Modified base material for treating acidic mine wastewater, preparation method of modified base material and method for treating acidic mine wastewater

By treating acidic mine wastewater with modified alkaline materials, utilizing the properties of carbonate rocks and biochar, and combining them with a multi-stage cascade platform, the problem of high cost and low efficiency in treating AMD in areas with abundant groundwater has been solved, achieving efficient, economical, and environmentally friendly wastewater treatment.

CN118954653AInactive Publication Date: 2024-11-15XIHUA UNIV

Patent Information

Application Number
CN202411287803.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention belongs to the field of acid mine wastewater treatment, and particularly discloses a modified base material for treating acid mine wastewater, a preparation method of the modified base material and a method for treating the acid mine wastewater. The modified base material is prepared from a main material and an auxiliary material; the main materials comprise a carbonate rock matrix and biomass charcoal, and the mass ratio of the carbonate rock matrix to the biomass charcoal is (5-25): 1; the auxiliary materials comprise clay, quartz sand and calcium oxide. According to the modified base material for treating the acid mine wastewater, the preparation method and the method for treating the acid mine wastewater, in the application process, the investment of chemical agents is not needed, secondary pollution caused by a large amount of sludge is avoided, the use cost is low, and the modified base material is environmentally friendly, economical, capable of being used continuously and capable of being recycled. The treatment efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of acid mine wastewater treatment, and in particular to a modified alkaline material for treating acid mine wastewater, a preparation method thereof, and a method for treating acid mine wastewater. Background Art

[0002] Acid mine drainage (AMD) is produced by the interaction of sulfide minerals in abandoned and operating mines and mining waste rock with air, water and bacteria (such as Thiobacillus). AMD has low pH and high SO4 2 - content, as well as the characteristics of containing a variety of high concentrations of metals and trace elements (Fe, Mn, Zn, Cu, Pb, As, Cd and Cr, etc.). If they are allowed to be discharged in an unordered manner, they will have serious impacts on groundwater, surface water, soil environment and even human health, and have attracted much attention. AMD mainly comes from the oxidation of sulfide minerals, which are exposed to the environment due to intensive mining activities. The chemical reactions of the soluble typical sulfide mineral pyrite (FeS2) under different oxidation conditions can explain the formation mechanism of AMD (Equations 1 to 6).

[0003]

[0004] Fe 3+ +3H2O→Fe(OH)3+3H + (Formula 3)

[0005]

[0006] FeS2+14Fe 3+ +8H2O→15Fe 2+ +2SO2 2- +16H + (Formula 5)

[0007]

[0008] The existing ideas for treating AMD mainly include inhibiting the production of AMD at the source and collecting and treating it at the end.

[0009] (1) Suppressing the generation of AMD at the source: This is to target the mechanism of AMD generation and go against the flow to block sulfide minerals from the influence of air, water and bacteria, thereby suppressing AMD. For example, tailings containing sulfide minerals are backfilled with clay, crushed aggregate, sand materials and cement or other adhesives to prevent air from contacting sulfide minerals, limit their oxidation process and minimize the formation of acid; for waste rock dumps and tailings ponds storing sulfide minerals, preventive measures such as dry cover, water cover and underwater tailings treatment are often used as oxygen barriers to suppress the generation of AMD; in addition, for abandoned mines that have reached their service life or have not been mined, channel blocking measures are taken to reduce AMD emissions, while restoring the oxidizing conditions of water-rock interaction to the original reducing conditions to control the generation of AMD from the source. Due to the persistence of AMD after its formation, suppressing the generation of AMD from the source is obviously the best strategy to deal with the AMD problem and minimize its environmental impact. However, in many parts of the world, sulfide ore layers are often associated with or sandwiched between coal seams, and the lithologic components of the stratigraphic layers adjacent to such ore layers are mostly carbonate rocks. For example, the coal seams of the Upper Permian Longtan Formation in southwest my country are adjacent to the carbonate rock layers of the Lower Qixia and Maokou Formations, and the coal seams of the Upper Triassic Xujiahe Formation are adjacent to the carbonate rock layers of the Middle Leikoupo Formation and the Lower Jialingjiang Formation. Mining activities in karst mountainous areas have created a close hydraulic connection between karst groundwater and AMD, making them extremely susceptible to pollution. Taking the Sichuan Shiping coal pyrite mining area as an example, the applicant identified the pollution patterns of AMD to the water environment in karst mountainous areas based on the runoff path of AMD, which can be divided into: 1) acidic water infiltrates into groundwater along the karst channel and then discharges to surface water; 2) acidic water is discharged along the tunnel and then pollutes surface water; 3) acidic water pollutes the water environment through alternating open and underground flows. In carbonate rock areas with abundant groundwater, the high heterogeneity of the water-bearing medium caused by the development of karst gaps and karst pipes makes it insufficient to improve or even repair the water environment by simply suppressing the production of AMD at the source.

[0010] (2) AMD terminal collection and disposal: According to the degree of human intervention, it can be divided into two main categories: "active management" and "passive management".

[0011] "Active treatment" technology: mainly through the addition of alkaline reagents to increase the pH of the water body, so that the metal ions form insoluble precipitation, ion exchange, and membrane technology. "Active treatment" technology requires the input of chemical agents and also needs to avoid "secondary pollution" caused by a large amount of sludge, resulting in high costs for harmless disposal of AMD.

[0012] "Passive treatment" technology: It is to remove pollutants from water by artificially regulating and strengthening the physical, chemical and biological processes in the natural environment. Technical methods have been developed, including lime conversion wells, open limestone ditches, anoxic limestone ditches, artificial wetlands, continuous alkali production systems and permeable reaction walls. Passive treatment does not require continuous consumption of chemicals and high sludge disposal costs, and is considered an economic alternative to "active treatment", but the treatment efficiency is low due to problems such as passivation of fillers and channel blockage.

[0013] The applicant has found that the prior art has at least the following technical problems:

[0014] In carbonate rock areas with abundant groundwater, the high heterogeneity of water-bearing media due to the development of karst crevices and karst pipes makes it insufficient to improve or even repair the water environment by simply suppressing the generation of AMD at the source. At the same time, the cost of harmless disposal of AMD is high due to the need for chemical input and the need to avoid "secondary pollution" caused by a large amount of sludge, while the "passive treatment" technology has low disposal efficiency due to problems such as passivation of fillers and channel blockage. Summary of the invention

[0015] The purpose of the present invention is to provide a modified alkaline material and preparation method for treating acid mine wastewater, and a method for treating acid mine wastewater, so as to solve the problem in the prior art that in carbonate rock areas with abundant groundwater, the high heterogeneity of the water-containing medium caused by the development of karst crevices and karst pipes makes it insufficient to improve or even repair the water environment by only inhibiting the production of AMD at the source. At the same time, the "active treatment" technology requires the input of chemical agents and the need to avoid "secondary pollution" caused by a large amount of sludge, so the cost of harmless disposal of AMD is high, while the "passive treatment" technology has the technical problem of low disposal efficiency due to problems such as passivation of fillers and channel blockage. The many technical effects that can be produced by the preferred technical scheme among the many technical schemes provided by the present invention are described in detail below.

[0016] To achieve the above object, the present invention provides the following technical solutions:

[0017] The present invention provides a modified alkaline material for treating acid mine wastewater, and its preparation includes main materials and auxiliary materials; wherein,

[0018] The main materials are carbonate matrix and biomass charcoal, and the mass ratio of the carbonate matrix to the biomass charcoal is 5-25:1;

[0019] The auxiliary materials are clay, quartz sand and calcium oxide; the amount of clay added is 15-25% of the mass of the main material; the amount of quartz sand added is 0.5-2% of the mass of the main material; and the amount of calcium oxide added is 0.5-2% of the mass of the main material.

[0020] Furthermore, the mass ratio of the carbonate rock matrix to the biochar in the main material is 9-19:1.

[0021] Furthermore, the mass ratio of the carbonate rock matrix to the biochar in the main material is 15:1.

[0022] Furthermore, the carbonate rock matrix is ​​limestone and dolomite, and the mass ratio of limestone to dolomite is 1-3:1-3.

[0023] Furthermore, the biochar is prepared from straw and coffee grounds into straw biochar and coffee grounds biochar respectively; the mass ratio of the straw biochar to the coffee grounds biochar in the biochar is 1-3:1-3.

[0024] Furthermore, the amount of clay added is 18-22% of the mass of the main material; the amount of quartz sand added is 1-1.5% of the mass of the main material; and the amount of calcium oxide added is 0.8-1.2% of the mass of the main material.

[0025] Furthermore, the amount of clay added is 20% of the mass of the main material; the amount of quartz sand added is 1% of the mass of the main material; and the amount of calcium oxide added is 1% of the mass of the main material.

[0026] The present invention provides a method for preparing a modified alkaline material for treating acid mine wastewater, comprising the following steps:

[0027] A1. Grind the carbonate rock matrix, clay and calcium oxide into carbonate rock matrix powder, clay powder and calcium oxide powder respectively;

[0028] A2. Prepare biochar using straw and / or coffee grounds and crush them into biochar powder;

[0029] A3, mixing the carbonate matrix powder, clay powder, calcium oxide powder obtained by crushing in step A1 in proportion, the biomass charcoal powder prepared in step A2, and quartz sand evenly to obtain a mixture;

[0030] A4. Granulate the mixture obtained in step A3 to obtain carbonate rock-based modified alkali material.

[0031] Furthermore, in the step A1 and the step A2, the carbonate matrix powder, the clay powder, the calcium oxide powder and the biochar powder are screened through a 60-100 mesh sieve;

[0032] In the step A4, the granulation is performed by a disc granulator, and the obtained carbonate rock-based modified alkali material is spherical particles with a particle size of 2 to 5 mm.

[0033] The present invention provides a method for treating acid mine wastewater, comprising the following steps:

[0034] B1. Construct natural river channels or newly built channels into multi-level waterfall platforms;

[0035] B2. Filling the bottom of each level of the waterfall platform and the water-passing section with the above-mentioned modified base material or the modified base material prepared by the above-mentioned preparation method in layers;

[0036] B3. Through the multi-stage aeration of the waterfall platform, the rapid oxidation of ferrous ions and sulfides in the acidic mine wastewater is achieved. The modified alkaline materials filled in layers neutralize the acidic mine wastewater, provide attachment space for heavy metal ions, and the generated hydroxide reacts with the Fe2O3 formed by oxidation after the waterfall. 3+ The formed sediment also adheres to the modified material and the riverbed bottom, improving the treatment efficiency of acid mine drainage.

[0037] Based on the above technical solution, the embodiments of the present invention can at least produce the following technical effects:

[0038] The modified alkali material for treating acid mine wastewater provided by the present invention is a modified material prepared by adding biochar to a carbonate rock matrix; the carbonate rock matrix selects natural limestone and dolomite, which has the characteristics of abundant reserves and strong acid neutralization ability. In addition, carbonate also shows good metal ion affinity, and is suitable for treatment materials for removing heavy metals in water bodies; the added biochar selects straw biochar and coffee grounds biochar, which have loose and porous surfaces and rich active groups. Adding them to the carbonate rock matrix increases the specific surface area and alkali production efficiency of the carbonate rock matrix, and avoids surface passivation and channel blockage of the modified alkali material; the added clay, quartz sand and calcium oxide are auxiliary granulation materials, the main component of clay is aluminosilicate, which serves as a binder for the modified material, and calcium oxide is an alkali activator, which will strengthen the alkali activating effect of clay as a binder in the granulation process, and the quartz sand will improve the particle strength of the modified material to meet the granulation requirements. The modified alkaline material for treating acid mine wastewater provided by the present invention does not require the input of chemical agents when used, avoids "secondary pollution" caused by a large amount of sludge, has a low cost of use, and is a green, economical, sustainable and highly efficient acid mine wastewater treatment material.

[0039] The method for treating acid mine wastewater provided by the present invention firstly performs natural riverbed waterfall, which is a widely used method for water body self-purification. The principle is to increase the oxygen in the gas phase to enter the liquid phase, promote the reaction rate of formula (6), and accelerate the Fe 3+ The formation and reaction of OH in water - Reaction precipitation can achieve the removal effect, which is the pre-treatment technology for the treatment of modified alkaline materials; in the riverbed waterfall, Fe 3+ After the formation of the modified base material, OH- , forming the OH required for Fe(OH)3 precipitation - At the same time, the increased specific surface area of ​​the base-modified material will provide space for the attachment of precipitates. DETAILED DESCRIPTION

[0040] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0041] 1. Preparation of modified base materials

[0042] Embodiment 1:

[0043] 1.1 Raw materials:

[0044] Main ingredients: carbonate rock matrix and biochar, wherein the mass ratio of the carbonate rock matrix to the biochar is 15:1; the carbonate rock matrix is ​​limestone and dolomite, wherein the mass ratio of the limestone to the dolomite is 2:2; the biochar is prepared from straw and coffee grounds into straw biochar and coffee grounds biochar, respectively, wherein the mass ratio of the straw biochar to the coffee grounds biochar in the biochar is 2:2; the quartz sand is 60 mesh quartz sand;

[0045] Auxiliary materials: clay, quartz sand and calcium oxide; the amount of clay added is 20% of the mass of the main material; the amount of quartz sand added is 1% of the mass of the main material; the amount of calcium oxide added is 1% of the mass of the main material.

[0046] 1.2 Preparation method, comprising the following steps:

[0047] A1. Crush the carbonate rock matrix, clay and calcium oxide respectively and sieve through an 80-mesh sieve to obtain carbonate rock matrix powder, clay powder and calcium oxide powder;

[0048] A2, preparing biochar using straw and / or coffee grounds, and then crushing and sieving through an 80-mesh sieve to obtain biochar powder;

[0049] A3, mixing the carbonate matrix powder, clay powder, calcium oxide powder obtained by crushing in step A1 in proportion, the biomass charcoal powder prepared in step A2, and quartz sand evenly to obtain a mixture;

[0050] A4. Granulate the mixture obtained in step A3 using a disc granulator to obtain carbonate rock-based modified alkali material with spherical particles having a particle size of 2 to 5 mm.

[0051] Embodiment 2:

[0052] 2.1 Raw materials:

[0053] Main ingredients: carbonate rock matrix and biochar, wherein the mass ratio of the carbonate rock matrix to the biochar is 25:1; the carbonate rock matrix is ​​limestone and dolomite, wherein the mass ratio of the limestone to the dolomite is 3:1; the biochar is prepared from straw and coffee grounds into straw biochar and coffee grounds biochar, respectively, wherein the mass ratio of the straw biochar to the coffee grounds biochar in the biochar is 1:3; the quartz sand is 80 mesh quartz sand;

[0054] Auxiliary materials: clay, quartz sand and calcium oxide; the amount of clay added is 25% of the mass of the main material; the amount of quartz sand added is 2% of the mass of the main material; the amount of calcium oxide added is 0.5% of the mass of the main material.

[0055] 2.2 Preparation method, comprising the following steps:

[0056] A1. Crush the carbonate rock matrix, clay and calcium oxide respectively and sieve through an 80-mesh sieve to obtain carbonate rock matrix powder, clay powder and calcium oxide powder;

[0057] A2, preparing biochar using straw and / or coffee grounds, and then crushing and sieving through an 80-mesh sieve to obtain biochar powder;

[0058] A3, mixing the carbonate matrix powder, clay powder, calcium oxide powder obtained by crushing in step A1 in proportion, the biomass charcoal powder prepared in step A2, and quartz sand evenly to obtain a mixture;

[0059] A4. Granulate the mixture obtained in step A3 using a disc granulator to obtain carbonate rock-based modified alkali material with spherical particles having a particle size of 2 to 5 mm.

[0060] Embodiment 3:

[0061] 3.1 Raw materials:

[0062] Main ingredients: carbonate rock matrix and biochar, the mass ratio of the carbonate rock matrix to the biochar is 5:1; the carbonate rock matrix is ​​limestone and dolomite, and the mass ratio of the limestone to the dolomite is 1:3; the biochar is prepared from straw and coffee grounds into straw biochar and coffee grounds biochar, respectively, and the mass ratio of the straw biochar to the coffee grounds biochar in the biochar is 1:3; the quartz sand is 40 mesh quartz sand;

[0063] Auxiliary materials: clay, quartz sand and calcium oxide; the amount of clay added is 15% of the mass of the main material; the amount of quartz sand added is 0.5% of the mass of the main material; the amount of calcium oxide added is 2% of the mass of the main material.

[0064] 3.2 Preparation method, comprising the following steps:

[0065] A1. Crush the carbonate rock matrix, clay and calcium oxide respectively and sieve through an 80-mesh sieve to obtain carbonate rock matrix powder, clay powder and calcium oxide powder;

[0066] A2, preparing biochar using straw and / or coffee grounds, and then crushing and sieving through an 80-mesh sieve to obtain biochar powder;

[0067] A3, mixing the carbonate matrix powder, clay powder, calcium oxide powder obtained by crushing in step A1 in proportion, the biomass charcoal powder prepared in step A2, and quartz sand evenly to obtain a mixture;

[0068] A4. Granulate the mixture obtained in step A3 using a disc granulator to obtain carbonate rock-based modified alkali material with spherical particles having a particle size of 2 to 5 mm.

[0069] Embodiment 4:

[0070] 4.1 Raw materials:

[0071] Main ingredients: carbonate rock matrix and biochar, wherein the mass ratio of the carbonate rock matrix to the biochar is 10:1; the carbonate rock matrix is ​​limestone and dolomite, wherein the mass ratio of the limestone to the dolomite is 1.5:2; the biochar is prepared from straw and coffee grounds into straw biochar and coffee grounds biochar, respectively, wherein the mass ratio of the straw biochar to the coffee grounds biochar in the biochar is 2:1.5; the quartz sand is 60 mesh quartz sand;

[0072] Auxiliary materials: clay, quartz sand and calcium oxide; the amount of clay added is 18% of the mass of the main material; the amount of quartz sand added is 0.8% of the mass of the main material; the amount of calcium oxide added is 1% of the mass of the main material.

[0073] 4.2 Preparation method, comprising the following steps:

[0074] A1. Crush the carbonate rock matrix, clay and calcium oxide respectively and sieve through an 80-mesh sieve to obtain carbonate rock matrix powder, clay powder and calcium oxide powder;

[0075] A2, preparing biochar using straw and / or coffee grounds, and then crushing and sieving through an 80-mesh sieve to obtain biochar powder;

[0076] A3, mixing the carbonate matrix powder, clay powder, calcium oxide powder obtained by crushing in step A1 in proportion, the biomass charcoal powder prepared in step A2, and quartz sand evenly to obtain a mixture;

[0077] A4. Granulate the mixture obtained in step A3 using a disc granulator to obtain carbonate rock-based modified alkali material with spherical particles having a particle size of 2 to 5 mm.

[0078] Embodiment 5:

[0079] 5.1 Raw materials:

[0080] Main ingredients: carbonate rock matrix and biochar, the mass ratio of the carbonate rock matrix to the biochar is 20:1; the carbonate rock matrix is ​​limestone and dolomite, and the mass ratio of the limestone to the dolomite is 2.5:1.5; the biochar is prepared from straw and coffee grounds into straw biochar and coffee grounds biochar, respectively, and the mass ratio of the straw biochar to the coffee grounds biochar in the biochar is 1.5:2; the quartz sand is 60 mesh quartz sand;

[0081] Auxiliary materials: clay, quartz sand and calcium oxide; the amount of clay added is 22% of the mass of the main material; the amount of quartz sand added is 1.5% of the mass of the main material; the amount of calcium oxide added is 1.2% of the mass of the main material.

[0082] 5.2 Preparation method, comprising the following steps:

[0083] A1. Crush the carbonate rock matrix, clay and calcium oxide respectively and sieve through an 80-mesh sieve to obtain carbonate rock matrix powder, clay powder and calcium oxide powder;

[0084] A2, preparing biochar using straw and / or coffee grounds, and then crushing and sieving through an 80-mesh sieve to obtain biochar powder;

[0085] A3, mixing the carbonate matrix powder, clay powder, calcium oxide powder obtained by crushing in step A1 in proportion, the biomass charcoal powder prepared in step A2, and quartz sand evenly to obtain a mixture;

[0086] A4. Granulate the mixture obtained in step A3 using a disc granulator to obtain carbonate rock-based modified alkali material with spherical particles having a particle size of 2 to 5 mm.

[0087] Embodiment 6:

[0088] 6.1 Raw materials:

[0089] Main ingredients: carbonate rock matrix and biochar, the mass ratio of the carbonate rock matrix to the biochar is 18:1; the carbonate rock matrix is ​​limestone and dolomite, and the mass ratio of the limestone to the dolomite is 2.2:1; the biochar is prepared from straw and coffee grounds into straw biochar and coffee grounds biochar, respectively, and the mass ratio of the straw biochar to the coffee grounds biochar in the biochar is 1.5:3; the quartz sand is 60 mesh quartz sand;

[0090] Auxiliary materials: clay, quartz sand and calcium oxide; the amount of clay added is 15% of the mass of the main material; the amount of quartz sand added is 0.5% of the mass of the main material; the amount of calcium oxide added is 2% of the mass of the main material.

[0091] 6.2 Preparation method, comprising the following steps:

[0092] A1. Crush the carbonate rock matrix, clay and calcium oxide respectively and sieve through an 80-mesh sieve to obtain carbonate rock matrix powder, clay powder and calcium oxide powder;

[0093] A2, preparing biochar using straw and / or coffee grounds, and then crushing and sieving through an 80-mesh sieve to obtain biochar powder;

[0094] A3, mixing the carbonate matrix powder, clay powder, calcium oxide powder obtained by crushing in step A1 in proportion, the biomass charcoal powder prepared in step A2, and quartz sand evenly to obtain a mixture;

[0095] A4. Granulate the mixture obtained in step A3 using a disc granulator to obtain carbonate rock-based modified alkali material with spherical particles having a particle size of 2 to 5 mm.

[0096] The method for using the carbonate rock-based modified alkali material prepared in the present invention is:

[0097] (1) Natural riverbed waterfall

[0098] Natural riverbed waterfalls are not an innovative step, but a widely used method for water self-purification. The principle is to increase the oxygen in the gas phase into the liquid phase, promote the reaction rate of (Equation 6), and accelerate the Fe 3+ The formation and reaction of OH in water - Reaction precipitation achieves the removal effect. It is the pre-treatment technology for the disposal of modified alkali materials.

[0099]

[0100] Fe 3+ +3H2O→Fe(OH)3+3H + (Formula 3)

[0101]

[0102] FeS2+14Fe3++8H2O→15Fe 2+ +2SO2 2- +16H + (Formula 5)

[0103]

[0104] (2) Application of modified base materials

[0105] Riverbed waterfall accelerates Fe removal in acid mine drainage water 3+ After the formation of the modified base material, the OH required to form the Fe(OH)3 precipitate is provided. - At the same time, the increased specific surface area of ​​the modified material will provide space for the attachment of precipitates.

[0106] B1. Construct natural river channels or newly built channels into multi-level waterfall platforms;

[0107] B2. Filling the modified base materials in Example 1, Example 2, Example 3, Example 4, Example 5 or Example 6 in layers at the bottom of each level of the waterfall platform and the water-passing section;

[0108] B3. Through the multi-stage aeration of the waterfall platform, the rapid oxidation of ferrous ions and sulfides in the acidic mine wastewater is achieved. The modified alkaline materials filled in layers neutralize the acidic mine wastewater, provide attachment space for heavy metal ions, and the generated hydroxide reacts with the Fe2O3 formed by oxidation after the waterfall. 3+ The formed sediment also adheres to the modified material and the riverbed bottom, improving the treatment efficiency of acid mine drainage.

[0109] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A modified alkaline material for treating acidic mine wastewater, It is characterized in that Its preparation includes main ingredients and auxiliary materials; wherein, The main materials are carbonate matrix and biomass charcoal, and the mass ratio of the carbonate matrix to the biomass charcoal is 5-25:1; The auxiliary materials are clay, quartz sand and calcium oxide; the amount of clay added is 15-25% of the mass of the main material; the amount of quartz sand added is 0.5-2% of the mass of the main material; and the amount of calcium oxide added is 0.5-2% of the mass of the main material.

2. The modified alkaline material for treating acid mine wastewater according to claim 1, It is characterized in that The mass ratio of carbonate rock matrix to biomass charcoal in the main material is 9-19:

1.

3. The modified alkaline material for treating acid mine wastewater according to claim 1, It is characterized in that The mass ratio of the carbonate rock matrix to the biochar in the main material is 15:

1.

4. The modified alkaline material for treating acid mine wastewater according to claim 1, It is characterized in that The carbonate rock matrix is ​​limestone and dolomite, and the mass ratio of limestone to dolomite is 1-3:1-3.

5. The modified alkaline material for treating acid mine wastewater according to claim 1, It is characterized in that The biomass charcoal is prepared from straw and coffee grounds into straw biomass charcoal and coffee grounds biomass charcoal respectively; the mass ratio of the straw biomass charcoal to the coffee grounds biomass charcoal in the biomass charcoal is 1-3:1-3.

6. The modified alkaline material for treating acid mine wastewater according to claim 1, It is characterized in that The amount of clay added is 18-22% of the mass of the main material; the amount of quartz sand added is 1-1.5% of the mass of the main material; and the amount of calcium oxide added is 0.8-1.2% of the mass of the main material.

7. The modified alkaline material for treating acid mine wastewater according to claim 1, It is characterized in that The amount of clay added is 20% of the mass of the main material; the amount of quartz sand added is 1% of the mass of the main material; and the amount of calcium oxide added is 1% of the mass of the main material.

8. A method for preparing a modified alkaline material for treating acid mine wastewater according to any one of claims 1 to 7, It is characterized in that The steps include: A1. Grind the carbonate rock matrix, clay and calcium oxide into carbonate rock matrix powder, clay powder and calcium oxide powder respectively; A2. Prepare biochar using straw and / or coffee grounds and crush them into biochar powder; A3, mixing the carbonate matrix powder, clay powder, calcium oxide powder obtained by crushing in step A1 in proportion, the biomass charcoal powder prepared in step A2, and quartz sand evenly to obtain a mixture; S4, granulating the mixture obtained in step A3 to obtain a carbonate rock-based modified base material.

9. The method for preparing the modified alkaline material for treating acid mine wastewater according to claim 8, It is characterized in that In the step A1 and the step A2, the carbonate matrix powder, the clay powder, the calcium oxide powder and the biochar powder are screened through a 60-100 mesh sieve; In the step A4, the granulation is performed by a disc granulator, and the obtained carbonate rock-based modified alkali material is spherical particles with a particle size of 2 to 5 mm.

10. A method for treating acid mine drainage, It is characterized in that The steps include: B1. Construct natural river channels or newly built channels into multi-level waterfall platforms; B2. Filling the bottom of each level of the waterfall platform and the water-passing section with the modified base material described in any one of claims 1 to 7 or the modified base material prepared by the preparation method described in any one of claims 8 to 9 in layers; B3. Through the multi-stage aeration of the waterfall platform, the rapid oxidation of ferrous ions and sulfides in the acidic mine wastewater is achieved. The modified alkaline materials filled in layers neutralize the acidic mine wastewater and provide attachment space for heavy metal ions. The generated hydroxide reacts with the Fe2O3 formed by oxidation after the waterfall. 3+ The formed sediment also adheres to the modified material and the riverbed bottom, improving the treatment efficiency of acid mine drainage.

Citation Information

Patent Citations

  • Method for treating mine acidic wastewater by means of mixed packing of organic matter and carbonatite

    CN102674559A

  • Method for jointly treating acid mine wastewater by using organic matter and carbonate rock

    CN102701517A

  • Acid mine wastewater treatment process

    CN111377516A

  • Mine habitat reconstruction coupling ecological treatment system and method for acid mine wastewater

    CN114163066A

  • System and method for simply treating acidic mine wastewater containing heavy metal ions

    CN116969573A

Cited By

  • Material for treating acid mine wastewater, preparation method and wastewater treatment method

    CN120698636A

  • A material for treating acid mine drainage and a method of preparation and a method of treating wastewater

    CN120698636B