Preparation method and application of positive electrode material, battery positive electrode and sodium ion battery
The preparation of multi-element doped Prussian blue positive electrode material at room temperature by co-precipitation method, which solved the problem of poor electrochemical stability of the positive electrode material of sodium ion battery, and achieved efficient performance improvement and cost reduction of sodium ion battery. It is suitable for electric vehicles and Energy storage system.
Patent Information
- Application Number
- CN202411054097.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The electrochemical stability of the cathode material of sodium ion battery is poor, resulting in poor performance, and the existing preparation methods require high temperatures, which limits the industrial application of materials.
The multi-element doped Prussian blue positive electrode material was prepared at room temperature by co-precipitation method. The co-precipitation reaction was carried out by mixing solution A and solution B, combined with stirring and vacuum drying, and added conductive agent and water removal agent for grinding and drying, and control The water content and structure of the material are obtained to obtain Prussian blue positive electrode material with low water content and low vacancy.
The preparation of high-entropy Prussian blue cathode material at room temperature is realized, which improves cycle stability and structural stability, reduces production costs, and expands the application potential of the materials, especially suitable for electric vehicles and energy storage systems.
Smart Images

Figure CN118954539A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of positive electrode materials, and in particular to a preparation method and application of positive electrode materials, a battery positive electrode and a sodium ion battery. Background Art
[0002] With the increase in market demand, sodium-ion batteries have received extensive attention and research, thanks to the high abundance of sodium resources in the world and its low cost. Li + In comparison, the larger Na + The intercalation kinetics in tightly packed materials are much slower, usually causing more significant structural changes, resulting in poor electrochemical stability of active materials, which in turn affects the performance of cathode materials. Therefore, the development of high-performance cathode materials is crucial. x TM[Fe(CN) 6 ] y □ 1-y ·nH 2 O, TM represents transition metal ions (Fe, Mn, Co, Ni, Cu, etc., some people also use M to represent transition metal ions), □ represents Fe(CN) 6 Vacancy) or a transition metal ferrocyanide compound, due to its high theoretical capacity (170 mAhg-1), large interstitial position (approx. ), adjustable structure and chemical composition, good framework stability and other advantages, showing very excellent electrochemical performance, easy to industrialize, and has great potential for practical applications.
[0003] CN117038966A discloses a positive electrode material, a preparation method, an application, a battery positive electrode and a sodium ion battery. The positive electrode material is prepared by a hydrothermal method at a relatively high preparation temperature. Summary of the invention
[0004] In view of the shortcomings of the prior art, one of the purposes of the present application is to provide a preparation method and application of a positive electrode material, a battery positive electrode and a sodium ion battery, which have the advantage of being able to be prepared at room temperature.
[0005] The above-mentioned purpose of the present application is achieved through the following technical solutions:
[0006] The preparation method of the positive electrode material comprises the following steps: preparing solution A, dissolving a soluble sodium hexacyano salt of transition metal N in deionized water under a certain temperature and a protective atmosphere, and then adding an inorganic sodium salt to obtain solution A; preparing solution B, dissolving a soluble salt of transition metal M, a complexing agent sodium salt and an antioxidant in deionized water under a certain temperature and a protective atmosphere, and then adding an inorganic sodium salt to obtain solution B; and coprecipitating, mixing solution B and solution A under a certain temperature and a protective atmosphere to carry out a coprecipitation reaction, and then carrying out a stirring reaction, aging and standing after the reaction, and then carrying out solid-liquid separation, washing the precipitate, and vacuum drying at a certain temperature to obtain a Prussian blue type sodium ion battery positive electrode material to be treated.
[0007] In a preferred example, the present application can be further configured as follows: grinding, adding the untreated Prussian blue type sodium ion battery positive electrode material obtained in the co-precipitation step, the conductive agent and the dehydrating agent to an anhydrous organic solvent, manually grinding, and separating the solid and liquid to obtain the undried Prussian blue type sodium ion battery positive electrode material.
[0008] In a preferred example, the present application can be further configured as follows: drying, coating the undried Prussian blue type sodium ion battery positive electrode material and placing it in an oven for drying to obtain a low-water content and low-vacancy Prussian blue type sodium ion battery positive electrode material.
[0009] In a preferred example, the present application can be further configured as follows: the transition metals N and M in the hexacyano sodium salt of transition metal N and the transition metal M salt are independently selected from any one of Ti, Cr, Mn, Fe, Co, Cu, Ni, Zn, and Zr.
[0010] In a preferred example, the present application can be further configured as follows: the concentration of the soluble sodium hexacyano salt of transition metal N in solution A is 0.01-10M.
[0011] In a preferred example, the present application can be further configured as follows: the concentration of the soluble transition metal M salt in solution B is 0.01 to 10 M; the concentration of the antioxidant in solution B is 0.001 to 0.1 M; the weight ratio of the complexing agent sodium salt to the transition metal M salt is (1 to 10):1.
[0012] In a preferred example, the present application can be further configured as follows: in the drying step, the ratio of the Prussian blue sodium ion battery positive electrode material to be treated to the anhydrous organic solvent is: (1-10) g: 100 mL; the concentration of the dehydrating agent in the anhydrous organic solvent is 0.001-0.1 M.
[0013] An application of a positive electrode material, and an application of the positive electrode material obtained by any of the above-mentioned methods for preparing a positive electrode material in a positive electrode of a sodium ion battery.
[0014] A battery positive electrode comprises a current collector, a conductive material, a binder and an active material, wherein the binder binds the conductive material and the active material to the current collector, and the active material is a positive electrode material obtained by any one of the above-mentioned methods for preparing the positive electrode material.
[0015] A sodium ion battery comprises a positive electrode, a negative electrode, an electrolyte and a separator, wherein the positive electrode is the positive electrode of the battery mentioned above.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] 1. High-entropy Prussian blue positive electrode materials for sodium-ion batteries doped with a variety of transition elements can be prepared at room temperature. Compared with single-element doped layered oxide positive electrode materials, they have better cycle stability and a smaller volume change rate during the charge and discharge process. The multi-element doped structure has better stability in water or air.
[0018] 2. The sodium source used in this application is more abundant in the earth's crust resources, so the raw materials of sodium ion batteries are easier to obtain and the cost is low, which greatly reduces the production cost of sodium ion batteries.
[0019] 3. The sodium-ion battery of the present application has more competitive characteristics and can be widely used in electric vehicles, energy storage systems and other fields. At the same time, the cycle life of the sodium-ion battery is relatively long, which can reduce the frequency of battery replacement, reduce maintenance costs, and is more environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a scanning electron microscope (SEM) morphology image of a high entropy structure sodium ion battery Prussian blue positive electrode material particle prepared in Example 1 of the present application.
[0021] Figure 2 This is a scanning electron microscope (SEM) morphology image of a high entropy structure sodium ion battery Prussian blue positive electrode material particle prepared in Example 2 of the present application.
[0022] Figure 3 This is a long-period cycle curve diagram of Example 1 of the present application at 0.1C. DETAILED DESCRIPTION
[0023] The present application is further described in detail below in conjunction with the accompanying drawings.
[0024] Reference Figure 1-Figure 3, which is a preparation method of the positive electrode material disclosed in the present application, and is prepared by using a chelating agent and a simple coprecipitation method. The chelating agent is sodium citrate. The sodium source, cobalt nitrate, nickel nitrate, copper nitrate, manganese nitrate, and zinc nitrate are weighed according to a ratio, a chelating agent and an antioxidant are added, mixed evenly, aged, centrifuged, washed, and dried at different temperatures in a vacuum drying oven to obtain a high entropy Prussian blue sodium ion battery positive electrode material. Under a scanning electron microscope, the multi-metal co-doped Prussian blue analog positive electrode material is irregular nanoparticles, and the multi-metal co-doped Prussian blue analog positive electrode material has an open three-dimensional framework structure.
[0025] That is, the preparation process of the salt solution before coprecipitation is to add antioxidant, sodium citrate chelating agent, cobalt nitrate hexahydrate, nickel nitrate hexahydrate, copper nitrate trihydrate, manganese nitrate tetrahydrate, and zinc nitrate hexahydrate into deionized water and fully dissolve them into solution A, add potassium ferrocyanide into deionized water and fully dissolve them into solution B, directly pour the clear solution B into the clear solution A at room temperature and stir continuously to form a mixed solution C, and let it stand at room temperature to carry out coprecipitation reaction. The temperature of coprecipitation is room temperature, and the reaction time is 24h.
[0026] More specific steps are as follows. It is worth noting that S1-S5 in the following text are only used to refer to steps and do not represent the order of the steps.
[0027] S1 (preparation of solution A), dissolving a soluble transition metal N hexacyano sodium salt in deionized water at a certain temperature and in a protective atmosphere, and then adding an inorganic sodium salt to obtain solution A;
[0028] S2 (preparation of solution B), at a certain temperature and under a protective atmosphere, dissolve a soluble transition metal M salt, a complexing agent sodium salt, and an antioxidant in deionized water, and then add an inorganic sodium salt to obtain solution B;
[0029] S3 (co-precipitation), under a certain temperature and protective atmosphere, slowly drop solution B into solution A to carry out a co-precipitation reaction, and then carry out a stirring reaction, and then carry out aging and standing after the reaction, and then carry out solid-liquid separation, and the precipitate is washed and vacuum dried at a certain temperature to obtain a Prussian blue sodium ion battery positive electrode material to be treated;
[0030] S4 (grinding), adding the untreated Prussian blue type sodium ion battery positive electrode material, the conductive agent and the water removing agent obtained in step S3 to an anhydrous organic solvent, manually grinding, and performing solid-liquid separation to obtain an undried Prussian blue type sodium ion battery positive electrode material;
[0031] S5 (drying), coating the undried Prussian blue type sodium ion battery positive electrode material and placing it in an oven for drying to obtain a low-water-content and low-vacancy Prussian blue type sodium ion battery positive electrode material.
[0032] The transition metals N and M in the sodium hexacyano salt of transition metal N and the transition metal M salt are each independently selected from any one of Ti, Cr, Mn, Fe, Co, Cu, Ni, Zn, and Zr.
[0033] The hexacyano sodium salt of transition metal N is sodium ferrocyanide decahydrate or sodium manganese cyanide decahydrate.
[0034] The transition metal M salt is any one of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, copper nitrate trihydrate, manganese nitrate tetrahydrate, and zinc nitrate hexahydrate.
[0035] In step S1, the concentration of the soluble sodium hexacyano salt of transition metal N in solution A is 0.01 to 10 M;
[0036] In step S2, the complexing agent sodium salt is selected from at least one of sodium citrate dihydrate, sodium oxalate, disodium ethylenediaminetetraacetate, sodium gluconate, sodium tartrate or sodium acetate.
[0037] In step S2, the antioxidant is at least one of butylated hydroxyanisole, butylated hydroxytoluene, tert-butylhydroquinone or ascorbic acid.
[0038] In step S2, the concentration of the soluble transition metal M salt in solution B is 0.01 to 10 M; the concentration of the antioxidant in solution B is 0.001 to 0.1 M; the weight ratio of the complexing agent sodium salt to the transition metal M salt is (1 to 10): 1;
[0039] The temperature range in step S2 and step S3 is 55°C to 95°C;
[0040] In step S4, the dehydrating agent is at least one of sodium cyanate and sodium thiocyanate.
[0041] In step S4, the anhydrous organic solvent is one or a combination of anhydrous ethanol, toluene, acetone, NMP, ethyl acetate, DMF, and dioxane.
[0042] In step S4, the ratio of the Prussian blue sodium ion battery positive electrode material to be treated to the anhydrous organic solvent is: (1-10) g: 100 mL; the concentration of the dehydrating agent in the anhydrous organic solvent is 0.001-0.1 M.
[0043] The manual grinding time in step S4 is 1 to 3 hours;
[0044] The high entropy Prussian blue-based sodium-ion battery cathode material is denoted as HE-PBA, and five high entropy alloy elements are selected: Co, Ni, Cu, Mn, and Zn.
[0045] Example 1
[0046] (1) Preparation of positive electrode
[0047] 0.968gNa 4 Fe(CN) 6 ·10H2O was dissolved in 50ml deionized water, then 2.92gNaCl was added and stirred to obtain Na 4 Fe(CN) 6 Solution; 1.164 g Co(NO 3 ) 2 6H 2 O, 1.164gNi(NO 3 ) 2 6H 2 O, 1.184gCu(NO 3 ) 2 ·3H 2 O, 1.148 gMn(NO 3 ) 2 ·4H 2 O, 1.188gZn(NO 3 ) 2 6H 2 O and 0.6615 g Na 3 C 6 H 5 O 7 ·2H 2 O and 0.1354g ascorbic acid were dissolved in 50ml deionized water, and then 2.92g NaCl was added; the metal salt mixed solution was obtained after stirring evenly; the former was slowly dripped into the latter solution, and the stirring was continuously carried out for 10min, and the obtained mixed solution was aged at room temperature for 24h; the product was collected by centrifugation, and repeatedly washed with deionized water and ethanol, respectively, and finally dried at 60℃ for 24h to obtain a high entropy Prussian blue positive electrode material sample.
[0048] The above sample, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 8:1:1, and the solvent N-methylpyrrolidone was added while grinding. The positive electrode slurry was evenly obtained, and then coated on a positive electrode current collector aluminum foil with a thickness of 15 μm. After drying at 80°C, it was punched into a positive electrode sheet with a diameter of 14 mm.
[0049] (2) Preparation of negative electrode
[0050] The negative electrode sheet is directly selected from the metallic sodium sheet.
[0051] (3) Preparation of electrolyte
[0052] Making NaClO 4 The concentration of the electrolyte is 1 mol / L.
[0053] (4) Preparation of isolation membrane
[0054] A glass fiber membrane (produced by Whatman) was used as an isolation membrane.
[0055] (5) Preparation of button batteries
[0056] Stack the positive electrode sheet, the separator, and the negative electrode sheet in order, so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, inject the prepared electrolyte into the dried battery cell, and assemble it into a battery, such as a CR2032 button battery or a CR2025 button battery.
[0057] Example 2
[0058] The preparation process of the button cell is the same as that of Example 1, except that:
[0059] (1) Preparation of positive electrode
[0060] 0.968gNa 4 Fe(CN) 6 10H 2 O was dissolved in 50 ml of deionized water, followed by adding 2.92 g of NaCl and stirring to obtain Na 4 Fe(CN) 6 Solution; 1.164 g Co(NO 3 ) 2 6H 2 O, 1.164gNi(NO 3 ) 2 6H 2 O, 1.184gCu(NO 3 ) 2 ·3H 2 O, 1.148 gMn(NO 3 ) 2 ·4H 2 O, 1.188gZn(NO 3 ) 2 6H 2 O and 0.7653 g Na 3 C 6 H 5 O 7 ·2H 2 O and 0.1354g ascorbic acid were dissolved in 50ml deionized water, and then 2.92g NaCl was added; the metal salt mixed solution was obtained after stirring evenly; the former was slowly dripped into the latter solution, and the stirring was continuously carried out for 10min, and the obtained mixed solution was aged at room temperature for 12h; the product was collected by centrifugation, and repeatedly washed with deionized water and ethanol, respectively, and finally dried at 60℃ for 12h to obtain a high entropy Prussian blue positive electrode material sample.
[0061] Example 3
[0062] The preparation process of the button cell is the same as that of Example 1, except that:
[0063] (1) Preparation of positive electrode
[0064] 0.968gNa 4 Fe(CN) 6 10H 2 O was dissolved in 50 ml of deionized water, followed by adding 2.92 g of NaCl and stirring to obtain Na 4 Fe(CN) 6 Solution; 1.164 g Co(NO 3 ) 2 6H 2 O, 1.164gNi(NO 3 ) 2 6H 2 O, 1.184gCu(NO 3 ) 2 ·3H 2 O, 1.148 gMn(NO 3 ) 2 ·4H 2 O, 1.188gZn(NO 3 ) 2 6H 2 O and 0.9052 g Na 3 C 6 H 5 O 7 ·2H 2 O and 0.1354g ascorbic acid were dissolved in 50ml deionized water, and then 2.92g NaCl was added; after stirring evenly, a mixed solution of metal salts was obtained; the former was slowly dripped into the latter solution, and the stirring was continued for 10min, and the obtained mixed solution was aged at room temperature for 8h; the product was collected by centrifugation, and repeatedly washed with deionized water and ethanol, respectively, and finally dried at 90°C for 12h to obtain a high entropy Prussian blue positive electrode material sample.
[0065] The present application also discloses an application of a positive electrode material, and an application of the positive electrode material obtained by any of the above-mentioned methods for preparing the positive electrode material in a positive electrode of a sodium ion battery.
[0066] The present application also discloses a battery positive electrode, comprising a current collector, a conductive material, a binder and an active material, wherein the binder bonds the conductive material and the active material to the current collector, and the active material is a positive electrode material obtained by any one of the above-mentioned methods for preparing the positive electrode material.
[0067] The present application also discloses a sodium ion battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator, wherein the positive electrode is the positive electrode of the battery mentioned above.
[0068] The implementation principle of this embodiment is as follows: This application adopts the coprecipitation method to prepare the Prussian blue positive electrode material, and realizes the slow growth of the material crystal by regulating the complexing agent sodium salt and the reaction temperature of the reaction system, and then introduces a dehydrating agent, a reducing agent, etc., and removes part of the crystal water of the material system by grinding and drying to prevent the internal Fe2+ from being oxidized, thereby obtaining a low-water-content and low-vacancy Prussian blue sodium ion battery positive electrode material, which solves the problems existing in conventional Prussian blue positive electrode materials, thereby improving the electrochemical performance of sodium ion batteries. .
[0069] The embodiments of this specific implementation method are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. Therefore, all equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a positive electrode material, characterized in that: Solution A is prepared by dissolving a soluble sodium hexacyano salt of transition metal N in deionized water at a certain temperature and in a protective atmosphere, and then adding an inorganic sodium salt to obtain solution A; Solution B is prepared by dissolving a soluble salt of transition metal M, a complexing agent sodium salt, and an antioxidant in deionized water at a certain temperature and in a protective atmosphere, and then adding an inorganic sodium salt to obtain solution B; Co-precipitation is carried out by mixing solution B and solution A at a certain temperature and in a protective atmosphere, and then stirring the solution, and then aging and standing the solution after the reaction, and then solid-liquid separation, and the precipitate is washed and vacuum dried at a certain temperature to obtain the Prussian blue sodium ion battery positive electrode material to be treated.
2. The method for preparing the positive electrode material according to claim 1, characterized in that: Grinding, adding the untreated Prussian blue type sodium ion battery positive electrode material obtained in the coprecipitation step, the conductive agent and the dehydrating agent into an anhydrous organic solvent, manually grinding, and performing solid-liquid separation to obtain the undried Prussian blue type sodium ion battery positive electrode material.
3. The method for preparing the positive electrode material according to claim 2, characterized in that: Drying, coating the undried Prussian blue type sodium ion battery positive electrode material and drying it in an oven to obtain a low-water-content and low-vacancy Prussian blue type sodium ion battery positive electrode material.
4. The method for preparing the positive electrode material according to claim 3, characterized in that: The transition metals N and M in the sodium hexacyano salt of transition metal N and the transition metal M salt are each independently selected from any one of Ti, Cr, Mn, Fe, Co, Cu, Ni, Zn, and Zr.
5. The method for preparing the positive electrode material according to claim 1, characterized in that: The concentration of the soluble sodium hexacyano salt of transition metal N in solution A is 0.01 to 10M.
6. The method for preparing the positive electrode material according to claim 1, characterized in that: The concentration of the soluble transition metal M salt in solution B is 0.01-10M; the concentration of the antioxidant in solution B is 0.001-0.1M; and the weight ratio of the complexing agent sodium salt to the transition metal M salt is (1-10):
1.
7. The method for preparing the positive electrode material according to claim 3, characterized in that: In the drying step, the ratio of the Prussian blue sodium ion battery positive electrode material to be treated to the anhydrous organic solvent is: (1-10) g: 100 mL; the concentration of the dehydrating agent in the anhydrous organic solvent is 0.001-0.1 M.
8. An application of a positive electrode material, characterized in that: Application of the positive electrode material obtained by the method for preparing the positive electrode material according to any one of claims 1 to 7 in the positive electrode of a sodium ion battery.
9. A positive electrode of a battery, characterized in that: The invention comprises a current collector, a conductive material, a binder and an active material, wherein the binder binds the conductive material and the active material to the current collector, and the active material is a positive electrode material obtained by the preparation method of the positive electrode material according to any one of claims 1 to 7.
10. A sodium ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode, an electrolyte and a separator, wherein the positive electrode is the positive electrode of the battery as claimed in claim 9.
Citation Information
Patent Citations
Prussian blue cathode material with high sodium content, preparation method and applications thereof, and sodium ion battery
CN110235292A
Preparation method and application of Prussian blue sodium ion battery positive electrode material
CN115611296A
Prussian blue analog having core-shell structure, preparation method thereof, and sodium-ion secondary battery comprising the same
US20220399536A1