Activated carbon-zirconium-based metal organic framework composite material and preparation method thereof
Through the preparation of activated carbon-zirconium-based metal organic framework composite materials, the problems of activated carbon insufficient adsorption capacity of small molecule ring gas and difficulty in forming metal organic framework materials are solved, and composite materials with multi-stage pore structures are formed, which is toxic to industrialization Efficient purification of gas.
Patent Information
- Application Number
- CN202411197149.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, activated carbon has insufficient adsorption capacity to small molecule cyclic gases such as ethylene oxide, and metal organic framework materials have problems of forming difficulties and high cost in industrial applications, which limits its industrial toxic gas purification field. Widely used.
Using activated carbon-zirconium-based metal organic framework composite material, UIO-66 or UIO-66-NH2 matrix is synthesized through hydrothermal reaction, and mixed with activated carbon, and then bonded molding and secondary carbonization to form a composite with a multi-stage pore structure. Material, improve adsorption performance.
It significantly improves the micropore adsorption capacity of activated carbon, achieves efficient purification of small-molecular ring gases and macromolecular gases, overcomes the shortcomings of single activated carbon and metal organic framework materials, and is suitable for broad-spectrum adsorption and purification of industrial toxic gases.
Smart Images

Figure BDA0005016792240000111 
Figure BDA0005016792240000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of industrial toxic gas adsorption and purification, and specifically relates to an activated carbon-zirconium-based metal organic framework composite material and a preparation method thereof. Background Art
[0002] In the field of industrial toxic gas adsorption and environmental governance, high-efficiency adsorption materials are needed to deal with harmful substances in industrial waste gas. Adsorption materials must have excellent adsorption capacity for various toxic gases. By using adsorption materials, industrial waste gas can be effectively purified, and the harm caused by toxic gases to the environment and human health can be reduced, thereby achieving the purpose of environmental governance and protection.
[0003] As a traditional adsorption material, activated carbon has been widely used in the fields of adsorption and separation because of its rich pore structure, high specific surface area, low price and easy modification in the later stage. Especially in the adsorption of industrial toxic gases, the developed microporous structure of activated carbon provides abundant adsorption sites, as well as mesopores and macropores as diffusion and transmission channels, which can achieve efficient adsorption of most gas molecules. It is often called a "universal adsorbent". However, some cyclic small molecule gases, such as ethylene oxide and propylene oxide, require catalytic ring-opening reactions, so a single activated carbon material shows weak capture ability and poor adsorption performance. Metal organic framework materials (MOFs) are an emerging adsorption material with their large specific surface area and pore volume, which perform well in gas adsorption and separation. The pore structure can be precisely controlled by repairing the synthesis method to achieve selective adsorption of specific molecules. In addition, MOFs have good chemical stability and sustainability. Through the pore structure, they can provide a highly selective adsorption environment, which helps to introduce the target molecules near the catalytic active sites and promote specific reactions through surface functional groups, showing potential application prospects in the fields of adsorption and catalysis. According to the different metal ions and organic ligands that constitute MOFs, MOFs can be divided into many types, such as ZIFs, MILs, UIOs, etc. Each type has unique physical and chemical properties and application characteristics. In particular, zirconium-based metal organic framework materials are known for their highly adjustable pore structure, chemical stability and good thermal stability. Their excellent surface area and pore size adjustment capabilities make them suitable for various gas adsorption, catalysis and separation applications. However, MOFs also have some shortcomings, such as difficult molding, complex synthesis process, and high cost, which limit their promotion and application in industrial applications. Therefore, it is necessary to develop new adsorption materials with excellent broad-spectrum performance for industrial toxic gases, and new composite materials that can comprehensively and effectively adsorb and purify small molecule organic gases and large molecule organic gases, so as to achieve their wider application in the field of adsorption materials. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] The present invention provides an activated carbon-zirconium-based metal organic framework composite material and a preparation method thereof, in order to solve the technical problem of how to improve the microporous adsorption capacity of activated carbon so that it can effectively purify small molecular cyclic gases such as ethylene oxide and propylene oxide.
[0006] (II) Technical solution
[0007] In order to solve the above technical problems, the present invention provides a method for preparing an activated carbon-zirconium-based metal organic framework composite material, which comprises the following steps:
[0008] S1. Dissolve zirconium oxychloride and organic ligand in a mixed solution of N,N-dimethylformamide and glacial acetic acid, perform hydrothermal reaction at 110-150°C, wash the obtained product with N,N-dimethylformamide and ethanol by centrifugation in sequence, and dry it in vacuo; wherein, when the organic ligand is terephthalic acid, a UIO-66 matrix is obtained; when the organic ligand is 2-aminoterephthalic acid, a UIO-66-NH2 matrix is obtained; when the organic ligand is a combination of terephthalic acid and 2-aminoterephthalic acid, a UIO-66 / UIO-66-NH2 composite matrix is obtained;
[0009] S2. The activated carbon, the UIO-66 matrix, the UIO-66-NH2 matrix or the UIO-66 / UIO-66-NH2 composite matrix obtained in step S1 are ground into powders and dried;
[0010] S3. The dried powdered activated carbon, and UIO-66, UIO-66-NH2 or UIO-66 / UIO-66-NH2 matrix powder were placed in a beaker and deionized water was added to mix well;
[0011] S4. After the mixed material obtained in step S3 is precipitated at the bottom of the beaker, the supernatant is removed, the mixed material at the bottom is taken and placed in a mixer, and then the binder is dissolved in hot water and injected into the mixer. After bonding, it is extruded by a molding extrusion device to obtain a strip composite sample;
[0012] S5. The strip composite sample extruded in step S4 is dried to completely remove moisture, and after drying, the sample is crushed and screened;
[0013] S6. Under nitrogen protection, the crushed sample obtained in step S5 is subjected to secondary carbonization and activation, so that part of the binder is volatilized and a secondary pore structure is formed, while the strength of the composite material is maintained, thereby obtaining an activated carbon-zirconium-based metal organic framework composite material.
[0014] Furthermore, the preparation method specifically comprises the following steps:
[0015] S1. Dissolve zirconium oxychloride and organic ligand in a mass ratio of 1:(1-1.5) in a mixed solution of N,N-dimethylformamide and glacial acetic acid in a mass ratio of 1:(1-1.5), and perform hydrothermal reaction at 110-150°C for 18-36h. Wash the obtained product by centrifugation with N,N-dimethylformamide and ethanol at a speed of 4000-7000rpm for 3 times, each time for 3-5min, and vacuum dry at 100-120°C for 8-12h. When the organic ligand is terephthalic acid, a UIO-66 matrix is obtained; when the organic ligand is 2-aminoterephthalic acid, a UIO-66-NH2 matrix is obtained; when the organic ligand is a combination of terephthalic acid and 2-aminoterephthalic acid, a UIO-66 / UIO-66-NH2 composite matrix is obtained.
[0016] S2. The activated carbon, the UIO-66 matrix obtained in step S1, the UIO-66-NH2 matrix or the UIO-66 / UIO-66-NH2 composite matrix were ground into powders and dried in an oven at 110°C;
[0017] S3. Place 70-90% of the powdered activated carbon dried in step S3 and 10-30% of the UIO-66, UIO-66-NH2 or UIO-66 / UIO-66-NH2 matrix powder in a beaker, add 100-150 ml of deionized water, and stir at 5000-7000 rpm for 10-30 min to fully mix;
[0018] S4. After the mixed material obtained in step S3 is precipitated at the bottom of the beaker, the supernatant is removed, the mixed material at the bottom is taken and placed in a mixer, and then a binder having a mass fraction of 4 to 10% of the mixed material is dissolved in hot water at 70 to 90°C, and injected into the mixer by spraying, and after bonding, extrusion is performed by a molding extrusion device to obtain a strip-shaped composite sample;
[0019] S5. The composite strip sample extruded in step S4 is placed in a 120°C blast oven for heating and drying for 6 to 8 hours to completely remove moisture, and after drying, the sample is crushed and screened according to a 10 to 24 mesh standard;
[0020] S6. Under nitrogen protection, the crushed sample obtained in step S5 is kept at 160-200° C. in a tubular furnace for 2 hours for secondary carbonization and activation, so that part of the binder is volatilized and a secondary pore structure is formed while maintaining the strength of the composite material, thereby obtaining an activated carbon-zirconium-based metal organic framework composite material.
[0021] Furthermore, in step S1, when the organic ligand is a combination of terephthalic acid and 2-aminoterephthalic acid, the molar ratio of terephthalic acid to 2-aminoterephthalic acid is 7:3 or 3:7.
[0022] Furthermore, in step S2, the activated carbon is selected from coal-based activated carbon or coconut shell activated carbon.
[0023] Furthermore, in step S2, the particle size of the activated carbon powder is 160-200 mesh and the specific surface area is 800-1400m 2 / g.
[0024] Furthermore, in step S2, the particle size of the UIO-66, UIO-66-NH2 or UIO-66 / UIO-66-NH2 matrix powder is 160-200 mesh and the specific surface area is 600-1000m 2 / g.
[0025] Furthermore, in step S3, the binder is hydroxypropyl methylcellulose or polypropylene alcohol.
[0026] In addition, the present invention also provides an activated carbon-zirconium-based metal organic framework composite material, and the activated carbon-zirconium-based metal organic framework composite material is prepared by the above method.
[0027] (III) Beneficial effects
[0028] The present invention proposes an activated carbon-zirconium-based metal organic framework composite material and a preparation method thereof, which breaks through the shortcomings of the weak adsorption capacity of activated carbon for small molecular cyclic substances and the difficulty in molding metal organic framework materials. The composite material with high specific surface area is formed by mixed molding and strong synergistic effect, which can significantly improve the microporous adsorption capacity of activated carbon, and has the adsorption and purification capacity for small molecular cyclic gases, such as ethylene oxide, and larger molecular gases, such as toluene. Through the adsorption test of toluene, it is shown that the introduction of the metal organic framework has little effect on large molecular cyclic gases mainly by physical adsorption. Through reasonable design and preparation, the present invention utilizes the dual adsorption characteristics of activated carbon and zirconium-based metal organic framework composite materials, so that the composite material exhibits a broad spectrum of adsorption characteristics for substances of various molecular sizes in the adsorption environment, can effectively deal with toxic gases of different molecular sizes and structures, and is applied to the fields of chemical protection equipment and air purification to achieve efficient purification of industrial toxic gases, providing a reliable gas treatment solution for industrial production.
[0029] The technical effects of the present invention are mainly reflected in the following aspects:
[0030] (1) This method utilizes the multi-level pore structure of activated carbon-zirconium-based metal organic framework composite materials to show significant capture ability for small molecule targets. This technology can not only improve the adsorption performance of activated carbon micropores, but also enhance its synergistic effect with zirconium-based metal organic framework materials to improve the efficient and broad-spectrum adsorption capacity for various pollutants.
[0031] (2) The combination of metal organic framework materials and activated carbon can fully utilize the advantages of both: the metal organic framework material provides catalytic activity, and the activated carbon improves the adsorption efficiency through its large surface area and pore structure. The composite material can not only effectively catalyze the conversion of toxic gases, but also maintain a high physical adsorption performance, thereby achieving efficient purification and treatment of complex industrial waste gas.
[0032] (3) This composite material can overcome the challenges of the previous pure activated carbon's insufficient adsorption capacity for small molecule cyclic substances and the difficulty in molding pure metal organic framework materials. By mixing and molding activated carbon and metal organic framework materials, this method successfully prepared a composite material with excellent performance without destroying the crystal structure of the two. This preparation method is not only simple but also has good repeatability and is suitable for large-scale production.
[0033] The present invention significantly improves the adsorption and purification efficiency of specific industrial toxic gases through innovative material combination and preparation process, and demonstrates great potential in practical applications. DETAILED DESCRIPTION
[0034] In order to make the purpose, content and advantages of the present invention more clear, the specific implementation methods of the present invention are further described in detail below in conjunction with embodiments.
[0035] Example 1
[0036] 1) Dissolve 1 mmol of zirconium oxychloride and 1 mmol of terephthalic acid in 10 ml of a mixed solution of N, N-dimethylformamide and glacial acetic acid, and perform a hydrothermal reaction at 120°C for 24 h. Wash the obtained product with N, N-dimethylformamide and ethanol by centrifugation at 5000 rpm for 3 times, each time for 5 min. Dry the product in vacuum at 120°C for 8 h to obtain a UIO-66 matrix.
[0037] 2) Grind DX-09 coal-based activated carbon and UIO-66 into powders of 160-200 mesh respectively, and dry them in a forced air drying oven at 120°C for 8 hours;
[0038] 3) 200 g of activated carbon powder and 50 g of UIO-66 powder in step 2) were placed in a beaker, 750 ml of deionized water were added, and the mixture was stirred at 5000 rpm for 20 min to fully mix;
[0039] 4) After the composite material prepared in step 3) is precipitated at the bottom of the beaker, the upper clear liquid is removed, and the bottom composite material is placed in a mixer, and then 15 g of hydroxypropyl methylcellulose is dissolved in 30 ml of 70° C. hot water, and injected into the mixer by spraying. After bonding and forming, it is extruded into a Φ3 mm strip in a molding extrusion device;
[0040] 5) placing the extruded strip composite sample in step 4) in a 120° C. forced air oven for heating and drying for 8 hours to completely remove moisture, and after drying, crushing and screening the sample according to a 10-24 mesh standard;
[0041] 6) The crushed sample in step 5) is placed in a tubular furnace at 160° C. for 2 h under nitrogen protection for secondary carbonization and activation, so that part of the binder volatilizes at this temperature and forms secondary pores while maintaining a high strength, thereby obtaining a composite material product.
[0042] Example 2
[0043] 1) Dissolve 1 mmol of zirconium oxychloride and 1 mmol of 2-aminoterephthalic acid in 10 ml of a mixed solution of N,N-dimethylformamide and glacial acetic acid, and perform a hydrothermal reaction at 120°C for 24 h. Wash the obtained product with N,N-dimethylformamide and ethanol by centrifugation at 5000 rpm for 3 times, each time for 5 min. Dry the product in vacuum at 120°C for 8 h to obtain a UIO-66-NH2 matrix.
[0044] 2) Grind DX-09 coal-based activated carbon and UIO-66-NH2 into powders of 160-200 mesh respectively, and dry them in a forced air drying oven at 120°C for 8 hours;
[0045] 3) 200 g of activated carbon powder and 50 g of UIO-66-NH2 powder in step 2) were placed in a beaker, 750 ml of deionized water were added, and the mixture was stirred at 5000 rpm for 20 min to fully mix;
[0046] 4) After the composite material prepared in step 3) is precipitated at the bottom of the beaker, the upper clear liquid is removed, and the bottom composite material is placed in a mixer, and then 15 g of hydroxypropyl methylcellulose is dissolved in 30 ml of 70° C. hot water, and injected into the mixer by spraying. After bonding and forming, it is extruded into a Φ3 mm strip in a molding extrusion device;
[0047] 5) placing the extruded strip composite sample in step 4) in a 120° C. forced air oven for heating and drying for 8 hours to completely remove moisture, and after drying, crushing and screening the sample according to a 10-24 mesh standard;
[0048] 6) The crushed sample in step 5) is placed in a tubular furnace at 160° C. for 2 h under nitrogen protection for secondary carbonization and activation, so that part of the binder volatilizes at this temperature and forms secondary pores while maintaining a high strength, thereby obtaining a composite material product.
[0049] Example 3
[0050] 1) 1 mmol of zirconium oxychloride, 0.7 mmol of terephthalic acid and 0.3 mmol of 2-aminoterephthalic acid were dissolved in 10 ml of a mixed solution of N,N-dimethylformamide and glacial acetic acid, and subjected to hydrothermal reaction at 120°C for 24 h. The obtained product was centrifugally washed with N,N-dimethylformamide and ethanol at 5000 rpm for 3 times, each time for 5 min, and dried in vacuo at 120°C for 8 h to obtain a UIO-66 / UIO-66-NH2 (7:3) matrix.
[0051] 2) Grind DX-09 coal-based activated carbon and UIO-66 / UIO-66-NH2 (7:3) into powders of 160-200 mesh respectively, and dry them in a forced air drying oven at 120°C for 8 h;
[0052] 3) 200 g of activated carbon powder and 50 g of UIO-66 / UIO-66-NH2 (7:3) powder in step 2) were placed in a beaker, 750 ml of deionized water were added, and the mixture was stirred at 5000 rpm for 20 min to fully mix;
[0053] 4) After the composite material prepared in step 3) is precipitated at the bottom of the beaker, the upper clear liquid is removed, and the bottom composite material is placed in a mixer, and then 15 g of hydroxypropyl methylcellulose is dissolved in 30 ml of 70° C. hot water, and injected into the mixer by spraying. After bonding and forming, it is extruded into a Φ3 mm strip in a molding extrusion device;
[0054] 5) placing the extruded strip composite sample in step 4) in a 120° C. forced air oven for heating and drying for 8 hours to completely remove moisture, and after drying, crushing and screening the sample according to a 10-24 mesh standard;
[0055] 6) The crushed sample in step 5) is placed in a tubular furnace at 160° C. for 2 h under nitrogen protection for secondary carbonization and activation, so that part of the binder volatilizes at this temperature and forms secondary pores while maintaining a high strength, thereby obtaining a composite material product.
[0056] Example 4
[0057] 1) 1 mmol of zirconium oxychloride, 0.3 mmol of terephthalic acid and 0.7 mmol of 2-aminoterephthalic acid were dissolved in 10 ml of a mixed solution of N,N-dimethylformamide and glacial acetic acid, and subjected to hydrothermal reaction at 120°C for 24 h. The obtained product was centrifugally washed with N,N-dimethylformamide and ethanol at 5000 rpm for 3 times, each time for 5 min, and dried in vacuo at 120°C for 8 h to obtain a UIO-66 / UIO-66-NH2 (3:7) matrix.
[0058] 2) Grind DX-09 coal-based activated carbon and UIO-66 / UIO-66-NH2 (3:7) into powders of 160-200 mesh, and dry them in a forced air drying oven at 120°C for 8 h;
[0059] 3) 200 g of activated carbon powder and 50 g of UIO-66 / UIO-66-NH2 (3:7) powder in step 2) were placed in a beaker, 750 ml of deionized water were added, and the mixture was stirred at 5000 rpm for 20 min to fully mix;
[0060] 4) After the composite material prepared in step 3) is precipitated at the bottom of the beaker, the upper clear liquid is removed, and the bottom composite material is placed in a mixer, and then 15 g of hydroxypropyl methylcellulose is dissolved in 30 ml of 70° C. hot water, and injected into the mixer by spraying. After bonding and forming, it is extruded into a Φ3 mm strip in a molding extrusion device;
[0061] 5) placing the extruded strip composite sample in step 4) in a 120° C. forced air oven for heating and drying for 8 hours to completely remove moisture, and after drying, crushing and screening the sample according to a 10-24 mesh standard;
[0062] 6) The crushed sample in step 5) is placed in a tubular furnace at 160° C. for 2 h under nitrogen protection for secondary carbonization and activation, so that part of the binder volatilizes at this temperature and forms secondary pores while maintaining a high strength, thereby obtaining a composite material product.
[0063] Example 5
[0064] 1) 1 mmol of zirconium oxychloride, 0.7 mmol of terephthalic acid and 0.3 mmol of 2-aminoterephthalic acid were dissolved in 10 ml of a mixed solution of N,N-dimethylformamide and glacial acetic acid, and subjected to hydrothermal reaction at 120°C for 24 h. The obtained product was centrifugally washed with N,N-dimethylformamide and ethanol at 5000 rpm for 3 times, each time for 5 min, and dried in vacuo at 120°C for 8 h to obtain a UIO-66 / UIO-66-NH2 (7:3) matrix.
[0065] 2) Grind KP coconut shell activated carbon and UIO-66 / UIO-66-NH2 (7:3) into 160-200 mesh powders respectively, and dry them in a forced air drying oven at 120°C for 8 h;
[0066] 3) 200 g of activated carbon powder and 50 g of UIO-66 / UIO-66-NH2 (7:3) powder in step 2) were placed in a beaker, 750 ml of deionized water were added, and the mixture was stirred at 5000 rpm for 20 min to fully mix;
[0067] 4) After the composite material prepared in step 3) is precipitated at the bottom of the beaker, the upper clear liquid is removed, and the bottom composite material is placed in a mixer, and then 50 g of polypropylene alcohol is dissolved in 50 ml of 80° C. hot water, and injected into the mixer by spraying. After bonding and forming, it is extruded into a Φ3 mm profile in a molding extrusion device;
[0068] 5) placing the extruded strip composite sample in step 4) in a 120° C. forced air oven for heating and drying for 8 hours to completely remove moisture, and after drying, crushing and screening the sample according to a 10-24 mesh standard;
[0069] 6) The crushed sample in step 5) is placed in a tubular furnace at 160° C. for 2 h under nitrogen protection for secondary carbonization and activation, so that part of the binder volatilizes at this temperature and forms secondary pores while maintaining a high strength, thereby obtaining a composite material product.
[0070] Example 6
[0071] 1) 1 mmol of zirconium oxychloride, 0.7 mmol of terephthalic acid and 0.3 mmol of 2-aminoterephthalic acid were dissolved in 10 ml of a mixed solution of N,N-dimethylformamide and glacial acetic acid, and subjected to hydrothermal reaction at 120°C for 24 h. The obtained product was centrifugally washed three times with N,N-dimethylformamide and ethanol at 7000 rpm for 3 min each time, and dried in vacuo at 120°C for 8 h to obtain a UIO-66 / UIO-66-NH2 (7:3) matrix.
[0072] 2) Grind DX-09 coal-based activated carbon and UIO-66 / UIO-66-NH2 (7:3) into powders of 160-200 mesh, and dry them in a forced air drying oven at 110°C for 8 h;
[0073] 3) 200 g of activated carbon powder and 50 g of UIO-66 / UIO-66-NH2 (7:3) powder in step 2) were placed in a beaker, 750 ml of deionized water were added, and the mixture was stirred at 5000 rpm for 20 min to fully mix;
[0074] 4) After the composite material prepared in step 3) is precipitated at the bottom of the beaker, the upper clear liquid is removed, and the bottom composite material is placed in a mixer, and then 50 g of polypropylene alcohol is dissolved in 50 ml of 80° C. hot water, and injected into the mixer by spraying. After bonding and forming, it is extruded into a Φ3 mm profile in a molding extrusion device;
[0075] 5) placing the extruded strip composite sample in step 4) in a 120° C. forced air oven for heating and drying for 8 hours to completely remove moisture, and after drying, crushing and screening the sample according to a 10-24 mesh standard;
[0076] 6) The crushed sample in step 5) is placed in a tubular furnace at 160° C. for 2 h under nitrogen protection for secondary carbonization and activation, so that part of the binder volatilizes at this temperature and forms secondary pores while maintaining a high strength, thereby obtaining a composite material product.
[0077] Example 7
[0078] 1) 1 mmol of zirconium oxychloride, 0.7 mmol of terephthalic acid and 0.3 mmol of 2-aminoterephthalic acid were dissolved in 10 ml of a mixed solution of N,N-dimethylformamide and glacial acetic acid, and subjected to hydrothermal reaction at 120°C for 24 h. The obtained product was centrifugally washed three times with N,N-dimethylformamide and ethanol at 7000 rpm for 3 min each time, and dried in vacuo at 120°C for 8 h to obtain a UIO-66 / UIO-66-NH2 (7:3) matrix.
[0079] 2) Grind KP coconut shell activated carbon and UIO-66 / UIO-66-NH2 (7:3) into 160-200 mesh powders respectively, and dry them in a forced air drying oven at 120°C for 8 h;
[0080] 3) 200 g of activated carbon powder and 50 g of UIO-66 / UIO-66-NH2 (7:3) powder in step 2) were placed in a beaker, 750 ml of deionized water were added, and the mixture was stirred at 5000 rpm for 20 min to fully mix;
[0081] 4) After the composite material prepared in step 3) is precipitated at the bottom of the beaker, the upper clear liquid is removed, and the bottom composite material is placed in a mixer, and then 30 g of hydroxypropyl methylcellulose is dissolved in 60 ml of 70° C. hot water, and injected into the mixer by spraying. After bonding and forming, it is extruded into a Φ3 mm strip in a molding extrusion device;
[0082] 5) placing the extruded strip composite sample in step 4) in a 120° C. forced air oven for heating and drying for 8 hours to completely remove moisture, and after drying, crushing and screening the sample according to a 10-24 mesh standard;
[0083] 6) The crushed sample in step 5) is placed in a tubular furnace at 160° C. for 2 h under nitrogen protection for secondary carbonization and activation, so that part of the binder volatilizes at this temperature and forms secondary pores while maintaining a high strength, thereby obtaining a composite material product.
[0084] The test results of various physical properties of Examples 1 to 7 and Comparative Example 1 (DX-09 activated carbon sample), Comparative Example 2 (KP activated carbon sample), Comparative Example 3 (UIO-66), Comparative Example 4 (UIO-66-NH2), Comparative Example 5 (UIO-66 / UIO-66-NH2 (7:3)), and Comparative Example 6 (UIO-66 / UIO-66-NH2 (3:7) are shown in Table 1.
[0085] Table 1 Physical properties test results of each sample
[0086]
[0087] As can be seen from Table 1, among the samples prepared in Examples 1 to 7, the sample in Example 5 has the largest specific surface area, a high volume of micropores and mesopores, and a sample strength of up to 90%. The specific surface area and strength of Example 7 are second only to those of Example 5. In contrast, the metal organic framework materials prepared in Examples 3 to 6 are bonded and extruded in the same manner, and have lower strengths, especially the strength of Example 4, which is only 76%. It can be seen that the metal organic framework material powder molding still has a relatively low strength, and activated carbon needs to be combined to maintain a high strength. In addition, the composite material prepared by using polypropylene alcohol as a mixed adhesive in Examples 3 and 6 also has the best comprehensive performance.
[0088] The present invention studies the dynamic adsorption performance of the above 8 activated carbon-zirconium-based metal organic framework composite materials on ethylene oxide and toluene through fixed bed adsorption experiments. The dynamic adsorption experiment was carried out under the conditions of airflow relative humidity of 10%, 50% and 90% respectively to evaluate the adsorption capacity of the material on different substances under extremely dry, normal and extremely wet conditions. The fixed bed used in the experiment had a diameter of 2 cm, a sample filling layer height of 2 cm, and an airflow rate set to 0.78 L / min; the initial concentration of ethylene oxide was 200 ppm, the initial concentration of toluene was 3000 ppm, and the breakthrough concentration was set to 10 ppm. The initial concentration and breakthrough concentration of the two substances were monitored in real time by a GC-8890 chromatograph to determine the protection time of the bed.
[0089] Table 2 Test results of protection performance of each sample
[0090]
[0091] According to the data listed in Table 2, it is observed that the two activated carbon samples (Comparative Example 1 and Comparative Example 2) have good protection performance for toluene at 10%, 50% and 90% air humidity, but the protection effect on ethylene oxide is poor. In contrast, the adsorption performance of the four metal organic framework samples for toluene is slightly lower than that of the activated carbon sample, but they show a certain protection time in the adsorption of ethylene oxide. This difference can be explained by the fact that toluene is mainly achieved through microporous physical adsorption, while the adsorption pore structure of the metal organic framework material affects the adsorption of toluene, so its protection time is not as good as that of the activated carbon material. For the removal of ethylene oxide, it mainly depends on the acidic sites on the surface of the metal organic framework material for chemical adsorption. In addition, as the air humidity increases, the competitive adsorption of water molecules will also increase, thereby weakening the material's adsorption capacity for the target. Therefore, the excellent catalytic performance of the metal organic framework material can effectively improve the adsorption capacity for ethylene oxide. The new composite material is innovatively made by combining activated carbon and metal organic framework at the atomic scale, spraying with a binder and extruding, and then calcining at high temperature. It has the advantages of both activated carbon and metal organic framework adsorption materials. The introduction of metal organic framework material makes fuller use of the micropores of activated carbon, greatly improves the adsorption capacity of ethylene oxide, and forms a powerful "synergistic effect". For example, in Example 7, the metal organic framework material only accounts for 20% of the total mass, but under different humidity conditions, the protection time for ethylene oxide reaches 28min, 22min and 15min respectively. At the same time, the metal organic framework material not only solves the molding problem of the composite material, but also the composite with the activated carbon material makes the adsorption capacity of toluene under different humidity conditions still maintain a high level. These results further verify the potential of the composite material in protecting harmful gases and provide new ideas for material design and application.
[0092] The present invention provides a new application of an activated carbon-zirconium-based metal organic framework composite material in the field of industrial toxic gas adsorption and purification. At present, the existing technology mainly focuses on the modification of activated carbon and metal organic framework materials, and their application in some industrial chemical toxic gases. However, the application of activated carbon-zirconium-based metal organic framework composite materials in the adsorption and purification of industrial toxic gases such as small organic molecule rings and larger organic molecule gases is still rare. The organic chemical gases involved in the present invention include small molecule heterocyclic compounds and larger molecule cyclic compounds, represented by ethylene oxide and toluene respectively. The concentration range of toxic gases in industrial environments is generally between 5ppm and 3000ppm, and the relative humidity of the air is usually between 10% and 90%.
[0093] Through experimental verification, the present invention uses the activated carbon-zirconium-based metal organic framework composite material to adsorb and purify two typical industrial toxic gases, ethylene oxide and toluene, thereby proving the effectiveness of the material in specific application fields.
[0094] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an activated carbon-zirconium-based metal organic framework composite material, characterized in that: The preparation method comprises the following steps: S1. Dissolve zirconium oxychloride and organic ligand in a mixed solution of N,N-dimethylformamide and glacial acetic acid, perform hydrothermal reaction at 110-150°C, wash the obtained product with N,N-dimethylformamide and ethanol by centrifugation in sequence, and dry it in vacuo; wherein, when the organic ligand is terephthalic acid, a UIO-66 matrix is obtained; when the organic ligand is 2-aminoterephthalic acid, a UIO-66-NH2 matrix is obtained; when the organic ligand is a combination of terephthalic acid and 2-aminoterephthalic acid, a UIO-66 / UIO-66-NH2 composite matrix is obtained; S2. The activated carbon, the UIO-66 matrix, the UIO-66-NH2 matrix or the UIO-66 / UIO-66-NH2 composite matrix obtained in step S1 are ground into powders and dried; S3. The dried activated carbon powder, as well as UIO-66, UIO-66-NH2 or UIO-66 / UIO-66-NH2 matrix powder were placed in a beaker and deionized water was added to mix well; S4. After the mixed material obtained in step S3 is precipitated at the bottom of the beaker, the supernatant is removed, the mixed material at the bottom is taken and placed in a mixer, and then the binder is dissolved in hot water and injected into the mixer. After bonding, it is extruded by a molding extrusion device to obtain a strip composite sample; S5. The strip composite sample extruded in step S4 is dried to completely remove moisture, and after drying, the sample is crushed and screened; S6. Under nitrogen protection, the crushed sample obtained in step S5 is subjected to secondary carbonization and activation, so that part of the binder is volatilized and a secondary pore structure is formed, while the strength of the composite material is maintained, thereby obtaining an activated carbon-zirconium-based metal organic framework composite material.
2. The method for preparing the activated carbon-zirconium-based metal organic framework composite material according to claim 1, characterized in that: The preparation method specifically comprises the following steps: S1. Dissolve zirconium oxychloride and organic ligand in a mass ratio of 1:(1-1.5) in a mixed solution of N,N-dimethylformamide and glacial acetic acid in a mass ratio of 1:(1-1.5), and perform hydrothermal reaction at 110-150°C for 18-36h. Wash the obtained product by centrifugation with N,N-dimethylformamide and ethanol at a speed of 4000-7000rpm for 3 times, each time for 3-5min, and vacuum dry at 100-120°C for 8-12h. When the organic ligand is terephthalic acid, a UIO-66 matrix is obtained; when the organic ligand is 2-aminoterephthalic acid, a UIO-66-NH2 matrix is obtained; when the organic ligand is a combination of terephthalic acid and 2-aminoterephthalic acid, a UIO-66 / UIO-66-NH2 composite matrix is obtained. S2. The activated carbon, the UIO-66 matrix obtained in step S1, the UIO-66-NH2 matrix or the UIO-66 / UIO-66-NH2 composite matrix were ground into powders and dried in an oven at 110°C; S3. Place 70-90% of the powdered activated carbon dried in step S3 and 10-30% of the UIO-66, UIO-66-NH2 or UIO-66 / UIO-66-NH2 matrix powder in a beaker, add 100-150 ml of deionized water, and stir at 5000-7000 rpm for 10-30 min to fully mix; S4. After the mixed material obtained in step S3 is precipitated at the bottom of the beaker, the supernatant is removed, the mixed material at the bottom is taken and placed in a mixer, and then a binder having a mass fraction of 4 to 10% of the mixed material is dissolved in hot water at 70 to 90°C, and injected into the mixer by spraying, and after bonding, extrusion is performed by a molding extrusion device to obtain a strip-shaped composite sample; S5. The composite strip sample extruded in step S4 is placed in a 120°C blast oven for heating and drying for 6 to 8 hours to completely remove moisture, and after drying, the sample is crushed and screened according to a 10 to 24 mesh standard; S6. Under nitrogen protection, the crushed sample obtained in step S5 is kept at 160-200° C. in a tubular furnace for 2 hours for secondary carbonization and activation, so that part of the binder is volatilized and a secondary pore structure is formed while maintaining the strength of the composite material, thereby obtaining an activated carbon-zirconium-based metal organic framework composite material.
3. The method for preparing an activated carbon-zirconium-based metal organic framework composite material according to claim 1 or 2, characterized in that: In step S1, when the organic ligand is a combination of terephthalic acid and 2-aminoterephthalic acid, the molar ratio of terephthalic acid to 2-aminoterephthalic acid is 7:3 or 3:
7.
4. The method for preparing an activated carbon-zirconium-based metal organic framework composite material according to claim 1 or 2, characterized in that: In step S2, the activated carbon is selected from coal-based activated carbon or coconut shell activated carbon.
5. The method for preparing an activated carbon-zirconium-based metal organic framework composite material according to claim 1 or 2, characterized in that: In step S2, the particle size of the activated carbon powder is 160-200 mesh and the specific surface area is 800-1400m 2 / g.
6. The method for preparing an activated carbon-zirconium-based metal organic framework composite material according to claim 1 or 2, characterized in that: In step S2, the particle size of the UIO-66, UIO-66-NH2 or UIO-66 / UIO-66-NH2 matrix powder is 160-200 mesh and the specific surface area is 600-1000m 2 / g.
7. The method for preparing an activated carbon-zirconium-based metal organic framework composite material according to claim 1 or 2, characterized in that: In step S3, the binder is hydroxypropyl methylcellulose or polypropylene alcohol.
8. An activated carbon-zirconium-based metal organic framework composite material, characterized in that: The activated carbon-zirconium-based metal organic framework composite material is prepared by the method according to any one of claims 1 to 7.