Catalyst support comprising uniformly distributed titanium dioxide and method for production thereof
By adjusting the pH of the alumina suspension and adding a titanium compound solution to form a catalyst support after heating and drying, the problem of uneven distribution of titanium compounds is solved and the performance of the catalyst is improved.
Patent Information
- Application Number
- CN202411007540.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-01-22
- Filing Date
- 2019-01-21
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the distribution of titanium compounds on the catalyst support is uneven, resulting in poor catalyst performance.
By preparing an alumina suspension and adjusting its pH to 4-5, a titanium compound solution is added to form an alumina/titanium compound suspension, followed by heating and drying to form a uniformly distributed catalyst support.
The uniform distribution of titanium compounds on the alumina catalyst support is significantly improved, and the performance and efficiency of the catalyst are improved.
Smart Images

Figure CN118949962A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese patent application No. 201980006763.8, filed on January 21, 2019, entitled “Catalyst carrier containing uniformly distributed titanium dioxide and production method thereof”. Technical Field
[0002] The present invention relates to a method for preparing a catalyst support comprising at least uniformly distributed titanium dioxide and aluminum oxide, and to a catalyst support prepared by this method. Background Art
[0003] WO 2014 / 020507A2 describes a method for introducing a titanium compound into a catalyst support material by impregnation. A suitable impregnation liquid medium can be used to achieve contact between the titanium compound and the catalyst support material. The examples of WO 2014 / 020507A2 disclose the use of ethanol as an organic liquid medium for contacting the catalyst support material with the titanium compound during the preparation of the titanium compound-modified catalyst support. Although not illustrated, WO 2014 / 020507A2 also discloses that an inorganic liquid medium such as water can be used to contact the catalyst support material with the titanium compound.
[0004] WO 2013 / 114098 A1 discloses a process in which an aqueous composition of a carboxylic acid and a titanium compound is prepared and added simultaneously to a catalyst support material, ie it is a mixture of the titanium compound and the carboxylic acid which is added to the catalyst support material.
[0005] US2005 / 0124490 discloses a homogeneous, amorphous catalyst support comprising a modifying metal oxide and an alkali metal oxide, wherein the modifying metal oxide is uniformly distributed throughout the alkali metal oxide. US2005 / 0124490 describes a precipitation process in which an alumina salt is used as a raw material to produce modified alumina.
[0006] The preparation methods of the prior art vary or result in the production of catalysts in which the titanium compound is not uniformly dispersed on the catalyst support. Therefore, there is a need to improve such methods. Summary of the invention
[0007] According to a first aspect of the present invention, there is provided a method for preparing a catalyst carrier, the method comprising:
[0008] i) preparing an alumina suspension having a pH of 6-8; wherein the alumina suspension comprises alumina selected from the group consisting of transition alumina, boehmite and mixtures thereof, and preferably γ-alumina;
[0009] ii) preparing a titanium compound solution;
[0010] iii) adding an acid to the alumina suspension until the pH of the alumina suspension is between 4 and 5 to form an acid-modified alumina suspension; and
[0011] iv) adding the titanium compound solution to the acid-modified alumina suspension to form an alumina / titanium compound suspension.
[0012] The method may further comprise the step of adding an acid to the alumina / titanium compound suspension to form an acid-modified alumina / titanium compound suspension.
[0013] The method may further comprise the step of heating the alumina / titanium compound suspension or the acid-modified alumina / titanium compound suspension to form a heated alumina / titanium compound suspension or a heated acid-modified alumina / titanium compound suspension. The heating occurs at a temperature in the range of 30°C to 70°C, typically about 50°C, for 2 to 4 hours.
[0014] The process may comprise the step of drying the heated aluminium oxide / titanium compound suspension or the heated acid-modified aluminium oxide / titanium compound suspension.
[0015] The method may include the step of drying the acid-modified alumina suspension to form a dried alumina acid-modified mixture prior to adding the titanium compound solution.
[0016] According to a first option of the first aspect of the present invention, there is provided a method for preparing a catalyst carrier, the method comprising:
[0017] i) preparing an alumina suspension having a pH of 6-8; wherein the alumina suspension comprises alumina selected from the group consisting of transition alumina, boehmite and mixtures thereof, and preferably γ-alumina;
[0018] ii) preparing a titanium compound solution;
[0019] iii) adding an acid to the alumina suspension until the pH of the alumina suspension is between 4 and 5 to form an acid-modified alumina suspension;
[0020] iv) adding the titanium compound solution to the acid-modified alumina suspension to form an alumina / titanium compound suspension; and
[0021] v) drying the alumina / titanium compound suspension to form a dry alumina / titanium compound mixture.
[0022] According to the second option of the first aspect of the present invention, there is provided a method for preparing a catalyst carrier, the method comprising:
[0023] i) preparing an alumina suspension having a pH of 6-8; wherein the alumina suspension comprises alumina selected from the group consisting of transition alumina, boehmite and mixtures thereof, and preferably γ-alumina;
[0024] ii) preparing a titanium compound solution;
[0025] iii) adding an acid to the alumina suspension until the pH of the alumina suspension is between 4 and 5 to form an acid-modified alumina suspension;
[0026] iv) adding the titanium compound solution to the acid-modified alumina suspension to form an alumina / titanium compound suspension;
[0027] v) adding an acid to the alumina / titanium compound suspension to form an acid-modified alumina / titanium compound suspension; and
[0028] vi) drying the acid-modified alumina / titanium compound suspension to form a dry pH-modified alumina / titanium compound mixture.
[0029] The first and second options of the first aspect of the invention may further comprise the step of heating the alumina / titanium compound suspension or the acid-modified alumina / titanium suspension. Heating may occur at a temperature in the range of 30°C to 70°C, typically about 50°C, and preferably for 2-4 hours.
[0030] When the method of the present invention does not include a step of drying the acid-modified alumina suspension before adding the titanium compound solution, the acid added to the alumina suspension is preferably formic acid, lactic acid, citric acid or a mixture thereof, more preferably lactic acid, citric acid or a mixture thereof, and most preferably citric acid.
[0031] The percentage of acid added to the alumina suspension may be 5 wt% to 30 wt% of the acid-modified alumina suspension, preferably 5 wt% to 20 wt% of the acid-modified alumina suspension. However, it should be understood that the amount of acid added must be sufficient to reduce the pH of the alumina suspension from pH 6-8 to pH 4-5.
[0032] According to a third option of the first aspect of the present invention, there is provided a method for preparing a catalyst carrier, the method comprising:
[0033] i) preparing an alumina suspension having a pH of 6-8; wherein the alumina suspension comprises alumina selected from the group consisting of transition alumina, boehmite and mixtures thereof, and preferably γ-alumina;
[0034] ii) preparing a titanium compound solution;
[0035] iii) adding an acid to the alumina suspension until the pH of the alumina suspension is between 4 and 5 to form an acid-modified alumina suspension;
[0036] iv) drying the acid-modified alumina suspension to form a dried alumina acid-modified mixture;
[0037] v) adding the titanium compound solution to the dried alumina acid-modified mixture to form an alumina / titanium compound suspension; and
[0038] vi) drying the alumina / titanium compound suspension to form a dry alumina / titanium compound mixture.
[0039] According to a fourth option of the first aspect of the present invention, there is provided a method for preparing a catalyst carrier, the method comprising:
[0040] i) preparing an alumina suspension having a pH of 6-8; wherein the alumina suspension comprises alumina selected from the group consisting of transition alumina, boehmite and mixtures thereof, and preferably γ-alumina;
[0041] ii) preparing a titanium compound solution;
[0042] iii) adding an acid to the alumina suspension until the pH of the alumina suspension is between 4 and 5 to form an acid-modified alumina suspension;
[0043] iv) drying the acid-modified alumina suspension to form a dried alumina acid-modified mixture;
[0044] v) adding the titanium compound solution to the dried alumina acid-modified mixture to form an alumina / titanium compound suspension;
[0045] vi) adding an acid to the alumina / titanium compound suspension to form an acid-modified alumina / titanium compound suspension; and
[0046] vii) drying the acid-modified alumina / titanium compound suspension to form a dry acid-modified alumina / titanium compound mixture.
[0047] The third and fourth options of the first aspect of the invention may further comprise the step of heating the alumina / titanium compound suspension or the acid-modified alumina / titanium compound suspension. Heating may occur at a temperature in the range of 30°C to 70°C, typically about 50°C, and preferably for 2-4 hours.
[0048] It will be appreciated that the amount of acid added in step vi) of the fourth option of the first aspect of the invention is sufficient to ensure that the pH of the aluminium oxide / titanium compound suspension is maintained at pH 4-5.
[0049] Where the process of the invention comprises drying the acid-modified alumina suspension prior to adding the titanium compound solution, the added acid is preferably a carboxylic acid (an organic compound comprising at least one carboxyl group (C(=O)OH)) including formic acid, lactic acid, citric acid or mixtures thereof.
[0050] The percentage of acid added to the alumina suspension is 5 wt% to 30 wt% of the acid-modified alumina suspension, preferably 5 wt% to 20 wt% of the acid-modified alumina suspension. However, it should be understood that the amount of acid added must be sufficient to reduce the pH of the alumina suspension from pH 6-8 to pH 4-5.
[0051] It is preferred that the acid-modified alumina suspension is not dried before adding the titanium compound solution, such as according to the first and second options of the first aspect of the present invention (called balanced sedimentation filtration "EDF"), while it is preferred that the acid-modified alumina suspension is dried before adding the titanium compound solution (called incipient wetness "IW") according to the third and fourth options of the first aspect of the present invention.
[0052] The method (and option) of the first aspect of the invention may include a final step of calcining the dried alumina / titanium compound mixture or the dried acid-modified alumina / titanium compound mixture. Calcination is generally carried out at a temperature of 100° C. to 1000° C., preferably 400° C. to 600° C., each preferably for a period of 2 to 5 hours to produce a calcined catalyst support.
[0053] The transition alumina is preferably gamma-alumina (γ), delta-alumina (δ), theta-alumina (θ) or a mixture thereof. Most preferably, the transition alumina is gamma-alumina.
[0054] The alumina suspension is preferably prepared by suspending an alumina selected from the group consisting of transition alumina, boehmite and mixtures thereof, preferably gamma-alumina, in at least water, wherein the percentage of the alumina in the suspension is 5% to 60% relative to the entire alumina suspension, preferably 40% to 50% relative to the entire alumina suspension.
[0055] Preferably, the alumina in the alumina suspension is only alumina selected from the group consisting of transition alumina, boehmite and mixtures thereof, and preferably only gamma-alumina.
[0056] The titanium compound solution is prepared by dissolving a titanium precursor in at least water. Water-soluble titanium precursors that can be used include potassium titanium oxalate, ammonium titanium oxalate, ammonium titanium lactate or mixtures thereof. If necessary, the temperature of the at least water can be raised to 90°C to accelerate the dissolution process. The concentration of the titanium precursor in the solution should be as high as possible and is limited only by the solubility of the titanium precursor in the at least water. The preferred titanium solution is an aqueous solution of potassium titanium oxalate dehydrate made with a concentration of 1 wt% to 4 wt% calculated as TiO2. Before the titanium solution is added to the alumina suspension, it can be magnetically stirred for about 30 minutes. The titanium solution is preferably passed through an ion exchange column to remove any impurities, such as potassium, before being added to the alumina suspension. Therefore, before the titanium solution is added to the alumina suspension, it is preferably magnetically stirred for a period of time and (also independently therefrom) passed through an ion exchange column.
[0057] Any drying method known in the art can be used in the method of the present invention. Drying is generally carried out at a temperature of 80°C to 120°C for a period of 0.5 to 5 hours.
[0058] The alumina / titanium compound suspension comprises 99wt%-95wt%, most preferably 97wt%-99wt% of alumina calculated as Al2O3 and preferably 1wt%-5wt%, most preferably 1wt%-3wt% of titanium compound calculated as TiO2, relative to the sum of the alumina calculated as Al2O3 and the titanium compound calculated as TiO2.
[0059] The dry (including acid / pH modified) alumina / titanium compound mixture preferably comprises 99 wt% to 95 wt%, most preferably 99 wt% to 97 wt%, of alumina calculated as Al2O3 and preferably 1 wt% to 5 wt%, most preferably 1-3 wt% of titanium compound calculated as TiO2, relative to the total dry (including acid / pH modified) alumina / titanium compound mixture.
[0060] According to a second aspect of the present invention, there is provided a catalyst support prepared according to the first aspect of the present invention.
[0061] According to a third aspect of the present invention, there is provided a calcined catalyst support comprising an alumina support coated with 1 wt% to 5 wt% of TiO2 relative to the alumina support (Al2O3), the TiO2 being uniformly dispersed on the alumina support.
[0062] "Coating" refers to a surface covering formed on a support material, including coating the surfaces of the inner pore walls of the support material (but not within the bulk of the support).
[0063] The catalyst support preferably comprises an alumina support coated with 3 wt % to 5 wt % TiO 2 (measured after calcination) relative to the alumina support (Al 2 O 3 ).
[0064] The wt% of TiO2 in the catalyst support prepared according to the first aspect of the present invention is expressed based on the total weight of the catalyst support.
[0065] Most surprisingly, it has been found that the uniform distribution of the titanium compound on the alumina catalyst support is improved if the alumina suspension is first treated with an acid before contacting it with a solution of the titanium compound.
[0066] According to a fourth aspect of the present invention, there is provided a method for preparing a promoted catalyst support, the method comprising:
[0067] i) preparing a catalyst support according to the first aspect of the invention; and
[0068] ii) introducing a promoter onto and / or into the catalyst support, thereby obtaining a promoted catalyst support.
[0069] The promoter is preferably a manganese compound, including, for example, manganese hydroxide, manganese oxide and / or manganese oxihydroxide. Manganese can be added to the catalyst support together with the titanium compound solution, i.e. by mixing a manganese precursor, for example, manganese acetate, with the titanium compound solution of step ii) of the first aspect of the invention. Alternatively, the calcined catalyst support is impregnated with a manganese precursor, for example, manganese acetate.
[0070] The fourth aspect of the present invention may include a final step of calcination.
[0071] The catalyst support or promoted catalyst support prepared according to the present invention can be used in Fischer-Tropsch catalysts, hydrocarbon synthesis catalysts, hydrodesulfurization catalysts, hydrotreating catalysts, photocatalysts for NO oxidation, and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] The present invention will now be described in more detail with reference to the accompanying drawings and the following non-limiting examples, in which:
[0073] Figure 1 is a cross-sectional SEM image of Comparative Example 3, wherein white dots indicate TiO2 enrichment; and
[0074] Figure 2 is a cross-sectional SEM of Example 3. DETAILED DESCRIPTION
[0075] experiment:
[0076] The titanium(IV) dihydroxide (TALH) used was 1 wt% of the commercially available Aqueous solution of TALH of LA (calculated as TiO2).
[0077] In the following examples, the wt % of Ti in the catalyst support calculated as TiO2 is expressed based on the total weight of the catalyst support.
[0078] X-ray photoelectron spectroscopy (XPS) was used in the following examples to determine the distribution of TiO2 on the surface of the alumina. XPS is a surface-sensitive quantitative spectroscopic technique that can measure elemental composition in the range of a few parts per thousand. Since XPS is only sensitive to the surface, the samples were analyzed by XPS as is (as is the pellet) and after pulverization (crushing) using a pestle and mortar, and the ratios of the elements are reported. Approximately the same amount of sample was used for the grinding step (compared to the sample measuring the as is pellet) using a pestle and mortar, applying only enough force to break up the pellets.
[0079] XPS spectra were recorded on a KRATOS Axis Ultra DLD, which was operated with a fixed measurement spectrum pass energy of 160 eV and a single area pass energy of 20 eV. Measurements were made using an Al Kα monochromatic source. Due to the nature of the material, neutralization must be performed during acquisition. All spectra were energy corrected using C1s at 284.6 eV. All samples were mounted in a molybdenum sample holder in the form of loose powder. The peak area ratios of all carrier samples in the examples determined by XPS, as well as the calculated differences between the original particles and the crushed samples, are provided in Tables 1, 2 and 3. The greater the difference, the more inhomogeneous the sample. Homogeneous samples show very small or even negative values.
[0080] Embodiment - Option 1 and 2 of the first aspect of the invention
[0081] As previously mentioned, options 1 and 2 of the first aspect of the present invention do not include the step of drying the acid-modified alumina suspension prior to adding the titanium compound solution (referred to as equilibrium sedimentation filtration (hereinafter referred to as "EDF")).
[0082] Comparative Example 1: TALH Equilibrium Sedimentation Filtration (hereinafter referred to as "EDF") without Acid Addition
[0083] 38.8 g of Puralox SCCa-150 was suspended in 46.5 g of water to obtain a 45.5 wt% Al2O3 aqueous suspension. 164 g of TALH aqueous solution (1 wt% TiO2) was added to the alumina suspension and heated at 50° C. for 3 hours, filtered, dried and calcined at 550° C. The resulting modified support contained 1.1 wt% TiO2 (based on the total weight of the modified support).
[0084] Comparative Example 2 - Same method as described in WO 2013 / 114098A1: 1-step TALH with citric acid EDF-Premix
[0085] 38.6 g of Puralox SCCa-150 were suspended in 46 g of water (45.5 wt% suspension). 160 g of a mixed solution of TALH and citric acid were added to the suspension (1 wt% of TiO2 = 11 g TALH, 20 wt% citric acid, relative to the amount of TALH used = 2.2 g). The mixture was heated, stirred at 50°C for 3 h, filtered, dried and calcined at 550°C. The resulting modified support included 1.7 wt% of TiO2 (based on the total weight of the modified support).
[0086] Example 1: TALHEDF (AP15-171) using citric acid
[0087] 38.8 g of Puralox SCCa-150 was suspended in 46.5 g of water to obtain a 45.5 wt% Al2O3 aqueous suspension. 11.2 g of a 40 wt% citric acid solution was added to the suspension to adjust the pH of the suspension to pH 4, thereby producing an acid-modified alumina suspension. Then 164 g of a 1 wt% TiO2 aqueous TALH solution was added to the acid-modified alumina suspension, and the alumina / titanium compound suspension was heated at 50°C for 3 h with the pH controlled at 4 using citric acid, filtered, dried and calcined at 550°C. The resulting catalyst support included 2.2 wt% TiO2 (based on the total weight of the modified support).
[0088] The examples show that the addition of an acid to the alumina suspension prior to the addition of the Ti compound leads to a higher adsorption of TiO2 on the alumina compared to no acid treatment or premixing of the acid with titanium oxide (TiO2) according to Comparative Examples 1 and 2.
[0089] The Ti:Al ratios of the as-prepared particles of the catalyst support and the ground (crushed) samples prepared in Example 1 were found to be almost identical, and therefore the titania surface distribution was considered to be uniform over the entire inner and outer surfaces of the support particles. Functionalization of the alumina support with an acid (citric acid in this case, before TALH EDF impregnation as in Example 1) resulted in a uniform Ti distribution (see Table 1, Example 1 XPS Ti:Al peak ratios) compared to Comparative Example 2, in which the titanium compound and the carboxylic acid were contacted with the catalyst support simultaneously without pre-treating the catalyst support material with an acid, in which a non-uniform Ti distribution was obtained.
[0090] The results of the support modification confirmed that the improvement in adsorption was a function of pH and the fact that the alumina surface was acid functionalized.
[0091] These results are included in Table 1 below:
[0092] Table 1: XPS and ICP analysis of TALH EDF impregnation
[0093]
[0094] Embodiment - Option 3 and 4 of the first aspect of the invention
[0095] As previously mentioned, Options 3 and 4 of the first aspect of the present invention include the step of drying the acid-modified alumina suspension prior to adding the titanium compound solution (hereinafter referred to as incipient wetness "IW").
[0096] Comparative Example 3: TALH, without acid addition IW
[0097] 13.7 g TALH was dissolved in water to give 21 mL aqueous TALH solution. The TALH solution was then added dropwise to 54.4 g Puralox SCCa-2 / 150 suspension during intense mixing. Water was removed at 80°C under atmospheric pressure and calcined at 550°C for 3 hours. The resulting catalyst support contained 4.1 wt% TiO2, but the TiO2 distribution was not uniform (see Tables 2 and Figure 1 ).
[0098] Comparative Example 4: 1-step TALH using 20 wt% citric acid (expressed relative to TALH) IW(Premix)
[0099] 11.3 g TALH was dissolved in water to give 18 mL TALH aqueous solution. 2.3 g citric acid was added as a solid to the TALH solution. The solution was added to 38.8 g Puralox SCCa-2 / 150 suspension under vigorous mixing. Water was removed at 80°C under atmospheric pressure and calcined at 550°C for 3 hours. The resulting catalyst support had an uneven distribution of TiO2.
[0100] Example 2: 2-Step: 20 wt% Citric Acid, Dry, TALH IW
[0101] 18 mL of 20 wt% citric acid solution was added to 38.8 g of Puralox SCCa-2 / 150 suspension and mixed. The mixture was dried at 80°C under atmospheric pressure. 11.3 g of TALH was dissolved in water to obtain 18 mL of aqueous TALH solution. The solution was added to the dried acid-modified Puralox mixture to form an alumina / titanium compound suspension. The alumina / titanium dioxide compound suspension was then dried at 80°C to remove water and calcined at 550°C for 3 hours to obtain a catalyst support containing 4.1 wt% TiO2 and uniformly dispersed TiO2.
[0102] Example 3-2 - Steps: 5wt% citric acid, dry, TALH IW
[0103] A modified alumina support having 4.1 wt% TiO2 was prepared as described in Example 2, however, the Puralox was treated with a 5 wt% citric acid solution. The homogeneity of the dispersed TiO2 on the modified support was determined from Table 2 and Figure 2 is good.
[0104] Example 4: 2-step: 10 wt% lactic acid, dry, TALH IW
[0105] 14 mL of 10 wt% lactic acid solution was added to 29.2 g of Puralox SCCa-150 suspension and mixed. The mixture was dried at 80°C under atmospheric pressure. 8.5 g of TALH was dissolved in water to obtain 14 mL of aqueous TALH solution. This was added to the dried acid-treated Puralox mixture to form an alumina / titanium compound suspension. The alumina / titanium compound suspension was then dried at 80°C to remove water and calcined at 550°C for 3 hours to obtain a catalyst support having 4.1 wt% TiO2 and uniform Ti compound dispersion.
[0106] Example 5-2 - Steps: 5 wt% lactic acid, dry, TALH IW
[0107] 13 mL of 5 wt% lactic acid solution was added to 29.1 g of Puralox SCCa-150 suspension and mixed. The mixture was dried at 80°C under atmospheric pressure. 8.5 g of TALH was dissolved in water to obtain 13 mL of aqueous TALH solution. This was added to the dried acid-treated Puralox mixture prepared in the first step to form an alumina / titanium compound suspension. The alumina / titanium compound suspension was dried at 80°C to remove water and calcined at 550°C for 3 hours. The uniformity of the dispersed TiO2 on the catalyst support was good.
[0108] As outlined in the Examples and Table 2, adding the acid to the alumina suspension before contacting the alumina suspension or mixture with the titanium compound (TALH), i.e., a two-step treatment process, shows that TiO2 adsorption can be significantly improved and titanium oxide is evenly distributed on the inner and outer surfaces of the alumina support.
[0109] Table 2: XPS and ICP analysis of TALH IW impregnation:
[0110]
[0111] Embodiments of the fourth aspect of the present invention:
[0112] Mn impregnation example:
[0113] Comparative Example 5: TALH IW, MnAc IW without acid pretreatment
[0114] The catalyst support was prepared as described in Comparative Example 3, but manganese acetate (MnAc) was added via incipient wetness after calcination.
[0115] 26.9 g of TALH was dissolved in water to obtain 42 mL of TALH aqueous solution. This was added dropwise to 91.8 g of Puralox SCCa-150 and mixed with a Krups stirrer. Water was removed at 120°C under atmospheric pressure and calcined at 550°C for 3 hours. 12.5 g of manganese acetate tetrahydrate (Mn(CH3COO)2·4H2O) was dissolved in 42 mL of water and added dropwise to the calcined powder. The catalyst support was dried at 120°C and calcined again at 550°C for 3 hours to obtain a catalyst containing 3.9 wt% TiO2 and 4.7 wt% MnO2.
[0116] Comparative Example 6: 1-Step TALH IW, MnAc IW with 20 wt% Citric Acid
[0117] The catalyst support was prepared as described in Comparative Example 4, except that manganese acetate (MnAc) was added in a second incipient wetness step after drying.
[0118] 22.8 g TALH was dissolved in water to give 36 mL aqueous TALH solution. 4.6 g citric acid was added as a solid to the TALH solution. The solution was added dropwise to 78 g Puralox SCCa-2 / 150 while mixing with a Krups stirrer. Water was removed at 120°C under atmospheric pressure. 10.6 g manganese acetate tetrahydrate was dissolved in 36 mL water and added dropwise to the dried powder, dried at 120°C under atmospheric pressure and calcined in air at 550°C for 3 hours. The modified support contained 3.9 wt% TiO2 and 4.7 wt% MnO2
[0119] Comparative Example 7: 1-Step TALH IW, MnAc IW, using 20 wt% citric acid
[0120] The catalyst support was prepared as described in Comparative Example 4, but with the addition of MnAc during TALH-citric acid-IW:
[0121] 22.8 g TALH, 10.6 g manganese acetate tetrahydrate and 4.6 g citric acid were dissolved in water to give 36 mL of aqueous solution. The solution was added dropwise to 78 g Puralox SCCa-2 / 150 while mixing using a Krups stirrer. Water was removed at 120° C. under atmospheric pressure and the powder was calcined at 550° C. in air for 3 hours. The modified support contained 3.9 wt% TiO2 and 4.7 wt% MnO2.
[0122] Example 6: 2-Step: TALH and MnAc IW pretreated with 5 wt% citric acid
[0123] The catalyst support was prepared as described in Example 3, but with the addition of MnAc during the initial wetness of the TALH-citric acid:
[0124] 34 mL of 5 wt% citric acid solution was added to 73.9 g of Puralox SCCa-2 / 150 and mixed. The mixture was dried at 80° C. under atmospheric pressure. 21.5 g of TALH and 10 g of manganese (II) acetate tetrahydrate (Mn(CH3COO)2·4H2O) were dissolved in water to obtain 34 mL of TALH / Mn acetate aqueous solution.
[0125] In the second impregnation step, the TALH / MnAc aqueous solution was added to the dried acid-treated Puralox prepared in the first step, dried at 80°C to remove water, and calcined at 550°C for 3 hours to obtain a modified support with 4.1 wt% TiO2 and 4.7 wt% MnO2. Drying was performed at 80°C to prevent a large amount of acid loss during drying.
[0126] Example 7: 2-Step: TALH EDF, 5 wt% Citric Acid and Acetic Acid Mn IW
[0127] The catalyst support was prepared as described in Example 1, but with the addition of MnAc by incipient wetness after calcination:
[0128] An Al2O3 aqueous suspension was prepared by mixing 85.8 g of Puralox SCCa-2 / 150 with 102 mL of water, and the pH of the suspension was adjusted to 4 with a 40 wt% citric acid solution. 950 g of a 1 wt% TiO2TALH aqueous solution was then added to the suspension and heated to 50°C for 3 hours with the pH controlled at 4 using citric acid. The suspension was filtered, dried and calcined at 550°C. After calcination, 12.4 g of manganese acetate tetrahydrate was dissolved in 43 mL of water and added dropwise to the powder, dried at 120°C and calcined at 550°C for 3 hours.
[0129] Table 3 contains the XPS peak ratio results of Comparative Examples 5 and 6 for Ti and Mn modified samples prepared by the incipient wetness route, which shows that titanium oxide is mainly located on the inner surface of the support, while manganese is uniformly located on the inner and outer surfaces of the support.
[0130] The results are included in Table 3 below:
[0131] Table 3: XPS and ICP analysis of Mn(CH3COO)2·4H2O IW impregnation
[0132]
[0133] The present invention discloses the following
[0134] Item 1. A method for preparing a catalyst carrier, the method comprising the following steps:
[0135] i) preparing an alumina suspension having a pH of 6-8, wherein the alumina suspension comprises alumina selected from the group consisting of transition alumina, boehmite and mixtures thereof;
[0136] ii) preparing a titanium compound solution;
[0137] iii) adding an acid to the alumina suspension until the pH of the alumina suspension is
[0138] Between 4 and 5 to form an acid-modified alumina suspension; and
[0139] iv) adding the titanium compound solution to the acid-modified alumina suspension to form an alumina / titanium compound suspension.
[0140] Item 2. The method according to Item 1 further comprises the step of adding an acid to the aluminum oxide / titanium compound suspension to form an acid-modified aluminum oxide / titanium compound suspension.
[0141] Item 3. The method according to Item 1 or 2 further includes the step of heating the alumina / titanium compound suspension or the acid-modified alumina / titanium compound suspension to form a heated alumina / titanium compound suspension or a heated acid-modified alumina / titanium compound suspension.
[0142] Item 4. The method according to Item 1 further includes a step of drying the acid-modified alumina suspension to form a dried alumina acid-modified mixture before adding the titanium compound solution.
[0143] Item 5. The method according to any one of Items 1 to 3, wherein the acid added to the alumina suspension is formic acid, lactic acid, citric acid or a mixture thereof, preferably lactic acid, citric acid or a mixture thereof, and most preferably citric acid.
[0144] Item 6. A method according to any one of Items 1 to 5, wherein the aluminum oxide / titanium compound suspension contains 99wt% to 95wt%, most preferably 99wt% to 97wt%, of aluminum oxide calculated as Al2O3, and 1wt% to 5wt%, most preferably 1wt% to 3wt% of titanium compound calculated as TiO2, relative to the total amount of aluminum oxide calculated as Al2O3 and titanium compound calculated as TiO2.
[0145] Item 7. The method according to Item 4, wherein the added acid is a carboxylic acid selected from the group consisting of formic acid, lactic acid, citric acid and a mixture thereof.
[0146] Item 8. The method according to any one of Items 1 or 7, wherein the percentage of the acid added to the alumina suspension is 5 wt % to 30 wt % of the acid-modified alumina suspension.
[0147] wt%, preferably 5wt% to 20wt% of the acid-modified alumina suspension.
[0148] Item 9. The method according to any one of Items 1 to 8 comprises the following steps: drying a) an aluminum oxide / titanium compound suspension or a heated aluminum oxide / titanium compound suspension to form a dry aluminum oxide / titanium compound mixture, or b) an acid-modified aluminum oxide / titanium compound suspension or a heated acid-modified aluminum oxide / titanium compound suspension to form a dry acid-modified aluminum oxide / titanium compound mixture.
[0149] Item 10. The method according to any one of Items 1 to 9, comprising the step of calcining the dried alumina / titanium compound mixture or the dried acid-modified alumina / titanium compound mixture.
[0150] Item 11. The method according to any one of Items 1 to 10, wherein the transition alumina is γ-alumina, δ-alumina, θ-alumina or a mixture thereof, and is preferably γ-alumina.
[0151] Item 12. The method according to any one of Items 1 to 11, wherein the titanium compound solution is prepared by dissolving a titanium precursor in at least water.
[0152] Item 13. The method according to Item 12, wherein the titanium precursor is a water-soluble titanium precursor selected from the group consisting of potassium titanium oxalate, ammonium titanium oxalate, ammonium titanium lactate and mixtures thereof.
[0153] Item 14. A catalyst support prepared according to any one of items 1 to 13.
[0154] Item 15. A calcined catalyst support comprising an alumina support coated with 1 wt % to 5 wt % of TiO 2 relative to the alumina support (Al 2 O 3 ), the TiO 2 being uniformly dispersed on the alumina support.
[0155] Item 16. A method for preparing a promoter catalyst carrier, the method comprising:
[0156] i) preparing a catalyst support according to any one of items 1 to 13, and
[0157] ii) introducing a promoter onto and / or into the catalyst support, thereby obtaining a promoted catalyst support.
Claims
1. A calcined catalyst carrier comprising an alumina carrier coated with 1 wt % to 5 wt % TiO2 relative to the alumina carrier, wherein the TiO2 is uniformly dispersed on the alumina carrier to form a surface coating on the alumina carrier, including coating the surface of the inner pore wall of the alumina carrier that is not within the body of the alumina carrier, wherein the difference in the X-ray photoelectron spectroscopy peak area ratio of Ti:Al between the original catalyst carrier and the catalyst carrier crushed using a pestle and mortar is very small or negative.
2. The catalyst carrier according to claim 1, wherein the difference in the X-ray photoelectron spectroscopy peak area ratio of Ti:Al between the catalyst carrier as is and the catalyst carrier after pulverization using a pestle and mortar is 0.067 or less.
3. The catalyst support according to claim 1, comprising an alumina support coated with 3 wt% to 5 wt% TiO2 relative to the alumina support.
Citation Information
Patent Citations
Homogeneous modified-alumina fischer-tropsch catalyst supports
US20050124490A1
Treating of catalyst carrier, fischer - tropsch catalysts and method of preparation thereof
WO2013114098A1
catalysts
WO2014020507A2
Manufacturing method of titania-coated alumina particle
JP2004331444A
Hydrogenation catalyst for heavy oil and manufacturing method thereof
JP2006061845A