Aerogel-expanded perlite composite slurry as well as preparation method and application thereof

By preparing an oil-absorbing box using superhydrophobic silica aerogel powder and expanded perlite composite material, the problems of high cost and environmental pollution of oil-absorbing materials in range hoods are solved, achieving efficient adsorption and environmentally friendly oil absorption effect.

CN118955083APending Publication Date: 2024-11-15THE HIGH SCHOOL AFFILIATED TO SHANGHAI JIAOTONG UNIV JIADING BRANCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411127799.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing oil-absorbing materials used in range hoods suffer from problems such as complex manufacturing processes, high costs, and difficulty in effectively absorbing waste oil. Furthermore, traditional cleaning methods are harmful to the environment.

Method used

A composite slurry of aerogel-expanded perlite was prepared by combining superhydrophobic silica aerogel powder with open-pore expanded perlite, and then using binders, surface modifiers, fibers and thickeners. After curing, the slurry was applied to the oil suction box of a range hood, utilizing its micron and nanopores to adsorb waste oil.

Benefits of technology

It achieves efficient adsorption of kitchen smoke condensate waste oil, avoids channel blockage, reduces production costs, avoids environmental pollution caused by chemical cleaning, and supports the reuse of the oil suction box.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955083A_ABST
    Figure CN118955083A_ABST
Patent Text Reader

Abstract

The invention relates to aerogel-expanded perlite composite slurry as well as a preparation method and application thereof. The aerogel-expanded perlite composite slurry is prepared from aerogel powder, expanded perlite, water, a surface modifier, an inorganic silicon adhesive, fibers and a thickening agent; the aerogel-expanded perlite composite slurry is prepared from the following components in percentage by mass: 5 to 10 percent of aerogel powder, 10 to 30 percent of expanded perlite, 30 to 73.45 percent of water, 0.5 to 2 percent of surface modifier, 10 to 25 percent of inorganic silicon adhesive, 1 to 2.5 percent of fiber and 0.05 to 0.5 percent of thickening agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil absorbing materials, and in particular relates to an aerogel-expanded perlite composite slurry and a preparation method and application thereof. Background Art

[0002] Range hoods are an indispensable kitchen appliance in today's families. While protecting human health, they also produce a lot of waste oil. Unlike ordinary cooking oil, this waste oil has a strong adhesive force. When pouring, a thick layer of oil will adhere to the bottom and sides of the oil collection box, which is difficult to remove. At the same time, the cleaning and discharge of waste oil will inevitably use a large amount of chemical detergents and cooking oil cleaners, which will cause great harm to the environment. Therefore, there is an urgent need for an efficient, environmentally friendly and convenient oil suction box.

[0003] Superhydrophobic silica aerogel powder is a porous nanomaterial with high oleophilic properties, featuring high porosity, large specific surface area, and large pore volume. The surface of its silica nanoparticles is loaded with a large number of methyl functional groups, so it has a strong affinity for oily materials. However, the density of superhydrophobic silica aerogel powder is very low, and the commercial powder density is only 0.03-0.05g / cm 3 , it is very easy to be affected by the disturbance of the ambient air and disperse. Therefore, the aerogel powder needs to be solidified into a block material with a certain strength to avoid the influence of environmental factors.

[0004] There have been several studies on aerogel materials in the field of oil absorption. Chinese patent CN202311732779.1 discloses a method for preparing an elastic composite silicon aerogel oil-absorbing material based on nano carbon black, Chinese patent CN202311520554.X discloses a method for preparing a waste straw-based cellulose aerogel oil absorbent, and Chinese patent CN201811119941.1 discloses a peanut shell graphene composite aerogel oil-absorbing material and its preparation method, etc. However, the existing preparation methods of oil-absorbing aerogels are complex, or use expensive raw materials such as graphene, or use special preparation conditions such as high temperature and high pressure, which is not conducive to application in the field of oil absorption boxes of range hoods.

[0005] In addition, due to the raw materials and preparation process, the cost of aerogel materials is relatively high. Composite aerogel with other cheap porous materials to reduce the manufacturing cost of oil absorption boxes has important market value.

[0006] Literature research found that there are few reports on the application of expanded perlite in the field of oil absorption. For example, a doctoral dissertation (Lin Na, Harbin Institute of Technology, 2013) reported on the modification of expanded perlite and the research on emergency disposal of oil spill pollution. Chinese patent CN201710629461.9 discloses a method for preparing a perlite oil absorbent for absorbing oil on the water surface. However, there are no reports on the composite of expanded perlite and aerogel materials for use in the oil absorption box of range hoods. Summary of the invention

[0007] In view of the above problems, the present invention provides an aerogel-expanded perlite composite slurry and a preparation method and application thereof. Super-hydrophobic silica aerogel powder and open-pore expanded perlite are used as core adsorption raw materials, which are compounded with a binder, a surface modifier, a fiber, a thickener, etc., and prepared into an aerogel-expanded perlite composite slurry through a special stirring process. The slurry is then poured into an oil collecting box shell, and an aerogel-expanded perlite composite material is prepared through high-temperature curing and drying. The aerogel-expanded perlite composite material is applied to a high-efficiency and environmentally friendly oil absorption box for range hoods, making full use of the ultra-high pore volume and unique oleophilic properties of silica aerogel and the adsorption properties of the micron pores of the expanded perlite, so that the condensed waste oil is adsorbed into the nano-pores of the aerogel and the micron pores of the expanded perlite, thereby facilitating cleaning and avoiding waste oil and cleaning chemicals for cleaning the waste oil from polluting the environment.

[0008] In a first aspect, the present invention provides an aerogel-expanded perlite composite slurry, comprising: aerogel powder, expanded perlite, water, a surface modifier, an inorganic silica adhesive, fibers and a thickener; The composition of the aerogel-expanded perlite composite slurry includes, by mass percentage, 5-10% aerogel powder, 10-30% expanded perlite, 30-73.45% water, 0.5-2% surface modifier, 10-25% inorganic silica adhesive, 1-2.5% fiber, and 0.05-0.5% thickener.

[0009] Preferably, the aerogel powder is super hydrophobic silica aerogel powder; the particle size of the super hydrophobic silica aerogel powder is 10 to 40 μm; the tap density is 0.03 to 0.05 g / cm 3 ; The average pore diameter is less than 50nm; the pore volume is greater than 3ml / g; the water contact angle is greater than 150°.

[0010] Preferably, the expanded perlite is an open-pore expanded perlite; the tap density of the open-pore expanded perlite is 0.12 to 0.16 g / cm 3 ; The particle size is 50-70 mesh.

[0011] Preferably, the surfactant includes a cationic surfactant and / or a neutral surfactant; the cationic surfactant is at least one of cetyltrimethylammonium bromide, stearylamine hydrochloride, and dodecyldimethylbenzyl ammonium chloride; the neutral surfactant is at least one of Tween-20, OP-10, Span-80, and peregal.

[0012] Preferably, the inorganic silicon binder is at least one of sodium silicate water glass, potassium silicate water glass, lithium silicate water glass and silica sol; the mass percentage of silicon dioxide in the inorganic silicon binder is not less than 25%.

[0013] Preferably, the fiber is at least one of wood fiber, glass fiber and plastic fiber.

[0014] Preferably, the thickener is a water-soluble cellulose thickener; the water-soluble cellulose thickener is sodium carboxymethyl cellulose or hydroxypropyl methylcellulose.

[0015] Preferably, the viscosity of the aerogel-expanded perlite composite slurry is 30,000 to 60,000 cp.

[0016] In a second aspect, the present invention provides a method for preparing an aerogel-expanded perlite composite slurry, comprising: stirring and mixing water and a thickener, adding a surfactant, an inorganic silicone adhesive, and fibers in sequence, and then slowly adding aerogel powder under high-speed stirring, and after it is completely dispersed, finally adding expanded perlite and stirring at a low speed to obtain the aerogel-expanded perlite composite slurry.

[0017] Preferably, the high-speed stirring rate is 1000-2000 rpm; preferably 1300-1600 rpm.

[0018] Preferably, the low-speed stirring rate is 60 to 300 rpm; preferably 100 to 200 rpm.

[0019] In a third aspect, the present invention provides a method for preparing an aerogel-expanded perlite composite material, comprising: pouring the above-mentioned aerogel-expanded perlite composite slurry into an oil collecting box mold, placing it in a forced air drying oven, and curing and drying it to a constant weight to obtain the aerogel-expanded perlite composite material.

[0020] Preferably, after pouring the aerogel-expanded perlite composite slurry into the oil collecting box mold, the oil collecting box mold is vibrated on a rubber pad for several times to ensure uniform filling of the slurry; the number of vibrations is 50 to 200 times.

[0021] Preferably, the curing and drying temperature is 105-150° C.; the curing and drying time is 8-48 hours.

[0022] Preferably, the condition for curing and drying to constant weight is that the weight deviation measured three times consecutively every 1 hour is no more than 0.1 g.

[0023] In a fourth aspect, the present invention provides an aerogel-expanded perlite composite material prepared according to the above preparation method.

[0024] Preferably, the compressive strength of the aerogel-expanded perlite composite material is 0.1-0.2 MPa.

[0025] In a fifth aspect, the present invention provides an oil absorption box comprising the above-mentioned aerogel-expanded perlite composite material.

[0026] In a sixth aspect, the present invention provides an application of the above-mentioned oil suction box in a range hood.

[0027] In the oil absorption box containing the aerogel-expanded perlite composite material prepared by the above process, the aerogel powder and the expanded perlite particles are firmly bonded together by the inorganic silicone adhesive to form a block with a certain strength and a fixed shape, which fits well with the box wall without gaps. The compressive strength of the surface of the aerogel-expanded perlite composite material is about 0.1-0.2MPa.

[0028] After the oil absorption box containing the aerogel-expanded perlite composite material prepared by the present invention is used, the internal pores of the aerogel-expanded perlite composite material will be saturated with the absorption of oil smoke, and the appearance will change from white to the brown color of waste oil. The silica aerogel that absorbs oil stains can be pried out of the box with a hard tool and cleaned, thereby realizing the reuse of the oil absorption box.

[0029] Beneficial effects: (1) The present invention combines two highly efficient adsorption materials, namely, super hydrophobic silica aerogel powder with abundant nanopores and expanded perlite with abundant micropores, and utilizes the effective combination of their micropores and nanopores to fully adsorb waste oil molecules with different molecular weights and different molecular sizes in waste oil condensed from kitchen smoke, thereby making the adsorption more efficient and avoiding the pores being blocked by waste oil macromolecules, resulting in a large number of micropores / nanopores being unable to be effectively adsorbed; (2) The present invention uses open-pore expanded perlite particles to prepare a composite oil absorption box, which can maximize the structural characteristics of the expanded perlite micron pores for waste oil absorption; (3) The present invention uses environmentally friendly water and inorganic silicon binder as solvent and adhesive, which can avoid the emission of organic solvents and polluting the environment during the production process, and also effectively reduces the production cost and ensures production safety; (4) The strength of the aerogel-expanded perlite composite material prepared by the present invention after molding is maintained at a relatively low level (0.1-0.2 MPa). After the composite material is saturated with oil in the oil absorption box, the aerogel solid can be pried out by a hard tool and the box body can be cleaned, thereby realizing the reuse of the box body. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The figure is a flow chart of the preparation of the aerogel-expanded perlite composite oil absorption box of the present invention; Figure 2 The schematic diagram of the structure of the aerogel-expanded perlite composite oil absorption box prepared by the present invention; wherein, 1-the outer wall of the oil collecting box; 2-the porous structure formed by curing the aerogel and the inorganic silicon binder; 3-the expanded perlite particles; 4-the central column of the oil collecting box. DETAILED DESCRIPTION

[0031] To further explain the content, characteristics and practical effects of the present invention, the present invention is described in detail below in conjunction with the embodiments. It should be pointed out that the modification method of the design of the present invention is not limited to these specific embodiments. Without departing from the spirit and connotation of the design of the present invention, the equivalent replacement and modification made by those skilled in the art on the basis of reading the content of the present invention are also within the scope of the present invention. In the absence of special instructions, each percentage refers to the percentage by mass.

[0032] First, the present invention provides an aerogel-expanded perlite composite slurry, comprising: aerogel powder, expanded perlite, water, surface modifier, inorganic silicone adhesive, fiber and thickener. The composition of the aerogel-expanded perlite composite slurry comprises: in terms of mass percentage, 5-10% aerogel powder, 10-30% expanded perlite, 30-73.45% water, 0.5-2% surface modifier, 10-25% inorganic silicone adhesive, 1-2.5% fiber, and 0.05-0.5% thickener.

[0033] In an optional embodiment, the aerogel powder is a super hydrophobic silica aerogel powder; the particle size of the super hydrophobic silica aerogel powder is 10 to 40 μm; and the tap density is 0.03 to 0.05 g / cm 3 ; Average pore size less than 50nm; Pore volume greater than 3ml / g; Water contact angle greater than 150°. The material, type and characteristics of aerogel powders vary, which will significantly affect the oil absorption performance of the final molded product. For example, hydrophilic silica aerogel powders have poor oil absorption performance; aerogel powders with low pore volume have low total oil absorption capacity; products with too low water contact angles have hydrophilic groups that are not conducive to oil adsorption; products with too large or too fine particles will make slurry molding difficult or affect slurry consistency and adsorption characteristics.

[0034] In an optional embodiment, the expanded perlite is an open-pore expanded perlite; the tap density of the open-pore expanded perlite is 0.12 to 0.16 g / cm 3 The particle size is 50-70 mesh. The present invention should not use closed-cell expanded perlite, because its pores are closed and the oil absorption effect is poor; it should not use products with too high density, because the pore volume is relatively small, and the adsorption capacity is lower under the same volume; it should not use products with too small particle size or too small density, because the strength is low when the density or particle size is small, and the pore structure is easily destroyed during the mixing and stirring process, resulting in the loss of oil absorption function.

[0035] Expanded perlite is prepared through a high-temperature process. The high temperature expands its internal structure, thereby forming a porous structure. The resulting product has two types: closed-cell and open-cell, of which the open-cell type is more common. However, the open pores are not all the pores on the surface of the particles, but only a small proportion of the pores are open, which means that the expanded perlite particles are a semi-closed cage-like structure in microstructure, with a large internal space and small pores. Therefore, it is difficult for oil to be discharged after entering, so it is very suitable for use as an efficient oil absorption material. The present invention combines expanded perlite particles with abundant micron pores with super-hydrophobic silica aerogel powder rock with abundant nanopores, and utilizes the effective combination of micron and nanopores of the two highly efficient adsorption materials to fully adsorb waste oil molecules with different molecular weights and different molecular sizes in the waste oil condensed from kitchen smoke, thereby making the adsorption more efficient and avoiding the pores being blocked by waste oil macromolecules, causing a large number of micron / nanopores to be unable to be effectively adsorbed.

[0036] In an optional embodiment, the surfactant includes a cationic surfactant and / or a neutral surfactant; the cationic surfactant is at least one of hexadecyltrimethylammonium bromide, stearylamine hydrochloride, and dodecyldimethylbenzyl ammonium chloride; the neutral surfactant is at least one of Tween-20, OP-10, Span-80, and peregrin. The role of the surfactant used in the present invention is mainly to change the surface chemical state of the superhydrophobic silica aerogel particles so that it can be compatible with the aqueous system. The role of using cationic and / or neutral surfactants is mainly to consider the silanol (-SiOH) groups on the surface of the aerogel particles and the silanol groups in the inorganic silica sol, which are complexed with water molecules in aqueous solution to show negative, so the use of neutral or cationic surfactants can enhance the surface charge affinity of the two.

[0037] In an optional embodiment, the inorganic silicon binder is at least one of sodium silicate water glass, potassium silicate water glass, lithium silicate water glass, and silica sol; the mass percentage of silicon dioxide in the inorganic silicon binder is not less than 25%. For water glass adhesives, products with a modulus of 3.2 or more can be selected; for silica sol adhesives, acidic or neutral silica sol types are preferably selected.

[0038] In an optional embodiment, the fiber is at least one of wood fiber, glass fiber, and plastic fiber. The function of the fiber is to enhance the strength, toughness and structural integrity of the composite system and avoid cracking.

[0039] In an optional embodiment, the thickener is a water-soluble cellulose thickener; the water-soluble cellulose thickener is sodium carboxymethyl cellulose or hydroxypropyl methyl cellulose; its purpose is to increase the consistency and viscosity of the aqueous solution, so as to facilitate uniform mixing of solvents, adhesives, etc. with superhydrophobic aerogel particles.

[0040] In an optional embodiment, the viscosity of the aerogel-expanded perlite composite slurry is 30,000 to 60,000 cp.

[0041] The following is an exemplary description of the method for preparing the aerogel-expanded perlite composite slurry provided by the present invention.

[0042] The preparation method of the aerogel-expanded perlite composite slurry comprises: firstly stirring and mixing water and a thickener, after uniform dispersion, sequentially adding a surfactant, an inorganic silica adhesive, and fibers, stirring evenly, then slowly adding aerogel powder under high-speed stirring, after complete uniform dispersion, finally adding expanded perlite, stirring evenly at a low speed, and obtaining the aerogel-expanded perlite composite slurry.

[0043] In the preparation of the aerogel-expanded perlite composite slurry of the present invention, the following points should be noted: (1) Water and thickener must be mixed first; the raw materials of water-soluble cellulose thickeners are generally in powder form, dissolve slowly in water, and need to be stirred for a long time before they can be evenly dispersed in water. (2) After the water, thickener, surfactant, inorganic silicon binder, and fiber are evenly mixed, the aerogel powder is added. The purpose is to first form a high-viscosity slurry solution, which is conducive to the uniform dispersion of the added aerogel powder particles in the slurry. In addition, during the process of adding and mixing the aerogel powder, a high rotation speed and a slow feeding rate must be maintained to ensure that the aerogel powder is evenly dispersed in the slurry. (4) The purpose of adding expanded perlite particles and stirring at a low speed is to prevent the perlite particles from being damaged by the stirring paddle or crushed by adjacent particles during high-speed stirring, resulting in collapse of the pore structure.

[0044] The preparation method of the aerogel-expanded perlite composite material provided by the present invention specifically includes the steps of: mold preparation, composite slurry casting, curing and drying. The following is an exemplary description of the preparation method of the aerogel-expanded perlite composite material (eg Figure 1 shown).

[0045] Pour the above-mentioned aerogel-expanded perlite composite slurry into the cleaned oil collecting box mold, and vibrate it on the rubber pad several times (such as 100 times) to make the slurry fill evenly. Since the internal structure of most oil collecting boxes is relatively complex, there are cylinders and hooks in the middle for fixing, and the aerogel slurry is thicker, with a viscosity in the range of 30,000 to 60,000 cp, it is necessary to apply vibration to make the aerogel slurry evenly dispersed and densely filled in the narrow oil absorption box. The viscosity of the aerogel slurry should not be too low or too high. If the viscosity is low, the amount of solvent used is large, and the volume shrinks greatly after curing, resulting in a small volume of the aerogel oil absorption block; if the viscosity is high, it is more difficult to pour in the oil collecting box and it is more difficult to disperse evenly.

[0046] In an optional embodiment, the oil collecting box may be made of plastic or metal. The oil collecting box needs to be cleaned before use, and may be surface treated if necessary to enhance its affinity with the organic silicone adhesive.

[0047] The oil collecting box filled with the aerogel-expanded perlite composite slurry is placed in a 105-150° C. forced air drying oven for curing and drying to a constant weight to obtain the aerogel-expanded perlite composite material.

[0048] In the present invention, during the heating and curing process, water evaporates, and the polymerized silicate molecules in the water glass or silica sol and the aerogel particles and expanded perlite particles are entangled and overlapped with each other to form a composite porous structure with a certain strength, that is, the aerogel-expanded perlite composite material.

[0049] In an optional embodiment, the curing and drying time of the composite slurry is 8 to 48 hours depending on the size and internal structure of different types of oil collecting boxes. Due to the unique semi-closed cage structure of expanded perlite with fewer openings, it takes a long time to completely dry out the moisture therein. Therefore, the present invention sets the oil absorption box to be dried to a constant weight state. The evaluation standard for constant weight is: the weight deviation of three consecutive measurements every 1 hour is no more than 0.1g.

[0050] In an optional embodiment, the compressive strength of the aerogel-expanded perlite composite material is controlled at 0.1-0.2 MPa. If the compressive strength is too low, it is easy to be damaged, and if it is too high, it is difficult to remove after use.

[0051] The present invention also provides an oil absorption box including the above-mentioned aerogel-expanded perlite composite material (referred to as aerogel-expanded perlite composite oil absorption box), which can absorb the waste oil obtained by condensing oil smoke into the micron and nano pores inside the composite porous material, thereby facilitating the cleaning of the oil box and also avoiding the waste oil and cleaning chemicals used in the conventional cleaning process from polluting the environment.

[0052] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0053] Example 1 (1) Material selection: Laboratory-made super-hydrophobic silica aerogel powder with an average particle size of 32 μm and a tap density of 0.035 g / cm 3 The average pore size is less than 17nm, the pore volume is 5.5ml / g, and the water contact angle is greater than 158°; the commercial density is 0.12g / cm 3 , open-cell expanded perlite with a particle size of 60 mesh, deionized water, hexadecyltrimethylammonium bromide as surfactant, potassium silicate water glass with a modulus of 3.2 and a silica mass concentration of 26.7% as adhesive, 3 mm long chopped glass fibers, and 300-800 mPa.s sodium carboxymethyl cellulose as thickener. The raw material ratios are: 8 g aerogel powder, 25 g expanded perlite, 42.75 g water, 1 g surface modifier, 22 g inorganic silicone adhesive, 1 g fiber, and 0.25 g thickener. A commercially available stainless steel oil collecting box is selected as the shell and molding mold; (2) Preparation of aerogel-expanded perlite composite slurry: First, water and thickener were stirred and mixed for 1 hour. After uniform dispersion, surfactant, inorganic silicone adhesive, and fiber were added in sequence and stirred evenly. Then, the aerogel powder was slowly added while maintaining the agitator speed at 1500 rpm. After complete uniform dispersion, the agitator speed was adjusted to 150 rpm, and expanded perlite was added. After uniform dispersion, the agitator speed was adjusted to 150 rpm, and expanded perlite was added. After uniform dispersion, the mixture was set aside. (3) Composite slurry casting: pour the aerogel-expanded perlite composite slurry into the oil collecting box mold and vibrate it on a rubber pad for 100 times to ensure that the slurry is evenly filled; (4) Curing and drying: The oil collecting box filled with the aerogel-expanded perlite composite slurry is placed in a 150° C. forced air drying oven and heated for 36 hours for curing and drying. After being taken out and cooled, the finished aerogel-expanded perlite composite oil absorbing box is obtained.

[0054] The oil absorption box containing the aerogel-expanded perlite composite material prepared in Example 1 is as follows Figure 2The surface strength of the obtained aerogel-expanded perlite composite material is relatively hard. The compressive strength of the obtained aerogel-expanded perlite composite material is 0.156MPa when the sample made with the same raw materials, proportion and process is tested according to the method specified in GB / T5486-2008. The obtained aerogel-expanded perlite composite oil absorption box is installed on the range hood for two months. Its oil absorption performance is good, and there is no trace of oil on the surface of the oil absorption box. The aerogel in the box is earthy brown. The aerogel core that absorbs oil can be pried out of the box with a hard tool. After a simple scrubbing, the oil collection box can be reused.

[0055] Example 2 (1) Material selection: Laboratory-made super-hydrophobic silica aerogel powder with a particle size of 40 μm and a tap density of 0.043 g / cm 3 The average pore size is less than 15nm, the pore volume is 4.5ml / g, and the water contact angle is greater than 152°; the commercial density is 0.13g / cm 3 , open-cell expanded perlite with a particle size of 70 mesh, deionized water, Tween-20 surfactant, sodium silicate water glass with a modulus of 3.2 and a silica mass concentration of 27.3% as adhesive, wood fiber with a length of 3 mm as fiber, and sodium carboxymethyl cellulose with a specification of 300-800 mPa.s as thickener. The proportions of each raw material are: 5g aerogel powder, 30g expanded perlite, 34.4g water, 0.6g surface modifier, 28g inorganic silicone adhesive, 1.5g fiber, and 0.5g thickener. A commercially available stainless steel oil collecting box is selected as the shell and molding mold; (2) Preparation of aerogel-expanded perlite composite slurry: First, water and thickener were stirred and mixed for 1.5 hours. After uniform dispersion, surfactant, inorganic silicone adhesive, and fiber were added in sequence and stirred evenly. Then, the aerogel powder was slowly added while maintaining the stirrer speed at 1800 rpm. After complete uniform dispersion, the stirrer speed was adjusted to 120 rpm, and expanded perlite was added. After uniform dispersion, the mixture was set aside. (4) Composite slurry casting: pour the aerogel-expanded perlite composite slurry into the oil collecting box mold and vibrate it on a rubber pad for 100 times to ensure that the slurry is evenly filled; (5) Curing and drying: The oil collecting box filled with aerogel-expanded perlite composite slurry was placed in a 135° C. forced air drying oven and heated for 30 hours for curing and drying. After being taken out and cooled, the finished aerogel-expanded perlite composite oil absorbing box was obtained.

[0056] The surface strength of the aerogel-expanded perlite composite material obtained in Example 2 is relatively hard. A small sample made with the same raw materials, proportions and process was tested according to the method specified in GB / T5486-2008, and the compressive strength of the obtained aerogel-expanded perlite composite material was 0.187 MPa; the obtained aerogel-expanded perlite composite oil absorption box was installed on a range hood for actual measurement for 2 months, and the oil absorption and cleaning effects were good.

[0057] Example 3 (1) Material selection: Laboratory-made super-hydrophobic silica aerogel powder with a particle size of 10 μm and a tap density of 0.033 g / cm 3 The average pore size is less than 20nm, the pore volume is 5.5ml / g, and the water contact angle is greater than 153°; the commercial density is 0.15g / cm 3 , open-cell expanded perlite with a particle size of 55 mesh, deionized water, dodecyl dimethyl benzyl ammonium chloride and perchlorate (mass ratio 1:1) as surfactant, acidic silica sol with a silica mass concentration of 31% as adhesive, polyester fiber with a length of 3 mm, and hydroxypropyl methylcellulose with a specification of 300-800 mPa.s as thickener. The proportions of each raw material are: 9g aerogel powder, 22g expanded perlite, 34.4g water, 0.8g total surface modifier, 19g inorganic silicone adhesive, 1.2g fiber, and 0.2g thickener. A commercially available stainless steel oil collecting box is selected as the shell and molding mold; (2) Preparation of aerogel-expanded perlite composite slurry: First, water and thickener were stirred and mixed for 1.2 hours. After uniform dispersion, surfactant, inorganic silicone adhesive, and fiber were added in sequence and stirred evenly. Then, the aerogel powder was slowly added while maintaining the agitator speed at 1200 rpm. After complete uniform dispersion, the agitator speed was adjusted to 80 rpm, and expanded perlite was added. After uniform dispersion, the mixture was set aside. (3) Composite slurry casting: pour the aerogel-expanded perlite composite slurry into the oil collecting box mold and vibrate it on a rubber pad for 100 times to ensure that the slurry is evenly filled; (4) Curing and drying: The oil collecting box filled with aerogel-expanded perlite composite slurry is placed in a 125° C. forced air drying oven and heated for 46 hours for curing and drying. After being taken out and cooled, the finished aerogel-expanded perlite composite oil absorbing box is obtained.

[0058] The surface strength of the aerogel-expanded perlite composite material obtained in Example 3 is relatively hard. A small sample made with the same raw materials, proportions and process was tested according to the method specified in GB / T5486-2008, and the compressive strength of the obtained aerogel-expanded perlite composite material was 0.122 MPa; the obtained aerogel-expanded perlite composite oil absorption box was installed on a range hood for actual measurement for 2 months, and the oil absorption and cleaning effects were good.

[0059] Comparative Example 1

[0060] In this comparative example 1, the aerogel selected was commercially available hydrophilic silica aerogel powder to prepare an aerogel-expanded perlite composite oil absorption box, and other raw materials and preparation processes were the same as those in Example 1.

[0061] After heating and drying, the volume of the aerogel in the aerogel-expanded perlite composite oil absorption box obtained in this comparative example 1 shrinks to only 2 / 3 of the initial casting volume, and the surface hydrophilic silica aerogel is not suitable for the application of the aerogel-expanded perlite composite oil absorption box of the present invention.

[0062] Comparative Example 2

[0063] The materials and preparation process of the aerogel-expanded perlite composite oil absorption box in Comparative Example 2 are the same as those in Example 1, except that the expanded perlite selected is a closed-cell expanded perlite of the same specification.

[0064] The surface of the aerogel-expanded perlite composite material obtained in this comparative example 2 is relatively hard, but its oil absorption capacity is significantly smaller. When installed on a range hood, it reaches oil absorption saturation in only 13 days, indicating that the closed-cell expanded perlite is not suitable for application in the present invention.

[0065] Comparative Example 3

[0066] The materials and preparation process of the aerogel-expanded perlite composite oil absorption box in this comparative example 3 are the same as those in Example 1, except that the specifications of the expanded perlite selected are: the commercial density is 0.3g / cm 3 , open-pore expanded perlite with a particle size of 20 mesh.

[0067] The surface of the aerogel-expanded perlite composite material obtained in this comparative example 3 is relatively hard, but there are fine particles on the surface, and the surface particles can be peeled off by touching it lightly with hands. The compressive strength thereof is tested to be 0.083 MPa, and the oil absorption thereof is also significantly reduced compared with that of Example 1. This indicates that the expanded perlite with high density and large particle size is not suitable for the application of the present invention.

[0068] Comparative Example 4

[0069] The materials and preparation process of the aerogel-expanded perlite composite oil absorption box in this comparative example 4 are the same as those in Example 1, except that, during the preparation of the aerogel-expanded perlite composite slurry, the stirring speed when the expanded perlite is added is increased to 800 rpm.

[0070] The surface of the aerogel-expanded perlite composite material in Comparative Example 4 is very hard, and its compressive strength is 0.33 MPa, and its oil absorption is also significantly lower than that of Example 1. This indicates that the high stirring rate used when adding expanded perlite may destroy the porous structure of the expanded perlite, thereby increasing the surface strength of the oil-absorbing block, but reducing the oil absorption value.

[0071] Comparative Example 5

[0072] The materials and preparation process of the aerogel-expanded perlite composite oil absorption box in Comparative Example 5 are the same as those in Example 1, except that the drying time is 2 hours during the drying process and the box is not dried to a constant weight.

[0073] The surface of the aerogel-expanded perlite composite material in Comparative Example 5 is very hard. When installed on a range hood, it was measured to reach oil absorption saturation in only 40 days. This shows that if the oil absorption box obtained by the present invention is not completely dried, there will still be residual moisture in the expanded perlite particles, which will weaken its oil absorption effect to a certain extent.

[0074] Comparative Example 6

[0075] The materials and preparation process of the aerogel-expanded perlite composite oil absorption box in this comparative example 6 are the same as those in Example 1, except that the density of the open-pore expanded perlite used is 80 kg / m 3 .

[0076] The volume of the solidified body in the aerogel-expanded perlite composite oil absorption box prepared in Comparative Example 6 shrinks greatly, and is only 3 / 5 of the initial pouring volume. This is because the low-density expanded perlite itself has thin pore walls and low strength, and is very easy to break during the stirring process, resulting in the collapse of the particle pore structure and a significant reduction in the volume of the solidified body.

[0077] Comparative Example 7

[0078] The materials and preparation process of the aerogel-expanded perlite composite oil absorption box in this comparative example 7 are the same as those in Example 1, except that the ratio of each raw material is: 2g aerogel powder, 25g expanded perlite, 48.75g water, 1g surface modifier, 22g inorganic silicone adhesive, 1g fiber, and 0.25g thickener.

[0079] In this comparative example 7, the content of aerogel powder is relatively low, the volume of the solidified body in the obtained aerogel-expanded perlite composite oil absorption box is reduced to a certain extent, the surface of the hardened body is rough, and the granularity is obvious. It was found in actual measurement on the range hood that a lot of oil stains adhered to the hardened body and the inner wall of the oil collection box, which caused great obstacles to subsequent cleaning.

[0080] Comparative Example 8

[0081] The materials and preparation process of the aerogel-expanded perlite composite oil absorption box in this comparative example 8 are the same as those in Example 1, except that the ratio of each raw material is: 20g aerogel powder, 25g expanded perlite, 30.75g water, 1g surface modifier, 22g inorganic silicone adhesive, 1g fiber, and 0.25g thickener.

[0082] In this comparative example 8, the amount of aerogel powder used is relatively large, and it is found that in the process of preparing the composite slurry, all the aerogel powder cannot be completely dissolved in the precursor solution composed of water, thickener, inorganic binder, fiber, and surfactant. Comparative Examples 7 and 8 illustrate that the amount of aerogel powder should maintain an appropriate ratio with the amount of other raw materials such as water, surfactant, and inorganic binder.

[0083] Comparative Example 9

[0084] The materials and preparation process of the aerogel-expanded perlite composite oil absorption box in this comparative example 9 are the same as those in Example 1, except that the ratio of each raw material is: 8g aerogel powder, 5g expanded perlite, 62.75g water, 1g surface modifier, 22g inorganic silicone adhesive, 1g fiber, and 0.25g thickener.

[0085] In this comparative example 9, the amount of expanded perlite used is relatively small, and it is found that the volume of the solidified body in the obtained aerogel-expanded perlite composite oil absorption box is reduced to a certain extent. During the actual measurement of oil absorption on the range hood, it is found that the distribution of oil in the oil absorption box is still uneven, and some areas are white or light in color, and the oil absorption amount is small, indicating that the expanded perlite in the composite oil absorption body needs to be maintained at an appropriate proportion.

[0086] Comparative Example 10

[0087] The materials and preparation process of the aerogel-expanded perlite composite oil absorption box in this comparative example 10 are the same as those in Example 1, except that the ratio of each raw material is: 8g aerogel powder, 40g mass of expanded perlite, 27.75g water, 1g surface modifier, 22g inorganic silicone adhesive, 1g fiber, and 0.25g thickener.

[0088] In this comparative example 10, a large amount of expanded perlite was used. It was found that during the preparation of the composite slurry, although all the expanded perlite could be mixed with the aerogel slurry, the entire system had lost fluidity and could not be poured into the oil collecting box, indicating that the amount of expanded perlite should be kept in an appropriate proportion to the amount of other raw materials such as aerogel powder, water, surfactant, inorganic binder, etc.

Claims

1. An aerogel-expanded perlite composite slurry, characterized in that: include: Aerogel powder, expanded perlite, water, surface modifier, inorganic silicone adhesive, fiber and thickener; The composition of the aerogel-expanded perlite composite slurry includes, by mass percentage, 5-10% aerogel powder, 10-30% expanded perlite, 30-73.45% water, 0.5-2% surface modifier, 10-25% inorganic silica adhesive, 1-2.5% fiber, and 0.05-0.5% thickener.

2. The aerogel-expanded perlite composite slurry according to claim 1, characterized in that: The aerogel powder is a super hydrophobic silica aerogel powder; the particle size of the super hydrophobic silica aerogel powder is 10 to 40 μm; the tap density is 0.03 to 0.05 g / cm 3 ; Average pore size less than 50nm; Pore volume greater than 3ml / g; Water contact angle greater than 150°; The expanded perlite is an open-pore expanded perlite; the tap density of the open-pore expanded perlite is 0.12 to 0.16 g / cm 3 ; The particle size is 50-70 mesh.

3. The aerogel-expanded perlite composite slurry according to claim 1 or 2, characterized in that: The surfactant includes a cationic surfactant and / or a neutral surfactant; the cationic surfactant is at least one of cetyltrimethylammonium bromide, stearylamine hydrochloride, and dodecyldimethylbenzyl ammonium chloride; the neutral surfactant is at least one of Tween-20, OP-10, Span-80, and peregal; The inorganic silicon binder is at least one of sodium silicate water glass, potassium silicate water glass, lithium silicate water glass and silica sol; the mass percentage of silicon dioxide in the inorganic silicon binder is not less than 25%; The fiber is at least one of wood fiber, glass fiber, and plastic fiber; The thickener is a water-soluble cellulose thickener; the water-soluble cellulose thickener is sodium carboxymethyl cellulose or hydroxypropyl methyl cellulose.

4. The aerogel-expanded perlite composite slurry according to any one of claims 1 to 3, characterized in that: The viscosity of the aerogel-expanded perlite composite slurry is 30,000-60,000 cp.

5. A method for preparing an aerogel-expanded perlite composite slurry according to any one of claims 1 to 4, characterized in that: include: The water and thickener are stirred and mixed, and a surfactant, an inorganic silicone adhesive, and fibers are added in sequence. Then, aerogel powder is slowly added under high-speed stirring. After it is completely dispersed, expanded perlite is finally added and stirred at a low speed to obtain the aerogel-expanded perlite composite slurry.

6. The preparation method according to claim 5, characterized in that: The high-speed stirring rate is 1000-2000 rpm; preferably 1300-1600 rpm; The low-speed stirring rate is 60 to 300 rpm, preferably 100 to 200 rpm.

7. A method for preparing an aerogel-expanded perlite composite material, characterized in that: include: The aerogel-expanded perlite composite slurry according to any one of claims 1 to 4 is poured into an oil collecting box mold, and the aerogel-expanded perlite composite material is obtained by curing and drying to a constant weight.

8. The preparation method according to claim 7, characterized in that: The curing and drying temperature is 105 to 150° C.; the curing and drying time is 8 to 48 hours; The condition for curing and drying to constant weight is that the weight deviation measured three times every 1 hour is no more than 0.1 g.

9. An aerogel-expanded perlite composite material prepared according to the preparation method of claim 7 or 8, characterized in that: The compressive strength of the aerogel-expanded perlite composite material is 0.1-0.2 MPa.

10. An oil absorption box comprising the super aerogel-expanded perlite composite material according to claim 9.

11. Use of the oil suction box according to claim 10 in a range hood.