene fluoride-chlorotrifluoroethylene fluororubber (VDF-CTFE fluororubber), etc.; epoxy resins, etc. Among them, polyimide, styrene-butadiene rubber, carboxymethyl cellulose, polypropylene, polytetrafluoroethylene, polyacrylonitrile, and polyamide are more preferred.

[0047] The thickness of the negative electrode active material layer varies depending on the structure of the target secondary battery, but is preferably within a range of 0.1 to 1000 μm, for example.

[0048] [Solid electrolyte layer]

[0049] exist Figure 1 and Figure 2 In the stacked battery according to the embodiment shown, the solid electrolyte layer is a layer interposed between the positive electrode active material layer and the negative electrode active material layer and necessarily contains a solid electrolyte.

[0050] The specific form of the solid electrolyte contained in the solid electrolyte layer is not particularly limited, and the solid electrolytes and preferred embodiments thereof exemplified in the negative electrode active material layer can be used in the same manner. Depending on the situation, solid electrolytes other than the above-mentioned solid electrolytes may be used in combination.

[0051] The solid electrolyte layer may contain a binder in addition to the above-mentioned solid electrolyte. The examples and preferred embodiments described in the section of the negative electrode active material layer may be used similarly to the binder that may be contained in the solid electrolyte layer.

[0052] The thickness of the solid electrolyte layer also varies depending on the structure of the target lithium secondary battery. From the perspective of being able to increase the volume energy density of the battery, it is preferably 800 μm or less, more preferably 700 μm or less, and further preferably 600 μm or less. On the other hand, there is no particular restriction on the lower limit of the thickness of the solid electrolyte layer, but it is preferably 1 μm or more, more preferably 5 μm or more, and further preferably 10 μm or more.

[0053] [Positive electrode active material layer]

[0054] Figure 1 and Figure 2 In the stacked battery of the embodiment shown, the positive electrode active material layer includes a positive electrode material of one embodiment of the present invention. The positive electrode material contains: a porous carbon material, a positive electrode active material containing sulfur, and a lithium halide. Moreover, at least a portion of the positive electrode active material and at least a portion of the lithium halide are arranged in the pores of the porous carbon material.

[0055] (Positive electrode active material containing sulfur)

[0056] As the type of sulfur-containing positive electrode active material, there is no particular limitation. In addition to elemental sulfur (S), particles or films of organic sulfur compounds or inorganic sulfur compounds can also be listed, as long as it is a material that can release lithium ions during charging and absorb lithium ions during discharge by utilizing the redox reaction of sulfur. As organic sulfur compounds, disulfide compounds, sulfur-modified polyacrylonitrile represented by compounds described in International Publication No. 2010 / 044437, sulfur-modified polyisoprene, erythromycin (dithiooxamide), polysulfide carbon, etc. can be listed. Among them, disulfide compounds, sulfur-modified polyacrylonitrile and erythromycin are preferred, and sulfur-modified polyacrylonitrile is particularly preferred. As a disulfide compound, it is more preferred to have a dithiodiurea derivative, a thiourea group, a thioisocyanate or a thioamide group. Here, sulfur-modified polyacrylonitrile is a polyacrylonitrile containing sulfur atoms and modified by mixing sulfur powder with polyacrylonitrile and heating it under an inert gas or under reduced pressure. Its presumed structure is, for example, as shown in Chem. Mater. 2011, 23, 5024-5028, a structure in which polyacrylonitrile is ring-closed to form a polycyclic structure, and at least a part of S is bonded to C. The compound described in the document has a Raman spectrum at 1330 cm -1 and 1560cm -1 There is a strong peak signal near 307cm -1 、379cm-1 、472cm -1 、929cm -1 On the other hand, inorganic sulfur compounds are preferred due to their excellent stability, and specific examples include elemental sulfur (S), S-carbon complexes, TiS 2 、TiS 3 、TiS 4 、NiS、NiS 2 , CuS, FeS 2 , Li 2 S、MoS 2 、MoS 3 、MnS、MnS 2 , CoS, CoS 2 Among them, elemental sulfur (S), TiS 2 、TiS 3 、TiS 4 , FeS 2 and MoS 2 , more preferably elemental sulfur (S), TiS 2 and FeS 2 From the viewpoint of high capacity, elemental sulfur (S) is particularly preferred. It should be noted that as elemental sulfur (S), S 8 α-sulfur, β-sulfur or γ-sulfur of the structure.

[0057] The positive electrode material of this embodiment may include a sulfur-containing positive electrode active material and a sulfur-free positive electrode active material (other positive electrode active material). Examples of other positive electrode active materials include LiCoO 2 、LiMnO 2 、LiNiO 2 、LiVO 2 、Li(Ni-Mn-Co)O 2 Layered rock salt type active material; LiMn 2 O 4 、LiNi 0.5 Mn 1.5 O 4 Spinel active materials such as LiFePO 4 、LiMnPO 4 Olivine-type active materials; Li 2 FeSiO 4 , Li 2 MnSiO 4 Other oxide active materials other than the above include Li 4 Ti 5 O 12 .

[0058] According to the circumstances, two or more positive electrode active materials can be used in combination. It should be noted that positive electrode active materials other than the above can also be used. Among them, the proportion of the content of the sulfur-containing positive electrode active material in the total amount of 100% by mass of the positive electrode active material is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, further preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 100% by mass.

[0059] (Lithium Halide)

[0060] The positive electrode material of this mode comprises lithium halide (LiX, X is a halogen atom). As lithium halide, for example, lithium fluoride, lithium chloride, lithium bromide, lithium iodide, etc. can be listed. Among the positive electrode materials of this mode, lithium chloride or lithium iodide is preferred for excellent ion conductivity, and lithium iodide is more preferred. It is also possible to use a combination of two or more lithium halides.

[0061] (Porous Carbon Materials)

[0062] The positive electrode material of this embodiment must contain a carbon material having pores (porous carbon material). The specific form of the porous carbon material contained in the positive electrode material of this embodiment is not particularly limited as long as it is a carbon material having pores, and a conventionally known material can be appropriately used.

[0063] As porous carbon materials, for example, carbon particles (carbon carriers) formed by carbon blacks such as activated carbon, Ketjen black (registered trademark) (highly conductive carbon black), (oil) furnace black, channel black, acetylene black, thermal black, lamp black, coke, natural graphite, artificial graphite, etc. can be listed. In addition, a mold such as ceramic is mixed with a carbon raw material such as a resin, and fired under an inactive atmosphere. After that, the mold is melted with an acid, thereby synthesizing a carbon material with a porous structure having a shape of the mold transferred, which can be used as a carbon material. At this time, by appropriately adjusting the particle size of the mold and the mixing ratio of the carbon raw material, the pore size and pore volume of the porous carbon material obtained can be changed.

[0064] It should be noted that the porous carbon material preferably has carbon as its main component. Here, "main component is carbon" means that it contains carbon atoms as the main component, and is a concept including both being composed of only carbon atoms and being substantially composed of carbon atoms. "Substantially composed of carbon atoms" means that impurities of about 2 to 3 mass % or less can be accepted.

[0065] The BET specific surface area of ​​the porous carbon material is not particularly limited, but is preferably 200 m 2 / g or more, more preferably 500m 2 / g or more, more preferably 800m 2 / g or more, particularly preferably 1200m 2 / g or more, most preferably 1500m 2 / g or more. In addition, the total pore volume of the porous carbon material is preferably 1.0mL / g or more, more preferably 1.3mL / g or more, and further preferably 1.5mL / g or more. If the BET specific surface area and total pore volume of the porous carbon material are values ​​within this range, a sufficient amount of pores can be maintained, and further, a sufficient amount of positive electrode active material can be maintained. It should be noted that the values ​​of the BET specific surface area and total pore volume of the porous carbon material can be measured using nitrogen adsorption-desorption measurement. The nitrogen adsorption-desorption measurement was performed using BELSORP mini manufactured by MICROTRAC BEL, and was performed by a multi-point method at a temperature of -196°C. According to 0.01 <P / P 0 The BET specific surface area was calculated from the adsorption isotherm in the relative pressure range of 0.05. In addition, the total pore volume was calculated from the adsorption N 2 Calculate the volume of .

[0066] The average pore size of the porous carbon material is not particularly limited, and is preferably less than 100 nm, more preferably less than 50 nm, and particularly preferably less than 30 nm. If the average pore size of the porous carbon material is a value within these ranges, the contact area with the positive electrode active material or lithium halide can be increased, and the reaction area can be increased. In addition, electrons can be fully supplied to the active material that is present in the sulfur-containing positive electrode active material disposed inside the pore and is located away from the pore wall. As a result, the effect of the present invention can be more significantly obtained. It should be noted that the value of the average pore size of the porous carbon material can be calculated based on nitrogen adsorption and desorption measurements in the same way as the value of the BET specific surface area and the total pore volume. In this specification, the pore distribution of the porous carbon material is obtained by the BJH method. It should be noted that there is no special restriction on the lower limit of the average pore size of the porous carbon material, for example, it is greater than 1 nm.

[0067] In the positive electrode material of this embodiment, the porous carbon material preferably has pores with a pore diameter in the range of 1 to 100 nm. In addition, among the pores of the porous carbon material, the percentage of the pore volume of the pores with a pore diameter in the range of 1 to 4 nm relative to the pore volume of the pores with a pore diameter in the range of 1 to 100 nm is preferably 20% or less. As a result, the positive electrode active material and / or lithium halide can be easily retained until the inside of the hole. In addition, inside the hole, on the surface of the positive electrode active material, not only can the electrons of the porous carbon material enter and exit smoothly, but also the charge carriers of the lithium halide can enter and exit smoothly. As a result, the three-phase interface where the positive electrode active material, the porous carbon material and the lithium halide coexist is fully formed around the positive electrode active material located deep in the hole, and the charge and discharge reaction can be fully carried out. As a result, it is believed that the internal resistance of the battery is further reduced. It should be noted that from the perspective of further exerting the effect of reducing the internal resistance, the value of the above percentage is more preferably less than 18%, further preferably less than 15%, further more preferably less than 12%, and particularly preferably less than 9%. On the other hand, the lower limit of the percentage is not particularly limited, but is, for example, 3% or more.

[0068] The average particle size (primary particle size) of the porous carbon material is not particularly limited, and is preferably 0.05 to 50 μm, more preferably 0.1 to 20 μm, and further preferably 0.5 to 10 μm. It should be noted that in this specification, the "particle size of the porous carbon material" refers to the maximum distance L between any two points on the contour line of the particles of the porous carbon material. The value of the "average particle size of the porous carbon material" is calculated as the arithmetic mean of the particle sizes observed in several to dozens of fields of view using observation means such as a scanning electron microscope (SEM) and a transmission electron microscope (TEM).

[0069] The positive electrode material of this embodiment contains the porous carbon material, the positive electrode active material containing sulfur, and the lithium halide as described above, and at least a part of the positive electrode active material and at least a part of the lithium halide are arranged in the pores of the porous carbon material.

[0070] Figure 3 (a) is a cross-sectional schematic diagram of a conventional positive electrode material 100'. Figure 3 (b) is a schematic cross-sectional view of a positive electrode material 100 according to an embodiment of the present invention. Figure 3 (a) and Figure 3 In (b), the porous carbon material 110 has a large number of pores 110 a , and the interior of the pores 110 a is filled with the positive electrode active material 120 containing sulfur.

[0071] However, using Figure 3When the electrode is made of the positive electrode material 100' of (a), the reaction resistance of the electrode reaction is high. This is considered to be because the positive electrode active material 120 containing sulfur has low conductivity, and in addition, during the electrode reaction, the positive electrode active material 120 generates Li with low ion conductivity near the interface 140 between it and the solid electrolyte 130. 2 S increases the resistance to the diffusion of lithium ions in the positive electrode material.

[0072] In contrast, in the positive electrode material 100 of the present invention, lithium halide 150 is present inside the pores 110a of the porous carbon material 110. As a result, an ion conduction path that is conducive to the movement of lithium ions can be constructed in the positive electrode active material 120, and lithium ions can be efficiently introduced into the pores 110a of the porous carbon material 110 with the help of lithium halide 150. Moreover, on the surface of the positive electrode active material 120 located deep in the pores 110a, not only can the entry and exit of electrons with the help of the porous carbon material 110 be smoothly carried out, but also the entry and exit of lithium ions from the solid electrolyte 130 with the help of lithium halide 150 can be smoothly carried out. Therefore, in the positive electrode material 100 of the present invention, a reaction area is formed in which the positive electrode active material 120, the lithium halide 150, and the porous carbon material 110 coexist on the surface of the porous carbon material 110 and inside the pores 110a, and the electrode reaction can be fully carried out. As a result, it is considered that the positive electrode active material 120 existing in the inside of the pore 110 a can also be used as an active material for the electrode reaction, thereby sufficiently reducing the internal resistance of the battery.

[0073] In addition, the charge and discharge reaction of a battery using a general positive electrode material containing sulfur is represented by the following formula (1), while the charge and discharge reaction of a battery using the positive electrode material of the present invention is represented by the following formula (2). That is, as shown in formula (2), the number of electrons participating in the reaction increases, so it is believed that the exchange of electrons is promoted, the reaction of sulfur is promoted, and the battery reaction can be carried out more efficiently.

[0074] Existing cathode materials;

[0075]

[0076] The positive electrode material of the present invention:

[0077]

[0078] Here, for the confirmation of whether the positive electrode active material and lithium halide are configured inside the pores of the porous carbon material, various methods known in the past can be used. For example, based on the observation image of the cross section of the porous carbon material by transmission electron microscopy (TEM), energy dispersive X-ray spectroscopy (EDX) is used to perform element mapping from each material, and the count of the elements from each material relative to the count of all elements is used as an index to confirm the configuration of each material.

[0079] In the positive electrode material of this method, preferably, the lithium halide is more present inside the pores than outside the pores of the porous carbon material (i.e., the surface of the particles of the porous carbon material). Thus, the conductive path of lithium ions can be more advantageously constructed in the positive electrode material, thereby further reducing the internal resistance of the battery.

[0080] In addition, the positive electrode material of the present embodiment is preferably that in the X-ray diffraction measurement using CuKα rays of the positive electrode material, between the two strongest peaks belonging to the peak of lithium halide, there is a crystallization peak that does not belong to any of the porous carbon material, the positive electrode active material containing sulfur, and the lithium halide. That is, it is preferred that there is a new peak that does not belong to any of the raw materials (starting materials). The details are unclear, but it is believed that the crystal structure providing the new peak advantageously promotes the movement of ions and contributes to the reduction of resistance.

[0081] In the positive electrode material of the present invention, the content of lithium halide is, for example, 4% by mass or more, preferably 5% by mass or more and less than 50% by mass relative to the total mass of the positive electrode material. If the content of lithium halide is within the above range, sufficient resistance reduction effect can be easily obtained. More preferably, the content of lithium halide is 5 to 30% by mass, further preferably 10 to 30% by mass, and further more preferably 20 to 30% by mass. It should be noted that when two or more lithium halides are used in combination, the total amount is preferably within the above range.

[0082] The mass ratio of the positive electrode active material containing sulfur and the lithium halide in the positive electrode material of this embodiment is not particularly limited, for example, positive electrode active material: lithium halide = 100: 1 to 100: 10000. The above mass ratio is preferably positive electrode active material: lithium halide = 100: 1 to 100: 100, more preferably 100: 1 to 100: 50, and further preferably 100: 5 to 100: 45. If it is within the above range, the amount of positive electrode active material can be fully ensured, so a high-performance battery can be obtained. In addition, the ion conductivity of the positive electrode material can be ensured, and an ion conductive network is fully formed in the pores, so it is preferred.

[0083] In the positive electrode material of this embodiment, the mass ratio of the positive electrode active material containing sulfur to the porous carbon material is not particularly limited, and for example, the ratio (positive electrode active material containing sulfur / porous carbon material) is 0.5 to 10, preferably 2 to 8. Within the above range, the effects of the present invention can be more significantly obtained.

[0084] It should be noted that, in the positive electrode material of this method, there is no particular limitation, and it is preferred that the inside of the pores of the porous carbon material is filled with a solid electrolyte. Solid electrolytes are expensive, and in addition, they are very reactive with water. Therefore, when operating solid electrolytes, it is necessary not to be exposed to the atmospheric environment, such as an environment with a low dew point (dew point <-60°C), and a glove box or a super dry room must be used. The positive electrode material of this method is configured with lithium halide and the positive electrode active material inside the pores of the porous carbon material, so that an ion conduction path that is conducive to the movement of lithium ions can be constructed even if a solid electrolyte is not used. In addition, without using a solid electrolyte, it can be made cheaply in an atmospheric environment, and the equipment and the surrounding environment can be simplified. For the positive electrode material of this method, the content of the solid electrolyte in the components filled into the pores of the porous carbon material is preferably 3% by mass or less, more preferably 2% by mass or less, further preferably 1% by mass or less, and most preferably 0% by mass.

[0085] It should be noted that the positive electrode material of this embodiment is preferably filled with only a positive electrode active material containing sulfur and a lithium halide in the pores of the porous carbon material. In this way, the effect of the present invention can be more significantly obtained. In the positive electrode material of this embodiment, the total content of the positive electrode active material containing sulfur and the lithium halide in the components filled into the pores of the porous carbon material is preferably 95% by mass, more preferably 99% by mass or more, and most preferably 100% by mass.

[0086] The method for producing the positive electrode material of the present embodiment having the above-described structure is not particularly limited, and the following (Production Method 1) or (Production Method 2) can be preferably used. In particular, according to (Production Method 1), the effect of reducing the reaction resistance is more excellent.

[0087] (Manufacturing method 1)

[0088] In manufacturing method 1, first, lithium halide is introduced into the interior of the pores of the porous carbon material by solution infiltration. Next, the porous carbon material having lithium halide in the interior of the pores is further hot-infiltrated with a positive electrode active material containing sulfur and arranged in the interior of the pores of the porous carbon material. Specifically, first, a solution in which lithium halide is dissolved in a solvent is prepared, and the porous carbon material is dispersed therein to obtain a dispersion. As solvents, for example, water; alcohols such as methanol, ethanol, 1-propanol, 2-propanol, ethylene glycol, glycerol, octanol, lauryl alcohol, myristyl alcohol, cetyl alcohol, stearyl alcohol, oleyl alcohol, and linolenic alcohol; ethers such as ether, tetrahydrofuran, 1,4-dioxane, and 1,3-dioxolane; etc. In view of the high solubility of lithium halide, water or alcohols are preferred as solvents, and alcohols are more preferred. Thereafter, after removing the solvent, heat treatment is performed at a temperature of about 150 to 250°C for about 1 to 5 hours. Thus, a porous carbon material impregnated with lithium halide in the interior of the hole is obtained. Then, the porous carbon material impregnated with lithium halide in the interior of the hole is mixed with the positive electrode active material in a dry manner, and further heat treated under the same conditions as above. Thus, the positive electrode active material melts and penetrates into the interior of the pores of the porous carbon material, and a positive electrode material as a composite material in which lithium halide and positive electrode active material are simultaneously configured (filled) in the interior of the pores of the porous carbon material can be obtained.

[0089] (Manufacturing method 2)

[0090] In manufacturing method 2, first, a positive electrode active material containing sulfur is introduced into the interior of the pores of a porous carbon material by heat infiltration. Next, for the porous carbon material having a positive electrode active material in the interior of the pores, a lithium halide is further infiltrated with a solution and arranged in the interior of the pores of the porous carbon material. Specifically, first, the porous carbon material is mixed with the positive electrode active material in a dry manner, and a heat treatment is performed at a temperature of about 150 to 250°C for about 1 to 5 hours. Thus, a porous carbon material in which the interior of the pores is infiltrated with a positive electrode active material is obtained. Next, a solution in which lithium halide is dissolved in a solvent is prepared, and a porous carbon material in which the interior of the pores is infiltrated with a positive electrode active material is dispersed therein to obtain a dispersion. The specific example of the solvent is the same as above. Thereafter, after removing the solvent, a heat treatment is performed under the same conditions as above. Thus, a positive electrode material as a composite material in which lithium halide and a positive electrode active material are simultaneously arranged (filled) in the interior of the pores of a porous carbon material can be obtained.

[0091] It should be noted that the pore size of the porous carbon material is nanometer-scale. Therefore, only by mechanically mixing the lithium halide with the porous carbon material in a solid state, the lithium halide cannot be configured inside the pores of the porous carbon material. In this case, the lithium halide is only attached to the surface of the particles of the porous carbon material. Similarly, even if the lithium halide is mechanically mixed with the porous carbon material with the positive electrode active material in a solid state, the lithium halide cannot be introduced into the interior of the pores of the porous carbon material. In addition, with respect to the positive electrode active material, it is also impossible to introduce it into the pores of the porous carbon material by mechanical mixing only in a solid state.

[0092] The content of the positive electrode active material in the positive electrode active material layer is not particularly limited, and is preferably within the range of 35 to 99 mass %, and more preferably within the range of 40 to 90 mass %. It should be noted that the value of the content is calculated based on the mass of the positive electrode active material alone, excluding the porous carbon material and the lithium halide from the positive electrode material.

[0093] In addition, the positive electrode active material layer may further include a conductive aid (the positive electrode active material and the solid electrolyte are not kept inside the pores) and / or a binder, and the specific methods and preferred methods thereof may be similarly described in the above-mentioned negative electrode active material layer column. Similarly, the positive electrode active material layer preferably further includes a solid electrolyte, and particularly preferably further includes a sulfide solid electrolyte. Regarding the specific methods and preferred methods of solid electrolytes such as sulfide solid electrolytes, the contents described in the above-mentioned negative electrode active material layer column may also be similarly used.

[0094] The thickness of the positive electrode active material layer varies depending on the structure of the target secondary battery, but is preferably within a range of 0.1 to 1000 μm, for example.

[0095] [Positive electrode collector plate and negative electrode collector plate]

[0096] The material constituting the collector plate (25, 27) is not particularly limited, and a known high-conductivity material used in the past as a collector plate for a secondary battery can be used. As the constituent material of the collector plate, metal materials such as aluminum, copper, titanium, nickel, stainless steel (SUS), and their alloys are preferred. From the viewpoint of light weight, corrosion resistance, and high conductivity, aluminum and copper are more preferred, and aluminum is particularly preferred. It should be noted that the positive collector plate 27 and the negative collector plate 25 can use the same material or different materials.

[0097] [Positive lead and negative lead]

[0098] In addition, although the figure is omitted, the collector and the collector plate can be electrically connected by means of a positive lead and a negative lead. As the constituent materials of the positive and negative leads, the materials used in known lithium secondary batteries can be used in the same manner. It should be noted that the part taken out from the outer package is preferably covered with a heat-resistant insulating heat shrink tube, etc., so that it does not contact peripheral equipment, wiring, etc. and leak electricity or does not affect the product (such as automotive parts, especially electronic equipment, etc.).

[0099] [Battery outer packaging materials]

[0100] As the battery outer packaging material, in addition to the known metal can shell, you can also use Figure 1 and Figure 2 A bag-shaped shell obtained by using an aluminum-containing laminate film 29 that can cover the power generation element as shown. The laminate film can use, for example, a three-layer structure laminate film in which polypropylene (PP), aluminum, and nylon are stacked in sequence, but is not limited to them. From the perspective of high output, excellent cooling performance, and being suitable for batteries for large equipment for EV and HEV, the outer packaging material is ideally a laminate film. In addition, from the perspective of being able to easily adjust the group pressure applied to the power generation element from the outside, the outer packaging material is more preferably an aluminum-containing laminate film.

[0101] The stacked battery according to this embodiment has a structure in which a plurality of single cell layers are connected in parallel, so that the capacity is high and the cycle durability is excellent. Therefore, the stacked battery according to this embodiment can be suitably used as a driving power source for EVs and HEVs.

[0102] An embodiment of the lithium secondary battery has been described above, but the present invention is not limited to the configuration described in the above embodiment, and can be modified appropriately based on the description of the claims.

[0103] For example, as a type of battery using the lithium secondary battery described in the present invention, a bipolar battery comprising a bipolar electrode can also be listed, wherein the bipolar electrode has a positive electrode active material layer electrically connected to one side of the collector and a negative electrode active material layer electrically connected to the opposite side of the collector.

[0104] In addition, the secondary battery described in this embodiment may not be a fully solid-state battery. That is, the solid electrolyte layer may further contain a known liquid electrolyte (electrolyte). There is no particular limitation on the amount of liquid electrolyte (electrolyte) that may be contained in the solid electrolyte layer, but it is preferred that the shape of the solid electrolyte layer formed by the solid electrolyte is maintained, and the amount of the liquid electrolyte (electrolyte) does not leak.

[0105] The present invention includes the following schemes and methods:

[0106] 1. A positive electrode material, characterized in that it contains: a porous carbon material, a positive electrode active material containing sulfur and a lithium halide, wherein at least a portion of the positive electrode active material and at least a portion of the lithium halide are arranged in the pores of the porous carbon material;

[0107] 2. The positive electrode material according to 1. above, wherein, in an X-ray diffraction measurement, between the two strongest peaks belonging to the lithium halide, there exists a crystal peak that does not belong to any of the porous carbon material, the positive electrode active material and the lithium halide;

[0108] 3. The positive electrode material according to 1. or 2. above, wherein the content of the lithium halide is 5% by mass or more and less than 50% by mass;

[0109] 4. The positive electrode material according to any one of 1. to 3. above, wherein the lithium halide is present more inside the pores than outside the pores of the porous carbon material;

[0110] 5. The positive electrode material according to any one of 1. to 4. above, wherein the average pore diameter of the porous carbon material is 100 nm or less;

[0111] 6. The positive electrode material according to any one of 1. to 5. above, wherein the percentage of the pore volume of pores with a pore diameter in the range of 1 to 4 nm in the pores of the porous carbon material relative to the pore volume of pores with a pore diameter in the range of 1 to 100 nm is 20% or less;

[0112] 7. A secondary battery comprising the positive electrode material according to any one of 1. to 6. above.

[0113] Example

[0114] The present invention will be described in more detail below by way of examples, but the technical scope of the present invention is not limited to the following examples.

[0115] 《Example of making a test battery cell》

[0116] [Example 1]

[0117] (Preparation of positive electrode materials)

[0118] In a glove box with an argon atmosphere below -68°C dew point, 1.0 g of lithium iodide (manufactured by FUJIFILM Wako Chemicals Corporation, LiI) was added to 33 mL of super dehydrated ethanol (manufactured by FUJIFILM Wako Chemicals Corporation), and stirred until the solution became transparent to dissolve LiI in ethanol. 0.50 g of powder of porous carbon material (manufactured by Toyo Tanso Co., Ltd., Cnovel (registered trademark) P(3)010) was added to the obtained solution, and stirred thoroughly to disperse the porous carbon material thoroughly in the solution. The container containing the dispersion was connected to a vacuum device, and the dispersion in the container was stirred with a magnetic stirrer while a reduced pressure state of less than 1 Pa was formed in the container with an oil rotary pump. Ethanol as a solvent evaporates under reduced pressure, so that ethanol is removed over time, and the porous carbon material impregnated with LiI remains in the container. After the ethanol was removed under reduced pressure in this manner, the mixture was heated to 180° C. under reduced pressure and heat treated for 3 hours to prepare a LiI-impregnated porous carbon material.

[0119] Here, for the porous carbon material used in this example, the average pore size was measured by nitrogen adsorption-desorption measurement before the above treatment. The nitrogen adsorption-desorption measurement was performed using a BELSORP mini manufactured by Microtrac BEL Corp. at a temperature of -196°C by a multipoint method. <P / P 0 The BET specific surface area was calculated by the multi-point method based on the adsorption isotherms in the range of relative pressure <0.05. For the total pore volume, the adsorption N 2 The pore size distribution is determined by the BJH method. The average pore size d is determined by assuming cylindrical pores, based on the BET specific surface area S and the total pore volume V, and using d=4V / S. As a result, the average pore size of the porous carbon material used in this example is 10 nm.

[0120] The pore size distribution in the pore size range of 1 to 100 nm was measured according to the BJH method, and the percentage of the pore volume in the pore size range of 1 to 4 nm relative to the pore volume in the pore size range of 1 to 100 nm was calculated to be 9%.

[0121] Next, in a glove box of an argon atmosphere with a dew point of -68°C or less, 0.938 g of sulfur (manufactured by Aldrich) was added to 0.563 g of the LiI-impregnated porous carbon material prepared above, and after being fully mixed with an agate mortar, the mixed powder was placed in a sealed pressure-resistant autoclave container and heated at 170°C for 3 hours to melt the sulfur and infiltrate the LiI-impregnated porous carbon material. Thus, a porous carbon material filled with sulfur and LiI in the pores was prepared as a positive electrode material.

[0122] (TEM-EDX measurement)

[0123] It should be noted that, for the positive electrode material prepared in this example, it was confirmed by TEM-EDX that sulfur and lithium iodide were arranged inside the pores of the porous carbon material.

[0124] Specifically, a plasma focused ion beam processing device (Helios G4PFIB CXe manufactured by Thermo Scientific, accelerating voltage: 30 kV) is used to thin the powder particles of the positive electrode material to a thickness of about 100 nm. The thinned observation sample is transported to a TEM device (JEOL, multifunctional analytical transmission electron microscope JEM-F200, accelerating voltage: 200 kV) without being exposed to the atmosphere to confirm the fine structure, and the EDX device attached to the TEM (energy dispersive X-ray emission spectrometer, JEOL, Dual SDD, accelerating voltage: 200 kV) is used to obtain elemental image data corresponding to the part inside the particle (characteristic X-ray measurement energy band of EDX mapping: 0-5 keV). From the obtained elemental image data, it is confirmed that sulfur and lithium iodide are arranged inside the pores of the porous carbon material. It should be noted that in this embodiment, iodine or sulfur is used as a marker element to determine whether lithium iodide or the positive electrode active material is filled into the pores of the porous carbon material. It was also confirmed that lithium iodide was arranged more inside the pores of the porous carbon material than outside the pores. It should be noted that for lithium iodide, either iodine or lithium may be detected as a labeling element.

[0125] (Powder X-ray diffraction measurement)

[0126] The positive electrode material obtained above was subjected to powder X-ray diffraction measurement. The measurement was performed using SmartLab manufactured by Rigaku Corporation under the following conditions:

[0127] Scanning speed (2θ / θ): 2° / min

[0128] Step width (2θ / θ): 0.02°

[0129] Radiation source: CuKα:

[0130] The XRD spectrum of the positive electrode material obtained in this example is shown in Figure 4For comparison, the XRD spectrum of a sample obtained by hot-impregnating only elemental sulfur into a porous carbon material according to the same method as above and the XRD spectrum of LiI are shown together. In the positive electrode material obtained in this example, a new peak (indicated by the arrow) that does not belong to any of the starting materials is observed between the two strongest peaks shown in ▼ among the peaks belonging to LiI.

[0131] (Preparation of positive electrode mixture)

[0132] In a glove box with an argon atmosphere at a dew point of -68°C or less, 40 g of zirconia balls with a diameter of 5 mm, 0.762 g of the positive electrode material prepared above, and 0.238 g of a solid electrolyte (Li6PS 5Cl, manufactured by Ampcera) were placed in a 45 mL zirconia container, and a planetary ball mill (Premium line P-7, manufactured by Fritsch) was used to process at 370 rpm for 6 hours to obtain a powder of a positive electrode mixture. The composition of the obtained positive electrode mixture was set to sulfur: lithium iodide: solid electrolyte: porous carbon material = 48:19:24:10 (mass ratio).

[0133] (Fabrication of a test battery cell (all-solid lithium secondary battery))

[0134] The battery was fabricated in a glove box with an argon atmosphere at a dew point of -68°C or less.

[0135] A SUS cylindrical convex punch (10 mm in diameter) was inserted into one side of a glass ceramic cylindrical tube jig (tube inner diameter 10 mm, outer diameter 23 mm, height 20 mm), and a sulfide solid electrolyte (Ampcera, Li 6 PS 5Cl) 80mg. After that, another SUS cylindrical convex punch was inserted to clamp the sulfide solid electrolyte, and a hydraulic press was used to press at a pressure of 75MPa for 3 minutes, thereby forming a solid electrolyte layer with a diameter of 10mm and a thickness of about 0.6mm in the cylindrical tube fixture. Next, the cylindrical convex punch inserted from the upper side was temporarily pulled out, and 7.5mg of the positive electrode mixture prepared above was placed on one side of the solid electrolyte layer in the cylindrical tube, and the cylindrical convex punch (also a positive electrode collector) was inserted from the upper side again, and pressed at a pressure of 300MPa for 3 minutes, thereby forming a positive electrode active material layer with a diameter of 10mm and a thickness of about 0.06mm on one side of the solid electrolyte layer. Next, the cylindrical convex punch on the lower side (which also serves as the negative electrode collector) was pulled out, and as the negative electrode, a lithium foil (manufactured by The Nilaco Corporation, with a thickness of 0.20 mm) punched out to a diameter of 8 mm and an indium foil (manufactured by The Nilaco Corporation, with a thickness of 0.30 mm) punched out to a diameter of 9 mm were overlapped and placed from the lower side of the cylindrical tube jig in a manner such that the indium foil was located on one side of the solid electrolyte layer. The cylindrical convex punch was inserted again, and pressing was performed at a pressure of 75 MPa for 3 minutes to form a lithium-indium negative electrode.

[0136] As described above, a test battery cell (all-solid lithium secondary battery) was prepared in which a negative electrode collector (punch), a lithium-indium negative electrode, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode collector (punch) were stacked in this order.

[0137] [Example 2]

[0138] (Preparation of positive electrode materials)

[0139] In a glove box with an argon atmosphere at a dew point of -68°C or less, 2.5 g of sulfur (manufactured by Aldrich) as a positive electrode active material and 0.5 g of a porous carbon material powder (manufactured by Toyo Tanso Co., Ltd., Cnovel (registered trademark) P(3)010) were fully mixed in an agate mortar, and the mixed powder was placed in a sealed pressure-resistant autoclave container and heated at 170°C for 3 hours to melt the sulfur and infiltrate the porous carbon material with sulfur. Thus, a sulfur-impregnated porous carbon material was prepared.

[0140] In a glove box with an argon atmosphere below -68°C dew point, 1.0 g of lithium iodide (manufactured by FUJIFILM Wako Chemicals Corporation, LiI) was added to 33 mL of super dehydrated ethanol (manufactured by FUJIFILM Wako Chemicals Corporation), and stirred until the solution became transparent to dissolve LiI in ethanol. 3.0 g of the sulfur-impregnated porous carbon material prepared above was added to the obtained solution, and stirred thoroughly to disperse the sulfur-impregnated porous carbon material in the solution. The container containing the dispersion was connected to a vacuum device, and the dispersion in the container was stirred with a magnetic stirrer while an oil rotary pump was used to form a reduced pressure state of less than 1 Pa in the container. Ethanol as a solvent evaporates under reduced pressure, so that ethanol is removed over time, and the porous carbon material filled with sulfur and LiI in the pores remains in the container. After the ethanol is removed under reduced pressure in this way, it is heated to 180°C under reduced pressure and heat treated for 3 hours to prepare a positive electrode material.

[0141] Except for the above, an all-solid lithium secondary battery was prepared in the same manner as in Example 1. In Example 2, the composition of the positive electrode mixture was sulfur: lithium iodide: solid electrolyte: porous carbon material = 48:19:24:10 (mass ratio).

[0142] [Example 3]

[0143] In the preparation of the positive electrode material of Example 1, 1.0 g of lithium iodide in the preparation of the LiI-impregnated porous carbon material is changed to 0.5 g. In addition, 2.5 g of sulfur is impregnated into the obtained 1.0 g of LiI-impregnated porous carbon material. In addition to the above, the above method is the same as Example 1 to prepare an all-solid lithium secondary battery. It should be noted that in Example 3, the composition of the positive electrode mixture is set to sulfur: lithium iodide: solid electrolyte: porous carbon material = 55:11:24:11 (mass ratio).

[0144] [Example 4]

[0145] In the preparation of the positive electrode material of Example 1, 1.0 g of lithium iodide in the preparation of the LiI-impregnated porous carbon material was changed to 0.15 g. In addition, 2.5 g of sulfur was impregnated into 0.65 g of the obtained LiI-impregnated porous carbon material. In addition to the above, the above method was used to prepare an all-solid lithium secondary battery in the same manner as in Example 1. It should be noted that in Example 4, the composition of the positive electrode mixture was set to sulfur: lithium iodide: solid electrolyte: porous carbon material = 60:4:24:12 (mass ratio).

[0146] [Example 5]

[0147] In the preparation of the positive electrode material, the super dehydrated ethanol was changed to ultrapure water, and the all-solid lithium secondary battery was prepared according to the same method as in the above-mentioned Example 1. It should be noted that in Example 5, the composition of the positive electrode mixture was set to sulfur: lithium iodide: solid electrolyte: porous carbon material = 48:19:24:10 (mass ratio).

[0148] In the positive electrode materials prepared in Examples 2 to 5, according to the same TEM-EDX measurement as above, it was confirmed that sulfur and lithium iodide were arranged inside the pores of the porous carbon material. In addition, it was confirmed that lithium iodide was arranged inside the pores more than outside the pores of the porous carbon material. Furthermore, in the positive electrode materials prepared in Examples 2 to 5, as described above, a new peak was observed between the two strongest peaks belonging to LiI in the XRD spectrum. It was confirmed that in Examples 3 and 4, the intensity of the new peak decreased as the content of lithium iodide decreased.

[0149] [Example 6]

[0150] In the preparation of the positive electrode material, lithium iodide was replaced with lithium chloride (LiCl), and an all-solid lithium secondary battery was prepared according to the same method as in Example 1. It should be noted that in Example 6, the composition of the obtained positive electrode mixture was sulfur: lithium chloride: solid electrolyte: porous carbon material = 48:19:24:10 (mass ratio).

[0151] In the positive electrode material prepared in Example 6, the same TEM-EDX measurement as above confirmed that sulfur and lithium chloride were arranged inside the pores of the porous carbon material. It was also confirmed that lithium chloride was arranged more inside the pores of the porous carbon material than outside the pores.

[0152] The XRD spectrum of the positive electrode material obtained in Example 6 was measured in the same manner as above. The results are shown in Figure 5 For comparison, the XRD spectrum of the sample obtained by thermally impregnating only elemental sulfur into the porous carbon material and the XRD spectrum of LiCl are shown together. In the positive electrode material obtained in Example 6, a new peak (indicated by the arrow) not belonging to any of the starting materials was observed between the two strongest peaks indicated by ▼ among the peaks belonging to LiCl.

[0153] [Example 7]

[0154] In the preparation of the positive electrode material, lithium iodide was replaced with lithium bromide (LiBr), and an all-solid lithium secondary battery was prepared according to the same method as in Example 1. It should be noted that in Example 7, the composition of the obtained positive electrode mixture was set to sulfur: lithium bromide: solid electrolyte: porous carbon material = 48:19:24:10 (mass ratio).

[0155] In the positive electrode material prepared in Example 7, according to the same TEM-EDX measurement as above, it was confirmed that sulfur and lithium bromide were arranged inside the pores of the porous carbon material. In addition, it was confirmed that lithium bromide was arranged inside the pores more than the outside of the pores of the porous carbon material. Further, for the positive electrode material obtained in Example 7, the XRD spectrum was measured in the same manner as above. In the positive electrode material obtained in Example 7, in the XRD spectrum, among the peaks belonging to LiBr, a new peak not belonging to any of the starting materials was observed between the two strongest peaks.

[0156] [Example 8]

[0157] In the preparation of the positive electrode material, lithium iodide was replaced with lithium fluoride (LiF), and an all-solid lithium secondary battery was prepared according to the same method as in Example 1. It should be noted that in Example 8, the composition of the obtained positive electrode mixture was sulfur: lithium fluoride: solid electrolyte: porous carbon material = 48:19:24:10 (mass ratio).

[0158] In the positive electrode material prepared in Example 8, according to the same TEM-EDX measurement as above, it was confirmed that sulfur and lithium fluoride were configured inside the pores of the porous carbon material. In addition, it was confirmed that lithium fluoride was more configured inside the pores than the outside of the pores of the porous carbon material. Further, for the positive electrode material obtained in Example 8, the XRD spectrum was measured in the same manner as above. In the positive electrode material obtained in Example 8, in the XRD spectrum, a new peak that does not belong to any of the starting materials was observed between the two strongest peaks in the peaks belonging to LiF.

[0159] [Comparative Example 1]

[0160] In a glove box of argon atmosphere with a dew point below -68°C, 40 g of zirconia balls with a diameter of 5 mm, 2.5 g of sulfur (manufactured by Aldrich), 0.5 g of powder of porous carbon material (manufactured by Toyo Tanso Co., Ltd., Cnovel (registered trademark) P(3)010) and 1.0 g of lithium iodide (manufactured by FUJIFILM Wako Chemicals Corporation, LiI) were placed in a 45 ml zirconia container, and the mixture was treated at 370 rpm for 6 hours using a planetary ball mill to obtain a positive electrode material of a sulfur / LiI / porous carbon material mixed powder. Except for the above, an all-solid lithium secondary battery was prepared in the same manner as in Example 1. It should be noted that in Comparative Example 1, the composition of the obtained positive electrode mixture was set to sulfur: lithium iodide: solid electrolyte: porous carbon material = 48:19:24:10 (mass ratio).

[0161] In the positive electrode material prepared in Comparative Example 1, TEM-EDX measurement was performed in the same manner as above. As a result, lithium iodide was present outside the pores of the porous carbon material and was not arranged inside the pores.

[0162] The XRD spectrum of the positive electrode material obtained in Comparative Example 1 was measured in the same manner as above. The results are shown in Figure 6 For comparison, the XRD spectra of elemental sulfur and the XRD spectra of the positive electrode material of Example 1 are shown together. In the positive electrode material of Comparative Example 1, peaks derived from starting materials such as elemental sulfur and LiI were observed, but no new peak was observed between the two strongest peaks attributable to LiI.

[0163] [Comparative Example 2]

[0164] In a glove box with an argon atmosphere at a dew point below -68°C, 40 g of zirconia balls with a diameter of 5 mm, 2.5 g of sulfur (manufactured by Aldrich), 0.5 g of porous carbon material powder (manufactured by Toyo Tanso Co., Ltd., Cnovel (registered trademark) P(3)010) and 1.0 g of lithium chloride (LiCl) were placed in a 45 ml zirconia container, and treated at 370 rpm for 6 hours using a planetary ball mill to obtain a positive electrode material belonging to a sulfur / LiCl / porous carbon material mixed powder. In addition to the above, an all-solid lithium secondary battery was prepared according to the same method as Example 1. It should be noted that in Comparative Example 2, the composition of the obtained positive electrode mixture was set to sulfur: lithium chloride: solid electrolyte: porous carbon material = 48:19:24:10 (mass ratio).

[0165] In the positive electrode material prepared in Comparative Example 2, TEM-EDX measurement was performed in the same manner as above. As a result, lithium chloride was present outside the pores of the porous carbon material and was not arranged inside the pores.

[0166] The XRD spectrum of the positive electrode material obtained in Comparative Example 2 was measured in the same manner as above. The results are shown in Figure 7 For comparison, the XRD spectra of elemental sulfur and the XRD spectra of the positive electrode material of Example 6 are shown together. In the positive electrode material of Comparative Example 2, peaks derived from starting materials such as elemental sulfur and LiCl were observed, but no new peak was observed between the two strongest peaks attributable to LiCl.

[0167] [Comparative Example 3]

[0168] (Preparation of positive electrode materials)

[0169] In a glove box with an argon atmosphere below -68°C dew point, 2.5 g of sulfur (manufactured by Aldrich) as a positive electrode active material and 0.5 g of a porous carbon material powder (manufactured by Toyo Tanso Co., Ltd., Cnovel (registered trademark) P(3)010) were thoroughly mixed in an agate mortar, and the mixed powder was placed in a sealed pressure-resistant autoclave container and heated at 170°C for 3 hours to melt the sulfur and infiltrate the porous carbon material. Thus, a sulfur-impregnated porous carbon material was prepared as a positive electrode material. In addition to the above, an all-solid lithium secondary battery was prepared according to the same method as Example 1. It should be noted that in Comparative Example 3, the composition of the obtained positive electrode mixture was set to sulfur: solid electrolyte: porous carbon material = 50:24:10 (mass ratio).

[0170] [Comparative Example 4]

[0171] In the preparation of the positive electrode material of Example 1, lithium iodide was replaced with a sulfide solid electrolyte (produced by Ampcera, Li 6 PS 5 Cl), and the operation in the glove box with an argon atmosphere with a dew point of less than -68°C was changed to the operation under the atmosphere, and an all-solid lithium secondary battery was prepared according to the same method as in Example 1. It should be noted that in Comparative Example 4, the composition of the obtained positive electrode mixture was set to sulfur: solid electrolyte: porous carbon material = 48:43:10 (mass ratio).

[0172] 《Evaluation example of test battery cell》

[0173] The resistance values ​​of the test battery cells prepared in the comparative examples and examples were measured by the following method. It should be noted that all the following measurements were performed in a constant temperature chamber set at 25°C using a charge and discharge tester (HJ-SD8 manufactured by Hokuto Denko Co., Ltd.).

[0174] (Measurement of resistance)

[0175] As a measuring device, a high-performance electrochemical measuring system "SP-200" manufactured by Bio-Logic (Bio-Logic SAS (France)) was used. The impedance as an electrochemical characteristic was measured under the measuring conditions of a frequency range of 7MHz to 0.1Hz, a temperature condition of room temperature, and an applied voltage of 50mV. The test battery cell was set in a constant temperature chamber, and the evaluation was carried out after the battery cell temperature became constant. The results are shown in Table 1 below. It should be noted that the resistance of the battery in Comparative Example 4 was too high to be measured.

[0176] [Table 1]

[0177] Table 1

[0178]

[0179] From the results shown in Table 1, it is understood that the positive electrode material of the present invention can further reduce the internal resistance of a secondary battery using a positive electrode active material containing sulfur.

[0180] This application is based on Japanese Patent Application No. 2022-058716 filed on March 31, 2022, the disclosure of which is incorporated herein by reference in its entirety.

[0181] Description of Reference Numerals

[0182] 10a stacked battery, 11' negative electrode collector, 11" positive electrode collector, 13 negative electrode active material layer, 15 positive electrode active material layer, 17 solid electrolyte layer, 19 single battery layer, 21 power generation element, 25 negative electrode collector plate, 27 positive electrode collector plate, 29 laminated film, 100, 100' positive electrode material, 110 porous carbon material, 110a pores, 120 positive electrode active material containing sulfur, 130 solid electrolyte, 140 region near the interface, 150 lithium halide.

Claims

1. A positive electrode material, characterized in that: Contains: porous carbon material, positive electrode active material containing sulfur and lithium halide, At least a portion of the positive electrode active material and at least a portion of the lithium halide are disposed in the pores of the porous carbon material.

2. The positive electrode material according to claim 1, wherein In the X-ray diffraction measurement, between the two strongest peaks attributable to the lithium halide, there exists a crystal peak that is not attributable to any of the porous carbon material, the positive electrode active material, and the lithium halide.

3. The positive electrode material according to claim 1 or 2, wherein The content of the lithium halide is 5 mass % or more and less than 50 mass %.

4. The positive electrode material according to claim 1 or 2, wherein The lithium halide is present more inside the pores than outside the pores of the porous carbon material.

5. The positive electrode material according to claim 1 or 2, wherein The average pore diameter of the porous carbon material is less than 100 nm.

6. The positive electrode material according to claim 1 or 2, wherein The percentage of the pore volume of pores having a pore diameter range of 1 to 4 nm in the pores of the porous carbon material relative to the pore volume of pores having a pore diameter range of 1 to 100 nm is 20% or less. 7 . A secondary battery comprising the positive electrode material according to claim 1 .