Battery cell shell surface defect repairing method
Through laser welding and scanning technology for surface defects of the battery cell shell, the problem of lithium battery shell defects exceeding the specifications is solved, efficient resource utilization and battery safety improvement are achieved, and the reliability and performance recovery of battery products are ensured. .
Patent Information
- Application Number
- CN202411102880.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-15
AI Technical Summary
Defects such as pits and indentations on the surface of the lithium battery cell shell exceed specification requirements, resulting in battery performance and safety threats. Existing treatment methods such as scrapping or downgrading increase production costs and cause waste of resources.
Using repair strategies for different types of defects, by identifying defects on the surface of the battery cell shell, laser welding or laser scanning filling is used to use the same repair material as the shell material to form a uniform repair layer to ensure the consistency of material performance and Structural integrity.
It significantly reduces the scrap ratio in battery production, improves resource utilization efficiency, ensures the safety and reliability of battery products, optimizes the uniformity and compactness of the repair layer, and restores the mechanical and electrochemical properties of the battery cell shell.
Smart Images

Figure CN118951590A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery cell shell repair, and further to a method for repairing surface defects of a battery cell shell. Background Art
[0002] Lithium batteries are now widely used in various power tools and electronic devices. They are favored for their excellent energy density, long cycle life, high safety and portability. Among many lithium-ion batteries, aluminum shell batteries have become the mainstream choice in the market due to their excellent safety performance.
[0003] However, in the production process of batteries, appearance quality control is an important link. Surface defects such as pits and indentations on the battery shell often exceed the specification requirements, posing a threat to the overall performance and safety of the battery. At present, when faced with these batteries that exceed the specifications, battery manufacturers generally adopt the method of scrapping or downgrading, which not only increases production costs, but also causes a huge waste of resources. Summary of the invention
[0004] In response to the above technical problems, the purpose of the present application is to provide a method for repairing surface defects of a battery cell shell, which can repair the surface defects of the battery cell shell, so as to significantly reduce the scrap rate in battery production, improve resource utilization efficiency, and at the same time ensure the safety and reliability of battery products.
[0005] In order to achieve the above-mentioned object, the present application provides a method for repairing surface defects of a battery cell shell, comprising the steps of:
[0006] Identify defects on the surface of the battery cell casing;
[0007] When the target defect is a first type defect, a repair welding material is arranged at the position of the target defect, and the repair welding material is processed by laser technology to be integrated with the battery cell shell, and the material of the repair welding material is the same as that of the battery cell shell;
[0008] When the type of the target defect is a second type defect, laser scanning is performed at the position of the target defect to remelt a portion of the surface of the battery cell shell, thereby filling the target defect.
[0009] In some embodiments, arranging the repair welding material at the location of the target defect specifically includes:
[0010] Cleaning at least the position on the battery cell housing where the target defect is located;
[0011] The repair welding material is placed on the surface of the target defect, and the edge contour of the repair welding material is flush with the edge contour of the target defect, or exceeds the edge contour of the target defect.
[0012] In some embodiments, the processing of the repair welding material by laser technology so that it merges with the battery cell shell specifically includes:
[0013] Firstly, laser spot welding is performed to preliminarily process the repair welding material, so as to preliminarily fuse the repair welding material and the battery cell shell, thereby forming a repair layer on the target defect surface;
[0014] The repair layer is then laser scanned to further repair the target defect.
[0015] In some embodiments, before the laser scanning is performed on the repair layer, the method further comprises the following steps:
[0016] The repair layer is polished to remove irregularities or protrusions.
[0017] In some embodiments, the laser spot welding is first performed to perform preliminary processing on the repair welding material, specifically including:
[0018] Determining the power and pulse frequency of laser spot welding according to the depth of the target defect and the thickness of the repair welding material;
[0019] Adjusting the focal position of the laser device that outputs the laser to ensure that the laser energy is concentrated on the bonding area between the repair welding material and the battery cell housing;
[0020] Controlling the spot spacing and overlap of laser spot welding so that the laser spot welding can evenly cover the bonding area between the repair welding material and the battery cell housing;
[0021] Laser spot welding is started to achieve preliminary fusion of the repair welding material and the battery cell shell.
[0022] In some embodiments, the laser scanning comprises the steps of:
[0023] Set the laser scanning speed and the preset path of the laser scanning;
[0024] The laser scanning head is controlled to move along the preset path for continuous scanning to form a cladding layer that uniformly fills the target defect.
[0025] In some embodiments, the cladding layer includes a plurality of cladding segments, each of which is formed by laser dotting, and controlling the laser scanning head to move along the preset path specifically includes:
[0026] Determine the starting end, the ending end, and the corresponding laser dot parameters of each cladding section, so that the starting ends of the plurality of cladding sections together form a specific contour;
[0027] The laser scanning head is controlled to scan so that the starting end of a single cladding section points from the center of the target defect to the periphery, and multiple cladding sections form multiple fillings in the center of the target defect.
[0028] In some embodiments, the specific profile is a spiral profile, and the starting end of the spiral profile is located at the center of the target defect or a predetermined starting point;
[0029] As the spiral profile expands outward from the center of the target defect, the density of the corresponding laser dots decreases monotonically.
[0030] In some embodiments, different cladding sections have different extension directions, and the extension direction of each cladding section is deflected at a preset angle relative to the extension direction of an adjacent cladding section, so as to jointly form a petal-shaped cladding layer.
[0031] In some embodiments, the depth of the first type of defects is greater than or equal to the depth of the second type of defects;
[0032] And / or, the diameter of the first type of defects is greater than the diameter of the second type of defects.
[0033] In some embodiments, the first type of defect is one of a shell pit, a shell depression, and a shell hole, and the diameter of the first type of defect is greater than 5 mm and the depth is greater than 0.3 mm;
[0034] And / or, the second type of defect is one of a shell scratch, a shell bump, and a shell crack, and the width of the second type of defect is greater than 3 mm and the depth is greater than 0.3 mm.
[0035] Compared with the prior art, the method for repairing surface defects of a battery cell shell provided in this application has the following beneficial effects:
[0036] 1. In this application, targeted repair strategies are adopted according to the type of defects. For the first type of defects, such as large pits, laser repair welding is performed by arranging repair welding materials of the same material as the battery shell at the defect location to ensure the consistency of material properties of the repaired battery shell; for the second type of defects, such as scratches or small cracks, laser scanning can cause the shell surface to remelt, thereby effectively filling the defects and restoring the original surface state of the battery shell.
[0037] 2. In this application, for the first type of defects, the repair material is first precisely processed by laser spot welding technology to achieve initial fusion with the battery shell, forming a uniform repair layer, ensuring a strong metallurgical bond between the repair material and the shell, and then laser scanning technology is used to perform secondary processing on the formed repair layer to further refine and reinforce the target defect area. This continuous laser processing not only optimizes the heat-affected zone and reduces thermal damage to surrounding materials, but also significantly improves the uniformity and density of the repair layer, effectively restoring the mechanical and electrochemical properties of the battery shell.
[0038] 3. In this application, by controlling the laser scanning head to move along a preset path, the starting end of each cladding section extends outward from the center of the target defect, forming a multiple filling mode from the inside to the outside. The multiple fillings of the starting ends of multiple cladding sections in the center area of the target defect further enhance the mechanical strength and surface finish of the repair area, ensure the structural integrity of the battery shell, and ensure the effective fusion of the repair welding material and the battery shell through the high-intensity laser energy at the center. At the same time, the decreasing energy at the periphery helps to form a smooth cladding layer, avoiding excessive melting or material burning.
[0039] 4. In this application, the repair welding is designed to be performed along the spiral contour. The starting end of the spiral contour is precisely positioned at the center of the target defect or a predetermined starting point, ensuring that the repair process starts from the deepest part of the defect and gradually expands outward. As the spiral contour expands outward, the density of the laser dots decreases monotonically. This decrease in the density of the laser dots from the center to the periphery achieves a gradient transition of material filling and energy input, and promotes the formation of a more uniform cladding layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The preferred implementation scheme will be described below in a clear and understandable manner with reference to the accompanying drawings to further illustrate the above-mentioned characteristics, technical features, advantages and implementation methods of the present application.
[0041] Figure 1 is a repair flow chart of an embodiment provided by the present application;
[0042] Figure 2 It is a partial repair flow chart of an embodiment provided by the present application;
[0043] Figure 3 It is a partial repair flow chart of one of the embodiments provided in this application;
[0044] Figure 4 It is a partial repair flow chart of one of the embodiments provided in this application;
[0045] Figure 5 It is a schematic diagram of the structure of the cladding layer in an embodiment provided in the present application.
[0046] Description of the accompanying drawings: cladding layer 10; cladding section 100. DETAILED DESCRIPTION
[0047] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the specific implementation methods of the present application will be described below with reference to the accompanying drawings. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings and other implementation methods can be obtained based on these drawings without creative work.
[0048] In order to simplify the drawings, only the parts related to the application are schematically shown in each figure, and they do not represent the actual structure of the product. In addition, in order to simplify the drawings and facilitate understanding, in some figures, only one of the parts with the same structure or function is schematically drawn or marked. In this article, "one" not only means "only one", but also means "more than one".
[0049] It should be further understood that the term “and / or” used in the specification and appended claims refers to any combination and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0050] In this document, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0051] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0052] In addition, in the description of the present application, the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.
[0053] With the transformation of the global energy structure and the rapid development of mobile devices, lithium batteries, as clean and efficient energy storage media, have become one of the key technologies to promote the progress of modern society. Lithium batteries have been widely used in portable electronic devices, electric vehicles, energy storage systems and other fields due to their advantages such as high energy density, long cycle life, low self-discharge rate and environmental friendliness.
[0054] Lithium-ion batteries, as an important branch of lithium battery technology, have dominated the market with their excellent charge and discharge performance and high energy conversion efficiency. Among the many lithium-ion battery products, aluminum shell batteries are widely used in various consumer electronic products and power tools due to their low manufacturing cost, excellent safety performance, and easy large-scale production.
[0055] However, aluminum case batteries face many challenges during the production process, especially in terms of quality control. Tiny defects on the surface of the battery cell shell, such as pits and indentations, may occur during manufacturing, transportation or use. Although these surface defects are small, they can have a significant impact on the overall performance of the battery. Imperfections on the surface of the battery cell shell can reduce the uniformity of the blue film and its mechanical strength, which in turn affects the stability and safety of the battery. In extreme cases, these defects may cause the battery to short circuit, overheat or even catch fire, causing serious safety accidents.
[0056] Traditional methods of dealing with defects in battery cell shells, such as scrapping or downgrading, not only cause a huge waste of resources, but also increase production costs. In addition, simple mechanical grinding or filling material repairs often cannot meet the strict requirements of modern battery manufacturing industry for product quality.
[0057] To solve the above problems, the present application provides a more optimized method for repairing surface defects of battery cell shells, which can significantly improve the repair quality, reduce production costs, and improve the safety and reliability of battery products.
[0058] Reference Manual Attached Figure 1 The present application provides a method for repairing surface defects of a battery cell shell, comprising the steps of:
[0059] S100. Identify defects on the surface of the battery cell casing.
[0060] S200: When the target defect is a first type defect, a repair welding material is arranged at the location of the target defect, and the repair welding material is processed by laser technology to be integrated with the battery cell shell, and the material of the repair welding material is the same as that of the battery cell shell.
[0061] S300: When the target defect is a second type defect, laser scanning is performed at the location of the target defect to remelt a portion of the surface of the battery cell shell, thereby filling the target defect.
[0062] S400. Perform performance test on the battery cell shell after repair.
[0063] According to step S100, the method divides the surface defects of the battery cell shell into two categories according to the type and characteristics of the defects. Generally speaking, the depth and diameter of the first type of defects are greater than the depth and diameter of the second type of defects. The first type of defects are larger pits, depressions, etc. These defects may have a greater impact on the structural integrity and functionality of the battery cell shell, and may need to be repaired using welding materials and laser cladding technology to ensure sufficient material filling and metallurgical bonding. The second type of defects are smaller surface defects, such as nicks or cracks, etc., which focus more on surface treatment, such as laser scanning remelting or mechanical grinding, to restore the smoothness and integrity of the surface.
[0064] The identification process in step S100 not only involves accurate measurement of the defect size, but also includes accurate recording of the defect location, providing necessary spatial positioning for subsequent repair work. In other words, the present application obtains all measurement data of the defect through step S100, and corresponds to the subsequent repair plan based on these data.
[0065] More specifically, in other related embodiments, the first type of defects include shell pits, depressions and holes, whose diameter is greater than 5 mm and whose depth exceeds 0.3 mm. These larger defects may be caused by defects in the manufacturing process, material discontinuity or external mechanical impact. In contrast, the second type of defects covers shell scratches, gouges and cracks. Scratches and gouges may be caused by friction, collision or contact with hard objects during the production process, and cracks may be caused by internal material stress, thermal shock or cumulative effects of chemical corrosion. The width of this type of defect is greater than 3 mm and the depth also exceeds 0.3 mm, and its length may reach 50 mm.
[0066] For the repair of the first type of defects, the repair welding material is made of the same material as the battery shell to ensure that the repaired area has the same material properties as the original shell. Through laser technology, especially laser cladding technology, the repair welding material is fused with the surface of the battery shell to form a strong metallurgical bond. For the repair of the second type of defects, laser scanning technology is used to remelt the surface of the target area, and the defects are accurately filled and repaired by precisely controlling the energy and scanning speed of the laser.
[0067] The repair method in this embodiment realizes customized repair of different types of defects, improving the adaptability and flexibility of the repair. In addition, in some other embodiments, a high-precision imaging system and image processing algorithm can be used to comprehensively scan the surface of the battery shell to identify larger pit-like defects and smaller surface defects such as scratches or cracks, and then the power, speed and path of the laser scanning can be set according to the type of defect.
[0068] At the same time, as in step S400, the repaired battery cell shell should be finally tested for mechanical strength and electrochemical performance to ensure that the repair quality meets industrial standards, or the microstructure and surface quality should be evaluated to ensure that the repair effect meets expectations.
[0069] Further, such as Figure 2 As shown in step S100, the repair welding material is arranged at the location of the target defect, which specifically includes the steps of:
[0070] Step S101 : Clean at least the position with the target defect on the battery cell shell.
[0071] Step S102: placing a repair welding material on the surface of the target defect, with the edge contour of the repair welding material flush with the edge contour of the target defect, or exceeding the edge contour of the target defect.
[0072] Among them, the cleaning step S101 is aimed at removing pollutants in the target defect area on the surface of the battery shell, including grease, rust, oxides, dust and other foreign matter. Through cleaning, a clean and pollution-free surface is provided for the repair welding material, which is the prerequisite for achieving good metallurgical bonding and can effectively reduce cladding defects caused by surface pollutants, such as holes, inclusions and uneven fusion.
[0073] Specifically, solution cleaning can be used, such as using chemical solvents to clean the target defect area to remove grease and soluble contaminants, or mechanical methods such as brushing, sandblasting or ultrasonic cleaning can be used to remove stubborn dirt and oxide layers. When selecting a cleaning method, the characteristics of the cell shell material, surface state, and type of contaminants should be considered; the cleaning process should be strictly controlled to avoid introducing new contaminants or damaging the cell shell surface; after cleaning, subsequent repair welding material layout and cladding operations should be carried out in a timely manner to prevent the surface from being contaminated again.
[0074] More importantly, the flushing or exceeding of the edge of the target defect by the repair welding material in step S102 helps to evenly distribute the laser energy, avoid cladding defects caused by insufficient coverage, ensure a smooth transition between the repair welding material and the original material, and reduce stress concentration and potential microcracks. On the other hand, the thickness and width of the repair welding material should be optimized according to the depth and width of the laser cladding to ensure the uniformity and consistency of the material after cladding.
[0075] In one embodiment, Figure 3 In step S200, the repair welding material is processed by laser technology to make it merge with the battery cell shell, which specifically includes the following steps:
[0076] Step S201: First, laser spot welding is performed to preliminarily process the repair welding material, so as to preliminarily fuse the repair welding material and the battery cell shell, thereby forming a repair layer on the target defect surface.
[0077] Step S202: laser scan the repair layer again to further repair the target defect.
[0078] In step S201, the repair material is first processed by laser spot welding technology. In this process, appropriate laser power and pulse frequency can be selected according to the specific situation to form tiny but high-strength welds on the contact interface between the repair material and the battery cell shell. This preliminary processing not only ensures the initial connection between the repair material and the shell, but also lays the foundation for the next step of comprehensive integration. The high-precision characteristics of laser spot welding can effectively avoid excessive melting and material splashing, thereby ensuring the initial stability and uniformity of the repair layer.
[0079] Subsequently, in step S202, the repair layer that has been initially fixed by spot welding is laser scanned to further repair the target defect. The laser scanning adjusts the scanning speed and power to fully heat and melt the repair layer, achieving deep fusion of the repair welding material and the battery cell shell. This step ensures the metallurgical bonding between the repair layer and the battery cell shell, significantly improving the mechanical strength and corrosion resistance of the repair area. By precisely controlling the parameters of the laser scanning, the melting depth and width can be optimized to achieve the improvement and optimization of the repair effect.
[0080] Furthermore, a key parameter of the laser spot welding step in step S201 is the overlap of the laser points, which directly affects the quality and filling effect of the cladding layer. The overlap of the laser points refers to the ratio of each laser point overlapping with the previous point during continuous laser spot welding. In this embodiment, this ratio is at least 30%, which means that each new laser point has at least 30% of its area overlapping with the previous point, ensuring the continuous transmission and accumulation of laser energy at the contact interface between the repair welding material and the battery cell shell, achieving uniform coverage of the defective area, and helping to form a more uniform and dense cladding layer.
[0081] Based on the above embodiment, before step S202, laser scanning the repair layer to further repair the target defect, there is step S2015, grinding the repair layer to remove irregular or protruding parts. The surface of the repair layer after grinding is smoother, high points and irregular areas are reduced, the surface finish of the repair layer is improved, and it is helpful to improve the appearance quality and mechanical properties of the final repair area.
[0082] Specifically, in this grinding step, appropriate grinding tools, such as grinding wheels, sandpaper or polishing machines, can be used to treat the surface of the repair layer. On the other hand, according to the hardness and thickness of the repair layer, the appropriate grinding force and speed are selected to ensure that excess material is removed while avoiding damage to the base of the battery cell shell.
[0083] In one embodiment, step S201 in the above embodiment specifically includes:
[0084] Step S2011, determining the power and pulse frequency of the laser spot welding according to the depth of the target defect and the thickness of the repair welding material.
[0085] Step S2012: adjusting the focal position of the laser device that outputs the laser to ensure that the laser energy is concentrated on the bonding area between the repair welding material and the battery cell shell.
[0086] Step S2013, controlling the spot spacing and overlap of the laser spot welding so that the laser spot welding can evenly cover the joining area between the repair welding material and the battery cell shell.
[0087] Step S2014, start laser spot welding to achieve preliminary fusion of the repair welding material and the battery cell shell.
[0088] It should be noted that in this embodiment, the optimal power and frequency parameters are determined according to the depth of the target defect and the specific thickness of the repair welding material. For example, for deeper defects or thicker repair welding materials, higher power and appropriate pulse frequency may be required to achieve effective melting depth and width.
[0089] Similarly, adjust the focus of the laser equipment to ensure that the laser energy forms a concentrated heat-affected zone at the interface between the repair welding material and the battery cell shell, thereby minimizing the thermal impact on the surrounding materials while achieving precise fusion; please refer to the attached Figure 5 By precisely controlling the spacing and overlap of the dots, a uniform cladding layer 10 is formed, thereby improving the mechanical properties and corrosion resistance of the welding area.
[0090] In one embodiment, the laser scanning used in the repair method of the present application includes the steps of:
[0091] Step S500, setting the laser scanning speed and the laser scanning preset path.
[0092] Step S600: Control the laser scanning head to move along a preset path for continuous scanning to form a cladding layer that uniformly fills the target defect.
[0093] For step S500, in this step, firstly, the laser scanning speed is set according to the material properties of the battery shell and the specific conditions of the target defect, such as the size and depth of the defect. The setting of the scanning speed is directly related to the distribution density of the laser energy on the material. Too fast a speed may lead to insufficient cladding, while too slow a speed may cause excessive melting or even damage the material. Therefore, choosing a moderate scanning speed is crucial to forming a uniform and high-quality cladding layer 10.
[0094] The preset path of laser scanning is determined, and the design of this path is based on the geometry of the defect and the desired cladding effect. For example, for a pit-type defect with a deep center and shallow surroundings, a spiral or concentric circle path can be designed to ensure that the laser energy gradually covers the entire defect area from the center to the outside. The optimized design of the preset path helps to achieve uniform distribution of laser energy, avoid thermal damage in local areas, and ensure effective fusion of the cladding material and the base material.
[0095] Furthermore, after the preset parameters are determined, the laser scanning head is guided to move along the preset path through system control. In this process, the laser scanning head continuously emits laser at a set speed to accurately melt and remelt the repair welding material. Due to the high energy density characteristics of the laser, the material is rapidly heated to the melting point in a very short time to form a molten pool, which then quickly solidifies to form a cladding layer 10, thereby effectively repairing various surface defects.
[0096] In addition, if Figure 5 As shown, the cladding layer 10 in the above content includes a plurality of cladding sections 100. Specifically, each cladding section 100 is formed by laser dotting. First, the starting position of the laser dotting is accurately located. As the laser scanning head moves, the laser beam continuously dots on the moving path, and each dot melts and solidifies to form a part of a cladding section 100.
[0097] In one embodiment, if Figure 4 As shown, step S600 in the above embodiment specifically includes:
[0098] Step S601: determine the starting end, the ending end, and the corresponding laser dot parameters of each cladding section.
[0099] Step S602: Control the laser scanning head to scan so that the starting end of a single cladding section points from the center of the target defect to the periphery, and multiple cladding sections form multiple fillings at the center of the target defect.
[0100] It can be understood that in this embodiment, by controlling the movement of the laser scanning head, it is ensured that the starting end of each cladding section 100 is accurately positioned at the center point of the defect, which is crucial because it determines the starting quality of the cladding layer 10 and the uniformity of the subsequent layers. As the laser scanning head moves outward along the preset path, each cladding section 100 gradually expands to the periphery, forming a cladding pattern that diffuses from the center to the outside. This filling strategy from the inside out not only ensures sufficient filling of the central area of the defect, but also helps to achieve a more uniform material distribution and reduce stress concentration.
[0101] In addition, by performing multiple laser scans at the center of the target defect, the present embodiment achieves the superposition of multiple layers of cladding sections 100, which is particularly important when repairing deeper or larger defects. Each cladding is performed on the basis of the previous cladding, ensuring a good combination between the new and old claddings, while gradually building up a dense and uniform repair layer. This multiple cladding method not only improves the mechanical strength and durability of the cladding layer 10, but also helps to reduce the occurrence of defects such as holes and cracks.
[0102] Furthermore, in step S601 , the starting ends of the plurality of cladding sections 100 together form a specific profile, thereby optimizing the distribution of the cladding material.
[0103] In particular, this profile can be spiral, and the starting end of this spiral profile is precisely located at the center of the target defect or a predetermined starting point, ensuring the symmetry and uniformity of the repair process. As the spiral profile expands outward, the density of the laser dots decreases monotonically according to the preset pattern, achieving denser cladding in the central area, while gradually reducing the material filling outward, thus forming a gradient, transitional filling effect.
[0104] This design form of decreasing laser dot density from the center to the periphery has several key advantages. First, it ensures that the deepest part of the defect is filled with the most material and heat treated, which helps to improve the mechanical strength and durability of the repaired area. Second, the reduction in density as it expands outward helps to avoid excessive material accumulation and potential stress concentration, thereby reducing the risk of cracks or deformation in the repair layer. In addition, this design also helps to achieve a smoother surface transition and improve the appearance quality of the repaired battery shell.
[0105] A specific repair step in the present application can be summarized as follows: First, a continuous laser is used, and its power is set to 1500W to perform processing at a lower energy density. Such a power setting can ensure that the laser can effectively heat and melt the substrate while avoiding excessive thermal damage to the battery cell shell.
[0106] Next, the movement path of the laser scanning head is planned to ensure that it scans according to a specific spiral profile. The scanning speed is set to 500mm / s to ensure that the laser energy is evenly distributed on the surface of the battery cell shell to form a uniform cladding layer.
[0107] In some other embodiments, this profile has other settings, for example, concentric circles can be used as scanning profiles, starting from the center of the target defect, and gradually increasing the diameter of the ring layer by layer to achieve uniform layered filling. In addition, a grid-like profile can also be used to provide cladding in multiple directions to increase the structural strength of the repair layer. Of course, there may be other profile settings, which will not be described here.
[0108] On the basis of the above-mentioned embodiment, different cladding sections 100 have different extension directions, and the extension direction of each cladding section 100 is deflected at a preset angle relative to the extension direction of the adjacent cladding section 100, so as to jointly form a petal-shaped cladding layer 100, ensuring that the cladding material is fully filled in the central area of the defect and smoothly transitions to the periphery. On the other hand, each cladding section 100 is deflected at a preset angle relative to the adjacent section, and this deflection not only forms a continuous petal-shaped profile, but also realizes a uniform transition of energy and material between the cladding sections 100 through angle control, avoiding the hot spot problem caused by energy concentration.
[0109] It should be noted that the above embodiments can be freely combined as needed. The above are only preferred implementations of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications should also be regarded as the protection scope of the present application.
Claims
1. A method for repairing surface defects of a battery cell shell, characterized in that: Includes steps: Identify defects on the surface of the battery cell casing; When the target defect is a first type defect, a repair welding material is arranged at the position of the target defect, and the repair welding material is processed by laser technology to be integrated with the battery cell shell, and the material of the repair welding material is the same as that of the battery cell shell; When the type of the target defect is a second type defect, laser scanning is performed at the position of the target defect to remelt a portion of the surface of the battery cell shell, thereby filling the target defect.
2. The method for repairing surface defects of a battery cell shell according to claim 1, characterized in that: The step of arranging the repair welding material at the position of the target defect specifically includes: Cleaning at least the position on the battery cell housing where the target defect is located; The repair welding material is placed on the surface of the target defect, and the edge contour of the repair welding material is flush with the edge contour of the target defect, or exceeds the edge contour of the target defect.
3. The method for repairing surface defects of a battery cell shell according to claim 1, characterized in that: The method of processing the repair welding material by laser technology so that it can be integrated with the battery cell shell specifically includes: Firstly, laser spot welding is performed to preliminarily process the repair welding material, so as to preliminarily fuse the repair welding material and the battery cell shell, thereby forming a repair layer on the target defect surface; The repair layer is then laser scanned to further repair the target defect.
4. The method for repairing surface defects of a battery cell shell according to claim 3, characterized in that: Before the laser scanning is performed on the repair layer, the method further comprises the following steps: The repair layer is polished to remove irregularities or protrusions.
5. The method for repairing surface defects of a battery cell shell according to claim 3, characterized in that: The laser spot welding is first performed to perform preliminary processing on the repair welding material, specifically including: Determining the power and pulse frequency of laser spot welding according to the depth of the target defect and the thickness of the repair welding material; Adjusting the focal position of the laser device that outputs the laser to ensure that the laser energy is concentrated on the bonding area between the repair welding material and the battery cell housing; Controlling the spot spacing and overlap of laser spot welding so that the laser spot welding can evenly cover the bonding area between the repair welding material and the battery cell housing; Laser spot welding is started to achieve preliminary fusion of the repair welding material and the battery cell shell.
6. The method for repairing a surface defect of a battery cell shell according to any one of claims 1 to 5, characterized in that: The laser scanning comprises the steps of: Set the laser scanning speed and the preset path of the laser scanning; The laser scanning head is controlled to move along the preset path for continuous scanning to form a cladding layer that uniformly fills the target defect.
7. The method for repairing surface defects of a battery cell shell according to claim 6, characterized in that: The cladding layer includes a plurality of cladding sections, each of which is formed by laser dotting, and the control of the laser scanning head to move along the preset path for continuous scanning specifically includes: Determine the starting end, the ending end and the corresponding laser dot parameters of each cladding section, so that the starting ends of the plurality of cladding sections together form a specific contour; The laser scanning head is controlled to scan so that the starting end of a single cladding section points from the center of the target defect to the periphery, and multiple cladding sections form multiple fillings in the center of the target defect.
8. The method for repairing surface defects of a battery cell shell according to claim 7, characterized in that: The specific profile is a spiral profile, and the starting end of the spiral profile is located at the center of the target defect or a predetermined starting point; As the spiral profile expands outward from the center of the target defect, the density of the corresponding laser dots decreases monotonically.
9. The method for repairing surface defects of a battery cell casing according to claim 7 or 8, characterized in that: Different cladding sections have different extension directions, and the extension direction of each cladding section is deflected at a preset angle relative to the extension direction of an adjacent cladding section, so as to jointly form a petal-shaped cladding layer.
10. The method for repairing surface defects of a battery cell shell according to any one of claims 1 to 5, 7 and 8, characterized in that: The depth of the first type of defects is greater than or equal to the depth of the second type of defects; and / or, The diameter of the first type of defects is greater than the diameter of the second type of defects.
11. The method for repairing surface defects of a battery cell shell according to claim 10, characterized in that: The first type of defect is one of a shell pit, a shell depression, and a shell hole, and the diameter of the first type of defect is greater than 5 mm and the depth is greater than 0.3 mm; and / or, The second type of defect is one of a shell scratch, a shell bump, and a shell crack, and the width of the second type of defect is greater than 3 mm and the depth is greater than 0.3 mm.
Citation Information
Patent Citations
Ni3(Si,Ti)-WC composite coating material and preparation method thereof
CN101161864A
Method combining surfacing and remelting for repair welding of surface defects of roller
CN107378287A
Method for repairing metal defects through laser and precise argon arc composite welding technology
CN108772629A
Method for repairing laser welding burst point of power battery shell and top cover
CN110449737A
Repairing joint welding method for stress corrosion cracking of ammonia refrigeration container
CN111168207A
Cited By
Laser fine repairing method and device for surface defects of die-casting aluminum mobile phone middle frame