Coated diaphragm, preparation method of coated diaphragm and battery

CN118947017AActive Publication Date: 2024-11-12SHENZHEN SENIOR TECH MATERIAL
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202280089293.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-28
Filing Date
2022-09-26
Publication Date
2024-11-12
Estimated Expiration
2042-09-26

AI Technical Summary

Technical Problem

Existing lithium battery separators are prone to peeling off of the ceramic layer at high temperatures, reducing heat resistance, increasing lithium ion transmission distance, resulting in reduced conductivity, and poor retention of liquid electrolyte, affecting battery performance.

Method used

A coating separator with a double-layer structure is used. The first coating is composed of a large-scale first nanofiber and a large-diameter first ceramic particle. The second coating is composed of a small-scale second nanofiber and a small-diameter third ceramic particle. It is composed of two ceramic particles, which are mixed with nanofibers of similar sizes to form a mixed material layer with uniform pore size, which improves heat resistance and permeability, and improves the transmission capacity of lithium ions through lithium ion fast conductor functional groups.

Benefits of technology

It significantly improves the heat resistance and lithium ion conductivity of the separator, reduces the possibility of lithium dendrites, enhances electrochemical stability, and meets the battery capacity retention and conductivity requirements for high-temperature storage and long-term cycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118947017A_ABST
    Figure CN118947017A_ABST
Patent Text Reader

Abstract

A coated separator, a preparation method thereof, and a battery, by mixing first nanofibers (21) with similar dimensions in a first coating layer (20) and mixing second nanofibers (31) with similar dimensions in a second coating layer (30), it is avoided that the size difference between different nanofibers is too large, and the size difference between the different nanofibers is too large. The problem that the nano fibers with similar surface energy are easy to agglomerate due to large surface energy difference of the nano fibers is solved, and the mixing uniformity of the nano fibers is greatly improved. The first coating (20) is arranged to be formed by mixing large-scale first nanofibers (21) and large-particle-size first ceramic particles (22), and the second coating (30) is arranged to be formed by mixing small-scale second nanofibers (31) and small-particle-size second ceramic particles (32), so that the first coating (20) is large in pore diameter and has a very strong skeleton structure; the coated diaphragm can maintain high heat resistance and high permeability; the second coating (30) with small pore diameter can improve the transmission capability of lithium ions and reduce the electrochemical stability risk of high-temperature shelving or long-time circulation.
Need to check novelty before this filing date? Find Prior Art

Description

Coated diaphragm, method for preparing coated diaphragm, and battery Technical Field

[0001] The present invention relates to the technical field of battery separators, and in particular to a coated separator, a method for preparing the coated separator, and a battery. Background Art

[0002] The diaphragm is a core component of lithium-ion batteries. Its performance significantly impacts the overall performance of lithium-ion batteries and is a key technology limiting their development. As the application of lithium-ion batteries continues to expand and the impact of lithium-ion products on people's lives continues to deepen, the demand for lithium-ion battery performance is also increasing. To meet these development requirements, the diaphragm, as a key component of lithium-ion batteries, must not only possess excellent chemical stability and low manufacturing costs, but also improve the safety performance of lithium-ion batteries, which is a key trend in the current lithium-ion battery development.

[0003] In existing technologies, coated separators can include a base membrane and a coating applied to at least one surface of the base membrane. A ceramic layer can also be applied to the surface of the coated separator to improve its heat resistance. However, the interface between the ceramic layer and the separator is weak and easily separates at high temperatures, leading to ceramic layer flaking, melting of the separator substrate, and decreased heat resistance. Furthermore, the surface ceramic layer increases the distance lithium ions travel, thereby reducing lithium ion conductivity, and the large pores cannot effectively retain liquid electrolyte.

[0004] Summary of the Invention

[0005] The present invention provides a coated diaphragm, a method for preparing the coated diaphragm, and a battery, so as to improve the performance of the diaphragm.

[0006] According to a first aspect of the present invention, a coated diaphragm is provided, comprising a base membrane and a coating structure disposed on at least one surface of the base membrane, the coating structure comprising at least a first coating layer and a second coating layer, wherein the first coating layer is disposed on the surface of the base membrane, and the second coating layer is disposed on a side of the first coating layer away from the base membrane; the first coating layer comprises a first nanofiber material and first ceramic particles, and the second coating layer comprises a second nanofiber material and second ceramic particles;

[0007] The first nanofiber material includes a plurality of first nanofibers, and the second nanofiber material includes a plurality of second nanofibers;

[0008] The length difference between the several first nanofibers is no more than 500nm, the length difference between the several second nanofibers is no more than 200nm, the length of the first nanofiber is greater than the length of the second nanofiber, and the average particle size of the first ceramic particles is greater than the average particle size of the second ceramic particles.

[0009] Optionally, the length of the first nanofiber is 500-1000 nm; and the average particle size of the first ceramic particles is 100-600 nm.

[0010] Optionally, the mass ratio of the first nanofiber material to the first ceramic particles is 5:1-1:5.

[0011] Optionally, the length of the second nanofiber is 100-300 nm; and the average particle size of the second ceramic particles is 10-60 nm.

[0012] Optionally, the mass ratio of the second nanofiber material to the second ceramic particles is 5:1-1:5.

[0013] Optionally, the diameter of the first nanofiber is 5-50 nm, and the diameter of the second nanofiber is 5-50 nm.

[0014] Optionally, a thickness ratio of the first coating layer to the second coating layer is greater than 2.

[0015] Optionally, at least one additional coating layer is included between the first coating layer and the second coating layer.

[0016] Optionally, the surface of the second ceramic particles is grafted with lithium ion fast conductor functional groups;

[0017] Furthermore, the lithium ion fast conductor functional group includes any one of hydroxyl (-OH), carbonyl (-C=O), fluorine (-F), and carboxyl (-COOH).

[0018] Optionally, the first ceramic particles and / or the second ceramic particles are inorganic substances having a melting point of above 200° C., electrical insulation, and electrochemical stability within the operating range of lithium batteries.

[0019] Optionally, the coated diaphragm satisfies at least any of the following conditions:

[0020] a) Ionic conductivity ≥ 1.2 mS / cm;

[0021] b) Capacity retention rate ≥ 98%;

[0022] c) Thermal shrinkage at 180°C / h ≤5%.

[0023] According to a second aspect of the present invention, a method for preparing a coated diaphragm is provided, for preparing the coated diaphragm involved in the first aspect and its alternatives, the preparation method comprising:

[0024] Preparing slurries: preparing a first slurry comprising first ceramic particles and a first nanofiber material, and preparing a second slurry comprising second ceramic particles and a second nanofiber material;

[0025] Coating film formation: applying the first slurry to at least one surface of the base film to form a first coating layer, and applying the second slurry to the side of the first coating layer away from the base film to form a second coating layer;

[0026] Further,

[0027] Preparing the first slurry includes dispersing first ceramic particles in a first solvent to obtain a first ceramic dispersion, dispersing a first nanofiber material in a second solvent to obtain a first nanofiber dispersion, and mixing the first ceramic dispersion and the first nanofiber dispersion to obtain a first slurry;

[0028] The second slurry is prepared by dispersing the second ceramic particles in a third solvent to obtain a second ceramic dispersion, dispersing the second nanofiber material in a fourth solvent to obtain a second nanofiber dispersion, and mixing the second ceramic dispersion and the second nanofiber dispersion to obtain a second slurry.

[0029] Optionally, before preparing the slurry, the method further comprises:

[0030] Ceramic screening: selecting first ceramic particles and second ceramic particles of different particle sizes, wherein the average particle size of the first ceramic particles is 100-600 nm, and the average particle size of the second ceramic particles is 10-60 nm;

[0031] Furthermore, the method further comprises ceramic pretreatment: performing a grafting reaction on the second ceramic particles and the object to be grafted, so that the surfaces of the second ceramic particles are grafted with lithium ion fast conductor functional groups.

[0032] Optionally, the material to be grafted includes any one of polycarbonate, polylactic acid, polyurethane, perfluoropropyl vinyl ether, and methyl ethyl propyl ketone.

[0033] According to a third aspect of the present invention, there is provided a battery comprising the coated diaphragm according to the first aspect and its optional solutions or the coated diaphragm prepared by the method for preparing the coated diaphragm according to the second aspect and its optional solutions;

[0034] Furthermore, the battery is a lithium battery.

[0035] In the coated diaphragm, the preparation method of the coated diaphragm, and the battery provided by the present invention, by mixing first nanofibers of similar size in the first coating layer and second nanofibers of similar size in the second coating layer, the problem of large size difference between different nanofibers, which causes the nanofibers of similar surface energy to easily agglomerate due to the large difference in surface energy, is avoided, and the mixing uniformity between the nanofibers is greatly improved. In addition, by setting the first coating layer to be a mixture of large-scale first nanofibers and large-particle first ceramic particles to form a first mixed material layer with large pore size and uniformity, the first mixed material layer is provided on the surface of the base film. Due to its large pore size and strong skeleton structure, the coated diaphragm can maintain high heat resistance and high permeability; by setting the second coating layer to be a mixture of small-scale second nanofibers and small-particle second ceramic particles to form a second mixed material layer with small pore size and uniformity, due to capillary action, the small pore size has a strong adsorption capacity for the electrolyte, thereby improving the transmission capacity of lithium ions, thereby reducing the possibility of lithium dendrites, and reducing the risk of electrochemical stability during high-temperature storage or long-term cycling. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0037] FIG1 is a schematic diagram of a partial structure of a coated diaphragm in one embodiment of the present invention;

[0038] FIG2 is a schematic flow chart of a method for preparing a coated diaphragm according to an embodiment of the present invention.

[0039] Description of reference numerals:

[0040] 10-basement membrane;

[0041] 20-first coating;

[0042] 21-First Nanofiber

[0043] 22-first ceramic particles;

[0044] 30- second coating;

[0045] 31- second nanofiber;

[0046] 32-Second ceramic particles. DETAILED DESCRIPTION

[0047] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0048] In the description of the specification of the present invention, it should be understood that the orientations or positional relationships indicated by the terms "upper part", "lower part", "upper end", "lower end", "lower surface", "upper surface", etc. are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0049] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood to indicate or imply relative importance or implicitly specify the number of the technical features indicated. Therefore, features specified as "first" or "second" may explicitly or implicitly include one or more of such features.

[0050] In the description of the present invention, "plurality" means multiple, such as two, three, four, etc., unless otherwise clearly defined.

[0051] In the description of the present invention, unless otherwise specified or limited, the term "connection" and other terms should be understood in a broad sense. For example, it can mean fixed connection, detachable connection, or integration; it can mean mechanical connection, electrical connection, or mutual communication; it can mean direct connection or indirect connection through an intermediate medium; it can mean internal communication between two elements or interaction between two elements. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0052] The following specific embodiments are used to describe the technical solution of the present invention in detail. The following specific embodiments can be combined with each other, and the same or similar concepts or processes may not be described in detail in some embodiments.

[0053] Before filing this application, the applicant conducted a series of research and experiments on existing diaphragms:

[0054] In order to solve the problem of easy peeling of the ceramic layer, it has been proposed in the art that one-dimensional nanomaterials can be added to the coating.

[0055] In order to solve the problems of disordered stacking of one-dimensional nanomaterials in the coating, which easily leads to excessive gaps and few contact points, the applicant proposed a corresponding solution. By making the length of the one-dimensional nanomaterial decrease layer by layer with the coating (reflected in the decrease of the length description value of the one-dimensional nanomaterial of each material layer), since the gaps of the long nanomaterials are large, the gaps are larger at the bottom layer, and the shorter nanomaterials in the upper layer can fill these gaps to a certain extent. After layer-by-layer deposition, there are no excessive gaps inside the coating and there are more contact points. When heated, the tight structure of the coating can inhibit thermal deformation of the diaphragm, thereby improving the heat resistance of the coated diaphragm. For this solution, the applicant also filed a patent application (application number: PCT / CN2022 / 077087, application date: 2022.02.21), and this application hereby introduces the entire content of PCT / CN2022 / 077087, that is, the entire content of PCT / CN2022 / 077087 can serve as support for this application.

[0056] In order to solve the problem that the stacking density of one-dimensional nanofibers is too large due to the gradual decrease in the stacking mode, which hinders the transmission channel of lithium ions, affects the transmission rate of lithium ions, and limits the performance of the diaphragm, the applicant has proposed a corresponding solution. By introducing ceramic particles into the one-dimensional nanomaterial coating, the ion conduction rate can be effectively improved. For this solution, the applicant has also filed a patent application (application number: PCT / CN2022 / 108551, application date: 2022.07.28). This application hereby introduces the entire contents of PCT / CN2022 / 108551, that is, the entire contents of PCT / CN2022 / 108551 can serve as support for this application.

[0057] However, the applicant discovered in further research that although the above solution can use ceramic particles to avoid the excessive stacking density of one-dimensional nanomaterials, thereby forming a more effective lithium ion transmission channel and improving the lithium ion transmission rate; however, the overall performance of the diaphragm is still not ideal. Through research and experiments, the applicant found that the reason is that the size difference between different nanofibers is too large, which causes the nanofibers with similar surface energies to easily agglomerate due to their large surface energy differences. That is, small-sized nanofibers have large surface energy and are easy to agglomerate with each other to form agglomerates, and then come into contact and mix with large-sized nanofibers. This results in the small-sized nanofibers not being able to fully exert their due performance; and the ceramic particles do not make corresponding distinctions for nanofibers of different sizes, which limits the performance of the diaphragm.

[0058] Based on this discovery, the applicant, through a series of research, testing, and verification, has developed the technical solution of this application. Since the orderly arrangement of one-dimensional nanofibers is a major innovation of the applicant, the further research questions and solutions based on this orderly arrangement are also major innovations. The entire research process should be considered an integral part of this solution and should be considered as a whole when evaluating the inventiveness of this application.

[0059] Please refer to Figure 1. An embodiment of the present invention provides a coated diaphragm, including: a base film 10 and a coating structure provided on the base film 10, the coating structure including a first coating 20 and a second coating 30, wherein the first coating 20 is provided on the surface of the base film 10, and the second coating 30 is provided on the side of the first coating 20 away from the base film 10; the first coating 20 contains a first nanofiber material and first ceramic particles 22, and the second coating 30 contains a second nanofiber material and second ceramic particles 32; the first nanofiber material includes a plurality of first nanofibers 21, and the second nanofiber material includes a plurality of second nanofibers 31; the length difference between each first nanofiber 21 is not greater than 500nm, the length difference between each second nanofiber 31 is not greater than 200nm, and the length of the first nanofiber 21 is greater than the length of the second nanofiber 31, and the average particle size of the first ceramic particles 22 is greater than the average particle size of the second ceramic particles 32.

[0060] The present invention takes into account that due to the large size differences between different nanofibers, nanofibers with similar surface energies tend to agglomerate due to their large surface energy differences. In other words, small-sized nanofibers have large surface energies and tend to agglomerate with each other to form agglomerates, which are then contacted and mixed with large-sized nanofibers. This results in the small-sized nanofibers not being able to fully exert their expected performance. By mixing nanofibers of similar sizes, the mixing uniformity is greatly improved, thereby reducing the differences. The first coating is formed by mixing large-scale first nanofibers with large-size first ceramic particles to form a first mixed material layer with large and uniform pore size. This first mixed material layer is provided on the surface of the base membrane. Due to its large pore size and strong skeleton structure, it can maintain the high heat resistance and high permeability of the coated diaphragm. The second coating is formed by mixing small-scale second nanofibers with small-size second ceramic particles to form a second mixed material layer with small and uniform pore size. Due to capillary action, the small pore size has a strong adsorption capacity for the electrolyte, thereby improving the transmission capacity of lithium ions, thereby reducing the possibility of lithium dendrites and the risk of electrochemical stability during high-temperature storage or long-term cycling. This effectively improves the performance of the diaphragm.

[0061] In a preferred embodiment, the length of the first nanofibers 21 is 500-1000 nm, for example, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, etc.; the average particle size of the first ceramic particles 22 is 100-600 nm, for example, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, etc. The first coating layer containing the first nanofibers and first ceramic particles is applied to the surface of the base membrane to form a large pore size and a strong skeleton structure, thereby maintaining the high heat resistance and high permeability of the coated membrane.

[0062] As a preferred embodiment, the mass ratio of the first nanofiber material to the first ceramic particles 22 is 5:1-1:5; by setting the mass ratio of the first nanofiber material to the first ceramic particles 22 within this range, the coating can be maintained to have better heat resistance and lithium ion conductivity. As a specific embodiment, the mass ratio of the first nanofiber material to the first ceramic particles 22 can be, for example, any one of 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4, 1:5 or a range between any two of them. Of course, the mass ratio of the first nanomaterial to the first ceramic particles can also take other values, and the specific numerical value is not a limitation of the present invention. As long as the ratio is between 5:1-1:5, it is within the scope of protection of the present invention.

[0063] In a preferred embodiment, the second nanofibers 31 have a length of 100-300 nm, such as 100 nm, 150 nm, 200 nm, 250 nm, or 300 nm. The second ceramic particles 32 have an average particle size of 10-60 nm, such as 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, or 60 nm. The second coating layer, located on the side of the first coating layer away from the base film, is a mixture of the second nanofibers and the second ceramic particles. Due to capillary action, the small pores provide strong electrolyte adsorption, improving lithium ion transport and reducing the likelihood of lithium dendrite formation. This reduces the risk of electrochemical stability during high-temperature storage or prolonged cycling.

[0064] As a preferred embodiment, the mass ratio of the second nanofiber material to the second ceramic particles 32 is 5:1-1:5. By setting the mass ratio of the second nanofiber material to the second ceramic particles 32 within this range, the coating has better battery capacity retention and lithium ion conductivity. As a specific embodiment, the mass ratio of the second nanofiber material to the second ceramic particles 22 can be, for example, any one of 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4, 1:5, or a range between any two of them. Of course, the mass ratio of the second nanomaterial to the second ceramic particles can also take other values. The specific numerical value is not a limitation of the present invention. As long as the ratio is between 5:1 and 1:5, it is within the scope of protection of the present invention.

[0065] As a preferred embodiment, the diameter of the first nanofiber is 5-50 nm, and the diameter of the second nanofiber is 5-50 nm.

[0066] As a preferred embodiment, the thickness ratio of the first coating layer 20 to the second coating layer 30 is greater than 2; thereby, the heat resistance of the coated diaphragm can be further effectively improved.

[0067] As a preferred embodiment, at least one additional coating layer is further included between the first coating layer 20 and the second coating layer 30. For example, an additional coating layer, such as a third coating layer, may be included between the first coating layer 20 and the second coating layer 30; or two additional coating layers, such as a third coating layer and a fourth coating layer, may be included. Of course, other numbers of additional coating layers may also be included. The additional coating layer may be made of the same material and size as the first coating layer or the second coating layer, or may be made of different materials and sizes. That is, a third coating layer is provided between the first coating layer and the second coating layer, the third coating layer comprising third ceramic particles with an average particle size of 100-600nm and third nanofibers with an aspect ratio of ≤200, and the materials and sizes of the third ceramic particles and the third nanofibers are different from those of the second coating layer; or a third coating layer is provided between the first coating layer and the second coating layer, the third coating layer comprising third ceramic particles with an average particle size of 10-60nm and third nanofibers with an aspect ratio of ≤60, and the materials and sizes of the third ceramic particles and the third nanofibers are different from those of the first coating layer. It should be noted that the number of coating layers, the selection of materials between different layers, and the size setting of the coated diaphragm can be adjusted according to actual needs and should not be construed as limiting the present invention.

[0068] As a preferred embodiment, the surfaces of the second ceramic particles 32 are grafted with lithium-ion fast conductor functional groups. The presence of these fast conductor functional groups on the surfaces of the second ceramic particles can significantly improve lithium-ion transport capacity. Furthermore, the fast conductor functional groups include any one of hydroxyl (-OH), carbonyl (-C=O), fluorine (-F), and carboxyl (-COOH).

[0069] In a preferred embodiment, the first ceramic particles 22 and / or the second ceramic particles 32 are inorganic materials having a melting point of 200°C or higher, electrically insulating properties, and electrochemically stable within the operating range of lithium batteries. Examples include oxide-based ceramics such as aluminum oxide, silicon dioxide, titanium oxide, zirconium dioxide, magnesium oxide, cerium oxide, yttrium oxide, and zinc oxide; nitride-based ceramics such as silicon nitride, titanium nitride, and boron nitride; silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, basic alumina, potassium titanate, talc, kaolinite, clay, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, magnesia chlorite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand. These ceramics can be used alone or in combination.

[0070] As a preferred embodiment, the coated diaphragm satisfies at least any of the following conditions:

[0071] a) Ionic conductivity ≥ 1.2 mS / cm;

[0072] b) Capacity retention rate ≥ 98%;

[0073] c) Thermal shrinkage at 180°C / h ≤5%.

[0074] In addition, referring to FIG. 2 , an embodiment of the present invention further provides a method for preparing a coated diaphragm, which is used to prepare the coated diaphragm involved in the first aspect and its optional solutions. The preparation method comprises:

[0075] S1: preparing a first slurry: preparing a first slurry comprising first ceramic particles and a first nanofiber material;

[0076] S2: preparing a second slurry: preparing a second slurry comprising second ceramic particles and a second nanofiber material;

[0077] S3: Coating and film formation: applying the first slurry to at least one surface of the base film to form a first coating layer, and applying the second slurry to the side of the first coating layer away from the base film to form a second coating layer.

[0078] Specifically, preparing the first slurry includes dispersing first ceramic particles in a first solvent to obtain a first ceramic dispersion, dispersing the first nanofiber material in a second solvent to obtain a first nanofiber dispersion, and mixing the first ceramic dispersion and the first nanofiber dispersion to obtain the first slurry;

[0079] The second slurry is prepared by dispersing the second ceramic particles in a third solvent to obtain a second ceramic dispersion, dispersing the second nanofiber material in a fourth solvent to obtain a second nanofiber dispersion, and mixing the second ceramic dispersion and the second nanofiber dispersion to obtain a second slurry.

[0080] The first solvent, the second solvent, the third solvent, and the fourth solvent may be the same type of solvent, or may be different, and the present invention does not impose any limitation thereto.

[0081] The present invention does not limit the order of preparing the first slurry and the second slurry. The second slurry can also be prepared first and then the first slurry.

[0082] In one example, the first and third solvents are selected from water, N-methylpyrrolidone, ethanol, acetone, and the like. The first and second ceramic particles are uniformly dispersed in the solvent by high-speed stirring, high-pressure homogenization, sand milling, and the like. The mass concentration of the first and second ceramic particles in the dispersion is 2% to 40%.

[0083] In one example, the second solvent and the fourth solvent are selected from water, N-methylpyrrolidone, ethanol, acetone, etc. The first nanofiber material and the second nanofiber material are uniformly dispersed in the dispersant by high-speed stirring, high-pressure homogenization, sand milling, etc., and the mass concentration of the first nanofiber and the second nanofiber in the dispersant is 2%-30%.

[0084] The lengths of the first nanofibers can vary, as long as the length difference is no more than 500 nm, i.e., they are within a similar range. Similarly, the lengths of the second nanofibers can vary, as long as the length difference is no more than 200 nm, i.e., they are within a similar range.

[0085] Among them, nanofibers of different lengths are achieved based on the selection of raw materials for the nanofibers. For example, when nanofiber materials of different materials are selected, nanofibers of different lengths may be formed.

[0086] In other examples, nanofibers of different lengths can also be formed through corresponding technical means.

[0087] The raw material of the nanofiber material or the broken nanofiber material is broken, and nanofibers of different lengths are formed through one or more breaking steps.

[0088] By cutting the nanofiber material, a shorter nanofiber material can be formed based on a raw material of a nanofiber material of a certain length. For example, the nanofiber material can be cut into half of the raw material. In other examples, the method of cutting in half is not required.

[0089] Any existing or improved method for disconnecting the nanofiber material can be used as a specific example of an embodiment of the present invention. In a specific example, the disconnection can be achieved by etching the nanofiber material, for example, the nanofiber can be etched to half the length of the original material.

[0090] Based on the required layering, the raw material can be disconnected once or multiple times. For example, the nanofiber material can be etched to half the length of the raw material, and then half the length of the nanofiber material is retained, and then the other half of the length of the nanofiber material is disconnected to obtain a quarter of the length of the nanofiber material. In other examples, part of the quarter of the length of the nanofiber material can be further disconnected, and the number of disconnections can be arbitrarily configured according to needs.

[0091] Of course, at least one of the following joining processes may also be implemented, and nanofiber materials of different lengths may be formed through one or more joining processes:

[0092] Joining a raw material of nanofiber material to one end of another raw material;

[0093] joining the joined nanofiber material to one end of the raw material;

[0094] The joined nanofiber material is joined to one end of another joined nanofiber material.

[0095] It can be seen that the objects to be joined can be one end of a raw material and one end of another raw material, one end of a raw material and one end of a joined nanofiber material, or one end of a joined nanofiber material and one end of another joined nanofiber material.

[0096] Among them, by joining the nanofiber materials, a longer nanofiber material can be formed based on a raw material of a nanofiber material of one length. For example, two raw materials can be joined to form a nanofiber material of twice the length. In other examples, raw materials of different lengths (or joined nanofiber materials) can also be used to achieve this.

[0097] Any existing means or improved means for achieving the bonding of nanofiber materials can be used as a specific example of the embodiment of the present invention.

[0098] For example, the bonding of nanofiber materials can be achieved based on materials rich in hydroxyl functional groups (such as polyethylene glycol PEG). Furthermore, the bonding mentioned above may include:

[0099] The nanofiber material to be bonded is mixed with a material rich in hydroxyl functional groups (such as PEG) in a solution;

[0100] adding molecular sieve particles as a catalyst to the solution;

[0101] The solution is heated, then cooled, and filtered to remove the molecular sieve, thereby obtaining a joined nanofiber material.

[0102] For example, let's take nanocellulose as an example. The hydroxyl content at the end of nanocellulose is significantly higher than that in the middle region. In order to increase the length of nanocellulose, the activity of hydroxyl groups can be fully utilized as follows:

[0103] (1) Mixing nanocellulose with polyethylene glycol (PEG), wherein the molecular weight of PEG is 50,000-1,000,000 g / mol and PEG accounts for 1% of the nanocellulose, and stirring the two together to form a corresponding solution.

[0104] (2) adding 13A molecular sieve particles with a particle size of 1 mm to 10 mm to the above solution, the molecular sieve being a catalyst;

[0105] (3) Hydrothermal heating to 80 degrees for 1-2 hours;

[0106] (4) Cooling to room temperature, filtering to remove 13A molecular sieve particles, and obtaining the joined nanocellulose.

[0107] In the above scheme, by adding a material rich in hydroxyl functional groups (such as PEG), a bridge can be connected between the nanocelluloses, and using molecular sieves (such as 13A molecular sieves) as catalysts, the polymerization reaction between PEG and the nanocellulose can be accelerated, and finally a structure of nanocellulose-PEG-nanocellulose is formed. Based on the required layering, a single joining of the raw materials can be achieved, or multiple joinings can be achieved, for example: the raw material of the nanofiber material can be first joined to twice the raw material, then the nanofiber material of twice the length of the part is retained, and then the nanofiber material of twice the length of the other part is joined to the raw material or the nanofiber material of twice the length to obtain a nanofiber material of three times the length or four times the length. In other examples, it is also possible to further join, and the number of joinings can be arbitrarily configured according to demand.

[0108] Mixing the first ceramic dispersion with the first nanofiber dispersion to obtain the first slurry and mixing the second ceramic dispersion with the second nanofiber dispersion to obtain the second slurry both specifically include: mixing the first ceramic dispersion with the first nanofiber dispersion to obtain a first mixed solution; and mixing the second ceramic dispersion with the second nanofiber dispersion to obtain a second mixed solution; wherein the mixing is performed by high-speed stirring, high-pressure homogenization, sand milling, or other methods. Subsequently, an adhesive is added to each of the first and second mixed solutions to obtain the first and second slurries. The adhesive is at least one of polyvinyl alcohol, polyacrylonitrile, polyacrylic acid, styrene-butadiene rubber, carboxymethyl cellulose, polyvinylidene fluoride, polyvinyl pyrrolidone, and polyimide. The adhesive constitutes 1% to 10% of the solid mass of each of the first and second mixed solutions.

[0109] In one example, the coating membrane formation comprises: applying the first slurry prepared above to a base film by coating, and drying to obtain a first coating layer. Subsequently, a second slurry is applied to the first coating layer, and dried to obtain the coated membrane. The coating method includes spraying, dipping, micro-gravure roller coating, printing coating, extrusion coating, or wire rod coating. The base film is, for example, a polyolefin base film with a thickness of 3-30 microns, a drying temperature of 40-130 degrees Celsius, and a coating speed of 10-200 m / min.

[0110] Of course, it should be understood that drying is only one method for forming the first / second coating layer from the first slurry / second slurry. The first / second coating layer can also be formed from the first slurry / second slurry by phase inversion. The present invention does not limit the method for forming the first / second coating layer from the first slurry / second slurry.

[0111] Among them, as a preferred embodiment, before the dispersion of ceramics, ceramic screening and ceramic pretreatment are also included, specifically:

[0112] The ceramic screening is specifically as follows: selecting first ceramic particles and second ceramic particles of different particle sizes, wherein the average particle size of the first ceramic particles is 100-600 nm, and the average particle size of the second ceramic particles is 10-60 nm;

[0113] The ceramic pretreatment specifically involves adding the second ceramic particles to a reactor and then adding the grafted material to conduct a grafting reaction, thereby grafting lithium-ion fast conductor functional groups onto the surfaces of the second ceramic particles. Specifically, the second ceramic particles are added to a solvent and then placed together in a reactor. The grafted material is then added. By controlling the reaction temperature, pressure, and time, the lithium-ion fast conductor functional groups are grafted onto the second ceramic particles.

[0114] The second ceramic particles are not particularly limited, but preferably have a melting point of 200°C or higher, high electrical insulation, and are electrochemically stable within the operating range of lithium batteries. Examples include oxide-based ceramics such as alumina, silica, titanium oxide, zirconium dioxide, magnesium oxide, cerium oxide, yttrium oxide, and zinc oxide; nitride-based ceramics such as silicon nitride, titanium nitride, and boron nitride; silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, basic alumina (aluminum hydroxide oxide), potassium titanate, talc, kaolinite, clay, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, magnesia chlorite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand. These can be used alone or in combination.

[0115] The first ceramic particles are also not particularly limited. They are preferably materials with a melting point of more than 200°C, high electrical insulation, and electrochemical stability within the range of use of lithium batteries. They can also be made of the same or different inorganic materials as the second ceramic particles. The solvents are water, ethanol, acetone, NMP, etc., and the grafted materials are polycarbonate, polylactic acid, polyurethane, perfluoropropyl vinyl ether, methyl ethyl propyl ketone, etc. The reaction temperature is 100-200°C, the reaction pressure is 0.1-0.5Mpa, and the reaction time is 10-50min. After the reaction is completed, the liquid solvent is removed, leaving the solid, and the second ceramic particles grafted with the lithium ion fast conductor can be obtained.

[0116] On this basis, the dispersion of ceramics is specifically as follows:

[0117] The first ceramic particles and the pretreated second ceramic particles are dispersed in a first solvent and a third solvent respectively to obtain a first ceramic dispersion and a second ceramic dispersion respectively.

[0118] Furthermore, an embodiment of the present invention further provides a battery comprising the coated diaphragm according to the first aspect of the present invention and its optional solutions, or the coated diaphragm prepared using the second aspect of the present invention and its optional solutions, wherein the battery is, for example, a lithium battery.

[0119] The product performance of some embodiments of the present invention will be analyzed through experiments below.

[0120] Example 1

[0121] In this embodiment, the coated diaphragm is prepared by the following steps:

[0122] Ceramic screening: first ceramic particles and second ceramic particles of different particle sizes are selected, wherein the average particle size of the first ceramic particles is 300 nm, and the average particle size of the second ceramic particles is 40 nm; the first ceramic and the second ceramic are both aluminum oxide.

[0123] Ceramic dispersion: The first ceramic particles and the second ceramic particles are uniformly dispersed in N-methylpyrrolidone by high-speed stirring to obtain a first ceramic dispersion and a second ceramic dispersion, wherein the mass concentration of the first ceramic particles in the first ceramic dispersion and the mass concentration of the second ceramic particles in the second ceramic dispersion are both 20%.

[0124] Nanomaterial Dispersion: First and second nanofibers of different lengths were dispersed in N-methylpyrrolidone to obtain first and second nanofiber dispersions. The first nanofibers had a length (L50) of 600 nm, and the second nanofibers had a length (L50) of 300 nm. Dispersion was performed using high-speed stirring. The mass concentration of both the first and second nanofibers in the dispersant was 15%.

[0125] Mixed slurrying: A first ceramic dispersion and a first nanofiber dispersion are mixed to form a first mixed solution; a second ceramic dispersion and a second nanofiber dispersion are mixed to form a second mixed solution; the mixing is performed using high-speed stirring. An adhesive is then added to the first and second mixed solutions, respectively, to form first and second slurries. The adhesive is polyvinyl alcohol; the adhesive constitutes 8% of the solid mass of each of the first and second mixed solutions. The mass ratio of the first nanofibers to the first ceramic particles is 1:1, and the mass ratio of the second nanofibers to the second ceramic particles is 1:1.

[0126] Coating process: A first slurry is applied to one surface of a base film and dried to form a first coating layer, producing a semi-finished coated membrane. A second slurry is then applied to the first coating layer and dried to form a second coating layer on top of the first coating layer, producing the coated membrane. The base film is a polyethylene film with a thickness of 9 microns. The drying temperature is 100°C and the coating speed is 100 m / min. The resulting first coating layer is 0.8 microns thick, and the second coating layer is 0.3 microns thick.

[0127] The first nanofiber and the second nanofiber are specifically one-dimensional nanofibers, which are deposited on the surface of the base film to form a layered structure (i.e., nanomaterials of different lengths). During the deposition process on the base film, due to surface energy, the longest one-dimensional nanomaterial (which has the largest surface energy and is the most unstable, and is most likely to adhere once it contacts an interface with low surface energy) is deposited first, while longer ones are deposited later, and the shortest nanowires are deposited last, thus forming a layered structure that gradually accumulates from long to short. The present invention significantly improves the mixing uniformity by mixing nanofibers of similar sizes, thereby reducing differences.

[0128] The same method was used to obtain Examples 2-12 and Comparative Examples 1-5. For the performance of the corresponding membranes obtained in Examples 1-12 and Comparative Examples 1-5, please refer to Table 1. Except for the differences in the preparation parameters listed in Table 1, all other embodiments and comparative examples are consistent with Example 1, and thus are not further described.

[0129] Example 12, shown in Table 1, differs from Example 1 only in that a ceramic pretreatment step is performed on the second ceramic particles before dispersing the S2 ceramic: the second ceramic particles are added to a solvent and then placed together in a reactor. The grafted material is then added, and the reaction temperature, pressure, and time are maintained to graft lithium-ion fast conductor functional groups onto the second ceramic particles. The solvent is acetone, and the grafted material is polycarbonate. The reaction temperature is 150°C, the pressure is 0.3 MPa, and the reaction time is 20 minutes. After the reaction is complete, the liquid solvent is removed, leaving a solid, to obtain the second ceramic particles grafted with the lithium-ion fast conductor.

[0130]

[0131]

[0132] Table 1

[0133] From Table 1, it can be seen from the comparison of Examples 1-12 that when the first nanofiber is mixed with the first ceramic particle and the second nanofiber is mixed with the second ceramic particle, the thermal shrinkage at 180°C is less than 5%, the lithium ion conductivity is greater than 1.2mS / cm, and the battery capacity retention rate for 30 days is greater than 98%. When the thickness of the first coating is reduced and the thickness of the second coating is increased, the heat resistance decreases (Examples 1, 2, and 3). This is mainly because the first nanofiber and the first ceramic particle are the main skeletons and are in direct contact with the base film. Therefore, the first coating composed of the first nanofiber and the first ceramic particle has a direct effect on the heat resistance. If the thickness of the first coating is reduced, the heat resistance decreases directly. The second coating composed of the second nanofiber and the second ceramic particle is in direct contact with the pole piece, and its uniformity directly determines the battery capacity retention rate. The higher the uniformity, the higher the battery capacity retention rate. The thickness of the second coating can greatly improve the uniformity of the entire coating structure. Therefore, as the thickness of the second coating increases, the battery capacity retention rate is improved (Examples 1, 2, and 3).

[0134] From the comparison of Example 1, Example 5, and Comparative Example 3, it can be seen that when the particle size of the second ceramic particles in the second coating is too large, the high-temperature storage battery capacity retention rate decreases (Comparative Example 3); when the particle size of the second ceramic particles in the second coating decreases, the lithium ion conductivity decreases (Example 1, Example 5). From the comparison of Example 1 and Example 7, it can be seen that when the length of the second nanofibers in the second coating decreases, the lithium ion conductivity decreases; the reason for this phenomenon is that the length of the second nanofibers increases, resulting in an increase in the disorder of the pore size distribution in the second coating, which in turn leads to a decrease in the battery capacity retention rate, and the length of the second nanofibers decreases, resulting in a narrowing of the pore size, which in turn leads to a smaller lithium ion transmission channel. However, by grafting fast lithium ion conductor functional groups on the second ceramic, the lithium ion conductivity can be further improved, as shown in Example 12.

[0135] A comparison of Example 1, Comparative Example 2, and Comparative Example 4 shows that increasing the size of the first ceramic particles in the first coating decreases the heat resistance of the separator; increasing the length of the first nanofibers in the first coating also decreases the separator's heat resistance. This phenomenon is primarily due to the fact that excessive increases in size increase the gaps between the coating materials, limiting the contact points with the base membrane. This results in a failure to effectively suppress the separator's shrinkage when heated.

[0136] From the comparison of Example 1, Comparative Example 1, and Comparative Example 5, it can be seen that when the nanofibers and ceramic particles are randomly distributed, the high-temperature shelf battery capacity retention rate is only 95%, which is much lower than the result of stratification. And when the first nanofiber is mixed with the second ceramic particle, and the second nanofiber is mixed with the first ceramic particle, its lithium ion conductivity, high-temperature shelf battery capacity retention rate, and heat resistance further decrease. The reason for this phenomenon is that when the nanofibers and ceramics are randomly distributed, the pore size uniformity of the coating is poor, and the pore sizes are different, which leads to a decrease in the high-temperature shelf battery capacity retention rate. When the first coating is the second nanofiber and the second coating is the first nanofiber, the scale difference between the nanofiber and the ceramic increases, resulting in a decrease in the mixing consistency. In addition, the introduction of the second nanofiber in the second coating greatly increases the pore size and its inconsistency, resulting in a significant decrease in the high-temperature shelf battery capacity retention rate. The introduction of the first nanofiber in the first coating reduces the rigidity of the skeleton, resulting in a decrease in high-temperature heat resistance.

[0137] Throughout this specification, references to terms such as "one embodiment," "an example," "a specific implementation," or "an example" indicate that the specific features, structures, materials, or characteristics described in conjunction with that embodiment or example are included in at least one embodiment or example of the present invention. In this specification, schematic representations of these terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.

[0138] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A coated diaphragm, characterized in that: include: A base film and a coating structure disposed on at least one surface of the base film, the coating structure comprising at least a first coating and a second coating, wherein the first coating is disposed on the surface of the base film, and the second coating is disposed on a side of the first coating away from the base film; the first coating contains a first nanofiber material and first ceramic particles, and the second coating contains a second nanofiber material and second ceramic particles; The first nanofiber material includes a plurality of first nanofibers, and the second nanofiber material includes a plurality of second nanofibers; The length difference between the several first nanofibers is no more than 500nm, the length difference between the several second nanofibers is no more than 200nm, the length of the first nanofiber is greater than the length of the second nanofiber, and the average particle size of the first ceramic particles is greater than the average particle size of the second ceramic particles.

2. The coated diaphragm according to claim 1, characterized in that The length of the first nanofiber is 500-1000 nm; the average particle size of the first ceramic particles is 100-600 nm.

3. The coated diaphragm according to claim 2, characterized in that The mass ratio of the first nanofiber material to the first ceramic particles is 5:1-1:

5.

4. The coated diaphragm according to claim 1, characterized in that The length of the second nanofiber is 100-300 nm; the average particle size of the second ceramic particles is 10-60 nm.

5. The coated diaphragm according to claim 4, characterized in that The mass ratio of the second nanofiber material to the second ceramic particles is 5:1-1:

5.

6. The coated diaphragm according to claim 1, characterized in that The diameter of the first nanofiber is 5-50 nm, and the diameter of the second nanofiber is 5-50 nm.

7. The coated diaphragm according to claim 1, characterized in that A thickness ratio of the first coating layer to the second coating layer is greater than 2.

8. The coated diaphragm according to any one of claims 1 to 7, characterized in that: At least one additional coating layer is further included between the first coating layer and the second coating layer.

9. The coated diaphragm according to claims 1 to 7, characterized in that The surface of the second ceramic particles is grafted with lithium ion fast conductor functional groups; Furthermore, the lithium ion fast conductor functional group includes any one of hydroxyl (-OH), carbonyl (-C=O), fluorine (-F), and carboxyl (-COOH).

10. The coated diaphragm according to claims 1-7, characterized in that: The first ceramic particles and / or the second ceramic particles are inorganic substances having a melting point of 200° C. or higher, electrically insulating properties, and electrochemically stable within the operating range of lithium batteries.

11. The coated diaphragm according to claim 1, characterized in that The coated diaphragm satisfies at least any of the following conditions: a) Ionic conductivity ≥ 1.2 mS / cm; b) Capacity retention rate ≥ 98%; c) Thermal shrinkage at 180℃ / h ≤5%.

12. A method for preparing a coated diaphragm, characterized in that: For preparing the coated diaphragm according to any one of claims 1 to 11, the preparation method comprises: Preparing slurries: preparing a first slurry comprising first ceramic particles and a first nanofiber material, and preparing a second slurry comprising second ceramic particles and a second nanofiber material; Coating film formation: applying the first slurry to at least one surface of the base film to form a first coating layer, and applying the second slurry to the side of the first coating layer away from the base film to form a second coating layer; Furthermore, Preparing the first slurry includes dispersing first ceramic particles in a first solvent to obtain a first ceramic dispersion, dispersing a first nanofiber material in a second solvent to obtain a first nanofiber dispersion, and mixing the first ceramic dispersion and the first nanofiber dispersion to obtain a first slurry; The second slurry is prepared by dispersing the second ceramic particles in a third solvent to obtain a second ceramic dispersion, dispersing the second nanofiber material in a fourth solvent to obtain a second nanofiber dispersion, and mixing the second ceramic dispersion and the second nanofiber dispersion to obtain a second slurry.

13. The method for preparing the coated diaphragm according to claim 12, characterized in that: Before preparing the slurry, the method further comprises: Ceramic screening: selecting first ceramic particles and second ceramic particles of different particle sizes, wherein the average particle size of the first ceramic particles is 100-600 nm, and the average particle size of the second ceramic particles is 10-60 nm; Furthermore, the method further comprises ceramic pretreatment: performing a grafting reaction on the second ceramic particles and the object to be grafted, so that the surfaces of the second ceramic particles are grafted with lithium ion fast conductor functional groups.

14. The method for preparing the coated diaphragm according to claim 13, characterized in that: The object to be grafted includes any one of polycarbonate, polylactic acid, polyurethane, perfluoropropyl vinyl ether, and methyl ethyl propyl ketone.

15. A battery, characterized in that: A coated diaphragm comprising the coated diaphragm according to any one of claims 1 to 11 or a coated diaphragm prepared by the method for preparing the coated diaphragm according to any one of claims 12 to 14; Furthermore, the battery is a lithium battery.

Citation Information

Patent Citations

  • Ceramic diaphragm and preparation method and application thereof

    CN105529425A

  • Composite diaphragm for lithium ion batteries, production method thereof, and lithium ion battery

    CN107437603A

  • Coating Liquid for Lithium Ion Batteries, Lithium Ion Battery Separators and Lithium Ion Batteries

    CN109167004A

  • Composite diaphragm for lithium battery and preparation method of composite diaphragm

    CN113193303A

  • Lithium ion battery and preparation method thereof

    CN114024097A