Cerium oxide ceramic slurry suitable for photocuring 3D printing, and preparation and forming method thereof

By combining modified cerium oxide ceramic powder with low absorbance powder filler and using specific processes, the problem of low curing thickness of cerium oxide ceramic in photopolymerization 3D printing was solved, enabling the precise molding of complex porous structures and the preparation of high-performance cerium oxide ceramic parts.

CN118955134AActive Publication Date: 2024-11-15XI AN JIAOTONG UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411024471.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Existing photopolymerization 3D printing technology has difficulty in effectively forming cerium oxide ceramics, especially due to their high refractive index and strong light absorption characteristics, resulting in low cured thickness and making it difficult to prepare cerium oxide ceramic components with precise pore shapes and complex geometric features.

Method used

A cerium oxide ceramic slurry with high curing ability and fluidity was prepared by using surface-modified cerium oxide ceramic powder, low absorbance powder filler, slurry liquid phase and photoinitiator, through specific ball milling and pyrolysis processes combined with photopolymerization 3D printing technology.

Benefits of technology

It improves the curing performance and fluidity of cerium oxide ceramic slurry, ensures the structural integrity of the green body during pyrolysis and sintering, avoids cracking and warping defects, and achieves precise molding of complex porous structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955134A_ABST
    Figure CN118955134A_ABST
Patent Text Reader

Abstract

The invention discloses cerium oxide ceramic slurry suitable for photocuring 3D printing and a preparation and forming method, the cerium oxide ceramic slurry comprises surface-modified cerium oxide ceramic powder, a low-absorbance powder filler, a slurry liquid phase and a photoinitiator, and the surface-modified cerium oxide ceramic powder is cerium oxide ceramic powder with a dispersing agent attached to the surface; wherein the total mass of the cerium oxide ceramic powder and the low-absorbance powder filler accounts for 40-50% of the volume of the cerium oxide ceramic slurry, and the ratio of the volume of the cerium oxide ceramic powder to the volume of the low-absorbance powder filler is (1-4): 1; the volume of the slurry liquid phase accounts for 50-60% of the volume of the cerium oxide ceramic slurry; the mass of the dispersing agent accounts for 1-3% of that of the cerium oxide ceramic powder; the mass of the photoinitiator accounts for 1%-3% of the mass of the slurry liquid phase; the slurry liquid phase comprises the following components in percentage by mass: 40%-50% of 4-acryloylmorpholine serving as a photosensitive monomer, 10%-20% of ethyoxyl pentaerythritol tetraacrylate serving as a cross-linking agent and 30%-40% of polypropylene glycol-400 serving as a diluent. According to the method, photocuring 3D printing forming of the cerium oxide ceramic sample piece and preparation of a complex porous structure can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of cerium oxide ceramic photocuring 3D printing, and specifically relates to a cerium oxide ceramic slurry suitable for photocuring 3D printing, and a preparation and molding method thereof. Background Art

[0002] As a functional material, cerium oxide (CeO2) ceramics have shown extensive application potential in many high-tech fields due to their unique redox properties, excellent high-temperature stability and chemical inertness. Especially in the field of complex porous structures, such as the preparation of three-periodic minimal surface structures as heat exchanger structures, cerium oxide ceramics are an indispensable key material. Although traditional preparation methods such as organic foam impregnation method, foaming method, solid phase sintering method, chemical vapor deposition method and sol-gel method have achieved the preparation of cerium oxide ceramic products to a certain extent, the cerium oxide ceramic products prepared by these methods are mostly limited to disordered foam porous structures and have significant defects, such as uneven pore structure, insufficient mechanical strength, and low molding success rate. What is particularly critical is that these methods face huge challenges in preparing cerium oxide ceramic components with precise pore shape, porosity and complex geometric features, which seriously restricts the widespread application of high-performance cerium oxide ceramics.

[0003] Photocuring 3D printing technology has become a leader in additive manufacturing technology with its high-precision, high-efficiency forming capabilities and excellent performance in small and complex structures. This technology has been widely used in the forming of resin materials and some low-refractive index and low-absorbance ceramics (such as alumina and zirconia), showing its great potential in the field of ceramic material preparation. However, for cerium oxide ceramics, due to its high refractive index and strong absorbance, photocuring 3D printing technology has encountered huge obstacles in practical applications. Specifically, the curing thickness of cerium oxide ceramic slurry is low during the photocuring process, and it is difficult to effectively form, which has become a key factor restricting the application of photocuring 3D printing technology in the preparation of cerium oxide ceramic components. Therefore, there is an urgent need to develop a cerium oxide ceramic slurry suitable for photocuring 3D printing and a forming method thereof. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a cerium oxide ceramic slurry suitable for photocuring 3D printing, and a preparation and molding method, which can realize the photocuring 3D printing molding of cerium oxide ceramic samples and the preparation of complex porous structures.

[0005] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:

[0006] A cerium oxide ceramic slurry suitable for photocuring 3D printing, comprising a surface-modified cerium oxide ceramic powder, a low-absorbance powder filler, a slurry liquid phase and a photoinitiator, wherein the surface-modified cerium oxide ceramic powder is a cerium oxide ceramic powder with a dispersant attached to the surface;

[0007] in:

[0008] The total mass of the cerium oxide ceramic powder and the low-absorbance powder filler accounts for 40% to 50% of the volume of the cerium oxide ceramic slurry, and the ratio of the volume of the cerium oxide ceramic powder to the volume of the low-absorbance powder filler is (1 to 4): 1;

[0009] The volume of the slurry liquid phase accounts for 50% to 60% of the volume of the cerium oxide ceramic slurry;

[0010] The mass of the dispersant accounts for 1% to 3% of the mass of the cerium oxide ceramic powder;

[0011] The mass of the photoinitiator accounts for 1% to 3% of the mass of the slurry liquid phase;

[0012] In terms of mass percentage, the slurry liquid phase includes 40% to 50% of 4-acryloylmorpholine as a photosensitive monomer, 10% to 20% of ethoxy pentaerythritol tetraacrylate as a crosslinking agent, and 30% to 40% of polypropylene glycol-400 as a diluent.

[0013] Furthermore, the particle size of the cerium oxide ceramic powder is 15 μm to 20 μm.

[0014] Furthermore, the low-absorbency powder filler is soluble starch, and its particle size is 10 μm to 30 μm.

[0015] Furthermore, the dispersant is one of KD-1 or BYK-180.

[0016] Furthermore, the photoinitiator is one of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide or 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0017] A method for preparing a cerium oxide ceramic slurry suitable for photocuring 3D printing, comprising:

[0018] The cerium oxide ceramic powder and the dispersant are mixed in anhydrous ethanol and then ball-milled, the mixed solution after ball milling is dried, ground after drying, and sieved through a 80-150 mesh screen to obtain a surface-modified cerium oxide ceramic powder;

[0019] The surface-modified cerium oxide ceramic powder, the low-absorbance powder filler and the slurry liquid phase are mixed and then ball-milled, and finally a photoinitiator is added and ball-milled again to obtain a cerium oxide ceramic slurry suitable for photocuring 3D printing.

[0020] Furthermore, when the cerium oxide ceramic powder and the dispersant are mixed in anhydrous ethanol and then ball-milled, the ball-milling rate is 100 rpm to 150 rpm, and the ball-milling time is 5 h to 10 h;

[0021] When the mixed solution after ball milling is dried, the drying temperature is 50° C. to 100° C., and the drying time is 2 h to 6 h.

[0022] Furthermore, when the surface-modified cerium oxide ceramic powder, the low-absorbency powder filler and the slurry liquid phase are mixed and then ball-milled, the ball-milling rate is 100 rpm to 150 rpm, and the ball-milling time is 5 h to 10 h;

[0023] During the second ball milling, the ball milling rate is 100 rpm to 150 rpm, and the ball milling time is 0.5 h to 1 h.

[0024] A method for forming a cerium oxide ceramic slurry suitable for photocuring 3D printing, comprising:

[0025] The cerium oxide ceramic slurry was exposed to a laser with an energy density of 25 mW / cm 2 ~37.5mW / cm 2 , exposure time 7s ~ 15s, layer thickness 25μm ~ 50μm process parameters for light-curing 3D printing, to obtain cerium oxide ceramic blank;

[0026] The cerium oxide ceramic blank is pyrolyzed in an argon atmosphere according to a set pyrolysis process, and a pyrolysis piece is obtained after the pyrolysis is completed; the set pyrolysis process sequentially includes: a first pyrolysis stage, a pyrolysis temperature of 20°C to 200°C, a heating rate of 1°C / min to 1.5°C / min, and a heat preservation time of 0.5h to 1h; a second pyrolysis stage, a pyrolysis temperature of 200°C to 310°C, a heating rate of 0.5°C / min to 1°C / min, and a heat preservation time of 1h to 2h; a In the third pyrolysis stage, the pyrolysis temperature is 310℃~410℃, the heating rate is 0.5℃ / min~1℃ / min, and the holding time is 1h~2h; in the fourth pyrolysis stage, the pyrolysis temperature is 410℃~480℃, the heating rate is 0.5℃ / min~1℃ / min, and the holding time is 1h~2h; in the fifth pyrolysis stage, the pyrolysis temperature is 480℃~600℃, the heating rate is 1℃ / min~1.5℃ / min, and the holding time is 0.5h~1h;

[0027] The pyrolysis piece is sintered in an air atmosphere, with the temperature rising to 1550-1650°C at a heating rate of 5°C / min-10°C / min, and the heat preservation time is 1h-2h; then, it is cooled to room temperature at a cooling rate of 3°C / min-5°C / min to obtain a cerium oxide ceramic piece.

[0028] Compared with the prior art, the present invention has at least the following beneficial effects:

[0029] The present invention provides a cerium oxide ceramic slurry suitable for photocuring 3D printing, which is composed of surface-modified cerium oxide ceramic powder, low-absorbance powder filler, slurry liquid phase and photoinitiator, and is mixed with monofunctional photosensitive monomer 4-acryloylmorpholine, multifunctional crosslinking agent ethoxy pentaerythritol tetraacrylate and diluent polypropylene glycol-400. The slurry liquid phase with a high refractive index reduces the refractive index difference between the liquid phase and the powder, thereby improving the curing ability of the cerium oxide ceramic slurry and improving the curing performance of the cerium oxide ceramic slurry. At the same time, the introduction of low-absorbance powder filler reduces the overall absorbance of the ceramic slurry and improves the curing performance of the cerium oxide ceramic slurry. A dispersant is attached to the surface of the cerium oxide ceramic powder to achieve modification of the surface of the cerium oxide ceramic powder. The particle size of the modified cerium oxide ceramic powder is more uniform, and the agglomeration phenomenon of the cerium oxide ceramic powder is reduced. The modified cerium oxide ceramic powder is more easily dispersed in the slurry liquid phase, thereby greatly reducing the viscosity of the ceramic slurry and improving the fluidity of the slurry.

[0030] Furthermore, cerium oxide ceramic powder with a particle size of 15 μm to 20 μm and low-absorbance powder filler soluble starch powder with a particle size of 10 μm to 30 μm are selected. The higher powder particle size improves the curing ability of the cerium oxide ceramic slurry while reducing the viscosity of the slurry and improving the fluidity of the slurry.

[0031] The present invention provides a molding method of cerium oxide ceramic slurry suitable for photocuring 3D printing. According to the TG-DSC curve, argon is used as the pyrolysis atmosphere, and 5 pyrolysis processes are determined, which are 20°C to 200°C, 200°C to 310°C, 310°C to 410°C, 410°C to 480°C and 480°C to 600°C, respectively. The appropriate heating rate and holding time are selected to ensure that the structure of the photocuring ceramic blank is intact and crack-free during the pyrolysis process, and the organic matter inside the blank is discharged.

[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions in the specific implementation modes of the present invention, the drawings required for use in the description of the specific implementation modes will be briefly introduced below. Obviously, the drawings described below are some implementation modes of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 These are the test long blanks, pyrolysis parts and sintered parts printed out from the slurry prepared in Example 1.

[0035] Figure 2 These are the green blanks, pyrolysis parts and sintered parts of the three-periodic minimal surface porous structure printed out by preparing the slurry in Example 2. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] A method for preparing cerium oxide ceramic slurry suitable for photocuring 3D printing is as follows:

[0039] Step 1: Weigh 85 g of cerium oxide ceramic powder with an average powder particle size of 20 μm, weigh 1.7 g of dispersant KD-11, mix them in 50 ml of anhydrous ethanol, add ball milling beads, and ball mill at a rate of 120 rpm in a planetary ball mill for 8 hours. Place the mixed solution after ball milling in an oven at a temperature of 50°C for 6 hours, dry and grind, and sieve through a 100-mesh sieve to obtain surface-modified cerium oxide ceramic powder.

[0040] Step 2: Measure 12 ml of 4-acryloylmorpholine as a photosensitive monomer, 3.48 ml of ethoxypentaerythritol tetraacrylate as a cross-linking agent, and 8.52 ml of polypropylene glycol-400 as a diluent, and mix them to obtain a slurry liquid phase premix, wherein the mass ratio of the photosensitive monomer, the cross-linking agent and the diluent is 50:15:35.

[0041] Step 3: Weigh 6 g of soluble starch powder with an average particle size of 20 μm, and the volume ratio of cerium oxide ceramic powder to soluble starch powder is 3:1.

[0042] Step 4: Add the surface-modified cerium oxide ceramic powder and soluble starch powder to the slurry liquid premix, add ball milling beads, and ball mill at a rate of 150 rpm in a planetary ball mill for 8 hours. Finally, add 0.54 g of photoinitiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and ball mill again for 0.5 to 1 hour to obtain 40 ml of cerium oxide ceramic slurry, wherein the mass of cerium oxide ceramic powder and soluble starch powder together accounts for 40% of the volume of the cerium oxide ceramic slurry.

[0043] The cerium oxide ceramic slurry prepared in this embodiment is used as a printing slurry, and a cerium oxide ceramic blank is printed by a light-curing 3D printing technology, and the cerium oxide ceramic blank is heat-treated to obtain a cerium oxide ceramic sample. The specific operation is as follows:

[0044] 1) Use 3D design software to design a strip structure with a length of 35 mm, a width of 5 mm, and a height of 4 mm.

[0045] 2) Inject the prepared cerium oxide ceramic slurry into the slurry tank, slice the designed strip structure, and set the printing parameters: the light source wavelength of the light-curing 3D printing equipment is 405nm, and the laser exposure energy density is 37.5mW / cm 2 , exposure time 12s, layer thickness 25μm, and photocuring 3D printing equipment were used to prepare cerium oxide ceramic blanks with long strip structures.

[0046] 3) The cerium oxide ceramic blank is placed in a pyrolysis furnace for pyrolysis. In an argon atmosphere, the temperature is increased from room temperature to 200°C at a heating rate of 1°C / min, then increased to 310°C at a heating rate of 0.5°C / min, increased to 410°C at a heating rate of 0.5°C / min, increased to 480°C at a heating rate of 0.5°C / min, and increased to 600°C at 1°C / min. The temperatures are kept at 310°C, 410°C, 480°C, and 600°C for 1 h, respectively, and then cooled to room temperature at a cooling rate of 1°C / min to obtain a pyrolysis piece with a long strip structure.

[0047] 4) The pyrolysis piece is placed in a sintering furnace for sintering, the temperature is increased from room temperature to 1200°C at a heating rate of 6°C / min, the temperature is increased to 1600°C at a heating rate of 3°C / min, and it is kept at 1600°C for 1 hour, and then the temperature is cooled to room temperature at a cooling rate of 3°C / min to obtain a cerium oxide ceramic sample with a long strip structure.

[0048] Figure 1 The photocured test samples prepared from the cerium oxide ceramic slurry in Example 1 and their pyrolysis sintered parts can be seen from the figure that the green sample has no obvious stratification and deformation, and the dimensional accuracy is 150μm~250μm; the pyrolysis sample has no obvious deformation and cracking; the sintered part has no obvious warping and cracking defects.

[0049] Example 2

[0050] A method for preparing cerium oxide ceramic slurry suitable for photocuring 3D printing is as follows:

[0051] Step 1: Weigh 57 g of cerium oxide ceramic powder with an average powder particle size of 20 μm, weigh 1.14 g of dispersant KD-11, mix them in 50 ml of anhydrous ethanol, add ball milling beads, and ball mill for 5 hours at a rate of 150 rpm in a planetary ball mill. Place the mixed solution after ball milling in an oven at a temperature of 80°C for 4 hours, grind it after drying, and sieve it through a 100-mesh sieve to obtain surface-modified cerium oxide ceramic powder.

[0052] Step 2: Measure 12 ml of 4-acryloylmorpholine as a photosensitive monomer, 3.48 ml of ethoxypentaerythritol tetraacrylate as a cross-linking agent, and 8.52 ml of polypropylene glycol-400 as a diluent, and mix them to obtain a slurry liquid phase premix, in which the mass ratio of the photosensitive monomer, the cross-linking agent and the diluent is 50:15:35.

[0053] Step 3: Weigh 12 g of soluble starch powder with an average particle size of 20 μm, and the volume ratio of cerium oxide ceramic powder to soluble starch powder is 1:1.

[0054] Step 4: Add the surface-modified cerium oxide ceramic powder and soluble starch powder to the slurry liquid premix, add ball milling beads, and ball mill at a rate of 150 rpm in a planetary ball mill for 8 hours. Finally, add 0.54 g of photoinitiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and ball mill again for 0.5 to 1 hour to obtain 40 ml of cerium oxide ceramic slurry, wherein the mass of cerium oxide ceramic powder and soluble starch powder together accounts for 40% of the volume of the cerium oxide ceramic slurry.

[0055] The cerium oxide ceramic slurry prepared in this embodiment is used as a printing slurry, and a cerium oxide ceramic blank is printed by a light-curing 3D printing technology, and the cerium oxide ceramic blank is heat-treated to obtain a cerium oxide ceramic sample. The specific operation is as follows:

[0056] 1) A diamond three-period minimal surface structure with a porosity of 70% was designed using three-dimensional design software. The dimensions of the structure were a rectangular parallelepiped structure with a length of 30 mm, a width of 15 mm, and a height of 12 mm.

[0057] 2) Inject the prepared cerium oxide ceramic slurry into the slurry tank, slice the designed three-period minimal surface structure cuboid, and set the printing parameters: the light source wavelength of the light-curing 3D printing equipment is 405nm, and the laser exposure energy density is 30mW / cm 2, exposure time 7s, layer thickness 31.25μm, and the cerium oxide ceramic blank with a three-periodic minimal surface structure was prepared using a photocuring 3D printing device.

[0058] 3) Placing the cerium oxide ceramic blank in a pyrolysis furnace for pyrolysis, in an argon atmosphere, heating from room temperature to 200°C at a heating rate of 1°C / min, heating to 310°C at a heating rate of 0.7°C / min, heating to 410°C at a heating rate of 0.5°C / min, heating to 480°C at a heating rate of 0.5°C / min, heating to 600°C at 1°C / min, keeping at 310°C, 410°C, 480°C, and 600°C for 1 h, then cooling to room temperature at a cooling rate of 1°C / min, keeping at 310°C, 410°C, 480°C, and 600°C for 1 h, then cooling to room temperature at a cooling rate of 1°C / min, to obtain a pyrolysis piece with a rectangular parallelepiped structure of a three-period minimal surface.

[0059] 4) The pyrolysis piece is placed in a sintering furnace for sintering, the temperature is increased from room temperature to 1200°C at a heating rate of 10°C / min, the temperature is increased to 1600°C at a heating rate of 3°C / min, and it is kept at 1600°C for 1 hour, and then the temperature is cooled to room temperature at a cooling rate of 3°C / min to obtain a cuboid cerium oxide ceramic sample with a three-periodic minimal surface structure.

[0060] Figure 2 The photocured porous sample and its pyrolysis sintered part prepared by the cerium oxide ceramic slurry in Example 2 can be seen from the figure that the green sample has no obvious stratification and deformation, the pore structure is clear, and the dimensional accuracy is 150μm~250μm; the pyrolysis sample has no obvious cracking; and the sintered part has no obvious warping and cracking defects.

[0061] Example 3

[0062] A method for preparing cerium oxide ceramic slurry suitable for photocuring 3D printing is as follows:

[0063] Step 1: Weigh 68.5 g of cerium oxide ceramic powder with an average powder particle size of 18 μm, weigh 1.37 g of dispersant KD-11, mix them in 50 ml of anhydrous ethanol, add ball milling beads, and ball mill at a rate of 120 rpm in a planetary ball mill for 8 hours. Place the mixed solution after ball milling in an oven at 80°C for 4 hours, dry and grind, and sieve through a 100-mesh sieve to obtain surface-modified cerium oxide ceramic powder.

[0064] Step 2: Measure 12 ml of 4-acryloylmorpholine as a photosensitive monomer, 3.48 ml of ethoxypentaerythritol tetraacrylate as a cross-linking agent, and 8.52 ml of polypropylene glycol-400 as a diluent, and mix them to obtain a slurry liquid phase premix, in which the mass ratio of the photosensitive monomer, the cross-linking agent and the diluent is 50:15:35.

[0065] Step 3: Weigh 9.6 g of soluble starch powder with an average particle size of 25 μm, and the volume ratio of cerium oxide ceramic powder to soluble starch powder is 1.5:1.

[0066] Step 4: Add the surface-modified cerium oxide ceramic powder and soluble starch powder to the slurry liquid premix, add ball milling beads, and ball mill at a rate of 150 rpm in a planetary ball mill for 8 hours. Finally, add 0.54 g of photoinitiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and ball mill again for 0.5 to 1 hour to obtain 40 ml of cerium oxide ceramic slurry, wherein the mass of cerium oxide ceramic powder and soluble starch powder together accounts for 40% of the volume of the cerium oxide ceramic slurry.

[0067] The cerium oxide ceramic slurry prepared in this embodiment is used as a printing slurry, and a cerium oxide ceramic blank is printed by a light-curing 3D printing technology, and the cerium oxide ceramic blank is heat-treated to obtain a cerium oxide ceramic sample. The specific operation is as follows:

[0068] 1) A diamond three-period minimal surface structure with a porosity of 70% was designed using three-dimensional design software. The dimensions of the structure were a rectangular parallelepiped structure with a length of 30 mm, a width of 15 mm, and a height of 10 mm.

[0069] 2) Inject the prepared cerium oxide ceramic sample into the slurry tank, slice the designed three-period minimal surface structure cuboid, and set the printing parameters: the light source wavelength of the light-curing 3D printing equipment is 405nm, and the laser exposure energy density is 30mW / cm 2 , exposure time 8s, layer thickness 31.25μm, and the cerium oxide ceramic blank with a three-periodic minimal surface structure was prepared using a photocuring 3D printing device.

[0070] 3) The cerium oxide ceramic blank is placed in a pyrolysis furnace for pyrolysis. In an argon atmosphere, the temperature is increased from room temperature to 200°C at a heating rate of 1°C / min, then increased to 310°C at a heating rate of 0.5°C / min, increased to 410°C at a heating rate of 0.5°C / min, increased to 480°C at a heating rate of 1°C / min, and increased to 600°C at a heating rate of 1°C / min. The temperatures are kept at 310°C, 410°C, 480°C, and 600°C for 1 h, respectively, and then cooled to room temperature at a cooling rate of 1°C / min to obtain a pyrolysis piece with a rectangular parallelepiped structure of a three-period minimal surface.

[0071] 4) The pyrolysis piece is placed in a sintering furnace for sintering, with the temperature rising from room temperature to 1200°C at a heating rate of 6°C / min, then rising to 1600°C at a heating rate of 3°C / min, and kept at 1600°C for 1 hour, and then cooled to room temperature at a cooling rate of 3°C / min to obtain a cuboid cerium oxide ceramic sample with a three-periodic minimal surface structure.

[0072] The green blank sample prepared in this embodiment has no obvious delamination and deformation, a clear pore structure, and a dimensional accuracy of 150μm to 250μm; the pyrolysis sample has no obvious cracking; and the sintered part has no obvious warping and cracking defects.

[0073] Example 4

[0074] A method for preparing cerium oxide ceramic slurry suitable for photocuring 3D printing is as follows:

[0075] Step 1: Weigh 128.34 g of cerium oxide ceramic powder with an average powder particle size of 18 μm, weigh 3.85 g of dispersant BYK-180, mix them in 50 ml of anhydrous ethanol, add ball milling beads, and ball mill at a rate of 120 rpm in a planetary ball mill for 8 h. Place the mixed solution after ball milling in an oven at a temperature of 50 ° C for 6 h, dry and grind, and sieve through a 100-mesh sieve to obtain surface-modified cerium oxide ceramic powder.

[0076] Step 2: Measure 10.83 ml of 4-acryloylmorpholine as a photosensitive monomer, 4.64 ml of ethoxypentaerythritol tetraacrylate as a cross-linking agent, and 8.52 ml of polypropylene glycol-400 as a diluent, and mix them to obtain a slurry liquid phase premix, wherein the mass ratio of the photosensitive monomer, the cross-linking agent and the diluent is 45:20:35.

[0077] Step 3: Weigh 9 g of soluble starch powder with an average particle size of 15 μm, and the volume ratio of cerium oxide ceramic powder to soluble starch powder is 3:1.

[0078] Step 4: Add the surface-modified cerium oxide ceramic powder and soluble starch powder to the slurry liquid premix, add ball milling beads, and ball mill for 8 hours at 150 rpm in a planetary ball mill. Finally, add 0.62 g of photoinitiator phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, and ball mill again for 0.5 to 1 hour to obtain 48 ml of cerium oxide ceramic slurry, wherein the mass of cerium oxide ceramic powder and soluble starch powder together accounts for 50% of the volume of the cerium oxide ceramic slurry.

[0079] The cerium oxide ceramic slurry prepared in this embodiment is used as a printing slurry, and a cerium oxide ceramic blank is printed by a light-curing 3D printing technology, and the cerium oxide ceramic blank is heat-treated to obtain a cerium oxide ceramic sample. The specific operation is as follows:

[0080] 1) Use 3D design software to design a disc structure with a diameter of 20 mm and a height of 4 mm.

[0081] 2) The prepared cerium oxide ceramic slurry was injected into the slurry tank, the designed disc structure was sliced, and the printing parameters were set: the light source wavelength of the photocuring 3D printing equipment was 405nm, the laser exposure energy density was 37.5mW / cm2, the exposure time was 12s, the layer thickness was 25μm, and the cerium oxide ceramic blank with a disc structure was prepared using the photocuring 3D printing equipment.

[0082] 3) Placing the cerium oxide ceramic blank in a pyrolysis furnace for pyrolysis, in an argon atmosphere, heating the temperature from room temperature to 200°C at a heating rate of 1°C / min, heating the temperature to 310°C at a heating rate of 1°C / min, heating the temperature to 410°C at a heating rate of 0.5°C / min, heating the temperature to 480°C at a heating rate of 0.5°C / min, and heating the temperature to 600°C at 1°C / min, and keeping the temperatures at 310°C, 410°C, 480°C, and 600°C for 1 h, respectively, and then cooling the temperature to room temperature at a cooling rate of 1°C / min to obtain a pyrolysis piece with a wafer structure.

[0083] 4) The pyrolysis piece is placed in a sintering furnace for sintering, with the temperature rising from room temperature to 1200°C at a heating rate of 8°C / min, rising to 1600°C at a heating rate of 3°C / min, and being kept at 1600°C for 1.5 h, and then cooled to room temperature at a cooling rate of 3°C / min to obtain a cerium oxide ceramic sample with a disc structure.

[0084] The green blank samples prepared in this embodiment have no obvious delamination and deformation, and the dimensional accuracy is 150μm to 250μm; the pyrolysis samples have no obvious deformation and cracking; and the sintered parts have no obvious warping and cracking defects.

[0085] Example 5

[0086] A method for preparing cerium oxide ceramic slurry suitable for photocuring 3D printing is as follows:

[0087] Step 1: Weigh 62.74 g of cerium oxide ceramic powder with an average powder particle size of 15 μm, weigh 1.25 g of dispersant KD-11, mix them in 50 ml of anhydrous ethanol, add ball milling beads, and ball mill them in a planetary ball mill at a rate of 120 rpm for 8 h. Place the mixed solution after ball milling in an oven at a temperature of 50 ° C for 6 h, dry and grind it, and sieve it through a 100 mesh sieve to obtain surface-modified cerium oxide ceramic powder.

[0088] Step 2: Measure 11.24 ml of 4-acryloylmorpholine as a photosensitive monomer, 4.34 ml of ethoxypentaerythritol tetraacrylate as a cross-linking agent, and 6.82 ml of polypropylene glycol-400 as a diluent, and mix them to obtain a slurry liquid phase premix, wherein the mass ratio of the photosensitive monomer, the cross-linking agent and the diluent is 50:20:30.

[0089] Step 3: Weigh 13.2 g of soluble starch powder with an average particle size of 25 μm, and the volume ratio of cerium oxide ceramic powder to soluble starch powder is 1:1.

[0090] Step 4: Add the surface-modified cerium oxide ceramic powder and soluble starch powder to the slurry liquid premix, add ball milling beads, and ball mill for 8 hours at a rate of 150 rpm in a planetary ball mill. Finally, add 0.54 g of photoinitiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and ball mill again for 0.5 to 1 hour to obtain 40 ml of cerium oxide ceramic slurry, wherein the mass of cerium oxide ceramic powder and soluble starch powder together accounts for 44% of the volume of the cerium oxide ceramic slurry.

[0091] The cerium oxide ceramic slurry prepared in this embodiment is used as a printing slurry, and a cerium oxide ceramic blank is printed by a light-curing 3D printing technology, and the cerium oxide ceramic blank is heat-treated to obtain a cerium oxide ceramic sample. The specific operation is as follows:

[0092] 1) Use 3D design software to design a disc structure with a diameter of 20 mm and a height of 4 mm.

[0093] 2) The prepared cerium oxide ceramic slurry was injected into the slurry tank, the designed disc structure was sliced, and the printing parameters were set: the light source wavelength of the photocuring 3D printing equipment was 405nm, the laser exposure energy density was 25mW / cm2, the exposure time was 12s, the layer thickness was 25μm, and the cerium oxide ceramic blank with a disc structure was prepared using the photocuring 3D printing equipment.

[0094] 3) Placing the cerium oxide ceramic blank in a pyrolysis furnace for pyrolysis, in an argon atmosphere, heating the temperature from room temperature to 200°C at a heating rate of 1°C / min, heating the temperature to 310°C at a heating rate of 0.5°C / min, heating the temperature to 410°C at a heating rate of 0.5°C / min, heating the temperature to 480°C at a heating rate of 1°C / min, and heating the temperature to 600°C at a heating rate of 1°C / min, and keeping the temperatures at 310°C, 410°C, 480°C, and 600°C for 1 h, respectively, and then cooling the temperature to room temperature at a cooling rate of 1°C / min to obtain a pyrolysis piece with a wafer structure.

[0095] 4) placing the pyrolysis piece in a sintering furnace for sintering, heating the temperature from room temperature to 1200°C at a heating rate of 6°C / min, heating the temperature to 1600°C at a heating rate of 3°C / min, keeping the temperature at 1600°C for 1 hour, and then cooling the temperature to room temperature at a cooling rate of 3°C / min to obtain a cerium oxide ceramic sample with a disc structure.

[0096] The green blank samples prepared in this embodiment have no obvious delamination and deformation, and the dimensional accuracy is 150μm to 250μm; the pyrolysis samples have no obvious deformation and cracking; and the sintered parts have no obvious warping and cracking defects.

[0097] Example 6

[0098] A method for preparing cerium oxide ceramic slurry suitable for photocuring 3D printing is as follows:

[0099] Step 1: Weigh 85 g of cerium oxide ceramic powder with an average powder particle size of 16 μm, weigh 1.7 g of dispersant KD-11, mix them in 50 ml of anhydrous ethanol, add ball milling beads, and ball mill for 5 hours at a rate of 150 rpm in a planetary ball mill. Place the mixed solution after ball milling in an oven at a temperature of 85 ° C for 4 hours, dry and grind, and sieve through a 100 mesh sieve to obtain surface-modified cerium oxide ceramic powder.

[0100] Step 2: Measure 10.82 ml of 4-acryloylmorpholine as a photosensitive monomer, 3.48 ml of ethoxypentaerythritol tetraacrylate as a cross-linking agent, and 9.73 ml of polypropylene glycol-400 as a diluent, and mix them to obtain a slurry liquid phase premix, wherein the mass ratio of the photosensitive monomer, the cross-linking agent and the diluent is 45:15:40.

[0101] Step 3: Weigh 6 g of soluble starch powder with an average particle size of 30 μm, and the volume ratio of cerium oxide ceramic powder to soluble starch powder is 3:1.

[0102] Step 4: Add the surface-modified cerium oxide ceramic powder and soluble starch powder to the slurry liquid premix, add ball milling beads, and ball mill at a rate of 150 rpm in a planetary ball mill for 8 hours. Finally, add 0.54 g of photoinitiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and ball mill again for 0.5 to 1 hour to obtain 40 ml of cerium oxide ceramic slurry, wherein the mass of cerium oxide ceramic powder and soluble starch powder together accounts for 40% of the volume of the cerium oxide ceramic slurry.

[0103] The cerium oxide ceramic slurry prepared in this embodiment is used as a printing slurry, and a cerium oxide ceramic blank is printed by a light-curing 3D printing technology, and the cerium oxide ceramic blank is heat-treated to obtain a cerium oxide ceramic sample. The specific operation is as follows:

[0104] 1) Use 3D design software to design a disc structure with a diameter of 20 mm and a height of 4 mm.

[0105] 2) The prepared cerium oxide ceramic slurry was injected into the slurry tank, the designed disc structure was sliced, and the printing parameters were set: the light source wavelength of the photocuring 3D printing equipment was 405nm, the laser exposure energy density was 37.5mW / cm2, the exposure time was 12s, the layer thickness was 25μm, and the cerium oxide ceramic blank with a disc structure was prepared using the photocuring 3D printing equipment.

[0106] 3) The cerium oxide ceramic blank is placed in a pyrolysis furnace for pyrolysis. In an argon atmosphere, the temperature is increased from room temperature to 200°C at a heating rate of 1°C / min, then increased to 310°C at a heating rate of 1°C / min, increased to 410°C at a heating rate of 0.5°C / min, increased to 480°C at a heating rate of 1°C / min, and increased to 600°C at a heating rate of 1°C / min. The temperatures are kept at 310°C, 410°C, 480°C, and 600°C for 1 h, respectively, and then cooled to room temperature at a cooling rate of 1°C / min to obtain a pyrolysis piece with a wafer structure.

[0107] 4) placing the pyrolysis piece in a sintering furnace for sintering, heating the temperature from room temperature to 1200°C at a heating rate of 8°C / min, heating the temperature to 1600°C at a heating rate of 4°C / min, keeping the temperature at 1600°C for 1 hour, and then cooling the temperature to room temperature at a cooling rate of 3°C / min to obtain a cerium oxide ceramic sample with a disc structure.

[0108] The green blank samples prepared in this embodiment have no obvious delamination and deformation, and the dimensional accuracy is 150μm to 250μm; the pyrolysis samples have no obvious deformation and cracking; and the sintered parts have no obvious warping and cracking defects.

[0109] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0110] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A cerium oxide ceramic slurry suitable for photocuring 3D printing, characterized in that: The invention comprises a surface-modified cerium oxide ceramic powder, a low-absorbance powder filler, a slurry liquid phase and a photoinitiator, wherein the surface-modified cerium oxide ceramic powder is a cerium oxide ceramic powder with a dispersant attached to the surface; in: The total mass of the cerium oxide ceramic powder and the low-absorbance powder filler accounts for 40% to 50% of the volume of the cerium oxide ceramic slurry, and the ratio of the volume of the cerium oxide ceramic powder to the volume of the low-absorbance powder filler is (1 to 4): 1; The volume of the slurry liquid phase accounts for 50% to 60% of the volume of the cerium oxide ceramic slurry; The mass of the dispersant accounts for 1% to 3% of the mass of the cerium oxide ceramic powder; The mass of the photoinitiator accounts for 1% to 3% of the mass of the slurry liquid phase; In terms of mass percentage, the slurry liquid phase includes 40% to 50% of 4-acryloylmorpholine as a photosensitive monomer, 10% to 20% of ethoxy pentaerythritol tetraacrylate as a crosslinking agent, and 30% to 40% of polypropylene glycol-400 as a diluent.

2. The cerium oxide ceramic slurry suitable for photocuring 3D printing according to claim 1, characterized in that: The particle size of the cerium oxide ceramic powder is 15 μm to 20 μm.

3. The cerium oxide ceramic slurry suitable for photocuring 3D printing according to claim 1, characterized in that: The low-absorbency powder filler is soluble starch, and its particle size is 10 μm to 30 μm.

4. The cerium oxide ceramic slurry suitable for photocuring 3D printing according to claim 1, characterized in that: The dispersant is one of KD-1 or BYK-180.

5. The cerium oxide ceramic slurry suitable for photocuring 3D printing according to claim 1, characterized in that: The photoinitiator is one of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide or 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

6. A method for preparing a cerium oxide ceramic slurry suitable for photocuring 3D printing according to any one of claims 1 to 5, characterized in that: include: The cerium oxide ceramic powder and the dispersant are mixed in anhydrous ethanol and then ball-milled, the mixed solution after ball milling is dried, ground after drying, and sieved through a 80-150 mesh screen to obtain a surface-modified cerium oxide ceramic powder; The surface-modified cerium oxide ceramic powder, the low-absorbance powder filler and the slurry liquid phase are mixed and then ball-milled, and finally a photoinitiator is added and ball-milled again to obtain a cerium oxide ceramic slurry suitable for photocuring 3D printing.

7. The method for preparing a cerium oxide ceramic slurry suitable for photocuring 3D printing according to claim 6, characterized in that: When the cerium oxide ceramic powder and the dispersant are mixed in anhydrous ethanol and then ball-milled, the ball-milling rate is 100 rpm to 150 rpm, and the ball-milling time is 5 h to 10 h; When the mixed solution after ball milling is dried, the drying temperature is 50° C. to 100° C., and the drying time is 2 h to 6 h.

8. The method for preparing a cerium oxide ceramic slurry suitable for photocuring 3D printing according to claim 6, characterized in that: When the surface-modified cerium oxide ceramic powder, the low-absorbency powder filler and the slurry liquid phase are mixed and then ball-milled, the ball-milling rate is 100 rpm to 150 rpm, and the ball-milling time is 5 h to 10 h; During the second ball milling, the ball milling rate is 100 rpm to 150 rpm, and the ball milling time is 0.5 h to 1 h.

9. A method for forming a cerium oxide ceramic slurry suitable for photocuring 3D printing according to any one of claims 1 to 5, characterized in that: include: The cerium oxide ceramic slurry was exposed to a laser with an energy density of 25 mW / cm 2 ~37.5mW / cm 2 , exposure time 7s ~ 15s, layer thickness 25μm ~ 50μm process parameters for light-curing 3D printing, to obtain cerium oxide ceramic blank; Pyrolyzing the cerium oxide ceramic blank in an argon atmosphere according to a set pyrolysis process, and obtaining a pyrolysis piece after the pyrolysis is completed; The set pyrolysis process includes: a first pyrolysis stage, a pyrolysis temperature of 20°C to 200°C, a heating rate of 1°C / min to 1.5°C / min, and a heat preservation time of 0.5h to 1h; a second pyrolysis stage, a pyrolysis temperature of 200°C to 310°C, a heating rate of 0.5°C / min to 1°C / min, and a heat preservation time of 1h to 2h; a third pyrolysis stage, a pyrolysis temperature of 310°C to 410°C, a heating rate of 0.5°C / min to 1°C / min, and a heat preservation time of 1h to 2h; a fourth pyrolysis stage, a pyrolysis temperature of 410°C to 480°C, a heating rate of 0.5°C / min to 1°C / min, and a heat preservation time of 1h to 2h; a fifth pyrolysis stage, a pyrolysis temperature of 480°C to 600°C, a heating rate of 1°C / min to 1.5°C / min, and a heat preservation time of 0.5h to 1h; The pyrolysis piece is sintered in an air atmosphere, with the temperature rising to 1550-1650°C at a heating rate of 5°C / min-10°C / min, and the heat preservation time is 1h-2h; then, it is cooled to room temperature at a cooling rate of 3°C / min-5°C / min to obtain a cerium oxide ceramic piece.

Citation Information

Patent Citations

  • Ultraviolet-proof high-refractive-index composite nano coating and preparation method thereof

    CN111205747A

  • Preparation method of difficult-to-cure ceramic based on photocuring forming and product

    CN113880559A

  • High-refractive-index piezoelectric ceramic slurry for photocuring as well as preparation method and application of high-refractive-index piezoelectric ceramic slurry

    CN117586009A

  • Organic-inorganic hybrid composition with high refractive index

    KR1020170024836A

  • Compositions for additive manufacturing and methods of additive manufacturing, particularly of nuclear reactor components