Ceramic, preparation method thereof and wading device
By using a combination of glass silver-carrying antibacterial agent, matrix and binder in water-treated ceramics, combined with metal oxides, ceramics with excellent antibacterial effects and long-term sustained release are prepared, and the antibacterial effects and cycles in the prior art are solved. The difficult problem to take into account has achieved efficient and long-term antibacterial properties, while controlling production costs.
Patent Information
- Application Number
- CN202411042461.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing water-treated antibacterial agents are difficult to take into account both the antibacterial effect and the antibacterial cycle. They cannot guarantee good antibacterial effect or long antibacterial cycle, and have high production costs.
The ceramic consisting of glass silver-carrying antibacterial agent, matrix and binder is prepared by sintering process. The mass part of the ceramic is 10-32 parts, the binder is 5-31 parts, and the matrix is 35-85 parts, pore volume is 0.5-1cm3/g, combined with metal oxides, it forms excellent antibacterial effect and long-term sustained release.
The antibacterial rate of ceramics to E. coli in aqueous solution is achieved, and the silver ion sustained release effect is good, the service cycle can reach 1-3 years, and the cost is controlled within a reasonable range.
Smart Images

Figure BDA0004972712350000071 
Figure BDA0004972712350000081 
Figure BDA0004972712350000091
Abstract
Description
Technical Field
[0001] The invention relates to a ceramic and a preparation method thereof, and a wading device. Background Art
[0002] With the improvement of living standards, people have an increasing demand for antibacterial and anti-mildew products in daily life, especially in products that are in frequent contact with water, such as water purifiers, water dispensers, pressure tanks, etc. Antibacterial and anti-mildew products have become important considerations for products. This is not only related to the health of daily life, but also the key to improving the quality of life.
[0003] At present, conventional water treatment antibacterial agents are mostly based on porous alumina, activated carbon, molecular sieves, zeolites, etc. as carriers, and silver-loaded antibacterial balls are prepared by impregnation and calcination. When these silver-loaded antibacterial balls are used in water treatment systems, there will be problems such as either good antibacterial effect but short antibacterial cycle, or long antibacterial cycle but poor antibacterial effect.
[0004] Therefore, how to ensure that the antibacterial material has both good antibacterial effect and long antibacterial cycle, and how to improve the antibacterial effect without increasing production costs have become the main technical challenges facing the industry. Summary of the invention
[0005] Aiming at the defect that the antibacterial materials in the prior art cannot simultaneously ensure good antibacterial effect and long antibacterial period, a ceramic and a preparation method thereof, and a wading device are provided. The ceramic can simultaneously have excellent antibacterial effect and long antibacterial period.
[0006] The present invention solves the above technical problems through the following technical solutions.
[0007] The present invention also provides a ceramic, which comprises a glass-loaded silver antibacterial agent, a matrix and a binder, wherein, based on 100 parts by mass of the ceramic, the glass-loaded silver antibacterial agent is 10-32 parts, the binder is 5-31 parts, and the matrix is 35-85 parts; the pore volume of the ceramic is 0.5-1cm 3 / g.
[0008] In the present invention, the glass-loaded silver antibacterial agent refers to a silver-loaded glass material that can be used to provide an antibacterial effect, and the matrix refers to a material that can play a supporting role.
[0009] In the present invention, preferably, the glass-loaded silver antibacterial agent is a borosilicate-loaded silver antibacterial agent and / or a phosphate-loaded silver antibacterial agent.
[0010] In the present invention, preferably, the mass content of silver in the glass-supported silver antibacterial agent is 0.5%-2%, more preferably 0.5%-1%.
[0011] In the present invention, preferably, the particle size of the glass-supported silver antibacterial agent is 100-300 meshes, for example, 200 meshes.
[0012] In the present invention, preferably, the binder is an organic binder and / or an inorganic binder, preferably an inorganic binder.
[0013] The organic binder is, for example, one or more of sodium carboxymethyl cellulose, microcrystalline cellulose, polyvinyl alcohol and maltodextrin.
[0014] The inorganic binder is, for example, one or more of silica sol, clay, sodium silicate, aluminum phosphate and attapulgite. The clay is clay in the conventional sense in the art, and its main components are silicon oxide and aluminum oxide; the attapulgite is attapulgite in the conventional sense in the art, and its main components are water-containing magnesium-rich aluminum silicate clay minerals with a layered chain structure.
[0015] Wherein, the particle size of the clay is preferably 100-300 meshes.
[0016] Wherein, the particle size of the attapulgite is preferably 100-300 mesh.
[0017] Wherein, the modulus of the sodium silicate is preferably greater than 3. The modulus has the conventional meaning in the art, that is, the molar ratio of silicate ions to sodium ions in the sodium silicate.
[0018] Wherein, the mass proportion of silicon oxide in the silicon oxide sol is not less than 20%.
[0019] In certain preferred embodiments of the present invention, the binder is clay.
[0020] In the present invention, preferably, the matrix is an inorganic mineral containing silicate and / or aluminosilicate, and the inorganic mineral containing silicate and / or aluminosilicate is, for example, one or more of diatomaceous earth, kaolin and bentonite.
[0021] Wherein, the particle size of the diatomaceous earth is preferably 100-300 meshes.
[0022] In certain preferred embodiments of the present invention, the substrate is diatomaceous earth.
[0023] In the present invention, based on 100 parts by mass of the ceramic, the matrix is preferably 55-75 parts, for example, 59.69 parts, 63.32 parts or 71.88 parts.
[0024] In the present invention, preferably, the ceramic is spherical in shape.
[0025] The particle size of the ceramic is preferably 2-10 mm, more preferably 2-8 mm, further more preferably 3-8 mm, for example 5 mm.
[0026] In the present invention, preferably, based on 100 parts by mass of the ceramic, the glass-supported silver antibacterial agent is 10-25 parts, for example, 10.55 parts, 10.85 parts, 20.54 parts or 21.11 parts.
[0027] In the present invention, preferably, based on 100 parts by mass of the ceramic, the binder is 5-25 parts, for example, 5.13 parts, 10.55 parts, 21.11 parts or 21.71 parts.
[0028] In the present invention, preferably, the pore volume of the ceramic is 0.58-0.93 g / cm 3 , for example 0.63 g / cm 3 , 0.74g / cm 3 , 0.79g / cm 3 or 0.9g / cm 3 .
[0029] In the present invention, preferably, the compressive strength of the ceramic is greater than 50N, more preferably 75-163N, for example 83N, 110N, 127N or 154N.
[0030] In the present invention, preferably, the service life of the ceramic is more than 1 year, more preferably 1-3 years, for example, 1.65 years, 1.8 years, 2.14 years, 2.6 years, 2.8 years or 2.97 years. The service life means that within this time range, the antibacterial rate of the ceramic against Escherichia coli in aqueous solution is ≥99%.
[0031] In the present invention, preferably, the silver ion dissolution rate of the ceramic in 6 months is 15%-35%, for example, 16.5%, 17.8%, 19.23%, 23.4%, 27.7% or 30.2%.
[0032] In the present invention, preferably, the silver ion dissolution rate of the ceramic in one month is 3%-6%, for example, 3.04%, 3.26%, 3.33%, 4.29%, 5.08% or 5.54%.
[0033] In the present invention, preferably, the three-month silver ion dissolution ratio of the ceramic is 8%-16%, for example, 8.43%, 9.05%, 9.79%, 11.90%, 14.08% or 15.35%.
[0034] In the present invention, preferably, the ceramic also includes metal oxides, such as one or more of calcium oxide (i.e. calcium oxide CaO), aluminum oxide (i.e. aluminum oxide Al2O3), sodium oxide (i.e. sodium oxide Na2O) and magnesium oxide (i.e. magnesium oxide MgO).
[0035] Wherein, based on 100 parts by mass of the ceramic, the metal oxide is preferably 2-15 parts, more preferably 2-10 parts, for example, 2.45 parts, 5.03 parts or 7.75 parts.
[0036] In certain preferred embodiments of the present invention, the ceramic further comprises magnesium oxide.
[0037] In some specific embodiments of the present invention, the ceramic is composed of a glass-supported silver antibacterial agent, a matrix, a binder and a metal oxide.
[0038] The present invention provides a method for preparing ceramics, which comprises the following steps: sintering a mixture to obtain the ceramics, wherein the mixture comprises a ceramic raw material and a solvent;
[0039] Wherein, the ceramic raw material comprises a glass silver antibacterial agent, a matrix and a binder; based on 100 parts by mass of the ceramic raw material, the glass silver antibacterial agent is 10-25 parts, the binder is 5-25 parts, and the matrix is 35-80 parts;
[0040] Wherein, the sintering temperature is 700-900°C.
[0041] In the present invention, preferably, the glass-supported silver antibacterial agent is defined as described in any one of the present invention.
[0042] In the present invention, the ceramic raw material preferably further includes a pore former. The pore former means a material that can generate pores during the preparation process. The pore former used in the present invention can further regulate the pore structure of the ceramic and provide a suitable channel for the release of silver ions.
[0043] Preferably, the pore former is an inorganic pore former.
[0044] Wherein, the inorganic pore former is preferably one or more of carbonate, phosphate and metal hydroxide.
[0045] The carbonate is, for example, one or more of calcium carbonate, sodium carbonate and magnesium carbonate.
[0046] The phosphate is, for example, calcium phosphate and / or sodium phosphate.
[0047] The metal hydroxide is, for example, one or more of calcium hydroxide, aluminum hydroxide and magnesium hydroxide.
[0048] In certain preferred embodiments of the present invention, the pore former is magnesium carbonate.
[0049] Preferably, the particle size of the pore former is 100-300 mesh.
[0050] Preferably, based on 100 parts by mass of the ceramic raw material, the pore former is 5-15 parts, for example, 10 parts.
[0051] In the present invention, based on 100 parts by mass of the ceramic raw material, the glass-supported silver antibacterial agent is preferably 10-20 parts.
[0052] In the present invention, preferably, the binder is defined as described in any one of the present invention.
[0053] In the present invention, based on 100 parts by mass of the ceramic raw material, the binder is preferably 5-20 parts, for example, 10 parts.
[0054] In the present invention, preferably, the matrix is defined as described in any one of the present invention.
[0055] In certain preferred embodiments of the present invention, the substrate is diatomaceous earth.
[0056] In the present invention, preferably, based on 100 parts by mass of the ceramic raw material, the matrix accounts for 45-80 parts, for example, 55 parts, 60 parts or 70 parts.
[0057] In the present invention, the ceramic raw material is preferably composed of a glass-loaded silver antibacterial agent, a matrix and a binder, or is preferably composed of a glass-loaded silver antibacterial agent, a matrix, a pore-forming agent and a binder.
[0058] In some specific embodiments of the present invention, the glass-loaded silver antibacterial agent is a borosilicate-loaded silver antibacterial agent, the matrix is diatomaceous earth, the binder is clay, and the pore-forming agent is magnesium carbonate.
[0059] In other specific embodiments of the present invention, the glass-loaded silver antibacterial agent is a phosphate-loaded silver antibacterial agent, the matrix is diatomaceous earth, the binder is clay, and the pore-forming agent is magnesium carbonate.
[0060] In a specific embodiment of the present invention, based on 100 parts by mass of the ceramic raw material, the glass-based silver antibacterial agent is 10 parts, the matrix is 55 parts, the pore-forming agent is 15 parts, and the binder is 20 parts.
[0061] In a specific embodiment of the present invention, based on 100 parts by mass of the ceramic raw material, the glass-based silver antibacterial agent is 10 parts, the matrix is 60 parts, the pore-forming agent is 10 parts, and the binder is 20 parts.
[0062] In a specific embodiment of the present invention, based on 100 parts by mass of the ceramic raw material, the glass-based silver antibacterial agent is 20 parts, the matrix is 60 parts, the pore-forming agent is 10 parts, and the binder is 10 parts.
[0063] In a specific embodiment of the present invention, based on 100 parts by mass of the ceramic raw material, the glass-based silver antibacterial agent is 20 parts, the matrix is 70 parts, the pore former is 5 parts, and the binder is 5 parts.
[0064] In the present invention, preferably, the solvent is water.
[0065] The water is, for example, deionized water.
[0066] Wherein, based on 100 parts by mass of the ceramic raw material, the solvent is preferably 5-20 parts, more preferably 10-20 parts, for example 15 parts.
[0067] In the present invention, preferably, a ball-making step is further included before the sintering, and the ball-making step is to granulate the ceramic raw material by rolling to obtain wet balls.
[0068] Wherein, the ball making step is preferably carried out in a ball making machine.
[0069] The rotation speed of the ball making machine can be selected according to actual conditions, for example, 35 rpm / min.
[0070] Wherein, the particle size of the wet bulb is preferably 2-10 mm.
[0071] The time for making the balls is not particularly limited, as long as the particle size of the wet balls is 2-10 mm.
[0072] Preferably, the wet bulbs are dried to obtain dry bulbs.
[0073] The drying time is preferably 8-24 hours, more preferably 10-14 hours, for example 12 hours.
[0074] The drying temperature is preferably 60-150°C, for example 100°C or 120°C.
[0075] Those skilled in the art generally understand that the sintered ceramics can be sieved to obtain ceramics of a target size.
[0076] In the present invention, preferably, the sintering temperature is 700-800°C.
[0077] In the present invention, preferably, the sintering time is 2-8 hours, for example, 4 hours or 6 hours.
[0078] In the present invention, preferably, the ceramic is spherical in shape.
[0079] The particle size of the ceramic is preferably 2-10 mm, more preferably 2-8 mm, further more preferably 3-8 mm, for example 5 mm.
[0080] The invention also provides a ceramic prepared by the preparation method of the ceramic.
[0081] The present invention also provides a wading device, which comprises the ceramic.
[0082] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0083] The reagents and raw materials used in the present invention are commercially available.
[0084] The positive and progressive effects of the present invention are:
[0085] The present invention prepares ceramics with excellent antibacterial effect, silver ion sustained release effect and long-term antibacterial effect by matching the type of antibacterial agent in the ceramic raw material, the ratio of each component of the ceramic raw material and the sintering temperature. Compared with the prior art, the ceramic can have both excellent antibacterial effect and long antibacterial period. DETAILED DESCRIPTION
[0086] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0087] Examples 1-4 and Comparative Examples 1-6
[0088] The method for preparing the ceramic comprises the following steps:
[0089] Taking the ceramic raw material as 100 parts, weigh a 200-mesh glass silver-loaded antibacterial agent, a 200-mesh matrix, a 200-mesh pore-forming agent and a 200-mesh binder according to the mass proportion in Table 1, and use a mixer to mix them evenly to obtain a powder; add the powder to a ball-making machine, and add a solvent in multiple times, the solvent is proportioned according to the mass proportion in Table 1, and the ball-making machine is rolled at 35 rpm / min to obtain wet balls, and the particle size of the wet balls is 2-10 mm; dry the wet balls to obtain dry balls, the drying temperature is 120°C, and the drying time is 12 hours; sinter and sieve the dry balls to obtain ceramics, and the sintering temperature and time are listed in Table 1.
[0090] The prepared ceramics include a glass-supported silver antibacterial agent, a matrix and a binder, and the pore-forming agent is completely decomposed to form pores in the ceramics.
[0091] The mass content of silver in the glass-loaded silver antibacterial agent is 1%.
[0092] Among them, borosilicate silver-loaded antibacterial agent was purchased from Shanghai Langyi Functional Materials Co., Ltd., model B110; phosphate silver-loaded antibacterial agent was purchased from Shanghai Langyi Functional Materials Co., Ltd., model BP110; magnesium carbonate was purchased from Wuxi Zemei New Materials Technology Co., Ltd., model ZH-200; clay was purchased from Lingshou County Dingsheng Mining Processing Plant, model DS-250; diatomaceous earth was purchased from Yixing Junlian Diatomaceous Earth Co., Ltd., model SZ-200.
[0093] Table 1
[0094]
[0095]
[0096] Note: “ / ” in the table means that the substance is not contained.
[0097] Effect Example 1
[0098] The ceramics prepared in Examples 1-6 and Comparative Examples 1-6 were subjected to the following tests: 1. Ceramic appearance: The appearance of the ceramic balls was observed visually.
[0099] 2. Ceramic particle size: randomly select 50 prepared ceramics, use a vernier caliper to measure the diameter of each ceramic ball, and calculate the average value of the diameters of these 50 ceramics as the ceramic particle size.
[0100] 3. Compressive strength of ceramics: The compressive strength of ceramics is tested using a DL2 particle strength tester. The test method refers to standard HG / T 3927-2020.
[0101] 4. Test of ceramic pore volume: Use static adsorption instrument to test the pore volume of ceramics.
[0102] 5. The content of glass-based silver antibacterial agent, binder and metal oxide in ceramics is theoretically calculated based on the component content of the raw materials.
[0103] The above test results are listed in Table 2, wherein the ceramics prepared in Examples 1-6 and Comparative Examples 1-6 include a glass-loaded silver antibacterial agent, a matrix, a binder and a metal oxide. The types of the glass-loaded silver antibacterial agent, the matrix and the binder are listed in Table 1. The metal oxides prepared in Examples 1-6 and Comparative Examples 1-6 are all magnesium oxides (i.e., magnesium oxide MgO). The mass fraction of the ceramic is 100 parts, and the component contents are listed in Table 2.
[0104] Table 2
[0105]
[0106]
[0107] Note: “ / ” in the table means that the test cannot be performed.
[0108] Effect Example 2
[0109] The ceramics prepared in Examples 1-4 and Comparative Examples 1-6 were subjected to the following tests:
[0110] 1. 1d solution antibacterial rate: Add ceramics into deionized water at a ratio of 4% by mass of ceramics to deionized water. After soaking for one day, take the soaking liquid to test the antibacterial rate of Escherichia coli in the solution. The test method refers to QB / T2738.
[0111] 2. Silver ion dissolution ratio:
[0112] (1) Silver ion dissolution ratio in 6 months: ceramics were added to deionized water at a ratio of 4% by mass of ceramics to deionized water and immersed therein. After 6 months, the concentration of silver ions in the deionized water was tested by inductively coupled plasma emission spectroscopy (ICP). The silver ion dissolution ratio in 6 months was calculated as follows: Silver ion dissolution ratio in 6 months = (silver ion concentration in deionized water after 6 months * volume of deionized water) / (ceramic mass * silver content in ceramics), silver content in ceramics = number of glass-based silver antibacterial agents in ceramics * mass content of silver in glass-based silver antibacterial agents.
[0113] (2) 3-month silver ion dissolution ratio: The determination method and calculation are the same as the 6-month silver ion dissolution ratio, and the immersion time is adjusted to 3 months and tested.
[0114] (3) 1-month silver ion dissolution ratio: The determination method and calculation are the same as the 6-month silver ion dissolution ratio, and the immersion time is adjusted to 1 month and tested.
[0115] 3. Calculation method of usage cycle: 100% / (3-month silver ion dissolution ratio*4)
[0116] The above test results are listed in Table 3 below:
[0117] Table 3
[0118]
[0119]
[0120] Note: “ / ” in the table means that the test cannot be performed.
[0121] It can be seen from the data in Table 1-3 that the ceramics prepared in Examples 1-4 are uniformly spherical and have a compressive strength of 70-170N. The antibacterial rate of the 1d solution of the ceramics prepared in Examples 1-4 can reach more than 99%, indicating that it has a good antibacterial effect. On the basis of satisfying the excellent antibacterial effect of the ceramics, the 6-month silver ion dissolution ratio of the ceramics prepared in Examples 1-4 is 15%-35%, and the service life is 1-3 years, indicating that the silver ion sustained release effect in the ceramics is good and can have long-term antibacterial effect.
[0122] Compared with Example 3, the content of glass-based silver antibacterial agent in Comparative Example 1 is too low, resulting in the antibacterial rate of the ceramic solution in 1d being only 52%, and the antibacterial effect is poor. Although the silver ion dissolution ratio in 6 months can reach 42.6%, it cannot achieve a certain antibacterial performance, and therefore cannot achieve long-term antibacterial effect.
[0123] Compared with Example 3, the content of glass-based silver antibacterial agent in Comparative Example 2 is too high, resulting in the antibacterial rate of the ceramic solution in 1d being only 85%, with poor antibacterial effect, and the proportion of silver ion dissolution in 6 months being only 8.4%, which cannot achieve excellent sustained-release effect and long-term antibacterial effect. This may be due to the excessive content of glass-based silver antibacterial agent, which dissolves the components of the matrix during the sintering process, causing the ceramic structure to become dense, thereby affecting the release channel of silver ions, resulting in poor antibacterial effect and sustained-release effect.
[0124] Compared with Example 3, Comparative Example 3 did not add any adhesive, resulting in a compressive strength of only 3N, which made it unusable.
[0125] Compared with Example 3, the binder content in Comparative Example 4 is too high, and the ceramics with uniform spherical shapes cannot be formed, so the ceramics cannot be used. This may be because the high binder content causes the spheres to adhere to each other during the sintering process and cannot be separated.
[0126] Compared with Example 3, the sintering temperature of Comparative Example 5 is too high to form uniform spherical ceramics, and the spheres are stuck together, so the ceramics cannot be used. This may be because the sintering temperature is too high, which will melt the glass-loaded silver antibacterial agent, causing the ceramic spheres to stick together and cannot be separated.
[0127] Compared with Example 3, the sintering temperature of Comparative Example 6 is too low, so that its compressive strength is too high, which is 188N, and the antibacterial rate of the ceramic solution in 1d is only 68%, and the antibacterial effect is poor. The proportion of silver ion dissolution in 6 months is only 10.3%, and it is impossible to achieve an excellent sustained-release effect and long-term antibacterial. This may be because the sintering temperature is too low, resulting in the inability of the pore-forming agent to be effectively decomposed, making the structure of the ceramic too dense, and the compressive strength is too high, which affects the release channel of the silver ions, resulting in poor antibacterial effect and sustained-release effect.
Claims
1. A ceramic, It is characterized in that The ceramic comprises a glass-loaded silver antibacterial agent, a matrix and a binder, wherein, based on 100 parts by mass of the ceramic, the glass-loaded silver antibacterial agent is 10-32 parts, the binder is 5-31 parts, and the matrix is 35-85 parts; the pore volume of the ceramic is 0.5-1cm 3 / g.
2. The ceramic according to claim 1, It is characterized in that It meets one or more of the following conditions: (1) The glass silver-loaded antibacterial agent is a borosilicate silver-loaded antibacterial agent and / or a phosphate silver-loaded antibacterial agent; (2) The particle size of the glass-supported silver antibacterial agent is 100-300 mesh, for example, 200 mesh; (3) The mass content of silver in the glass-supported silver antibacterial agent is 0.5%-2%, preferably 0.5%-1%; (4) The binder is an organic binder and / or an inorganic binder; wherein the inorganic binder is, for example, one or more of silica sol, clay, sodium silicate, aluminum phosphate and attapulgite; wherein the particle size of the clay is preferably 100-300 mesh; wherein the particle size of the attapulgite is preferably 100-300 mesh; wherein the modulus of the sodium silicate is preferably greater than 3; wherein the mass proportion of silicon oxide in the silica sol is not less than 20%; wherein the organic binder is, for example, one or more of sodium carboxymethyl cellulose, microcrystalline cellulose, polyvinyl alcohol and maltodextrin; (5) The matrix is an inorganic mineral containing silicate and / or aluminosilicate, and the inorganic mineral containing silicate and / or aluminosilicate is, for example, one or more of diatomaceous earth, kaolin and bentonite; wherein the particle size of the diatomaceous earth is preferably 100-300 mesh; (6) Based on 100 parts by mass of the ceramic, the matrix is 55-75 parts, for example, 59.69 parts, 63.32 parts or 71.88 parts; (7) The shape of the ceramic is spherical; wherein the particle size of the ceramic is preferably 2-10 mm, more preferably 2-8 mm, further preferably 3-8 mm, for example 5 mm; (8) Based on 100 parts by mass of the ceramic, the glass-supported silver antibacterial agent is 10-25 parts, for example, 10.55 parts, 10.85 parts, 20.54 parts or 21.11 parts; (9) Based on 100 parts by mass of the ceramic, the binder is 5-25 parts, for example, 5.13 parts, 10.55 parts, 21.11 parts or 21.71 parts; (10) The pore volume of the ceramic is 0.58-0.93 g / cm 3 , for example 0.63 g / cm 3 , 0.74g / cm 3 , 0.79g / cm 3 or 0.9g / cm 3 ; (11) The compressive strength of the ceramic is greater than 50N, preferably 75-163N, for example 83N, 110N, 127N or 154N; (12) The ceramic has a service life of more than 1 year, preferably 1-3 years, for example, 1.65 years, 1.8 years, 2.14 years, 2.6 years, 2.8 years or 2.97 years; (13) The 6-month silver ion dissolution rate of the ceramic is 15%-35%, for example, 16.5%, 17.8%, 19.23%, 23.4%, 27.7% or 30.2%; (14) The silver ion dissolution rate of the ceramic in one month is 3%-6%, for example, 3.04%, 3.26%, 3.33%, 4.29%, 5.08% or 5.54%; (15) The three-month silver ion dissolution rate of the ceramic is 8%-16%, for example, 8.43%, 9.05%, 9.79%, 11.90%, 14.08% or 15.35%; (16) The ceramic also includes a metal oxide, such as one or more of calcium oxide, aluminum oxide, sodium oxide and magnesium oxide; wherein, based on 100 parts by mass of the ceramic, the metal oxide accounts for 2-15 parts, preferably 2-10 parts, for example, 2.45 parts, 5.03 parts or 7.75 parts.
3. A method for preparing ceramics, It is characterized in that It includes the following steps: Sintering the mixture to obtain ceramics, wherein the mixture includes ceramic raw materials and a solvent; Wherein, the ceramic raw material comprises a glass silver antibacterial agent, a matrix and a binder; based on 100 parts by mass of the ceramic raw material, the glass silver antibacterial agent is 10-25 parts, the binder is 5-25 parts, and the matrix is 35-80 parts; Wherein, the sintering temperature is 700-900°C.
4. The method for preparing the ceramic according to claim 3, It is characterized in that The ceramic raw material also includes a pore former; Wherein, the particle size of the pore-forming agent is preferably 100-300 mesh; Wherein, based on 100 parts by mass of the ceramic raw material, the pore former is preferably 5-15 parts, for example, 10 parts; Among them, the pore former is preferably an inorganic pore former; the inorganic pore former is preferably one or more of carbonates, phosphates and metal hydroxides; the carbonate is, for example, one or more of calcium carbonate, sodium carbonate and magnesium carbonate; the phosphate is, for example, calcium phosphate and / or sodium phosphate; the metal hydroxide is, for example, one or more of calcium hydroxide, aluminum hydroxide and magnesium hydroxide.
5. The method for preparing the ceramic according to claim 3, It is characterized in that It meets one or more of the following conditions: (1) The glass silver-loaded antibacterial agent is a borosilicate silver-loaded antibacterial agent and / or a phosphate silver-loaded antibacterial agent; (2) The mass content of silver in the glass-supported silver antibacterial agent is 0.5%-2%, preferably 0.5%-1%; (3) The particle size of the glass-supported silver antibacterial agent is 100-300 mesh, for example, 200 mesh; (4) Based on 100 parts by mass of the ceramic raw material, the glass-loaded silver antibacterial agent is 10-20 parts.
6. The method for preparing the ceramic according to claim 3, It is characterized in that It meets one or more of the following conditions: (1) The binder is an organic binder and / or an inorganic binder; Wherein, the inorganic binder is, for example, one or more of silica sol, clay, sodium silicate, aluminum phosphate and attapulgite; wherein the particle size of the clay is preferably 100-300 mesh; wherein the particle size of the attapulgite is preferably 100-300 mesh; wherein the modulus of the sodium silicate is preferably greater than 3; wherein the mass proportion of silicon oxide in the silica sol is not less than 20%; Wherein, the organic binder is, for example, one or more of sodium carboxymethyl cellulose, microcrystalline cellulose, polyvinyl alcohol and maltodextrin; (2) Based on 100 parts by mass of the ceramic raw material, the binder is 5-20 parts, for example, 10 parts; (3) The matrix is a natural inorganic mineral containing silicate and / or aluminosilicate, and the natural inorganic mineral containing silicate and / or aluminosilicate is, for example, one or more of diatomaceous earth, kaolin and bentonite; wherein the particle size of the diatomaceous earth is preferably 100-300 mesh; (4) Based on 100 parts by mass of the ceramic raw material, the matrix accounts for 45-80 parts, for example, 55 parts, 60 parts or 70 parts.
7. The method for preparing the ceramic according to claim 3, It is characterized in that It meets one or more of the following conditions: (1) The solvent is water; wherein, based on 100 parts by mass of the ceramic raw material, the solvent is preferably 5-20 parts, more preferably 10-20 parts; (2) Before the sintering, the process also includes a ball-making step, wherein the ceramic raw material is granulated by rolling to obtain wet balls; wherein the ball-making step is preferably performed in a ball-making machine; Wherein, the particle size of the wet bulb is preferably 2-10 mm; Wherein, the wet bulb is preferably dried to obtain a dry bulb; The drying time is preferably 8-24 hours, more preferably 10-14 hours, for example 12 hours; Wherein, the drying temperature is preferably 60-150°C, for example, 100°C or 120°C; (3) The sintering temperature is 700-800° C.; (4) The sintering time is 2-8 hours, for example, 4 hours or 6 hours; (5) The shape of the ceramic is spherical; wherein the particle size of the ceramic is preferably 2-10 mm, more preferably 2-8 mm, and further preferably 3-8 mm, for example 5 mm.
8. A method for preparing a ceramic according to any one of claims 3 to 7, It is characterized in that It meets any of the following conditions: (1) The ceramic raw material is composed of a glass-loaded silver antibacterial agent, a matrix, a pore-forming agent and a binder. Based on 100 parts by mass of the ceramic raw material, the glass-loaded silver antibacterial agent is 10 parts, the matrix is 55 parts, the pore-forming agent is 15 parts, and the binder is 20 parts; (2) The ceramic raw material is composed of a glass-loaded silver antibacterial agent, a matrix, a pore-forming agent and a binder. Based on 100 parts by mass of the ceramic raw material, the glass-loaded silver antibacterial agent is 10 parts, the matrix is 60 parts, the pore-forming agent is 10 parts, and the binder is 20 parts; (3) The ceramic raw material is composed of a glass-loaded silver antibacterial agent, a matrix, a pore-forming agent and a binder. Based on 100 parts by mass of the ceramic raw material, the glass-loaded silver antibacterial agent is 20 parts, the matrix is 60 parts, the pore-forming agent is 10 parts, and the binder is 10 parts; (4) The ceramic raw material is composed of a glass-loaded silver antibacterial agent, a matrix, a pore-forming agent and a binder. Based on 100 parts by mass of the ceramic raw material, the glass-loaded silver antibacterial agent is 20 parts, the matrix is 70 parts, the pore-forming agent is 5 parts, and the binder is 5 parts.
9. A ceramic obtained by the method for preparing a ceramic according to any one of claims 3 to 8.
10. A wading device, It is characterized in that It comprises the ceramic as claimed in any one of claims 1 to 2 and 9.
Citation Information
Patent Citations
Preparation method of modified silver-loaded floating bead-based ceramic filter material
CN108339324A
Glass silver-zinc-loaded antibacterial agent and preparation method thereof
CN113317324A
Special ceramic material with antibacterial and water activating functions and preparation method and application thereof
CN1621388A
Antibacterial composition and its production
JP1994024920A
Antibacterial ceramic body
JP2013233492A