Thermoplastic resin, method for producing same, and optical lens

By introducing specific structural units and melt condensation process into the thermoplastic resin, the problems of difficult to achieve high refractive index, low b value and moisture and heat resistance in the prior art are solved, and high-performance optical lenses suitable for electronic devices are manufactured.

CN118955256APending Publication Date: 2024-11-15MITSUBISHI GAS CHEM CO INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411003869.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-02-27
Filing Date
2020-02-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to provide small, lightweight thermoplastic resins and optical lenses with high refractive index, low b values ​​and high humidity resistance, especially when water and heat resistance are required in electronic devices.

Method used

By developing a thermoplastic resin containing specific structural units, such as polyester resin or polyester carbonate resin, manufactured by melt polycondensation process, the resin is ensured to contain structural units with high refractive index and low b values, and through specific structural design The proportion to the composition is improved to improve its moisture and heat resistance.

Benefits of technology

It achieves high refractive index, low b value and high humidity resistance, and is suitable for the manufacturing of lightweight optical lenses, meeting the water resistance and heat resistance requirements of electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955256A_ABST
    Figure CN118955256A_ABST
Patent Text Reader

Abstract

Provided are: a thermoplastic resin having a high refractive index, a low b value, and high wet heat resistance; an optical lens using the thermoplastic resin; and the like. According to one embodiment, a thermoplastic resin containing a structural unit represented by general formula (1) is provided. (In formula (1), R1 and R2 each independently represent a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, a monocyclic or polycyclic aryl group having 6 to 36 carbon atoms, a monocyclic or polycyclic heteroaryl group having 5 to 36 ring atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms, 1, 2, 3 or 4 of the ring atoms are selected from nitrogen, sulfur and oxygen, the other ring atoms are carbon, and X, a and b are respectively described in the specification. > # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This case is filed on February 27, 2020 、Application No. 202080017426.1(PCT / JP2020 / 008193) 、The name of the invention is Thermoplastic resin, method for producing the same, and optical lens Divisional application. Technical Field

[0002] The present invention relates to a thermoplastic resin, in particular, to a thermoplastic resin such as a polyester resin, a polyester carbonate resin, a polycarbonate resin, and a method for producing the same. The present invention also relates to an optical lens containing the thermoplastic resin. Background Art

[0003] Optical glass or optical resin is used as a material for optical lenses used in the optical systems of various cameras such as still cameras, film-integrated cameras, and video cameras. Although optical glass has excellent heat resistance, transparency, dimensional stability, and chemical resistance, it has problems such as high material cost, poor molding processability, and low productivity.

[0004] On the other hand, optical lenses made of optical resins have the advantage of being able to be mass-produced through injection molding. For example, thermoplastic resins are used in camera lenses. However, in recent years, as products have become thinner and smaller, there is a need to develop resins with a high refractive index (Patent Documents 1 to 4). Generally speaking, when the refractive index of an optical material is high, a lens element with the same refractive index can be realized with a surface of smaller curvature, which can reduce the amount of aberration generated on the surface. As a result, the number of lenses can be reduced, the decentering sensitivity of the lens can be reduced, and the thickness of the lens can be reduced to achieve lightweighting.

[0005] Furthermore, generally speaking, for lenses used in the optical system of a camera, in addition to having a high refractive index, the b value is also required to be not too high but maintained at a certain level in order to suppress chromatic aberration.

[0006] However, a thermoplastic resin and an optical lens having a sufficiently high refractive index and a low b value have not yet been provided.

[0007] Moreover, in recent years, water resistance and heat resistance are required for various electronic devices. As an environmental test to evaluate the water resistance and heat resistance of such electronic devices, the "PCT test" (pressure cooker test) is implemented. This test is a moisture and heat resistance test, which accelerates the intrusion of water into the inside of the sample over time and evaluates it. Therefore, the optical lens made of optical resin used in electronic devices is required not only to have a high refractive index and a low b value, but also to have high heat resistance and resistance to water decomposition.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2018-2893

[0011] Patent Document 2: Japanese Patent Application Publication No. 2018-2894

[0012] Patent Document 3: Japanese Patent Application Publication No. 2018-2895

[0013] Patent Document 4: Japanese Patent Application Publication No. 2018-59074 Summary of the invention

[0014] Technical problem to be solved by the invention

[0015] The technical problem to be solved by the present invention is to provide a thermoplastic resin having a high refractive index, a low b value and high resistance to moisture and heat, in particular a high refractive index. Also, the object is to provide an excellent optical lens by using the resin.

[0016] Technical solutions for solving technical problems

[0017] The inventors of the present invention have repeatedly conducted intensive studies to solve the above-mentioned technical problems, and as a result, have found that the above-mentioned technical problems can be solved by the following thermoplastic resin and optical lens, thereby arriving at the present invention.

[0018] The present invention is, for example, as follows.

[0019] [1] A thermoplastic resin comprising a structural unit represented by the following general formula (1):

[0020]

[0021] R1 and R2 in formula (1) each independently represent a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, a monocyclic or polycyclic aryl group having 6 to 36 carbon atoms, a monocyclic or polycyclic heteroaryl group having 5 to 36 ring atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms, wherein in the above heteroaryl group, 1, 2, 3 or 4 of the ring atoms are selected from nitrogen, sulfur and oxygen, and the other ring atoms are carbon,

[0022] The monocyclic or polycyclic aryl group and the monocyclic or polycyclic heteroaryl group may have no substituent, or may have one or two R selected from the group consisting of CN, CH3, OCH3, O-phenyl, O-naphthyl, S-phenyl, S-naphthyl and halogen. a base,

[0023] Wherein, R1 and R2 are not all hydrogen,

[0024] X is an alkylene group having 1 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0025] The alkylene group and the cycloalkylene group may be substituted to have a benzene ring, and a and b are integers of 1 to 10 respectively.

[0026] [2] The thermoplastic resin according to [1] above, wherein the thermoplastic resin is a polyester resin or a polyester carbonate resin.

[0027] [3] The thermoplastic resin according to [1] or [2], further comprising a structural unit represented by the following general formula (2).

[0028]

[0029] (In the general formula (2), Q is represented by the following formula (2a).

[0030]

[0031] (In formula (2a), R C Each independently represents a single bond or an alkylene group bonded to the CO group in the above formula (2), the alkylene group may have a substituent, has a total carbon number of 1 to 10, and contains a bonding point to the CO group in the above formula (2) at the terminal.

[0032] [4] The thermoplastic resin according to [3] above, wherein Q is represented by the following formula (2b).

[0033]

[0034] (In formula (2b), n and m each independently represent an integer of 0 to 5,

[0035] p and k each independently represent an integer of 1 to 5,

[0036] R1 and R2 are the same as R1 and R2 in formula (1),

[0037] a and b each independently represent an integer of 0 to 6,

[0038] * represents the bonding point with the CO group in the above formula (2).

[0039] [5] The thermoplastic resin according to [4] above, which has at least a structural unit containing the above Q represented by the following formula (2c).

[0040]

[0041] (In formula (2c), * represents the bonding point to the CO group in the above formula (2).)

[0042] [6] The thermoplastic resin according to any one of [1] to [5] above, which contains more than 50 mol% of the structural unit represented by the general formula (1).

[0043] [7] The thermoplastic resin according to any one of [1] to [6] above, wherein at least one of R1 and R2 in the general formula (1) is an aryl group having 6 to 20 carbon atoms.

[0044] [8] The thermoplastic resin according to [7] above, wherein at least two of R1 and R2 in the general formula (1) are aromatic groups having 6 to 14 carbon atoms.

[0045] [9] The thermoplastic resin according to any one of [1] to [8] above, wherein the structural unit represented by the general formula (1) contains at least one of the structural units represented by the following general formulas (A-1) to (A-7),

[0046]

[0047]

[0048]

[0049]

[10] The thermoplastic resin according to any one of [1] to [9] above, further comprising at least one of the structural units represented by the following general formulas (3) and (4).

[0050]

[0051] (R'1~R' in formula (3) 20 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms,

[0052] Y is an alkylene group having 1 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0053] c and d are integers from 1 to 10 respectively.)

[0054]

[0055] (R"1~R" in formula (4) 16 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms,

[0056] Z is an alkylene group having 1 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0057] e and f are integers from 1 to 10 respectively.)

[0058]

[11] The thermoplastic resin according to 10] above, comprising a copolymer containing at least the structural unit represented by the general formula (1) and the structural unit represented by the general formula (3).

[0059]

[12] The thermoplastic resin according to

[11] above, wherein the copolymer further contains a structural unit represented by the following general formula (3-1):

[0060]

[0061]

[13] The thermoplastic resin according to

[10] above, comprising a copolymer containing at least the structural unit represented by the general formula (1) and the structural unit represented by the general formula (4).

[0062]

[14] The thermoplastic resin according to

[13] above, wherein the copolymer further contains a structural unit represented by the following general formula (4-1):

[0063]

[0064]

[15] The thermoplastic resin according to any one of [1] to

[14] above, which contains 20 to 80 mol% in total of the structural units represented by the general formulae (3) and (4).

[0065]

[16] The thermoplastic resin according to [1] to

[15] above, further comprising at least one structural unit represented by the following general formula (5):

[0066]

[0067]

[17] The thermoplastic resin according to

[16] above, comprising at least a structural unit of BNEF (9,9-bis(6-(2-hydroxyethoxy)naphthalen-2-yl)fluorene).

[0068]

[18] The thermoplastic resin according to

[16] above, comprising at least a structural unit of 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthyl.

[0069]

[19] The thermoplastic resin according to

[16] , further comprising at least a BPPEF (9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene) structural unit.

[0070]

[20] A thermoplastic resin as described in any one of [1] to

[19] above, wherein the aromatic group is selected from the group consisting of pyrenyl, furanyl, benzodioxanyl, dihydrobenzofuranyl, piperonyl, benzofuranyl, dibenzofuranyl, pyrrolidinyl, isoquinolyl, pyrimidinyl and carbazolyl which may be substituted with an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms or an aromatic group having 6 to 16 carbon atoms.

[0071]

[21] The thermoplastic resin according to any one of [1] to

[20] above, wherein the refractive index of the thermoplastic resin is 1.655 or more.

[0072]

[22] The thermoplastic resin according to any one of [1] to

[20] above, wherein the R1 is the same as the R2.

[0073]

[23] The thermoplastic resin according to any one of [1] to

[20] above, wherein

[0074] The above R1 is the same as or different from the above R2 and is selected from a monocyclic or polycyclic aryl group having 6 to 36 carbon atoms, or a monocyclic or polycyclic heteroaryl group having 5 to 36 ring atoms, wherein in the above heteroaryl group, 1, 2, 3 or 4 of the ring atoms are selected from nitrogen, sulfur and oxygen, and the other ring atoms are carbon,

[0075] The monocyclic or polycyclic aryl group and the monocyclic or polycyclic heteroaryl group have no substituent.

[0076]

[24] The thermoplastic resin according to any one of [1] to

[23] above, wherein the R1 and R2 are selected from the following groups:

[0077] Azulene;

[0078] An unsubstituted indenyl group or an indenyl group which may be substituted with 2, 3, 4 or 5 substituents selected from phenyl and polycyclic aryl groups, wherein the polycyclic aryl groups have 2, 3 or 4 benzene rings which may be bonded to each other via single bonds, may be directly condensed to each other, and / or may be condensed with a saturated or unsaturated 4-10 membered monocyclic or bicyclic hydrocarbon ring;

[0079] Phenyl with no substituents;

[0080] Phenyl substituted with 1 or 2 CN groups;

[0081] A phenyl group which may be substituted with 2, 3, 4 or 5 substituents selected from a phenyl group and a polycyclic aryl group, wherein the polycyclic aryl group has 2, 3 or 4 benzene rings which may be bonded to each other via single bonds, may be directly condensed to each other, and / or may be condensed with a saturated or unsaturated 4-10 membered monocyclic or bicyclic hydrocarbon ring;

[0082] A polycyclic aromatic group having 2, 3 or 4 benzene rings which can be directly condensed with each other and / or condensed with a saturated or unsaturated 4-10 membered monocyclic or bicyclic hydrocarbon ring, the polycyclic aromatic group having no substituent or being substituted with 1 or 2 substituents selected from phenyl and a polycyclic aromatic group having 2 or 3 benzene rings, the 2 or 3 benzene rings can be bonded with each other via a single bond, can be directly condensed with each other and / or can be condensed with a saturated 4-10 membered monocyclic or bicyclic hydrocarbon ring, the benzene ring of the polycyclic aromatic group having no substituent or having 1 or 2 substituents R a .

[0083]

[25] The thermoplastic resin according to any one of [1] to

[24] above, wherein the R1 and R2 are selected from the following groups:

[0084] Phenyl which is unsubstituted or which may be substituted with 1, 2, 3, 4 or 5 phenyl groups;

[0085] Phenyl substituted with 1 or 2 CN groups;

[0086] A phenyl group which is substituted with one or two polycyclic aromatic groups selected from biphenyl, naphthyl, fluorenyl, anthracenyl, phenanthrenyl and pyrenyl, and which may be substituted with one phenyl group;

[0087] An unsubstituted naphthyl group or a naphthyl group substituted with one or two substituents selected from the group consisting of CN, phenyl and polycyclic aryl groups, wherein the polycyclic aryl group is selected from the group consisting of biphenyl, naphthyl, fluorenyl, anthracenyl, phenanthrenyl and pyrenyl;

[0088] biphenylenyl;

[0089] triphenylenyl;

[0090] tetraphenylenyl;

[0091] Fiki;

[0092] Pyrene base;

[0093] 9H-fluorenyl;

[0094] dibenzo[a,e][8]annulyl;

[0095] Perylenyl; and

[0096] 9,9'-Spirobi[9H-fluorenyl]yl.

[0097]

[26] The thermoplastic resin according to

[25] , wherein the R1 and R2 are selected from phenyl, 2-cyanophenyl, 3-cyanophenyl, 4-cyanophenyl, 2-naphthyl, 1-naphthyl and 9-naphthyl.

[0098]

[27] The thermoplastic resin according to any one of [1] to

[23] above, wherein the R1 and R2 are selected from the group consisting of:

[0099] a heteroaromatic monocyclic radical having 5 or 6 ring atoms, which has 1, 2, 3 or 4 nitrogen atoms, or has 1 oxygen atom and 0, 1, 2 or 3 nitrogen atoms, or has 1 sulfur atom and 0, 1, 2 or 3 nitrogen atoms, the other ring atoms being carbon atoms;

[0100] A heteroaromatic polycyclic group having the above-mentioned heteroaromatic monocyclic ring and 1, 2, 3, 4 or 5 additional aromatic rings selected from phenyl and heteroaromatic monocyclic rings, wherein the (hetero) aromatic rings of the polycyclic heteroaromatic group may be bound to each other by covalent bonds, may be directly condensed with each other, and / or may be condensed with a saturated or unsaturated 4-10 membered monocyclic or bicyclic hydrocarbon ring; and

[0101] A heteroaromatic polycyclic group having at least one saturated or partially unsaturated 5- or 6-membered heterocyclic ring containing one or two heteroatoms selected from oxygen, sulfur and nitrogen as ring atoms, and one, two, three, four or five other aromatic rings selected from phenyl and the above-mentioned heteroaromatic monocyclic rings, at least one of the above-mentioned other aromatic rings is directly condensed with the saturated or partially unsaturated 5- or 6-membered heterocyclic group, and the other other aromatic rings of the polycyclic heteroaryl aromatic ring may be bound to each other via a covalent bond or may be directly condensed with each other and / or may be condensed with a saturated or unsaturated 4- to 10-membered monocyclic or bicyclic hydrocarbon ring.

[0102]

[28] The thermoplastic resin according to

[27] , wherein R1 and R2 are selected from the group consisting of furyl, thienyl, pyrrolyl, imidazolyl, pyrazolyl, 1,2,3-triazolyl, 1,2,4-triazolyl, tetrazolyl, oxazolyl, isoxazolyl, 1,3,4-oxadiazolyl, 1,2,4-oxadiazolyl, pyridyl, pyrazinyl, pyridazinyl, pyrimidinyl, triazine, benzofuranyl, dibenzofuranyl, benzothiophenyl, dibenzothiophenyl, thianthrenyl, naphthofuranyl, benzothiophene, benzothiophene, benzothiazyl, benzothrene, benzothiazyl ... yl, furano[3,2-b]furanyl, furano[2,3-b]furanyl, furano[3,4-b]furanyl, oxanthrenyl, indolyl, isoindolyl, carbazolyl, indolizinyl, benzopyrazolyl, benzimidazolyl, benzoxazolyl, benzo[cd]indolyl, 1H-benzo[g]indolyl, quinolyl, isoquinolyl, acridinyl, phenazinyl, quinazolinyl, quinoxalinyl, phenoxazinyl, benzo[b][1,5]naphthyridinyl , cinnolinyl, 1,5-naphthyridinyl, 1,8-naphthyridinyl, phenylpyrrolyl, naphthylpyrrolyl, bipyridinyl, phenylpyridinyl, naphthylpyridinyl, pyrido[4,3-b]indolyl, pyrido[3,2-b]indolyl, pyrido[3,2-g]quinolinyl, pyrido[2,3-b][1,8]naphthyridinyl, pyrrolo[3,2-b]pyridinyl, pteridinyl, purinyl, 9H-xanthenyl benzo[g]benzopyranyl, pyrrolo[3,2,1-hi]indolyl, benzo[g]quinoxalinyl, benzo[f]quinoxalinyl and benzo[h]isoquinolyl.

[0103]

[29] The thermoplastic resin according to any one of [1] to

[28] above, wherein X is an ethylene group.

[0104]

[30] The thermoplastic resin according to any one of [1] to

[29] above, wherein the b value according to JIS K 7105 is 10 or less.

[0105]

[31] The thermoplastic resin according to any one of [1] to

[30] above, wherein the refractive index nD and the Abbe number ν satisfy the relationship -0.0002ν+1.6718<nD<-0.024ν+2.124.

[0106]

[32] The thermoplastic resin as described in

[31] above, wherein the refractive index nD and the Abbe number ν satisfy the relationship of -0.004v+1.744<nD<-0.024ν+2.124.

[0107]

[33] The thermoplastic resin as described in

[32] above, wherein the refractive index nD and the Abbe number ν satisfy the relationship of -0.02v+2.04<nD<-0.024ν+2.124.

[0108]

[34] An optical lens comprising the thermoplastic resin described in any one of [1] to

[33] above.

[0109]

[35] A method for producing a thermoplastic resin, for producing the thermoplastic resin described in any one of [1] to

[33] above, the method comprising the step of melt-polycondensing a dihydroxy compound represented by at least the following general formula (6) with at least one of a carboxylic acid, a carboxylic acid monoester and a carboxylic acid diester.

[0110]

[0111] (In the general formula (6), R1 and R2 each independently represent a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, a monocyclic or polycyclic aryl group having 6 to 36 carbon atoms, a monocyclic or polycyclic heteroaryl group having 5 to 36 ring atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms, wherein in the above heteroaryl group, 1, 2, 3 or 4 of the ring atoms are selected from nitrogen, sulfur and oxygen, and the other ring atoms are carbon,

[0112] The monocyclic or polycyclic aryl group and the monocyclic or polycyclic heteroaryl group may have no substituent, or may have one or two R selected from the group consisting of CN, CH3, OCH3, O-phenyl, O-naphthyl, S-phenyl, S-naphthyl and halogen. a base,

[0113] Wherein, R1 and R2 are not all hydrogen,

[0114] X is an alkylene group having 1 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0115] The above alkylene group and the above cycloalkylene group may be substituted to have a benzene ring,

[0116] a and b are integers from 1 to 10 respectively.)

[0117]

[36] A crystalline solvate of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, wherein:

[0118] The crystal contains 0.3 to 1.2 mol of an organic solvent per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl.

[0119] The organic solvent is selected from methanol, toluene and methyl ethyl ketone.

[0120]

[37] The crystalline solvate according to

[36] above, wherein the organic solvent is methanol.

[0121]

[38] The form of the crystalline solvate according to

[37] above, wherein

[0122] The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is:

[0123] The following three reflection peaks were shown as 2θ values: 13.0±0.2°, 14.9±0.2°, and 21.5±0.2°.

[0124] As 2θ values, at least three of the following reflection peaks are shown: 6.2±0.2°, 9.0±0.2°, 10.6±0.2°, 16.9±0.2°, 18.2±0.2°, 18.5±0.2°, 19.2±0.2°, 19.6±0.2°, 20.9±0.2°, 22.7±0.2°, 24.3±0.2°, 24.9±0.2°, 26.2±0.2°, 28.7±0.2° and 30.5±0.2°.

[0125]

[39] A crystalline solvate as described in

[37] or

[38] above, wherein, in differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min (or 20°C / min, the same below), it shows an endothermic peak with a starting point in the range of 97 to 101°C, and the maximum value of the peak is in the range of 108 to 115°C.

[0126]

[40] The crystalline solvate according to any one of

[37] to

[39] above, wherein the amount of methanol is 0.3 to 1.0 mol per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl.

[0127]

[41] The crystalline solvate according to

[36] above, wherein the organic solvent is toluene.

[0128]

[42] The form of the crystalline solvate according to

[41] above, wherein

[0129] The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is:

[0130] The following three reflection peaks were shown as 2θ values: 5.2±0.2°, 7.7±0.2°, and 21.6±0.2°.

[0131] As 2θ values, at least three of the following reflection peaks are shown: 8.2±0.2°, 9.1±0.2°, 10.6±0.2°, 10.8±0.2°, 11.6±0.2°, 12.6±0.2°, 13.6±0.2°, 14.7±0.2°, 15.0±0.2°, 15.7±0.2°, 16.7±0.2°, 17.1±0.2°, 18.4±0.2°, 19.8±0.2°, 20.1±0.2°, 21.3±0.2°, 22.4±0.2°, 23.9±0.2°, 24.8±0.2°, 25.9±0.2°, 26.1±0.2°, 27. 8.0±0.2°, 18.5±0.2°, 19.4±0.2°, 19.9±0.2°, 20.8±0.2°, 21.0±0.2°, 22.2±0.2°, 22.7±0.2°, 24.1±0.2°, 25.0±0.2°, 25.7±0.2°, 26.5±0.2°, 27.1±0.2° and 27.6±0.2°.

[0132]

[43] A crystalline solvate in the form of the above-mentioned

[41] or

[42] , wherein, in differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, an endothermic peak having an onset in the range of 105 to 108°C is shown, and the maximum value of the peak is in the range of 112 to 115°C.

[0133]

[44] The crystalline solvate according to any one of

[41] to

[43] above, wherein the amount of toluene is 0.3 to 0.5 mol per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl.

[0134]

[45] A crystalline form A, which is a crystalline form A of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, wherein:

[0135] The crystal contains less than 0.1 mol of an organic solvent per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl.

[0136] The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is:

[0137] The following three reflection peaks were shown as 2θ values: 20.9±0.2°, 21.4±0.2°, and 23.7±0.2°.

[0138] As 2θ values, at least three of the following reflection peaks are shown: 6.5±0.2°, 8.6±0.2°, 11.0±0.2°, 13.2±0.2°, 14.9±0.2°, 16.2±0.2°, 17.3±0.2°, 17.8±0.2°, 18.4±0.2°, and 19.0±0.2°.

[0139]

[46] A crystalline form as described in 45 above, wherein, in differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, an endothermic peak with a starting point in the range of 112 to 114°C is shown, and the maximum value of the peak is in the range of 124 to 126°C.

[0140]

[47] A crystalline form C, which is a crystalline form C of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, wherein:

[0141] The crystal contains less than 0.1 mol of an organic solvent per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl.

[0142] The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is:

[0143] The following three reflection peaks were shown as 2θ values: 5.1±0.2°, 7.6±0.2°, and 21.0±0.2°.

[0144] As 2θ values, at least three of the following reflection peaks are shown: 8.2±0.2°, 9.2±0.2°, 10.4±0.2°, 10.8±0.2°, 11.6±0.2°, 12.8±0.2°, 13.4±0.2°, 14.5±0.2°, 15.2±0.2°, 15.6±0.2°, 16.6±0.2°, 17.4±0.2°. .2°, 17.9±0.2°, 18.5±0.2°, 19.2±0.2°, 19.9±0.2°, 20.4±0.2°, 21.8±0.2°, 22.2±0.2°, 22.6±0.2°, 13.4±0.2°, 24.0±0.2°, 25.7±0.2°, 27.3±0.2° and 27.9±0.2°.

[0145]

[48] ​​A crystalline form as described in

[47] above, wherein, in differential scanning calorimetry (DSC) recorded in accordance with ISO11357-3:2018 at a heating rate of 20 K / min, an endothermic peak with a starting point in the range of 112 to 114°C is shown, and the maximum value of the peak is in the range of 124 to 126°C.

[0146]

[49] A crystal form as described in any one of

[33] to

[48] above, wherein the crystal has an aspect ratio of up to 5:1.

[0147]

[50] An amorphous form B, which is an amorphous form B of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, wherein:

[0148] The crystal has a purity of at least 99.0% by weight based on organic matter, wherein the crystal contains less than 0.1 mol of an organic solvent per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl.

[0149] The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is:

[0150] No reflection peak as a 2θ value is shown at multiple diffraction angles in the range of 5° to 40°.

[0151] In differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, no endothermic peak is shown in the range of 80 to 200°C.

[0152]

[51] A 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, wherein the total amount of impurities selected from 2-(2-hydroxyethoxy)-2′-hydroxy-6,6′-diphenyl-1,1′-binaphthyl, 2,2′-dihydroxy-6,6′-diphenyl-1,1′-binaphthyl and 2-(2-hydroxyethoxy)-2′-(2-(2-hydroxyethoxy)-ethoxy)-6,6′-diphenyl-1,1′-binaphthyl is less than 0.5% by weight, based on 100% by weight of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl.

[0153]

[52] A 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl having at least one of the following characteristics:

[0154] i. The yellowness index (YI) measured by a 5 w / w% dichloromethane solution of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl in accordance with ASTM E 313 is less than 3.0; and

[0155] ii. The haze measured using a 5 w / w% dichloromethane solution of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl is less than 1.0 ntu.

[0156]

[53] The 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl described in

[51] or

[52] above, which is in a crystalline form as described in any one of

[33] to

[49] above, or in an amorphous form as described in

[50] above.

[0157]

[54] The thermoplastic resin described in any one of [1] to

[33] above, which has structural units derived from the crystalline form described in

[33] to

[49] above and the amorphous form described in

[50] above.

[0158]

[55] The thermoplastic resin according to any one of [1] to

[33] above, which has a structural unit derived from the 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl according to

[51] or

[52] above.

[0159]

[56] An optical lens comprising the thermoplastic resin described in

[54] or

[55] above.

[0160] Effects of the Invention

[0161] The thermoplastic resin of the present invention has a high refractive index, a low b value, and high resistance to moisture and heat, and particularly has a high refractive index. Furthermore, by using such an excellent thermoplastic resin, an excellent optical lens can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0162] Figure 1 This is the H1-NMR spectrum of the resin (BINOL-2EO / BNEF=50 mol / 50 mol) produced in Example 2-B.

[0163] Figure 2 The X-ray powder diffraction pattern of Form A of 6,6′-DPBHBNA obtained in Example 21 is shown.

[0164] Figure 3 The NIR spectrum of Form A of 6,6′-DPBHBNA obtained in Example 21 is shown.

[0165] Figure 4The IR spectrum of Form A of 6,6′-DPBHBNA obtained in Example 21 is shown.

[0166] Figure 5 The DSC of Form A of 6,6'-DPBHBNA obtained in Example 21 is shown.

[0167] Figure 6 The X-ray powder diffraction pattern of the methanol solvate of 6,6′-DPBHBNA obtained in Example 22 is shown.

[0168] Figure 7 The NIR spectrum of the methanol solvate of 6,6′-DPBHBNA obtained in Example 22 is shown.

[0169] Figure 8 The NR spectrum of the methanol solvate of 6,6′-DPBHBNA obtained in Example 22 is shown.

[0170] Fig. 9 The DSC of the methanol solvate of 6,6'-DPBHBNA obtained in Example 22 is shown.

[0171] Fig.10 The X-ray powder diffraction pattern of the crystalline material obtained in Example 23 is shown.

[0172] Fig.11 The NIR spectrum of the crystalline material obtained in Example 23 is shown.

[0173] Fig.12 The NR spectrum of the crystalline material obtained in Example 23 is shown.

[0174] Fig.13 The DSC of the crystalline material obtained from Example 23 is shown.

[0175] Fig.14 A microscopic photograph of the toluene solvate of 6,6′-DPBHBNA obtained in Example 24 is shown.

[0176] Fig.15 The X-ray powder diffraction pattern of the toluene solvate of 6,6′-DPBHBNA obtained in Example 24 is shown.

[0177] Fig.16 The NIR spectrum of the toluene solvate of 6,6′-DPBHBNA obtained in Example 24 is shown.

[0178] Fig.17 The NR spectrum of the toluene solvate of 6,6′-DPBHBNA obtained in Example 24 is shown.

[0179] Fig.18The DSC of the toluene solvate of 6,6'-DPBHBNA obtained in Example 24 is shown.

[0180] Fig.19 A microscopic photograph of the MEK solvate of 6,6′-DPBHBNA obtained in Example 25 is shown.

[0181] Fig. 20 The NIR spectrum of the MEK solvate of 6,6′-DPBHBNA obtained in Example 25 is shown.

[0182] Fig.21 The DSC of the MEK solvate of 6,6'-DPBHBNA obtained in Example 25 is shown.

[0183] Fig. 22 The X-ray powder diffraction pattern of the MEK solvate of 6,6′-DPBHBNA obtained in Example 25 is shown.

[0184] Fig.23 The X-ray powder diffraction pattern of the amorphous form B of 6,6′-DPBHBNA obtained in Example 26 is shown.

[0185] Fig.24 The NIR spectrum of the amorphous form B of 6,6′-DPBHBNA obtained in Example 26 is shown.

[0186] Fig.25 The IR spectrum of the amorphous form B of 6,6′-DPBHBNA obtained in Example 26 is shown.

[0187] Fig.26 The X-ray powder diffraction pattern of Form C of 6,6′-DPBHBNA obtained in Example 27 is shown.

[0188] Fig. 27 The NIR spectrum of Form C of 6,6′-DPBHBNA obtained in Example 27 is shown.

[0189] Fig.28 The IR spectrum of Form C of 6,6′-DPBHBNA obtained in Example 27 is shown.

[0190] Fig.29 The DSC of Form C of 6,6'-DPBHBNA obtained in Example 27 is shown.

[0191] Fig.30 This is a first graph having the Abbe number (v) of the thermoplastic resins of Examples and Comparative Examples as the horizontal axis and the refractive index (nD) as the vertical axis.

[0192] Fig.31This is a second graph having the Abbe number (v) of the thermoplastic resins of Examples and Comparative Examples as the horizontal axis and the refractive index (nD) as the vertical axis. DETAILED DESCRIPTION

[0193] Hereinafter, the present invention will be described in detail.

[0194] (1) Components (structural units) of thermoplastic resins

[0195] The thermoplastic resin of the present invention contains a structural unit represented by the following general formula (1). The type of the thermoplastic resin is not particularly limited as long as it has the following structural unit, and is preferably a polyester resin, a polyester carbonate resin, a polycarbonate resin, or a mixture of at least two of these.

[0196] Furthermore, among thermoplastic resins, polyester resin is a resin having a polyester structural unit (repeating unit) containing a (-RCO-O-) site but excluding a polycarbonate structural unit (repeating unit) containing a (-RO-CO-O-) site, polycarbonate resin is a resin having a polycarbonate structural unit (repeating unit) containing a (-RO-CO-O-) site but excluding a polyester structural unit (repeating unit) containing a (-RCO-O-) site, and polyester carbonate resin is a resin having both a polyester structural unit (repeating unit) containing a (-RO-CO-) site and a polycarbonate structural unit (repeating unit) containing a (-RO-CO-O-) site (R is a hydrocarbon group, etc.).

[0197]

[0198] (In formula (1), R1 and R2 each independently represent a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, a monocyclic or polycyclic aryl group having 6 to 36 carbon atoms, a monocyclic or polycyclic heteroaryl group having 5 to 36 ring atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms, wherein in the above heteroaryl group, 1, 2, 3 or 4 of the ring atoms are selected from nitrogen, sulfur and oxygen, and the other ring atoms are carbon,

[0199] The monocyclic or polycyclic aryl group and the monocyclic or polycyclic heteroaryl group may have no substituent, or may have one or two R selected from the group consisting of CN, CH3, OCH3, O-phenyl, O-naphthyl, S-phenyl, S-naphthyl and halogen. a base,

[0200] Wherein, R1 and R2 are not all hydrogen,

[0201] X is an alkylene group having 1 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0202] The above alkylene group and the above cycloalkylene group may be substituted with a benzene ring, and a and b are integers of 1 to 10.

[0203] R1 and R2 in the general formula (1) are each preferably a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 30 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and even more preferably an aryl group having 6 to 14 carbon atoms. 10 At least one of them is preferably an aryl group having 6 to 20 carbon atoms, more preferably an aryl group having 6 to 14 carbon atoms, and particularly preferably R1 to R 10 At least two of them are aryl groups having 6 to 14 carbon atoms or 6 to 12 carbon atoms.

[0204] R1 and R2 may be the same, for example.

[0205] In addition, R1 and R2 are the same or different and may be selected from a monocyclic or polycyclic aryl group having 6 to 36 carbon atoms, or a monocyclic or polycyclic heteroaryl group having 5 to 36 ring atoms, wherein 1, 2, 3 or 4 of the ring atoms in the heteroaryl group are selected from nitrogen, sulfur and oxygen, and the other ring atoms are carbon. The monocyclic or polycyclic aryl group and the monocyclic or polycyclic heteroaryl group may have no substituent.

[0206] R1 and R2 can be selected from the following groups.

[0207] Azulene;

[0208] An unsubstituted indenyl group or an indenyl group which may be substituted with 2, 3, 4 or 5 substituents selected from phenyl and polycyclic aryl groups, wherein the polycyclic aryl groups have 2, 3 or 4 benzene rings which may be bonded to each other via single bonds, may be directly condensed to each other, and / or may be condensed with a saturated or unsaturated 4-10 membered monocyclic or bicyclic hydrocarbon ring;

[0209] Phenyl with no substituents;

[0210] Phenyl substituted with 1 or 2 CN groups;

[0211] A phenyl group which may be substituted with 2, 3, 4 or 5 substituents selected from a phenyl group and a polycyclic aryl group, wherein the polycyclic aryl group has 2, 3 or 4 benzene rings which may be bonded to each other via single bonds, may be directly condensed to each other, and / or may be condensed with a saturated or unsaturated 4-10 membered monocyclic or bicyclic hydrocarbon ring;

[0212] A polycyclic aromatic group having 2, 3 or 4 benzene rings which can be directly condensed with each other and / or condensed with a saturated or unsaturated 4-10 membered monocyclic or bicyclic hydrocarbon ring, the polycyclic aromatic group having no substituent or being substituted with 1 or 2 substituents selected from phenyl and a polycyclic aromatic group having 2 or 3 benzene rings, the 2 or 3 benzene rings can be bonded with each other via a single bond, can be directly condensed with each other and / or can be condensed with a saturated 4-10 membered monocyclic or bicyclic hydrocarbon ring, the benzene ring of the polycyclic aromatic group having no substituent or having 1 or 2 substituents R a .

[0213] In addition, R1 and R2 can be selected from the following groups.

[0214] Phenyl which is unsubstituted or which may be substituted with 1, 2, 3, 4 or 5 phenyl groups;

[0215] Phenyl substituted with 1 or 2 CN groups;

[0216] A phenyl group which is substituted with one or two polycyclic aromatic groups selected from biphenyl, naphthyl, fluorenyl, anthracenyl, phenanthrenyl and pyrenyl, and which may be substituted with one phenyl group;

[0217] An unsubstituted naphthyl group or a naphthyl group substituted with one or two substituents selected from the group consisting of CN, phenyl and polycyclic aryl groups, wherein the polycyclic aryl group is selected from the group consisting of biphenyl, naphthyl, fluorenyl, anthracenyl, phenanthrenyl and pyrenyl;

[0218] Biphenylene;

[0219] Triphenylene;

[0220] Tetraphenylene;

[0221] Fiki;

[0222] Pyrene base;

[0223] 9H-fluorenyl;

[0224] dibenzo[a,e][8]annulyl;

[0225] Perylenyl; and

[0226] 9,9'-Spirobi[9H-fluorenyl]yl.

[0227] Among them, R1 and R2 are preferably selected from phenyl, 2-cyanophenyl, 3-cyanophenyl, 4-cyanophenyl, 2-naphthyl, 1-naphthyl and 9-naphthyl.

[0228] In addition, R1 and R2 can be selected from the following groups.

[0229] a heteroaromatic monocyclic radical having 5 or 6 ring atoms, which has 1, 2, 3 or 4 nitrogen atoms, or has 1 oxygen atom and 0, 1, 2 or 3 nitrogen atoms, or has 1 sulfur atom and 0, 1, 2 or 3 nitrogen atoms, the other ring atoms being carbon atoms;

[0230] A heteroaromatic polycyclic group having the above-mentioned heteroaromatic monocyclic ring and 1, 2, 3, 4 or 5 additional aromatic rings selected from phenyl and heteroaromatic monocyclic rings, wherein the (hetero) aromatic rings of the polycyclic heteroaromatic group may be bound to each other by covalent bonds, may be directly condensed with each other, and / or may be condensed with a saturated or unsaturated 4-10 membered monocyclic or bicyclic hydrocarbon ring; and

[0231] A heteroaromatic polycyclic group having at least one saturated or partially unsaturated 5- or 6-membered heterocyclic ring containing one or two heteroatoms selected from oxygen, sulfur and nitrogen as ring atoms and one, two, three, four or five additional aromatic rings selected from phenyl and the above-mentioned heteroaromatic monocyclic rings, at least one additional aromatic ring being directly condensed with the saturated or partially unsaturated 5- or 6-membered heterocyclic group, and the other additional aromatic rings of the polycyclic heteroaryl aromatic ring may be bound to each other via a covalent bond or may be directly condensed with each other and / or may be condensed with a saturated or unsaturated 4- to 10-membered monocyclic or bicyclic hydrocarbon ring.

[0232] In addition, R1 and R2 may be selected from the following groups: furanyl, thienyl, pyrrolyl, imidazolyl, pyrazolyl, 1,2,3-triazolyl, 1,2,4-triazolyl, tetrazolyl, oxazolyl, isoxazolyl, 1,3,4-oxadiazolyl, 1,2,4-oxadiazolyl, pyridyl, pyrazinyl, pyridazinyl, pyrimidinyl, triazinyl, benzofuranyl, dibenzofuranyl, benzothienyl, dibenzothienyl, thianthrenyl, naphthofuranyl, furano[3,2-b]furanyl, furano[2,3-b]furanyl, ] furanyl, furano[3,4-b] furanyl, oxanthrenyl, indolyl, isoindolyl, carbazolyl, indolizinyl, benzopyrazolyl, benzimidazolyl, benzoxazolyl, benzo[cd]indolyl, 1H-benzo[g]indolyl, quinolyl, isoquinolyl, acridinyl, phenazinyl, quinazolinyl, quinoxalinyl, phenoxazinyl, benzo[b][1,5]naphthyridinyl, cinnolinyl, 1,5-naphthyridinyl, 1,8- naphthyridinyl, phenylpyrrolyl, naphthylpyrrolyl, bipyridinyl, phenylpyridinyl, naphthylpyridinyl, pyrido[4,3-b]indolyl, pyrido[3,2-b]indolyl, pyrido[3,2-g]quinolyl, pyrido[2,3-b][1,8]naphthyridinyl, pyrrolo[3,2-b]pyridinyl, pteridinyl, purinyl, 9H-xanthenyl, 2 H-benzopyranyl, phenanthridinyl, phenanthrolinyl, furo[3,2-f][1]benzofuranyl, furo[2,3-f][1]benzofuranyl, furo[3,2-g]quinolyl, furo[2,3-g]quinolyl, furo[2,3-g]quinoxalinyl, benzo[g]benzopyranyl, pyrrolo[3,2,1-hi]indolyl, benzo[g]quinoxalinyl, benzo[f]quinoxalinyl and benzo[h]isoquinolyl.

[0233] X in the general formula (1) is preferably an alkylene group having 2 to 4 carbon atoms, a cycloalkylene group having 5 to 8 carbon atoms, or an arylene group having 6 to 14 carbon atoms, more preferably an alkylene group having 2 or 3 carbon atoms, a cycloalkylene group having 5 to 6 carbon atoms, or an arylene group having 6 to 10 carbon atoms, and particularly preferably an alkylene group having 2 or 3 carbon atoms, such as ethylene.

[0234] In addition, a and b in the general formula (1) are each preferably an integer of 1 to 6, more preferably 1 to 4, and particularly preferably 2 or 3.

[0235] The thermoplastic resin is, for example, a polyester resin or a polyester carbonate resin. Furthermore, the polyester resin or the polyester carbonate resin preferably further contains a structural unit represented by the following general formula (2).

[0236]

[0237] In the general formula (2), Q is represented by the following formula (2a).

[0238]

[0239] In formula (2a), R C Each of them is independently a single bond to the CO group of formula (2), or an alkylene group which may have a substituent, has a total of 1 to 10 carbon atoms and contains a bonding point to the CO group of formula (2) at the terminal. C It is preferably a single bond or an alkylene group having 1 to 3 carbon atoms in total.

[0240] Q in the formula (2) is preferably represented by the following formula (2b).

[0241]

[0242] In formula (2b), n and m are each independently an integer of 0-5, preferably an integer of 1-3.

[0243] p and k are each independently an integer of 1-5, preferably an integer of 1-3.

[0244] R1 and R2 have the same meanings as R1 and R2 in formula (1).

[0245] a and b are each independently an integer of 0 to 6, preferably an integer of 1 to 3, and more preferably an integer of 1 or 2.

[0246] Furthermore, * indicates a bonding point to the CO group of formula (2).

[0247] More preferably, Q in the formula (2) is represented by the following formula (2c).

[0248]

[0249] In formula (2c), * is the bonding point with the CO group of formula (2).

[0250] The structural unit represented by the general formula (1) preferably includes at least one of the structural units represented by the following general formulae (A-1) to (A-7).

[0251]

[0252]

[0253] That is, the structural unit represented by the general formula (1) preferably contains a structural unit derived from (BINL-2EO (2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl) represented by the general formula (A-1), a structural unit derived from DNBINOL-2EO (2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-1-yl)-1,1'-binaphthyl) represented by the general formula (A-2), a structural unit derived from 2DNBINOL-2EO (2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-2-yl)-1,1'-binaphthyl) represented by the general formula (A-3), and a structural unit derived from 9DPNBINOL-2EO (2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-2-yl)-1,1'-binaphthyl) represented by the general formula (A-4). The present invention further comprises at least one of a structural unit derived from (6,6′-di(3-cyanophenyl)-2,2′-bis-(2-hydroxyethoxy)-1,1′-binaphthyl) represented by the general formula (A-5), a structural unit derived from (FUR-BNA(6,6′-di(dibenzo[b,d]furan-4-yl)-2,2′-bis-(2-hydroxyethoxy)-1,1′-binaphthyl) represented by the general formula (A-6), and a structural unit derived from (THI-BNA(6,6′-di(dibenzo[b,d]thiophen-4-yl)-2,2′-bis-(2-hydroxyethoxy)-1,1′-binaphthyl) represented by the general formula (A-7).

[0254] The thermoplastic resin of the present invention preferably contains more than 50 mol%, more preferably more than 60 mol%, even more preferably more than 70 mol%, particularly preferably more than 80 mol%, or preferably more than 90 mol%. In addition, the thermoplastic resin of the present invention may be composed only of the structural unit represented by the general formula (1).

[0255] The thermoplastic resin of the present invention may contain one or more other structural units in addition to the structural unit represented by the general formula (1) (structural unit (1)). As the other structural unit, a fluorene derivative unit is preferred.

[0256] Specifically, the thermoplastic resin of the present invention preferably further contains at least one of the structural units represented by the general formulae (3) and (4).

[0257]

[0258] (R'1~R' in formula (3) 20each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms,

[0259] Y is an alkylene group having 1 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0260] c and d are integers from 1 to 10 respectively.)

[0261] In the above general formula (3), R'1 to R" 20 Each of them is preferably a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms, and more preferably hydrogen.

[0262] In the above general formula (3), Y is preferably an alkylene group having 2 to 4 carbon atoms, a cycloalkylene group having 5 to 8 carbon atoms, or an arylene group having 6 to 14 carbon atoms, more preferably an alkylene group having 2 or 3 carbon atoms, a cycloalkylene group having 5 to 6 carbon atoms, or an arylene group having 6 to 10 carbon atoms, and particularly preferably an alkylene group having 2 or 3 carbon atoms.

[0263] In addition, c and d in the general formula (3) are each preferably an integer of 1 to 6, more preferably 1 to 4, and particularly preferably 2 or 3.

[0264]

[0265] (R"1~R" in formula (4) 16 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms,

[0266] Z is an alkylene group having 1 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0267] e and f are integers from 1 to 10 respectively.)

[0268] In the above general formula (4), R1 to R 16 Each of them is preferably a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or an aralkyl group having 7 to 12 carbon atoms, and more preferably hydrogen or an aryl group having 6 to 10 carbon atoms.

[0269] Z in the above general formula (4) is preferably an alkylene group having 2 to 4 carbon atoms, a cycloalkylene group having 5 to 8 carbon atoms, or an arylene group having 6 to 14 carbon atoms, more preferably an alkylene group having 2 or 3 carbon atoms, a cycloalkylene group having 5 to 6 carbon atoms, or an arylene group having 6 to 10 carbon atoms, and particularly preferably an alkylene group having 2 or 3 carbon atoms.

[0270] In addition, e and f in the general formula (4) are each preferably an integer of 1 to 6, more preferably 1 to 4, and particularly preferably 2 or 3.

[0271] The thermoplastic resin of the present invention preferably contains the structural unit (1) and, as the structural unit represented by the above-mentioned general formula (3) or (4), further contains at least one structural unit represented by the following general formula (5).

[0272]

[0273] That is, the thermoplastic resin of the present invention preferably contains, together with the structural unit (1), at least any one of a structural unit derived from BNEF (9,9-bis(6-(2-hydroxyethoxy)naphth-2-yl)fluorene) represented by the above general formula (5), a structural unit derived from BNE (2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthyl), and a structural unit derived from BPPEF (9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene).

[0274] The thermoplastic resin of the present invention may contain 20 to 80 mol% of structural units other than the structural unit (1), preferably the structural units represented by the general formulae (3) and (4), for example, 25 to 75 mol%. The thermoplastic resin may contain 30 to 70 mol%, 35 to 65 mol%, or 40 to 60 mol% of the structural units represented by the general formulae (3) and (4), for example.

[0275] That is, the molar ratio of the structural unit (1) to the structural unit (3) represented by the general formula (3) in the thermoplastic resin composition of the present invention is, for example, 4:1 to 1:4 or 7:3 to 3:7. The molar ratio may also be 65:35 to 35:65, 3:2 to 2:3 or 1:1. However, since the thermoplastic resin composition preferably contains more than 50 mol% of the structural unit (1) as described above, specific preferred examples of the molar ratio of the structural unit (1) to the structural unit (3) are 4:1 to 1:1, 7:3 to 1:1, 65:35 to 1:1 and 3:2 to 1:1.

[0276] The molar ratio of the structural unit (1) to the structural unit (4) represented by the general formula (4) is also the same as the molar ratio of the structural unit (1) to the structural unit (3).

[0277] The thermoplastic resin of the present invention may include any structure of random, block and alternating copolymer structures. Furthermore, in the thermoplastic resin of the present invention, not all of the above-mentioned structural unit (1), structural unit (3) and structural unit (4) may be included in the same polymer molecule. That is, as long as the above-mentioned structural unit is included in a plurality of polymer molecules as a whole, the thermoplastic resin of the present invention may also be a blended resin. For example, as a thermoplastic resin containing all of the above-mentioned structural unit (1), structural unit (3) and structural unit (4), it may be a copolymer containing all of the structural units (1), (3) and (4), or a mixture of a homopolymer or copolymer containing the structural unit (1), a homopolymer or copolymer containing the structural unit (2) and a homopolymer or copolymer containing the structural unit (4), or a blended resin of a copolymer containing the structural units (1) and (3) and a copolymer containing the structural units (1) and (4).

[0278] The thermoplastic resin of the present invention may be blended with other resins to produce a molded article. For example, when the thermoplastic resin is any of polyester, polyester carbonate, and polycarbonate, examples of the other resin include polyamide, polyacetal, polycarbonate of a type different from the thermoplastic resin, modified polyphenylene ether, polyethylene terephthalate, and polybutylene terephthalate.

[0279] Furthermore, it is preferred to add an antioxidant, a mold release agent, a processing stabilizer, an ultraviolet absorber, a fluidity modifier, a crystal nucleating agent, a reinforcing agent, a dye, an antistatic agent, an antibacterial agent, or the like to the thermoplastic resin composition of the present invention.

[0280] Examples of the antioxidant include triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, The antioxidant may be butyl-4-hydroxybenzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid amide), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, and 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane. Among these, pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is preferred. The content of the antioxidant in the thermoplastic resin composition is preferably 0.001 to 0.3 parts by weight relative to 100 parts by weight of the thermoplastic resin.

[0281] As a release agent, it is preferred that 90% by weight or more of the release agent is composed of an ester of an alcohol and a fatty acid. As the ester of an alcohol and a fatty acid, specifically, there can be mentioned an ester of a monohydric alcohol and a fatty acid, and a partial ester or full ester of a polyhydric alcohol and a fatty acid. As the ester of the monohydric alcohol and a fatty acid, an ester of a monohydric alcohol having 1 to 20 carbon atoms and a saturated fatty acid having 10 to 30 carbon atoms is preferred. In addition, as a partial ester or full ester of a polyhydric alcohol and a fatty acid, a partial ester or full ester of a polyhydric alcohol having 1 to 25 carbon atoms and a saturated fatty acid having 10 to 30 carbon atoms is preferred.

[0282] Specifically, as the ester of monohydric alcohol and saturated fatty acid, octadecyl stearate, palmityl palmitate, butyl stearate, methyl laurate, isopropyl palmitate, etc. can be cited. As the partial ester or full ester of polyhydric alcohol and saturated fatty acid, stearic acid monoglyceride, stearic acid diglyceride, stearic acid triglyceride, stearic acid monosorbitol ester, behenic acid monoglyceride, capric acid monoglyceride, lauric acid monoglyceride, pentaerythritol monostearate, pentaerythritol tetrastearate, pentaerythritol tetrapelargonate, propylene glycol monostearate, biphenyl biphenyl ester, sorbitan monostearate, 2-ethylhexyl stearate, dipentaerythritol hexastearate, etc., full ester or partial ester of dipentaerythritol, etc. can be cited. Among these, stearic acid monoglyceride and lauric acid monoglyceride are particularly preferred. The content of these release agents is preferably in the range of 0.005 to 2.0 parts by weight, more preferably 0.01 to 0.6 parts by weight, and even more preferably 0.02 to 0.5 parts by weight, based on 100 parts by weight of the thermoplastic resin.

[0283] Examples of the processing stabilizer include phosphorus-based processing heat stabilizers, sulfur-based processing heat stabilizers, etc. Examples of the phosphorus-based processing heat stabilizer include phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid, and esters thereof. Specific examples thereof include triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,6-di-tert-butylphenyl)phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, bis(nonylphenyl)pentaerythritol diphosphite, and bis(2,4-dicumylphenyl)pentaerythritol diphosphite. , bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, tributyl phosphate, triethyl phosphate, trimethyl phosphate, triphenyl phosphate, diphenyl mono-o-biphenyl phosphate, dibutyl phosphate, dioctyl phosphate, diisopropyl phosphate, dimethyl phenylphosphonate, diethyl phenylphosphonate, dipropyl phenylphosphonate, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite, bis(2,4-di-tert-butylphenyl)-4-phenyl-phenyl phosphonite and bis(2,4-di-tert-butylphenyl)-3-phenyl-phenyl phosphonite, etc. Among these, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite is preferred. The content of the phosphorus-based processing heat stabilizer in the thermoplastic resin composition is preferably 0.001 to 0.2 parts by weight relative to 100 parts by weight of the thermoplastic resin.

[0284] Examples of the sulfur-based processing heat stabilizer include pentaerythritol-tetrakis (3-lauryl thiopropionate), pentaerythritol-tetrakis (3-myristyl thiopropionate), pentaerythritol-tetrakis (3-stearyl thiopropionate), dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, and distearyl-3,3'-thiodipropionate. The content of the sulfur-based processing heat stabilizer in the thermoplastic resin composition is preferably 0.001 to 0.2 parts by weight relative to 100 parts by weight of the thermoplastic resin.

[0285] As the ultraviolet absorber, at least one ultraviolet absorber selected from benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, triazine ultraviolet absorbers, cyclic iminoester ultraviolet absorbers and cyanoacrylate ultraviolet absorbers is preferred. That is, any one of the ultraviolet absorbers listed below may be used alone, or two or more may be used in combination.

[0286] Examples of the benzotriazole ultraviolet absorber include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, and 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole. 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octyloxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazin-4-one), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole, etc.

[0287] Examples of the benzophenone-based ultraviolet absorber include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid hydrate, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodium sulfonatebenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.

[0288] Examples of the triazine-based ultraviolet absorber include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol and 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-[(octyl)oxy]-phenol.

[0289] Examples of the cyclic urethane ultraviolet absorber include 2,2'-bis(3,1-benzoxazin-4-one), 2,2'-p-phenylenebis(3,1-benzoxazin-4-one), 2,2'-m-phenylenebis(3,1-benzoxazin-4-one), 2,2'-(4,4'-diphenylene)bis(3,1-benzoxazin-4-one), 2,2'-(2,6-naphthylene)bis(3 ,1-benzoxazine-4-one), 2,2'-(1,5-naphthalene)bis(3,1-benzoxazine-4-one), 2,2'-(2-methyl-p-phenylene)bis(3,1-benzoxazine-4-one), 2,2'-(2-nitro-p-phenylene)bis(3,1-benzoxazine-4-one) and 2,2'-(2-chloro-p-phenylene)bis(3,1-benzoxazine-4-one).

[0290] Examples of the cyanoacrylate-based ultraviolet absorber include 1,3-bis-[(2′-cyano-3′,3′-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.

[0291] The content of the ultraviolet absorber is preferably 0.01 to 3.0 parts by weight, more preferably 0.02 to 1.0 parts by weight, and even more preferably 0.05 to 0.8 parts by weight relative to 100 parts by weight of the thermoplastic resin. Within this range, the thermoplastic resin composition can be provided with sufficient weather resistance depending on the application.

[0292] In a thermoplastic resin composition, such as a polycarbonate resin composition, there are phenols generated during production and unreacted and residual carbonic acid diesters as impurities. The phenol content in the thermoplastic resin composition is preferably 0.1 to 3000 ppm, more preferably 0.1 to 2000 ppm, more preferably 1 to 1000 ppm, 1 to 800 ppm, 1 to 500 ppm or 1 to 300 ppm. In addition, the carbonic acid diester content in the thermoplastic resin composition is preferably 0.1 to 1000 ppm, more preferably 0.1 to 500 ppm, and particularly preferably 1 to 100 ppm. By adjusting the amount of phenol and carbonic acid diester contained in the thermoplastic resin composition, a resin having properties that meet the purpose can be obtained. The adjustment of the content of phenol and carbonic acid diester can be appropriately carried out by changing the conditions and equipment of polycondensation. In addition, it can also be adjusted by the conditions of the extrusion process after polycondensation.

[0293] When the content of phenol or carbonic acid diester exceeds the above range, there may be problems such as reduced strength of the obtained resin molded product and generation of odor. On the other hand, when the content of phenol or carbonic acid diester is below the above range, there is a concern that the plasticity of the resin when melted may be reduced.

[0294] (2) Properties of thermoplastic resins

[0295] The viscosity average molecular weight (Mv) of the thermoplastic resin of the present invention is preferably 8,000 to 20,000, more preferably 9,000 to 15,000, and even more preferably 10,000 to 14,000.

[0296] When the Mv value is less than 8,000, the molded product may become brittle. When the Mv value is greater than 20,000, the melt viscosity becomes high, making it difficult to remove the produced resin, and the fluidity may deteriorate, making it difficult to perform injection molding in a molten state.

[0297] The refractive index (nD) of the thermoplastic resin of the present invention at 23°C and a wavelength of 589nm is preferably 1.635 or more, more preferably 1.645 or more, even more preferably 1.655 or more, particularly preferably 1.665 or more, or greater than these values. For example, the refractive index of the thermoplastic resin of the present invention is preferably 1.640 to 1.710, more preferably 1.645 to 1.700, even more preferably 1.650 to 1.697, and particularly preferably 1.655 to 1.695. The thermoplastic resin of the present invention has a high refractive index (nD) and is suitable for optical lens materials. The refractive index can be measured by using an Abbe refractometer for a film with a thickness of 0.1 mm according to the method of JIS-K-7142.

[0298] The Abbe number (ν) of the thermoplastic resin of the present invention is preferably 24 or less, more preferably 22 or less, and still more preferably 20 or less. The Abbe number can be calculated from the refractive index at wavelengths of 486 nm, 589 nm, and 656 nm at 23° C. by the following formula.

[0299] ν=(nD-1) / (nF-nC)

[0300] nD: refractive index at a wavelength of 589nm

[0301] nC: refractive index at a wavelength of 656nm

[0302] nF: refractive index at a wavelength of 486nm

[0303] Considering the use for injection molding, the preferred glass transition temperature (Tg) of the thermoplastic resin of the present invention is 90 to 185°C, more preferably 95 to 180°C, and even more preferably 100 to 175°C. When Tg is lower than 90°C, the use temperature range may be narrowed. In addition, when it exceeds 185°C, the melting temperature of the resin becomes high, and there is a concern that the resin is easily decomposed and colored. When the glass transition temperature of the resin is too high, the difference between the mold temperature and the glass transition temperature of the resin becomes large when using a conventional mold temperature controller. Therefore, in applications that require strict surface accuracy for products, it may be difficult to use resins with too high a glass transition temperature. In addition, from the viewpoint of molding fluidity and molding heat resistance, the lower limit of Tg is preferably 130°C, more preferably 135°C, and the upper limit of Tg is preferably 185°C, more preferably 175°C.

[0304] The total light transmittance of the optical molded body obtained using the thermoplastic resin of the present invention is preferably 85% or more, more preferably 87% or more, and particularly preferably 88% or more. When the total light transmittance is 85% or more, it is comparable to bisphenol A polycarbonate resin and the like.

[0305] The thermoplastic resin of the present invention has high resistance to moisture and heat. Resistance to moisture and heat can be evaluated by conducting a "PCT test" (pressure cooker test) on an optical molded body obtained using the thermoplastic resin and measuring the total light transmittance of the optical molded body after the test. The PCT test can be performed by maintaining an injection molded body with a diameter of 50 mm and a thickness of 3 mm under conditions of 120°C, 0.2 MPa, 100% RH, and 20 hours. The total light transmittance of the thermoplastic resin of the present invention after the PCT test is 60% or more, preferably 70% or more, more preferably 75% or more, even more preferably 80% or more, and particularly preferably 85% or more. When the total light transmittance is 60% or more, it can be said that it has high resistance to moisture and heat relative to existing thermoplastic resins.

[0306] The b value indicating the hue of the thermoplastic resin of the present invention is preferably not more than 5. A smaller b value indicates less yellowishness and better hue.

[0307] (3) Method for producing thermoplastic resin

[0308] When the thermoplastic resin having the structural unit represented by the general formula (1) is a polycarbonate resin, the production method thereof includes, for example, the step of melt-polycondensing a dihydroxy compound represented by the following general formula (6) and a carbonic acid diester.

[0309]

[0310] (In the general formula (6), R1 and R2 each independently represent a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, a monocyclic or polycyclic aryl group having 6 to 36 carbon atoms, a monocyclic or polycyclic heteroaryl group having 5 to 36 ring atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms, wherein in the above heteroaryl group, 1, 2, 3 or 4 of the ring atoms are selected from nitrogen, sulfur and oxygen, and the other ring atoms are carbon,

[0311] Wherein, R1 and R2 are not all hydrogen,

[0312] X is an alkylene group having 1 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0313] The above alkylene group and the above cycloalkylene group may be substituted with a benzene ring, and a and b are integers of 1 to 10.

[0314] That is, use the compound shown in the above-mentioned general formula (6) as dihydroxy component, make it and carbonate precursor material reaction such as carbonic acid diester, can manufacture polycarbonate resin.Specifically, the compound shown in the general formula (6) and carbonate precursor materials such as carbonic acid diester in the presence of basic compound catalyst or transesterification catalyst or containing its both sides of mixed catalyst, or under the situation of catalyst-free, can react and manufacture by melt polycondensation method.

[0315] Furthermore, polyester carbonate resin and polyester resin can also be obtained by using the dihydroxy compound represented by the above general formula (6) as a raw material (monomer).

[0316] The polyester carbonate resin or polyester resin can be produced, for example, by subjecting the dihydroxy compound represented by the general formula (6) to melt polycondensation with at least one of carboxylic acid, carboxylic acid monoester and carboxylic acid diester.

[0317] For example, specific examples of carboxylic acids, carboxylic acid monoesters and carboxylic acid diesters include dicarboxylic acid, monocarboxylic acid monoesters and diesters of 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl (BINL-2EO), 9,9-fluorene-dipropionic acid, and 9,9-fluorene-dipropionic acid methyl ester (FDPM) as a monoester and diester of 9,9-fluorene-dipropionic acid.

[0318] Specific examples of carboxylic acids, carboxylic acid monoesters and carboxylic acid diesters include 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-1-yl)-1,1'-binaphthyl (DNBINOL-2EO), 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-2-yl)-1,1'-binaphthyl (2DNBINOL-2EO), 2,2'-bis(2-hydroxyethoxy)-6,6'-di(phenanthrene-9-yl)-1,1'-binaphthyl (9DPNBINO dicarboxylic acids, monocarboxylic acid monoesters, diesters, etc. of 6,6'-di-(3-cyanophenyl)-2,2'-bis-(2-hydroxyethoxy)-1,1'-binaphthyl (CN-BNA), 6,6'-di-(dibenzo[b,d]furan-4-yl)-2,2'-bis-(2-hydroxyethoxy)-1,1'-binaphthyl (FUR-BNA), and 6,6'-di-(3-cyanophenyl)-2,2'-bis-(2-hydroxyethoxy)-1,1'-binaphthyl (CN-BNA).

[0319] Examples of the compound of the general formula (6) include 2,2'-bis(hydroxy(poly)alkoxy)-diaryl-1,1'-binaphthyls and 2,2'-bis(hydroxy(poly)alkoxy)-dinaphthyl-1,1'-binaphthyls. For example, 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphth-1-yl)-1,1'-binaphthyl, 2,2'-bis(2-hydroxymethoxy)-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-bis(2-hydroxymethoxy)-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-bis(2-hydroxymethoxy)-6,6'-di(naphth-1-yl)-1,1'-binaphthyl, 2,2'-bis(2-hydroxypropoxy)-6,6'-diphenyl-1,1'-binaphthyl, and 2,2'-bis(2-hydroxypropoxy)-6,6'-di(naphth-1-yl)-1,1'-binaphthyl are preferred. These may be used alone or in combination of two or more.

[0320] In addition, the monomer used to produce the thermoplastic resin may contain, together with the dihydroxy compound represented by the general formula (6), as an impurity, a dihydroxy compound in which the values ​​of a and b in the general formula (6) are both 0, or a dihydroxy compound in which either a or b in the general formula (6) is 0.

[0321] Thus, the total amount of dihydroxy compounds having different values ​​from at least any one of a and b in the above-mentioned general formula (6) is preferably contained in a monomer having the dihydroxy compound represented by the above-mentioned general formula (6) as the main component in an amount of 1000 ppm or less, more preferably 500 ppm or less, even more preferably 200 ppm or less, and particularly preferably 100 ppm or less, and the total amount of dihydroxy compounds having different values ​​from at least any one of a and b in the above-mentioned general formula (6) in the above-mentioned monomer is preferably 50 ppm or less, and more preferably 20 ppm or less.

[0322] The compound of general formula (6) can be produced by various synthesis methods. For example, as described in Japanese Patent Publication Nos. 2014-227387, 2014-227388, 2015-168658 and 2015-187098, it can be produced by: (a) a method of reacting 1,1'-binaphthol with ethylene glycol monotoluenesulfonate, (b) a method of reacting binaphthols with alkylene oxides, halogenated alkanols or alkylene carbonates, (c) a method of reacting 1,1'-binaphthol with ethylene carbonate, (d) a method of reacting 1,1'-binaphthol with ethylene carbonate, etc.

[0323] The monomer of general formula (6) may contain impurities that may have adverse effects on the properties of the thermoplastic resin, especially on the optical properties. In particular, the monomer of general formula (6) may contain one or more of the following by-products of general formulas (6a) and (6b) as impurities generated from its production process.

[0324]

[0325] In one embodiment, the monomer of the general formula (6) may contain the following by-products of the general formula (6c) as impurities generated in the production process in addition to or instead of the impurities of the formulae (6a) and (6b).

[0326] In formulae (6a), (6b) and (6c), substituents R1, R2 and X are the same as defined in the monomer of formula (6). In formulae (6a) and (6c), as in the monomer of formula (6), a is an integer in the range of 1 to 10, preferably an integer in the range of 1 to 4, and more preferably 1, 2 or 3. In formulae (6c), variables b, c and d are integers in the range of 1 to 10, preferably an integer in the range of 1 to 4, and more preferably 1, 2 or 3. In formulae (6a) and (6c), as in the monomer of formula (6), substituent X is preferably an alkylene group having 1 to 4 carbon atoms, and more preferably an ethylene group, i.e., 1,2-ethylenediyl or -CH2CH2-.

[0327] In formulae (6a), (6b) and (6c), as in the monomer of formula (6), the substituents R1 and R2 are preferably monocyclic or polycyclic aromatic groups having 6 to 36 carbon atoms, or monocyclic or polycyclic heteroaromatic groups having 6 to 36 ring atoms, more preferably monocyclic or polycyclic aromatic groups having 6 to 20 carbon atoms, even more preferably aromatic groups having 6 to 14 carbon atoms, and particularly preferably selected from phenyl, 1-naphthyl, 2-naphthyl, 9-phenanthrenyl, 4-dibenzo[b,d]furanyl and 4-dibenzo[b,d]thienyl.

[0328] The total weight of the impurities of formula (6a) and (6b) in the monomer of formula (6) used in the method of the present invention is preferably not more than 5000 ppm based on 1 part by weight of the monomer of formula (6). In particular, the total weight of the impurities of formula (6a) and (6b) is preferably not more than 4000 ppm, more preferably not more than 3000 ppm, and even more preferably not more than 2000 ppm based on 1 part by weight of the monomer of formula (6). It is particularly preferred that the weight of each impurity of formula (6a) and (6b) is not more than 2000 ppm, more preferably not more than 1500 ppm, and even more preferably not more than 1000 ppm based on 1 part by weight of the monomer of formula (6). If present, the amount of the impurity (6c) is not more than 2000 ppm, and is usually not more than 1500 ppm, based on 1 part by weight of the monomer of formula (6).

[0329] In a specific embodiment of the invention regarding the thermoplastic resin produced by the method of the present invention, the variables (a) and (b) of the monomer of formula (6) are 1, and this is hereinafter referred to as monomer (6-1). Monomer (6-1) may contain one or more by-products of the following formulas (6a-1), (6-2) and (6b), and may contain (6c-1) as an impurity as appropriate.

[0330]

[0331] In formula (6-1), (6a-1), (6-2) and (6c-1), the substituent X is preferably an alkylene group having 1 to 4 carbon atoms, and more preferably an ethylene group, that is, 1,2-ethanediyl or -CH2CH2-. In formula (6-2), the variable e is a variable defined as the variable a, and may be 2 or 3 in particular. In formulae (6-1), (6a-1), (6-2), (6-b) and (6c-1), the substituents R1 and R2 are preferably monocyclic or polycyclic aryl groups having 6 to 36 carbon atoms, or monocyclic or polycyclic heteroaryl groups having 6 to 36 ring atoms, more preferably monocyclic or polycyclic aryl groups having 6 to 20 carbon atoms, even more preferably aryl groups having 6 to 14 carbon atoms, and particularly preferably selected from phenyl, 1-naphthyl, 2-naphthyl, 9-phenanthrenyl, 4-dibenzo[b,d]furanyl and 4-dibenzo[b,d]thienyl.

[0332] The total weight of the impurities of formula (6a-1), (6-2) and (6b) in the monomer of formula (6-1) used in the method of the present invention is preferably not more than 5000 ppm based on 1 part by weight of the monomer of formula (6). In particular, the total weight of the impurities of formula (6a-1), (6-2) and (6b) is preferably not more than 4000 ppm, more preferably not more than 3000 ppm, and even more preferably not more than 2000 ppm based on 1 part by weight of the monomer of formula (6-1). In particular, the weight of each impurity of formula (6a-1), (6-2) and (6b) is preferably not more than 2000 ppm, more preferably not more than 1500 ppm, and even more preferably not more than 1000 ppm based on 1 part by weight of the monomer of formula (6-1). If present, the amount of the impurity (6c-1) is not more than 2000 ppm, and is usually not more than 1500 ppm, based on 1 part by weight of the monomer of formula (6-1).

[0333] In a specific embodiment of the invention regarding the thermoplastic resin produced by the method of the present invention, the monomer of formula (6) is 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl, that is, in formula (6), variables (a) and (b) are both 1, X is 1,2-ethanediyl, and substituents of R1 and R2 are both phenyl. Here and elsewhere in the present specification, 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl may be abbreviated as 6,6'-DPBHBNA.

[0334] 6,6'-DPBHBNA may contain one or more impurities in which the substituent X in the above formulas (6a-1), (6-2), (6b) and (6c-1) is 1,2-ethanediyl, all R1 and R2 substituents are phenyl, and the variable e in formula (6-2) is 2 or 3, especially 2.

[0335] In formula (6a-1), the chemical name of the compound in which the substituent X is 1,2-ethanediyl and the substituents of R1 and R2 are both phenyl is 2-(2-hydroxyethoxy)-2'-hydroxy-6,6'-diphenyl-1,1'-binaphthyl.

[0336] In formula (6-2), the chemical name of the compound in which the substituent X is 1,2-ethanediyl, e is 2, and the substituents of R1 and R2 are both phenyl is 2-(2-hydroxyethoxy)-2'-(2-(2-hydroxyethoxy)-ethoxy)-6,6'-diphenyl-1,1'-binaphthyl (6,6'-diphenyl-2-(2-hydroxyethoxy)-2'-(2-(2-hydroxyethoxy)-ethoxy)-1,1'-binaphthyl).

[0337] In the formula (6b), the chemical name of the compound in which both R1 and R2 are phenyl groups is 2,2′-dihydroxy-6,6′-diphenyl-1,1′-binaphthyl.

[0338] In the formula (6c-1), the chemical name of the compound in which the substituent X is 1,2-ethanediyl and all the substituents of R1 and R2 are phenyl is bis[2-[[1-[2-(2-hydroxyethoxy)-6-phenyl-1-naphthyl]-6-phenyl-2-naphth yl]-oxy]-ethyl] carbonate.

[0339] In the 6,6'-DPBHBNA used in the method of the present invention, the total weight of impurities in which the substituent X is 1,2-ethanediyl and all R1 and R2 substituents are phenyl groups as impurities of formula (6a-1), (6-2) and (6b) is preferably not more than 5000 ppm based on 1 part by weight of 6,6'-DPBHBNA. Thus, 6,6'-DPBHBNA containing a small amount of the above impurities is a novel substance, and therefore, it is also included in the present invention. In particular, the total weight of impurities in which the substituent X is 1,2-ethanediyl and all R1 and R2 substituents are phenyl groups in formula (6a-1), (6-2) and (6b) is preferably not more than 4000 ppm, more preferably not more than 3000 ppm, and even more preferably not more than 2000 ppm, based on 1 part by weight of 6,6'-DPBHBNA. In particular, the weight of each impurity in which the substituent X is 1,2-ethanediyl and all R1 and R2 substituents are phenyl groups is preferably 2000 ppm or less, more preferably 1500 ppm or less, and further preferably 1000 ppm or less, based on 1 part by weight of the monomer of 6,6'-DPBHBNA in formula (6a-1), (6-2) and (6b). If present, the amount of impurities in which the substituent X is 1,2-ethanediyl and all R1 and R2 substituents are phenyl groups in formula (6c-1) is usually not more than 2000 ppm, and is generally 1500 ppm or less, based on 1 part by weight of the monomer of 6,6'-DPBHBNA.

[0340] 6,6'-DPBHBNA has a tendency to form solvates with certain organic solvents, particularly with aliphatic ketones such as methanol, toluene, anisole, xylene, chlorobenzene, tetrahydrofuran, 2-butanone also known as methyl ethyl ketone (MEK), and 4-methyl-2-pentanone also known as methyl isobutyl ketone (MIBK). In these solvents, the amount of each organic solvent is generally in the range of 0.3 to 1.5 moles per 1 mole of 6,6'-DPBHBNA. Here and elsewhere in the specification of this application, the term solvate is understood to mean a crystalline form containing a solvent in the crystal lattice of the crystalline form. These solvates are generally referred to as "pseudo polymorphisms" to distinguish them from polymorphisms that are substantially free of solvent. In the crystalline solvates of 6,6'-DPBHBNA, the amount of solvent need not be a stoichiometric amount relative to the amount of 6,6'-DPBHBNA, but may vary. Although not being bound by theory, the solvent molecules present in the crystalline solvate of 6,6'-DPBHBNA generally fill the gaps or holes in the crystal lattice formed by the molecules of 6,6'-DPBHBNA.

[0341] Among the above solvents, methanol, toluene and methyl ethyl ketone are particularly preferred. These crystalline solvates formed with 6,6'-DPBHBNA are usually obtained in the form of compact crystals with a low aspect ratio. Such crystals tend to have high purity 6,6'-DPBHBNA without adhering to the mother liquid. Therefore, these crystalline solvates also form part of the present invention.

[0342] The solvate of 6,6'-DPBHBNA with an organic solvent selected from methanol, toluene and methyl ethyl ketone can improve the purity of 6,6'-DPBHBNA to more than 99%, particularly at least 99.5% or more, and further 99.7% or more.

[0343] In particular, unless otherwise indicated, a purity of more than 99% here or in the context of solid forms of 6,6'-DPBHBNA means that the total amount of organic impurities, i.e., organic compounds other than 6,6'-DPBHBNA and optionally the solvent, contained in the respective solid form of 6,6'-DPBHBNA is less than 1% by weight. Similarly, a purity of at least 99.5% or at least 99.7% means that the total amount of organic impurities, i.e., organic compounds other than 6,6'-DPBHBNA and optionally the solvent, contained in the respective solid form of 6,6'-DPBHBNA is at most 0.5% by weight or at most 0.3% by weight.

[0344] In the crystalline solvate of 6,6'-DPBHBNA in the present invention, the total amount of impurities having a 1,1'-binaphthyl moiety selected from 2-(2-hydroxyethoxy)-2'-hydroxy-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-dihydroxy-6,6'-diphenyl-1,1'-binaphthyl and 2-(2-hydroxyethoxy)-2'-(2-(2-hydroxyethoxy)-ethoxy)-6,6'-diphenyl-1,1'-binaphthyl is generally at most 5000 ppm (0.50 wt%) or less, preferably at most 4000 ppm (0.40 wt%) or less, particularly preferably at most 3000 ppm (0.30 wt%) or less, and further preferably at most 2000 ppm (0.20 wt%) or less, based on 1 part by weight of 6,6'-DPBHBNA contained in the crystal of the crystalline solvate. It is particularly preferred that the weight of each of these impurities is 2000 ppm or less, more preferably 1500 ppm or less, and even more preferably 1000 ppm or less, based on 1 part by weight of 6,6'-DPBHBNA. If each solvate contains bis[2-[[1-[2-(2-hydroxyethoxy)-6-phenyl-1-naphthyl]-6-phenyl-2-naphthyl]-oxy]-ethyl] carbonate, its amount is usually not more than 2000 ppm, and may be 1500 ppm or less, based on 1 part by weight of 6,6'-DPBHBNA.

[0345] In the crystalline solvate of the present invention, the amount of the solvent may vary, but is usually in the range of 0.3 to 1.5 mol, particularly in the range of 0.3 to 1.2 mol, per 1 mol of 6,6'-DPBHBNA.

[0346] A specific embodiment of the present invention relates to a crystalline solvate of 6,6′-DPBHBNA and methanol, which is hereinafter referred to as a methanol solvate.

[0347] In the methanol solvate, the amount of methanol is usually in the range of 0.3 to 1.5 mol, particularly in the range of 0.4 to 1.2 mol, and further in the range of 0.6 to 1.1 mol per 1 mol of 6,6'-DPBHBNA.

[0348] In the X-ray powder diffraction pattern recorded by irradiation with Cu Kα1 rays at 22°C, the methanol solvate generally shows the following three reflection peaks as 2θ values, namely, 13.0±0.2°, 14.9±0.2° and 21.5±0.2°;

[0349] showing as 2θ values ​​at least 3, in particular at least 5, at least 7 or all of the following reflection peaks: 6.2±0.2°, 9.0±0.2°, 10.6±0.2°, 16.9±0.2°, 18.2±0.2°, 18.5±0.2°, 19.2±0.2°, 19.6±0.2°, 20.9±0.2°, 22.7±0.2°, 24.3±0.2°, 24.9±0.2°, 26.2±0.2°, 28.7±0.2° and 30.5±0.2°; and

[0350] Arbitrarily, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 reflection peaks are shown as 2θ values ​​among the following: 8.4±0.2°, 11.8±0.2°, 12.5±0.2°, 16.0±0.2°, 17.7±0.2°, 22.1±0.2°, 26.6±0.2°, 27.7±0.2°, 31.6±0.2° and 32.5±0.2°.

[0351] Methanol solvates can also be characterized by endothermic peaks that represent their decomposition. When methanol solvates are analyzed using a differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, methanol solvates generally show an endothermic peak with a starting point in the range of 97 to 101°C, and the maximum value of the peak is in the range of 108 to 115°C. In addition, the reaction point is generally in the range of 103 to 110°C. The reaction point is understood to be the inflection point on the lower side of the endothermic peak in the DSC curve. The above temperature can vary within the above range depending on the content of methanol, and the temperature rises when the content of methanol is high.

[0352] The methanol solvate can be obtained by crystallization of 6,6'-DPBHBNA from a high-temperature methanol solution of 6,6'-DPBHBNA or a solution of a mixture of high-temperature methanol and toluene of 6,6'-DPBHBNA. In order to obtain the desired methanol solvate, the 6,6'-DPBHBNA to be crystallized has a purity of at least 97% by weight with respect to organic matter other than the solvent. The 6,6'-DPBHBNA having a purity of at least 97% by weight is preferably dissolved in high-temperature methanol or a mixture of high-temperature methanol and toluene. In the mixture, the content of methanol is preferably at least 50 w / w% and less than 90 w / w% based on the total weight of the solvent (mixture), that is, the volume ratio of methanol to toluene is 1:1 to 9:1, particularly preferably 6:4 to 8:2, for example 7:3. Typically, the temperature of the high temperature solution of 6,6'-DPBHBNA is at least 45°C, and can be as high as reflux temperature, especially when the content of methanol is high. The concentration of 6,6'-DPBHBNA in the high temperature solution can vary depending on the amount of methanol used for crystallization. When the amount of methanol is large, a low concentration of 6,6'-DPBHBNA is generally allowed. The concentration of 6,6'-DPBHBNA is generally not more than 30% by weight, and is generally 2 to 25% by weight. Crystallization of the methanol solvate from the high temperature solution is generally achieved by cooling the high temperature solution to a temperature below 40°C, for example, a temperature in the range of -10 to below 40°C, and -5 to 30°C. Seed crystals can be added at a temperature below 40°C, for example, in the range of -5 to 30°C. The amount of seed crystals is generally 0.05 to 2% by weight, particularly 0.1 to 1% by weight, based on the amount of 6,6'-DPBHBNA crystallized as a methanol solvate. The time for completing the crystallization of the methanol solvate may vary depending on the concentration of 6,6'-DPBHBNA and the temperature applied, and is typically in the range of 4 to 24 hours. Crystallization of the methanol solvate may also be achieved by concentrating the high temperature solution, or by a combination of concentrating and cooling. Concentration of the solution may be achieved by distilling off a portion of the solvent.

[0353] Methanol solvates can be obtained by crystallization in the form of compact crystals with a low aspect ratio. The aspect ratio of methanol solvates is usually less than 5, and more specifically in the range of 1 to 4. The size of the crystals is usually in the range of 5 to 200 μm. Among them, the size of the crystals in the solvate form is the same as that of the non-solvate crystal form, and can be obtained by visual inspection using an optical microscope magnified 100 times. The size range given here is the longest dimension of the crystal.

[0354] The crystallization of the methanol solvate tends not to enclose a significant amount of mother liquor. Therefore, the crystalline solvate of 6,6'-DPBHBNA with methanol can increase the purity of 6,6'-DPBHBNA to at least 99%, and further to at least 99.5% or more, and further to 99.7% or more. This means that as mentioned above, the total amount of impurities other than methanol in the methanol solvate does not exceed 1% by weight, in particular 0.5% by weight, and further does not exceed 0.3% by weight.

[0355] On the other hand, the above-mentioned methanol solvate crystals are substances that can be very easily decomposed by long-term drying. Although it is preferably dried at a high temperature, it can be decomposed at a temperature lower than the melting point of the methanol solvate. Therefore, a new crystalline polymorph of 6,6'-DPBHBNA can be obtained, which is a crystalline polymorph that is basically free of organic solvents and cannot be obtained by crystallization from a solution of 6,6'-DPBHBNA. Hereinafter, this crystalline polymorph is referred to as crystalline form A of 6,6'-DPBHBNA or simply form A. Since form A does not contain a significant amount of solvent, it is particularly useful in the manufacture of the thermoplastic resin of the present invention.

[0356] In Form A, the organic solvent is usually contained in an amount of less than 0.1 mol, and in particular, less than 0.05 mol, per mol of 6,6'-DPBHBNA. The total amount of organic solvent in Form A is usually less than 1 wt%. In addition, the amount of methanol in Form A is usually less than 0.1 wt%.

[0357] In the X-ray powder diffraction pattern recorded by irradiation with Cu Kα1 rays at 22°C, Form A generally shows the following six reflection peaks as 2θ values, namely, 13.0±0.2°, 14.9±0.2°, 20.9±0.2°, 21.4±0.2°, 21.5±0.2° and 23.7±0.2°;

[0358] showing as 2θ values ​​at least 5, in particular at least 7, at least 9 or all reflection peaks among the following: 6.5±0.2°, 8.6±0.2°, 11.0±0.2°, 13.2±0.2°, 14.9±0.2°, 16.2±0.2°, 17.3±0.2°, 17.8±0.2°, 18.4±0.2° and 19.0±0.2°; and

[0359] Optionally, 1, 2, 3, 4, 5, 6, 7, 8 or 9 reflection peaks among the following are shown as 2θ values: 9.4±0.2°, 10.4±0.2°, 15.5±0.2°, 22.5±0.2°, 22.9±0.2°, 24.5±0.2°, 25.9±0.2°, 27.8±0.2° and 30.8±0.2°.

[0360] Form A can also be characterized by an endothermic peak indicating its dissolution. When Form A is analyzed by DSC recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, Form A generally shows an endothermic peak with an onset in the range of 112 to 114°C, and a peak maximum in the range of 124 to 126°C. Furthermore, the reaction point is generally in the range of 117 to 120°C.

[0361] Form A can be obtained by decomposition of a methanol solvate as a compact crystalline form with a low aspect ratio. The aspect ratio of the crystals of Form A is generally less than 5, and more particularly in the range of 1 to 4. The crystal size of Form A is generally in the range of 5 to 200 μm, and the crystal size of the solvate form can be obtained by visual inspection by magnifying 100 times with an optical microscope. The decomposition of the methanol solvate generally occurs by long-term drying, and although it is preferably dried at a high temperature, decomposition can occur at a temperature lower than the melting point of the methanol solvate. Typically, drying is performed until the amount of methanol in the obtained 6,6'-DPBHBNA is less than 0.1% by weight. Drying is performed at a temperature range of 30°C to 95°C, and in particular can be performed at 30°C to 70°C.

[0362] The crystals of form A of 6,6'-DPBHBNA generally have a purity of at least 99%, further at least 99.5% or more, and further at least 99.7%. As described above, this means that the total amount of impurities other than the solvent in form A does not exceed 1% by weight, particularly not more than 0.5% by weight, and further not more than 0.3% by weight. In particular, in Form A, the total amount of impurities selected from 2-(2-hydroxyethoxy)-2'-hydroxy-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-dihydroxy-6,6'-diphenyl-1,1'-binaphthyl and 2-(2-hydroxyethoxy)-2'-(2-(2-hydroxyethoxy)-ethoxy)-6,6'-diphenyl-1,1'-binaphthyl is generally 5000 ppm or less, preferably 4000 ppm or less, particularly preferably 3000 ppm or less, and further preferably 2000 ppm or less, based on 1 part by weight of 6,6'-DPBHBNA contained in the crystal of Form A. In particular, the weight of each of these impurities is 2000 ppm or less, more preferably 1500 ppm or less, and further preferably 1000 ppm or less, based on 1 part by weight of 6,6'-DPBHBNA contained in the crystal of Form A. When Form A contains bis[2-[[1-[2-(2-hydroxyethoxy)-6-phenyl-1-naphthyl]-6-phenyl-2-naphthyl]-oxy]-ethyl] carbonate, its amount is usually not more than 2000 ppm and may be up to 1500 ppm or less based on 1 part by weight of 6,6'-DPBHBNA contained in the crystals of Form A.

[0363] In addition, a specific embodiment of the present invention relates to a crystalline 6,6'-DPBHBNA, which is a mixture of a crystalline methanol solvate and form A of 6,6'-DPBHBNA. The mixture is usually obtained by incomplete decomposition of the methanol solvate. The mixture is characterized by reflecting peaks of the X-ray powder diffraction pattern showing both the methanol solvate and form A. In particular, the mixture shows the following three reflection peaks as 2θ values ​​in the X-ray powder diffraction pattern recorded by irradiation with Cu Kα1 rays at 22°C, namely, 20.9±0.2°, 21.4±0.2° and 23.7±0.2°; and

[0364] The invention shows at least 3, in particular at least 5, at least 7, or at least 9 reflection peaks among the following 2θ values: 6.2±0.2°, 6.5±0.2°, 8.6±0.2°, 9.0±0.2°, 10.6±0.2°, 11.0±0.2°, 13.2±0.2°, 14.9±0.2°, 16.2±0.2°, 16.9±0.2°, 17.3±0. 2°, 17.8±0.2°, 18.2±0.2°, 18.4±0.2°, 18.5±0.2°, 19.0±0.2°, 19.2±0.2°, 19.6±0.2°, 20.9±0.2°, 22.7±0.2°, 24.3±0.2°, 24.9±0.2°, 26.2±0.2°, 28.7±0.2°, and 30.5±0.2°;

[0365] Optionally, other reflection peaks observed in the methanol solvate and Form A described above may also be shown.

[0366] When the mixture of methanol solvate and Form A is analyzed by DSC recorded in accordance with ISO11357-3:2018 at a heating rate of 20 K / min, two endothermic peaks are generally observed. One peak has an onset in the range of 97-101°C and a peak maximum in the range of 108-115°C, and the second peak has an onset in the range of 112-114°C and a peak maximum in the range of 124-126°C.

[0367] The mixture of methanol solvate and Form A usually has a purity of at least 99%, more preferably at least 99.5% or more, and further preferably 99.7% or more. In the mixture, the total amount of impurities selected from 2-(2-hydroxyethoxy)-2'-hydroxy-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-dihydroxy-6,6'-diphenyl-1,1'-binaphthyl and 2-(2-hydroxyethoxy)-2'-(2-(2-hydroxyethoxy)-ethoxy)-6,6'-diphenyl-1,1'-binaphthyl is usually at most 5000 ppm or less, preferably at most 4000 ppm or less, particularly preferably at most 3000 ppm or less, and further preferably at most 2000 ppm or less, based on 1 part by weight of 6,6'-DPBHBNA contained in the mixture of methanol solvate and Form A.

[0368] Another specific embodiment of the present invention relates to a crystalline solvate of 6,6'-DPBHBNA and toluene, which is hereinafter referred to as a toluene solvate.

[0369] In the toluene solvate, the amount of toluene is generally in the range of 0.3 to 1.5 mol, particularly in the range of 0.3 to 1.2 mol, and further in the range of 0.3 to 0.5 mol per 1 mol of 6,6′-DPBHBNA.

[0370] In the X-ray powder diffraction pattern recorded by irradiation with Cu Kα1 rays at 22°C, the toluene solvate generally shows the following three reflection peaks as 2θ values, namely, 5.2±0.2°, 7.7±0.2° and 21.6±0.2°; and

[0371] The 2θ values ​​of the present invention are as follows: at least 3, in particular at least 5, at least 7 or all reflection peaks selected from the group consisting of 8.2±0.2°, 9.1±0.2°, 10.6±0.2°, 10.8±0.2°, 11.6±0.2°, 12.6±0.2°, 13.6±0.2°, 14.7±0.2°, 15.0±0.2°, 15.7±0.2°, 16.7±0.2°, 17. .1±0.2°, 18.0±0.2°, 18.5±0.2°, 19.4±0.2°, 19.9±0.2°, 20.8±0.2°, 21.0±0.2°, 22.2±0.2°, 22.7±0.2°, 24.1±0.2°, 25.0±0.2°, 25.7±0.2°, 26.5±0.2°, 27.1±0.2° and 27.6±0.2°.

[0372] Toluene solvates can also be characterized by an endothermic peak showing their decomposition. When the toluene solvates are analyzed by DSC recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, the toluene solvates generally show an endothermic peak with an onset in the range of 105 to 108°C, and the maximum value of the peak is in the range of 112 to 115°C. In addition, the reaction point is generally in the range of 109 to 112°C.

[0373] The toluene solvate can be obtained by crystallizing 6,6'-DPBHBNA from a high-temperature toluene solution of 6,6'-DPBHBNA, the toluene solution not containing more than 5% by weight of other organic solvents, in particular, not containing more than 1% by weight of methanol. In order to obtain the desired toluene solvate, the 6,6'-DPBHBNA to be crystallized has a purity of at least 97% by weight with respect to organic matter other than the solvent. Preferably, 6,6'-DPBHBNA having a purity of at least 97% by weight is dissolved in high-temperature toluene. Usually, the temperature of the high-temperature solution of 6,6'-DPBHBNA is at least 60°C, and can be as high as reflux temperature. The concentration of 6,6'-DPBHBNA in the high-temperature solution is usually not more than 50% by weight, and is usually 10 to 40% by weight. When the toluene solvate is crystallized from the high-temperature solution, it is usually achieved by cooling the high-temperature solution to a temperature below 50°C, for example, a temperature in the range of -10 to below 50°C, and -5 to 40°C. Seed crystals can be added at a temperature below 50°C, for example, in the range of -5 to 40°C. The amount of seed crystals is usually 0.05 to 2% by weight, particularly 0.1 to 1% by weight, based on the amount of 6,6'-DPBHBNA crystallized as a toluene solvate. The time for completing the crystallization of the toluene solvate can vary depending on the concentration of 6,6'-DPBHBNA and the temperature applied, but is typically in the range of 4 to 24 hours. The crystallization of the toluene solvate can also be achieved by concentrating the high-temperature solution, or by a combination of concentration and cooling. The concentration of the solution can be achieved by distilling off part of the toluene.

[0374] Toluene solvate can be obtained by crystallization in the form of compact crystals with a low aspect ratio. The aspect ratio of the toluene solvate is usually less than 5, and more specifically in the range of 1 to 4. The size of the crystals is usually in the range of 5 to 300 μm. There is a tendency for the crystals of the toluene solvate not to enclose a significant amount of mother liquor. Therefore, the crystalline solvate of 6,6'-DPBHBNA and toluene can increase the purity of 6,6'-DPBHBNA to at least 99%, further to at least 99.5% or more, and further to 99.7% or more.

[0375] Another specific embodiment of the present invention relates to a crystalline solvate of 6,6′-DPBHBNA and methyl ethyl ketone (MEK), which is hereinafter referred to as MEK solvate.

[0376] In the MEK solvate, the amount of MEK is generally in the range of 0.3 to 1.5 mol, particularly in the range of 0.4 to 1.0 mol, and further in the range of 0.5 to 0.8 mol, per 1 mol of 6,6′-DPBHBNA.

[0377] In an X-ray powder diffraction pattern recorded by irradiation with Cu Kα1 rays at 22° C., a MEK solvate generally shows the following three reflection peaks as 2θ values, namely, 7.0±0.2°, 16.8±0.2°, and 23.4±0.2°; and

[0378] At least 3, in particular at least 5, at least 7 or all of the following reflection peaks are shown as 2θ values: 5.0±0.2°, 7.5±0.2°, 12.6±0.2°, 13.4±0.2°, 14.5±0.2°, 15.4±0.2°, 15.7±0.2°, 18.3±0.2°, 19.4±0.2°, 20.6±0.2°, 21.5±0.2°, 22.7±0.2°, 24.1±0.2°, 25.6±0.2°, 26.2±0.2°, 26.6±0.2° and 30.8±0.2°.

[0379] MEK solvates can also be characterized by an endothermic peak that indicates their decomposition. When MEK solvates are analyzed by DSC recorded in accordance with ISO 11357-3:2018 at a heating rate of 20K / min, MEK solvates generally show an endothermic peak with an onset in the range of 87 to 91°C, and a peak maximum in the range of 95 to 100°C. Furthermore, the reaction point is generally in the range of 94 to 98°C.

[0380] MEK solvate can be obtained by crystallizing 6,6'-DPBHBNA from a high-temperature MEK solution of 6,6'-DPBHBNA, wherein the MEK does not contain more than 5% by weight of other organic solvents, particularly, does not contain more than 0.5% by weight of methanol. In order to obtain the desired MEK solvate, the 6,6'-DPBHBNA to be crystallized has a purity of at least 97% by weight with respect to organic matter other than the solvent. It is preferred to dissolve 6,6'-DPBHBNA having a purity of at least 97% by weight in high-temperature MEK. Generally, the temperature of the high-temperature solution of 6,6'-DPBHBNA is at least 60°C, and can be as high as reflux temperature. The concentration of 6,6'-DPBHBNA in the high-temperature solution is generally not more than 50% by weight, and is generally 10 to 40% by weight. When crystallizing the MEK solvate from the high-temperature solution, it is generally achieved by cooling the high-temperature solution to a temperature below 50°C, for example, a temperature in the range of -10 to below 50°C, or -5 to 40°C. Seed crystals may be added at a temperature below 50°C, for example, in the range of -5 to 40°C. The amount of seed crystals is generally 0.05 to 2% by weight, particularly 0.1 to 1% by weight, based on the amount of 6,6'-DPBHBNA crystallized as a MEK solvate. The time for completing the crystallization of the MEK solvate may vary depending on the concentration of 6,6'-DPBHBNA and the temperature applied, but is typically in the range of 4 to 24 hours. Crystallization of the MEK solvate may also be achieved by concentrating a high temperature solution, or by a combination of concentrating and cooling. Concentration of the solution may be achieved by distilling off a portion of the MEK.

[0381] MEK solvate can be obtained by crystallization in the form of compact crystals with a low aspect ratio. The aspect ratio of MEK solvate is usually less than 5, and more specifically in the range of 1 to 4. The size of the crystals is usually in the range of 1 to 300 μm. There is a tendency that the crystals of MEK solvate do not enclose a significant amount of mother liquid. Therefore, the crystalline solvate of 6,6'-DPBHBNA and MEK can increase the purity of 6,6'-DPBHBNA to at least 99%, and further to at least 99.5% or more, and further to 99.7% or more.

[0382] Although the above-mentioned crystalline forms of 6,6'-DPBHBNA have high purity, these can also be converted into amorphous form B. Amorphous form B is stable and has no tendency to crystallize even after long-term storage or crushing by grinding. Amorphous form B is prepared by melting any crystalline form and then rapidly cooling it. Preferably, each crystalline form is heated to a temperature at least 5K higher than its melting point until it is completely melted to obtain a clear melt. If a solvate is used as a starting material to prepare the melt, it is preferred that all the solvent is removed by vacuuming. Thereafter, the melt is preferably rapidly cooled at a cooling rate of at least 5K / min, for example, at a cooling rate of 5 to 50K / min. Thus, form B can be obtained as a solid amorphous (glass). In order to obtain a powder, the amorphous can be crushed by, for example, grinding. In order to prevent crystallization, the crushing operation (comminution) is performed at a temperature significantly lower than 100°C, for example, in the range of 5 to 40°C. In this powder, the particles still exist in the amorphous form B.

[0383] In the X-ray powder diffraction pattern recorded by irradiation with Cu Kα1 rays at 22°C, form B generally does not show a reflection peak as a 2θ value at multiple diffraction angles in the range of 5° to 40°, but instead a broad halo indicating that a crystal layer is substantially absent can be observed.

[0384] Form B is also characterized in that it does not show an endothermic peak in the range of 80 to 200° C. when analyzed by DSC recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min. In contrast, amorphous Form B can show a glass transition temperature of 105 to 125° C. under such conditions.

[0385] The amorphous form B of 6,6'-DPBHBNA generally has a purity of at least 99%, further at least 99.5% or more, and further at least 99.7%. As mentioned above, this means that the total amount of impurities other than the solvent in form B does not exceed 1% by weight, particularly not more than 0.5% by weight, and further not more than 0.3% by weight. In particular, in Form B, the total amount of impurities selected from 2-(2-hydroxyethoxy)-2'-hydroxy-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-dihydroxy-6,6'-diphenyl-1,1'-binaphthyl and 2-(2-hydroxyethoxy)-2'-(2-(2-hydroxyethoxy)-ethoxy)-6,6'-diphenyl-1,1'-binaphthyl is generally 5000 ppm or less, preferably 4000 ppm or less, particularly preferably 3000 ppm or less, and further preferably 2000 ppm or less, based on 1 part by weight of 6,6'-DPBHBNA contained in the crystal of Form B. In particular, the weight of each of these impurities is 2000 ppm or less, more preferably 1500 ppm or less, and further preferably 1000 ppm or less, based on 1 part by weight of 6,6'-DPBHBNA contained in the crystal of the amorphous Form B. If the amorphous form B contains bis[2-[[1-[2-(2-hydroxyethoxy)-6-phenyl-1-naphthyl]-6-phenyl-2-naphthyl]-oxy]-ethyl] carbonate, its amount is usually not more than 2000 ppm based on 1 part by weight of 6,6'-DPBHBNA contained in the crystal of the amorphous form B, and may be a maximum of 1500 ppm or less.

[0386] Surprisingly, what was crystallized from the ethanol solution of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl was not the ethanol solvate of 6,6′-DPBHBNA, but another novel polymorph of 6,6′-DPBHBNA, which is hereinafter referred to as Form C. Form C is particularly useful in the production of the thermoplastic resin of the present invention because it does not contain a significant amount of solvent.

[0387] Form C generally does not contain more than 0.1 mol of organic solvent per 1 mol of 6,6'-DPBHBNA, and particularly does not contain more than 0.05 mol of solvent. The total amount of organic solvent in Form C is generally less than 1 wt%, particularly up to 0.5 wt%, or up to 0.1 wt%.

[0388] In the X-ray powder diffraction pattern recorded by irradiation with Cu Kα1 rays at 22° C., Form C generally shows the following three reflection peaks as 2θ values, namely, 5.1±0.2°, 7.6±0.2°, and 21.0±0.2°; and

[0389] At least three, particularly preferably at least five, at least seven or all of the following reflection peaks are shown as 2θ values: 8.2±0.2°, 9.2±0.2°, 10.4±0.2°, 10.8±0.2°, 11.6±0.2°, 12.8±0.2°, 13.4±0.2°, 14.5±0.2°, 15.2±0.2°, 15.6±0.2°, 16.6±0. 2°, 17.4±0.2°, 17.9±0.2°, 18.5±0.2°, 19.2±0.2°, 19.9±0.2°, 20.4±0.2°, 21.8±0.2°, 22.2±0.2°, 22.6±0.2°, 13.4±0.2°, 24.0±0.2°, 25.7±0.2°, 27.3±0.2° and 27.9±0.2°.

[0390] The X-ray powder diffraction pattern of Form C is substantially the same as that of the toluene solvate, indicating that the molecules of 6,6′-DPBHBNA in Form C and the toluene solvate have the same arrangement in the crystal lattice.

[0391] Form C can also be characterized by an endothermic peak indicating its dissolution. When Form C is analyzed by DSC recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, Form C generally shows an endothermic peak with an onset in the range of 115 to 118°C, and a peak maximum in the range of 124 to 126°C. In addition, the reaction point is generally in the range of 120 to 122°C.

[0392] Form C can be obtained by crystallizing 6,6'-DPBHBNA from 6,6'-DPBHBNA in high temperature ethanol. In order to obtain the desired form C, the 6,6'-DPBHBNA to be crystallized usually has a purity of at least 97% by weight with respect to organic matter other than the solvent. It is preferred to dissolve 6,6'-DPBHBNA having a purity of at least 97% by weight in high temperature ethanol. Usually, the temperature of the high temperature solution of 6,6'-DPBHBNA is at least 45°C, and can be as high as reflux temperature. The concentration of 6,6'-DPBHBNA in the high temperature solution usually does not exceed 30% by weight, and is usually 2 to 25% by weight. When crystallizing form C from a high temperature solution, it is usually achieved by cooling the high temperature solution to a temperature below 40°C, for example, a temperature in the range of -10 to below 40°C, and -5 to 30°C. At a temperature below 40°C, for example, in the range of -5 to 30°C, a seed crystal can be added. The amount of seed crystals is usually 0.05 to 2% by weight, particularly 0.1 to 1% by weight, based on the amount of 6,6'-DPBHBNA crystallized as form C. The time for completing the crystallization of form C can vary depending on the concentration of 6,6'-DPBHBNA and the temperature applied, but is typically in the range of 4 to 24 hours. Crystallization of form C can also be achieved by concentrating a high-temperature solution, or by a combination of concentration and cooling. Concentration of the solution can be achieved by distilling off part of the solvent.

[0393] Form C can be obtained by crystallization in the form of compact crystals with a low aspect ratio. The aspect ratio of Form C is usually less than 5, and further in the range of 1 to 4. The size of the crystals is usually in the range of 2 to 250 μm.

[0394] Crystals of form C tend not to contain a significant amount of mother liquor. Therefore, the crystal form C of 6,6'-DPBHBNA can increase the purity of 6,6'-DPBHBNA to at least 99%, and further at least 99.5% or more, and further at least 99.7% or more. As described above, this means that the total amount of impurities other than the solvent in form C does not exceed 1% by weight, particularly 0.5% by weight, and further does not exceed 0.3% by weight. In particular, in Form C, the total amount of impurities selected from 2-(2-hydroxyethoxy)-2'-hydroxy-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-dihydroxy-6,6'-diphenyl-1,1'-binaphthyl and 2-(2-hydroxyethoxy)-2'-(2-(2-hydroxyethoxy)-ethoxy)-6,6'-diphenyl-1,1'-binaphthyl is generally 5000 ppm or less, preferably 4000 ppm or less, particularly preferably 2000 ppm or less, and further preferably 1000 ppm or less, based on 1 part by weight of 6,6'-DPBHBNA contained in the crystal of Form C. In particular, the weight of each of these impurities is 2000 ppm or less, more preferably 1500 ppm or less, and further preferably 1000 ppm or less, based on 1 part by weight of 6,6'-DPBHBNA contained in the crystal of Form C. When Form C contains bis[2-[[1-[2-(2-hydroxyethoxy)-6-phenyl-1-naphthyl]-6-phenyl-2-naphthyl]-oxy]-ethyl] carbonate, its amount is usually not more than 2000 ppm based on 1 part by weight of 6,6'-DPBHBNA contained in the crystal of Form C, and may be a maximum of 1500 ppm or less.

[0395] The solid form of 6,6'-DPBHBNA of the present invention, i.e., methanol solvate, toluene solvate, methyl ethyl ketone solvate, and crystalline forms A and C, like the amorphous form B, also has a yellowness (YI) as low as usually less than 3.0, sometimes less than 2.5 or less than 2.0, particularly less than 1.5, further less than 1.0 or less than 0.75, and further less than 0.5. All YI values ​​are values ​​measured using a 5 w / w% dichloromethane solution of 6,6'-DPBHBNA in accordance with ASTM E 313.

[0396] The solid form of 6,6'-DPBHBNA of the present invention generally has a low haze of less than 1.0 ntu, sometimes less than 0.8 ntu or less than 0.6 ntu when measured using a 5 w / w% dichloromethane solution of 6,6'-DPBHBNA. Turbidity is a value measured using a 5 w / w% dichloromethane solution of 6,6'-DPBHBNA and expressed in nephelometric turbidity units (ntu). The haze of the crystalline solid of 6,6'-DPBHBNA of the present invention can be further reduced to, for example, 0.4 ntu, less than 0.35 ntu, or less than 0.30 ntu, and can further reach about 0.2 ntu or less.

[0397] The thermoplastic resin of the present invention, that is, the polyester resin, polyester carbonate resin, polycarbonate resin, or a mixture of at least two of these resins, is preferably produced from a monomer having a predetermined amount of impurities, purity, and the like.

[0398] For example, if the dihydroxy compound represented by the general formula (6) is in the form of a crystalline solvate, it is preferred to use an organic solvent containing 0.3 to 1.2 mol of the organic solvent in the crystals per 1 mol of the dihydroxy compound to produce the thermoplastic resin. Examples of the organic solvent include methanol, toluene, and methyl ethyl ketone.

[0399] When a monomer containing an organic solvent in an appropriate range of content as described above is used as the monomer of formula (6), a thermoplastic resin can be efficiently produced. For example, when a monomer containing an organic solvent in an amount of about 0.3 to 1.2 mol, 0.3 to 1.0 mol, or 0.3 to 0.5 mol per 1 mol of the dihydroxy compound is used to produce a thermoplastic resin, the monomer can be prevented from scattering, and a high-purity thermoplastic resin can be produced.

[0400] When the dihydroxy compound represented by the general formula (6) is in the form of crystals, the thermoplastic resin may be produced by using a compound containing less than 0.1 mol of an organic solvent in the crystals.

[0401] Among the dihydroxy compounds in crystalline form, those having the aspect ratio of up to 5:1 can be used. For example, crystals having an aspect ratio of up to 3:1 or up to 1:1 can be used.

[0402] As the dihydroxy compound represented by the general formula (6), it is preferred to use a compound having a purity of at least 99.0% by weight (or more) based on an organic substance, preferably a compound having a purity of 99.5% by weight or more, and particularly preferably a compound having a purity of 99.7% by weight. In addition, the dihydroxy compound of the general formula (6) containing less than 0.1 mol of an organic solvent, for example, less than 0.05 mol of an organic solvent, preferably less than 0.03 mol of an organic solvent, can also be used to produce a thermoplastic resin.

[0403] The dihydroxy compound represented by the general formula (6) preferably has a yellowness index (YI) value of less than 3.0 as measured using a 5 w / w % dichloromethane solution in accordance with ASTM E313, more preferably less than 2.0, and even more preferably less than 1.0.

[0404] The dihydroxy compound represented by the general formula (6) preferably has a haze measured using a 5 w / w % dichloromethane solution of less than 1.0 ntu, more preferably less than 0.7 ntu, and even more preferably less than 0.5 ntu.

[0405] When a thermoplastic resin is produced using any dihydroxy compound represented by the general formula (6), the total amount of impurities such as dihydroxy compounds other than the dihydroxy compound, for example, impurities having a similar molecular structure, is preferably less than 0.5% by weight, more preferably less than 0.3% by weight, and even more preferably less than 0.1% by weight, based on the weight of the dihydroxy compound.

[0406] For example, when 6-6'DPBHBNA is used as a monomer, the total amount of impurities of 2-(2-hydroxyethoxy)-2'-hydroxy-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-dihydroxy-6,6'-diphenyl-1,1'-binaphthyl and 2-(2-hydroxyethoxy)-2'-(2-(2-hydroxyethoxy)-ethoxy)-6,6'-diphenyl-1,1'-binaphthyl is preferably less than 0.5% by weight, more preferably less than 0.3% by weight, and even more preferably less than 0.1% by weight, based on the weight of 6-6'DPBHBNA.

[0407] When the impurities in the specific dihydroxy compound are contained in an amount of 0.5% by mass or more, the reaction efficiency may be reduced and the molecular weight may be reduced. In addition, when the impurities containing a large number of hydroxyethoxy groups are repeated, the refractive index of the obtained thermoplastic resin tends to be reduced.

[0408] On the other hand, the impurities in the specific dihydroxy compound are less than 0.5% by mass. When contained, a structure similar to the basic structure is contained in the resin, the melt viscosity is reduced, the moldability is improved, that is, there is a tendency for the flow of the resin to become better, and the impact resistance of the molded body such as the optical lens to be improved.

[0409] For example, the impurity content is preferably within a range of not more than 1 ppb to 5000 ppm based on 1 part by weight of the monomer of formula (6).

[0410] In addition, it is preferred to use a monomer of formula (6) having an impurity content of less than 0.5% by mass, for example, to use a monomer containing a structural unit containing less than 0.5% by weight of impurities derived from 2-(2-hydroxyethoxy)-2'-hydroxy-6,6'-diphenyl-1,1'-binaphthyl, 2,2'-dihydroxy-6,6'-diphenyl-1,1'-binaphthyl and 2-(2-hydroxyethoxy)-2'-(2-(2-hydroxyethoxy)-ethoxy)-6,6'-diphenyl-1,1'-binaphthyl to produce a resin, a resin composition, an optical lens, an optical film, etc.

[0411] In addition, the thermoplastic resin preferably has properties particularly suitable for optical applications, for example, the refractive index and the Abbe number are preferably well balanced. Specifically, for the thermoplastic resin, the refractive index is preferably higher than 1.660, more preferably higher than 1.668, and the Abbe number is lower than 19, for example, 13 or more and lower than 19, or 15 or more and lower than 19. Furthermore, it is preferred that the refractive index nD and the Abbe number ν satisfy the relationship of -0.0002ν+1.6718<nD<-0.024ν+2.124 on the basis of satisfying the above-mentioned conditions of the refractive index and the Abbe number, more preferably the refractive index nD and the Abbe number ν satisfy the relationship of -0.004v+1.744<nD<-0.024ν+2.124, and even more preferably the refractive index nD and the Abbe number ν satisfy the relationship of -0.02v+2.04<nD<-0.024ν+2.124.

[0412] In the thermoplastic resin having the structural unit represented by the general formula (1) of the present invention, an aromatic dihydroxy compound or an aliphatic dihydroxy compound (for example, a dihydroxy compound having a fluorene skeleton or binaphthols) can be used as a dihydroxy component in addition to the compound represented by the general formula (6).

[0413] The thermoplastic resin of the present invention can be preferably produced by using, in addition to the compound represented by the above general formula (6), a compound represented by the following general formula (7) and / or a compound represented by the following general formula (8) as a dihydroxy component.

[0414]

[0415] Among them, R'1~R' in formula (7) 20 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms,

[0416] Y is an alkylene group having 1 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0417] c and d are integers of 1 to 10 respectively.

[0418] In addition, R"1~R" in formula (8) 16 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms,

[0419] Z is an alkylene group having 2 to 8 carbon atoms, a cycloalkylene group having 5 to 12 carbon atoms, or an arylene group having 6 to 20 carbon atoms,

[0420] e and f are integers of 1 to 10 respectively.

[0421] Examples of the dihydroxy compound represented by formula (7) include 2,2'-bis(1-hydroxymethoxy)-1,1'-binaphthyl, 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthyl, 2,2'-bis(3-hydroxypropyloxy)-1,1'-binaphthyl, and 2,2'-bis(4-hydroxybutoxy)-1,1'-binaphthyl. Among them, 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthyl is preferred. These may be used alone or in combination of two or more.

[0422] Examples of the dihydroxy compound represented by formula (8) include 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-methylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-tert-butylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-isopropylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-cyclohexylphenyl]fluorene, and 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene. Among them, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene are preferred. These can be used alone or in combination of two or more.

[0423] For example, examples of the dihydroxy compound represented by the formula (7) or (8) include compounds represented by the following general formula (9).

[0424]

[0425] In addition, the monomer used to produce the thermoplastic resin may contain, together with the dihydroxy compound represented by the general formula (6), a dihydroxy compound in which the values ​​of c and d in the general formula (6) are both 0 or a dihydroxy compound in which either c or d in the general formula (6) is 0 as an impurity.

[0426] Thus, the total amount of dihydroxy compounds whose values ​​of at least any one of c and d are different from those of the above-mentioned general formula (6) in the monomer having the dihydroxy compound represented by the above-mentioned general formula (6) as the main component is preferably 1000 ppm or less, more preferably 500 ppm or less, even more preferably 200 ppm or less, and particularly preferably 100 ppm or less, and the total content of dihydroxy compounds whose values ​​of at least any one of c and d are different from those of the above-mentioned general formula (6) in the above-mentioned monomer is preferably 50 ppm or less, and more preferably 20 ppm or less.

[0427] The content of impurities involved in the general formula (6) is the same in the dihydroxy compound represented by the general formula (7) or (8). That is, together with the dihydroxy compound represented by the general formula (7) or (8), a dihydroxy compound in which the values ​​of e and f in the general formula (7) or (8) are both 0 or a dihydroxy compound in which either e or f in the general formula (7) or (8) is 0 may be contained as an impurity.

[0428] Furthermore, the total amount of these impurities in the monomer having the dihydroxy compound represented by the above-mentioned general formula (7) or (8) as the main component is preferably 1000 ppm or less, more preferably 500 ppm or less, even more preferably 200 ppm or less, and particularly preferably 100 ppm or less. Moreover, the total content of the above-mentioned impurities in the above-mentioned monomer is preferably 50 ppm or less, and more preferably 20 ppm or less.

[0429] The compounds of the general formulae (7) and (8) can be produced by various synthetic methods. For example, as described in Japanese Patent No. 5442800 and Japanese Patent Application Laid-Open No. 2014-028806, 9,9-bis(hydroxynaphthyl)fluorenes are obtained by (a) reacting fluorenones with hydroxynaphthalenes in the presence of hydrogen chloride gas and mercaptocarboxylic acid, (b) reacting 9-fluorenones with hydroxynaphthalenes in the presence of an acid catalyst (and an alkyl mercaptan), (c) reacting fluorenones with hydroxynaphthalenes in the presence of hydrochloric acid and mercaptans (such as mercaptocarboxylic acid), (d) reacting fluorenones with hydroxynaphthalenes in the presence of sulfuric acid and mercaptans (such as mercaptocarboxylic acid), and crystallizing using a crystallization solvent composed of a hydrocarbon and a polar solvent to produce bis-naphthol fluorene. The fluorenones can be produced by reacting them with a compound corresponding to the [XO]a group and the [XO]b group (such as an alkylene oxide and a halogenated alkanol). For example, 9,9-bis[6-(2-hydroxyethoxy)naphthyl]fluorene can be obtained by reacting 9,9-bis[6-hydroxynaphthyl]fluorene with 2-chloroethanol under alkaline conditions.

[0430] Examples of aromatic dihydroxy compounds other than those mentioned above that can be used simultaneously include bisphenol A, bisphenol AP, bisphenol AF, bisphenol B, bisphenol BP, bisphenol C, bisphenol E, bisphenol F, bisphenol G, bisphenol M, bisphenol S, bisphenol P, bisphenol PH, bisphenol TMC and bisphenol Z.

[0431] (Vinyl terminal group amount)

[0432] The thermoplastic polyester resin, polyester carbonate resin and polycarbonate resin of the present invention are obtained by using the compounds represented by the above general formulas (6) to (9) as dihydroxy components and reacting them with carbonate precursors such as carbonic acid diesters. However, in the polymerization process for producing thermoplastic resins such as polycarbonates, impurities are generated in which one or both of the terminal -OROH groups of the compounds represented by the above general formulas (6) to (9) are converted into vinyl terminal groups represented by -OC=CH groups, for example.

[0433] For example, an impurity having a vinyl group represented by the following formula (v-1) may be present in the monomer, resin, resin composition, optical lens, and optical film described in the specification of the present application.

[0434]

[0435] (In the formula, ※ represents a polymer chain, and Hp represents a hydrogen atom)

[0436] (V-1)

[0437] The vinyl group may be generated during monomer synthesis and refining and contained in the monomer. In addition, it may be generated and increased during resin polymerization and additive mixing. The vinyl group may be considered as one of the causes of polymer coloration, but on the other hand, when the content is trace, it may sometimes improve the bending strength and impact resistance of the resin.

[0438] The amount of such impurities having a vinyl terminal structure is usually very small, and the produced polymer can be used as a thermoplastic resin without purification.

[0439] For example, the amount of vinyl groups in the polycarbonate resin can be determined by performing the following calculation as described in <9. Amount of vinyl terminal groups in polycarbonate resin> 1 The content is determined by the integrated ratio of the following formula (A) in H-NMR measurement: The amount of the vinyl terminal groups is preferably 0.0001 to 5.0, more preferably 0.01 to 3.0, and even more preferably 0.1 to 1.0.

[0440]

[0441] Here, Hk in the above formula (A) refers to Hk in the following formula (v-2) corresponding to the above formula (v-1).

[0442]

[0443] (where Hk represents a hydrogen atom)

[0444] (V-2)

[0445] In addition, in the resin of the present application, sometimes, oligomers with molecular weight (Mw) below 1000, cyclic structures formed by mutual carbonate bonding of more than 2 monomers are formed. Such oligomers and cyclic bodies can be analyzed by LC-MS etc., and for example, preferably contain below 2.5 mass %, more preferably contain below 2.0 mass %, more preferably contain below 1.0 mass %.

[0446] Regarding the metals contained in the monomer, the total amount of Li, Na, Mg, Al, K, Ca, Ti, Cr, Fe, Ni, Zn and Sn is preferably 1000 wtppm or less (e.g., 100 wtppm, 10 wtppm).

[0447] Regarding the metals in the obtained resin or resin composition, the total content of Li, Na, Mg, Al, K, Ca, Ti, Cr, Fe, Ni, Zn and Sn is preferably 1000 ppm by weight or less.

[0448] When the metal is less than 1000 ppm by weight, the obtained resin is less colored and there is less concern about the catalyst activity being reduced during polymerization. In addition, by preferably containing more than 1 ppb by weight (more preferably more than 1 ppm by weight), the operation of adding a catalyst can be omitted, and by exerting a catalyst effect, the amount of catalyst added may be reduced, and it is also possible to achieve a reduction in manufacturing costs. Such a metal concentration is measured, for example, by the following method.

[0449] <Metal Analysis>

[0450] After the sample was carbonized with sulfuric acid, the metal concentration was measured by ICP-MS.

[0451] That is, weigh 2g of the sample in a synthetic quartz measuring cup, add 2.5ml of sulfuric acid just before carbonization, add 0.1ml of sulfuric acid during carbonization, and heat on a hot plate for carbonization. After that, cover it with a quartz dish and heat it in an electric furnace at 500°C for 10 hours for carbonization. Then add sulfuric acid, heat it, and dry it, add nitric acid, heat it, and dry it, thereby performing thermal acid decomposition. Add nitric acid aqueous solution to make it 50mL, heat it to 50°C, and perform quantitative analysis using ICP-MS.

[0452] ICP-MS equipment: Shimadzu Corporation: ICPE-9000

[0453] As the carbonic acid diester used in the manufacture of polycarbonate resin and polyester carbonate resin, diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl) carbonate, meta-cresol carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, etc. can be cited. Among these, diphenyl carbonate is particularly preferred. Relative to 1 mol of the total of dihydroxy compounds, diphenyl carbonate is preferably used in a ratio of 0.97 to 1.20 mol, more preferably in a ratio of 0.98 to 1.10 mol.

[0454] The dicarboxylic acid, monocarboxylic acid monoester and diester compounds that can be used in the production of polyester resins and polyester carbonate resins are preferably used in a ratio of 0.97 to 1.20 mol, more preferably 0.98 to 1.10 mol, based on 1 mol of the total of the dihydroxy compounds.

[0455] Among the above-mentioned transesterification catalysts used in the production of thermoplastic resins, examples of basic compound catalysts include alkali metal compounds, alkaline earth metal compounds, and nitrogen-containing compounds.

[0456] As the alkali metal compound used in the present invention, for example, organic acid salts, inorganic salts, oxides, hydroxides, hydrides or alkoxides of alkali metals can be cited. Specifically, sodium hydroxide, potassium hydroxide, cesium hydroxide, lithium hydroxide, sodium bicarbonate, sodium carbonate, potassium carbonate, cesium carbonate, lithium carbonate, sodium acetate, potassium acetate, cesium acetate, lithium acetate, sodium stearate, potassium stearate, cesium stearate, lithium stearate, sodium borohydride, sodium phenylborate, sodium benzoate, potassium benzoate, cesium benzoate, lithium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, disodium phenylphosphate, disodium salt, dipotassium salt, dicesium salt or dilithium salt of bisphenol A, sodium salt, potassium salt, cesium salt or lithium salt of phenol can be used.

[0457] Examples of the alkaline earth metal compound include organic acid salts, inorganic salts, oxides, hydroxides, hydrides or alkoxides of alkaline earth metal compounds. Specifically, magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium hydrogen carbonate, calcium hydrogen carbonate, strontium hydrogen carbonate, barium hydrogen carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, magnesium acetate, calcium acetate, strontium acetate, barium acetate, magnesium stearate, calcium stearate, calcium benzoate, magnesium phenylphosphate and the like can be used.

[0458] Examples of nitrogen-containing compounds include quaternary ammonium hydroxides and salts thereof, amines, etc. Specifically, quaternary ammonium hydroxides having an alkyl group, an aryl group, etc., such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and trimethylbenzylammonium hydroxide; tertiary amines such as triethylamine, dimethylbenzylamine, and triphenylamine; secondary amines such as diethylamine and dibutylamine; primary amines such as propylamine and butylamine; imidazoles such as 2-methylimidazole, 2-phenylimidazole, and benzimidazole; or bases or basic salts such as ammonia, tetramethylammonium borohydride, tetrabutylammonium borohydride, tetrabutylammonium tetraphenylborate, and tetraphenylammonium tetraphenylborate.

[0459] As the transesterification catalyst, salts of titanium, zinc, tin, zirconium, lead or the like are preferably used, and these may be used alone or in combination.

[0460] Specifically, titanium alkoxides such as tetrabutoxytitanium, zinc acetate, zinc benzoate, zinc 2-ethylhexanoate, tin (II) chloride, tin (IV) chloride, tin (II) acetate, tin (IV) acetate, dibutyltin dilaurate, dibutyltin oxide, dibutyldimethoxytin, zirconium acetylacetonate, zirconium oxyacetate, tetrabutoxyzirconium, lead (II) acetate, lead (IV) acetate, and the like can be used as the transesterification catalyst.

[0461] These catalysts are used in an amount of 10 to 1 mol of the total dihydroxy compound. -9 ~10 -3 The molar ratio is preferably 10 -7 ~10 -4Molar ratios were used.

[0462] The melt polycondensation method is a method in which the above-mentioned raw materials and a catalyst are used to carry out melt polycondensation under heating and further under normal pressure or reduced pressure while removing by-products by an ester exchange reaction.

[0463] In the melt polycondensation of this composition system, it is desired to melt the compound shown in the general formula (6) and the carbonic acid diester in a reaction vessel, and then react in a state where the by-product monohydroxy compound is retained. In order to retain it, the reaction device can be closed, or the pressure can be controlled by reducing pressure or pressurizing. The reaction time of this process is more than 20 minutes and less than 240 minutes, preferably more than 40 minutes and less than 180 minutes, and particularly preferably more than 60 minutes and less than 150 minutes. At this time, if the by-product monohydroxy compound is distilled and removed immediately after its generation, the content of the high molecular weight body in the thermoplastic resin finally obtained is small. However, when the by-product monohydroxy compound is retained in the reaction vessel for a certain period of time, a resin with a high content of the high molecular weight body in the thermoplastic resin finally obtained can be obtained.

[0464] The melt polycondensation reaction can be carried out in a continuous or batch manner. The reaction apparatus used during the reaction can be a vertical type equipped with an anchor stirring paddle, a MAXBLEND stirring paddle, a spiral ribbon stirring paddle, etc., or a horizontal type equipped with a paddle blade, a lattice blade, a glasses blade, etc., or an extruder type equipped with a screw. In addition, it is preferred to use a reaction apparatus formed by appropriately combining these reaction apparatuses in consideration of the viscosity of the polymer.

[0465] In the method for producing the thermoplastic resin used in the present invention, after the polymerization reaction is completed, the catalyst may be removed or inactivated in order to maintain thermal stability and hydrolytic stability. A method for deactivating the catalyst by adding a known acidic substance can be appropriately performed. As the acidic substance, specifically, esters such as butyl benzoate, aromatic sulfonic acids such as p-toluenesulfonic acid; aromatic sulfonic acid esters such as butyl p-toluenesulfonate and hexyl p-toluenesulfonate; phosphoric acids such as phosphorous acid, phosphoric acid, and phosphonic acid; phosphites such as triphenyl phosphite, monophenyl phosphite, diphenyl phosphite, diethyl phosphite, di-n-propyl phosphite, di-n-butyl phosphite, di-n-hexyl phosphite, dioctyl phosphite, and monooctyl phosphite; triphenyl phosphate, diphenyl phosphate, phosphoric acid Phosphates such as monophenyl phosphate, dibutyl phosphate, dioctyl phosphate, and monooctyl phosphate; phosphonic acids such as diphenylphosphonic acid, dioctylphosphonic acid, and dibutylphosphonic acid; phosphonates such as diethyl phenylphosphonate; phosphines such as triphenylphosphine and bis(diphenylphosphino)ethane; boric acids such as boric acid and phenylboric acid; aromatic sulfonates such as tetrabutylphosphonium dodecylbenzenesulfonate; organic halides such as stearoyl chloride, benzoyl chloride, and p-toluenesulfonyl chloride; alkylsulfuric acid such as dimethylsulfuric acid; organic halides such as benzyl chloride, etc. These deactivators are used in an amount of 0.01 to 50 times the amount of the catalyst, preferably 0.3 to 20 times the amount of the catalyst. When the amount is less than 0.01 times the amount of the catalyst, the deactivation effect is insufficient, so it is not preferred. In addition, when the amount is more than 50 times the amount of the catalyst, the heat resistance of the resin decreases, and the molded body is easily colored, so it is not preferred.

[0466] After the catalyst is deactivated, a step of removing low boiling point compounds in the polymer by devolatilization at a pressure of 0.1 to 1 mmHg and a temperature of 200 to 350° C. can be provided. In this step, a horizontal device equipped with a stirring blade having excellent surface renewal performance, such as a paddle blade, a lattice blade, or a spectacled blade, or a thin film evaporator is preferably used.

[0467] The thermoplastic resin of the present invention is desired to have as little foreign matter as possible, and is suitable for filtering molten raw materials, filtering catalyst liquids, etc. The pore size of the filter is preferably 5 μm or less, and more preferably 1 μm or less. In addition, it is suitable to filter the generated resin through a polymer filter. The pore size of the polymer filter is preferably 100 μm or less, and more preferably 30 μm or less. In addition, the process of collecting the resin pellets must of course be in a low-dust environment, preferably below grade 6, and more preferably below grade 5.

[0468] In addition, as a molding method of the polycarbonate resin, compression molding, casting, roll processing, extrusion molding, stretching, etc. can be exemplified in addition to injection molding, but it is not limited to these.

[0469] (4) Optical molding

[0470] The thermoplastic resin of the present invention can be used to manufacture optical molded bodies. For example, it can be molded by any method such as injection molding, compression molding, extrusion molding, solution casting, etc. The thermoplastic resin of the present invention has excellent moldability and heat resistance, so it can be particularly advantageously used in optical lenses that require injection molding. During molding, the thermoplastic resin of the present invention can be mixed with other resins such as other polycarbonate resins and polyester resins. In addition, additives such as antioxidants, processing stabilizers, light stabilizers, polymer metal deactivators, flame retardants, lubricants, antistatic agents, surfactants, antibacterial agents, release agents, ultraviolet absorbers, plasticizers, and compatibilizers can also be mixed.

[0471] Examples of the antioxidant include triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, butyl-4-hydroxybenzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate and 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane. The content of the antioxidant in the thermoplastic resin is preferably 0.001 to 0.3 parts by weight relative to 100 parts by weight of the thermoplastic resin.

[0472] Examples of the processing stabilizer include phosphorus-based processing heat stabilizers, sulfur-based processing heat stabilizers, etc. Examples of the phosphorus-based processing heat stabilizer include phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid, and esters thereof. Specific examples thereof include triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,6-di-tert-butylphenyl)phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, bis(nonylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, Bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, distearylpentaerythritol diphosphite, tributyl phosphate, triethyl phosphate, trimethyl phosphate, triphenyl phosphate, diphenyl mono-o-biphenyl phosphate, dibutyl phosphate, dioctyl phosphate, diisopropyl phosphate, dimethyl phenylphosphonate, diethyl phenylphosphonate, dipropyl phenylphosphonate, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite, bis(2,4-di-tert-butylphenyl)-4-phenyl-phenyl phosphonite and bis(2,4-di-tert-butylphenyl)-3-phenyl-phenyl phosphonite, etc. The content of the phosphorus-based processing heat stabilizer in the thermoplastic resin is preferably 0.001 to 0.2 parts by weight based on 100 parts by weight of the thermoplastic resin.

[0473] Examples of the sulfur-based processing heat stabilizer include pentaerythritol-tetrakis (3-lauryl thiopropionate), pentaerythritol-tetrakis (3-myristyl thiopropionate), pentaerythritol-tetrakis (3-stearyl thiopropionate), dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, and distearyl-3,3'-thiodipropionate. The content of the sulfur-based processing heat stabilizer in the thermoplastic resin is preferably 0.001 to 0.2 parts by weight relative to 100 parts by weight of the thermoplastic resin.

[0474] As a release agent, it is preferred that 90% by weight or more of the release agent is composed of an ester of an alcohol and a fatty acid. As the ester of an alcohol and a fatty acid, specifically, esters of a monohydric alcohol and a fatty acid, and partial or full esters of a polyhydric alcohol and a fatty acid can be cited. As the ester of the monohydric alcohol and a fatty acid, an ester of a monohydric alcohol having 1 to 20 carbon atoms and a saturated fatty acid having 10 to 30 carbon atoms is preferred. In addition, as a partial or full ester of a polyhydric alcohol and a fatty acid, a partial or full ester of a polyhydric alcohol having 1 to 25 carbon atoms and a saturated fatty acid having 10 to 30 carbon atoms is preferred.

[0475] Specifically, examples of the esters of monohydric alcohols and saturated fatty acids include octadecyl stearate, palmityl palmitate, butyl stearate, methyl laurate, isopropyl palmitate, etc. Examples of partial or full esters of polyhydric alcohols and saturated fatty acids include stearic acid monoglyceride, stearic acid monoglyceride, stearic acid diglyceride, stearic acid triglyceride, stearic acid monosorbitol ester, behenic acid monoglyceride, capric acid monoglyceride, lauric acid monoglyceride, pentaerythritol monostearate, pentaerythritol tetrastearate, pentaerythritol tetrapelargonate, propylene glycol monostearate, biphenyl biphenyl ester, sorbitan monostearate, 2-ethylhexyl stearate, full or partial esters of dipentaerythritol such as dipentaerythritol hexastearate, etc. The content of these release agents is preferably in the range of 0.005 to 2.0 parts by weight, more preferably in the range of 0.01 to 0.6 parts by weight, and still more preferably in the range of 0.02 to 0.5 parts by weight, based on 100 parts by weight of the thermoplastic resin.

[0476] As the ultraviolet absorber, at least one ultraviolet absorber selected from benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, triazine ultraviolet absorbers, cyclic iminoester ultraviolet absorbers and cyanoacrylate ultraviolet absorbers is preferred. That is, any one of the ultraviolet absorbers listed below may be used alone, or two or more may be used in combination.

[0477] Examples of the benzotriazole ultraviolet absorber include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, and 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole. 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octyloxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazin-4-one), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole, etc.

[0478] Examples of the benzophenone-based ultraviolet absorber include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid hydrate, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodium sulfonatebenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.

[0479] Examples of the triazine-based ultraviolet absorber include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol and 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-[(octyl)oxy]-phenol.

[0480] Examples of the cyclic urethane ultraviolet absorber include 2,2'-bis(3,1-benzoxazin-4-one), 2,2'-p-phenylenebis(3,1-benzoxazin-4-one), 2,2'-m-phenylenebis(3,1-benzoxazin-4-one), 2,2'-(4,4'-diphenylene)bis(3,1-benzoxazin-4-one), 2,2'-(2,6-naphthylene)bis(3 ,1-benzoxazine-4-one), 2,2'-(1,5-naphthalene)bis(3,1-benzoxazine-4-one), 2,2'-(2-methyl-p-phenylene)bis(3,1-benzoxazine-4-one), 2,2'-(2-nitro-p-phenylene)bis(3,1-benzoxazine-4-one) and 2,2'-(2-chloro-p-phenylene)bis(3,1-benzoxazine-4-one).

[0481] Examples of the cyanoacrylate-based ultraviolet absorber include 1,3-bis-[(2′-cyano-3′,3′-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.

[0482] The content of the ultraviolet absorber is preferably 0.01 to 3.0 parts by weight, more preferably 0.02 to 1.0 parts by weight, and even more preferably 0.05 to 0.8 parts by weight, relative to 100 parts by weight of the thermoplastic resin. Within this range, the thermoplastic resin can be endowed with sufficient weather resistance depending on the application.

[0483] The thermoplastic resin of the present invention has a high refractive index and a low Abbe number. In addition to optical lenses, the optical molded body can also be preferably used as a structural material or functional material for optical parts such as transparent conductive substrates, optical disks, liquid crystal panels, optical memory cards, sheets, films, optical fibers, connectors, vapor-deposited plastic reflectors, and displays used in liquid crystal displays, organic EL displays, and solar cells.

[0484] On the surface of the optical molded body, a coating such as an anti-reflection layer or a hard coating may be provided as required. The anti-reflection layer may be a single layer or multiple layers, and may be an organic substance or an inorganic substance, preferably an inorganic substance. Specifically, oxides or fluorides such as silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, cerium oxide, magnesium oxide, and magnesium fluoride may be exemplified.

[0485] (5) Optical lens

[0486] The optical lens using thermoplastic resin of the present invention to make has high refractive index, low Abbe number, and has high resistance to moisture and heat, therefore can be used in the field of telescope, binoculars, TV projector etc., using expensive high refractive index glass lens at present, very useful.As required, preferably use in the form of aspheric lens.Aspheric lens can utilize 1 lens to make spherical aberration become zero in fact, therefore do not need to eliminate spherical aberration by combining multiple spherical lenses, can realize the reduction of lightweight and production cost.Therefore, aspheric lens is particularly useful as camera lens in optical lens.

[0487] The optical lens can be molded by any method, such as injection molding, compression molding, injection compression molding, etc. According to the present invention, a high refractive index low birefringence aspheric lens which is technically difficult to process using a glass lens can be obtained more easily.

[0488] In order to avoid foreign matter from entering the optical lens as much as possible, the molding environment must of course be a low-dust environment, preferably below level 6, and more preferably below level 5.

[0489] (6) Optical film

[0490] The optical film produced using the thermoplastic resin of the present invention has excellent transparency and heat resistance and is therefore suitable for use in films for liquid crystal substrates, optical memory cards, and the like.

[0491] In order to avoid foreign matter from being mixed into the optical film as much as possible, the molding environment must of course also be a low-dust environment, preferably level 6 or below, more preferably level 5 or below.

[0492] [Abbreviation]

[0493] 6,6'-DPBHBNA: 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl (Bis-2,2'-(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-bisnaphthyl); 6,6'-DPMHBNA: 2-(2-hydroxyethoxy)-2'-hydroxy-6,6'-diphenyl-1,1'-bisnaphthyl;

[0494] 6,6'-DPTHBNA: 2-(2-hydroxyethoxy)-2'-[(2-hydroxyethoxy)ethoxy]-6,6'-diphenyl-1,1'-bisnaphthyl;

[0495] %bw:% by weight;

[0496] DSC: differential scanning calorimetry;

[0497] LOD: Loss on drying;

[0498] mp: melting point;

[0499] MeOH: Methanol;

[0500] NaOH: sodium hydroxide;

[0501] NIR: near infrared;

[0502] PXRD: powder X-ray diffraction;

[0503] TLC: thin layer chromatography;

[0504] UPLC: Ultra Performance Liquid Chromatography.

[0505] [Example]

[0506] <1. Method for measuring weight average molecular weight (Mw)>

[0507] Based on JIS K 7252-3, the polystyrene conversion weight average molecular weight is obtained from a pre-prepared standard polystyrene calibration curve. That is, a standard polystyrene (PStQuick MP-M, manufactured by Tosoh Corporation) with a known molecular weight (molecular weight distribution = 1) is used to prepare a calibration curve, and the dissolution time and molecular weight value of each peak are marked from the measured standard polystyrene, and a cubic approximation is performed to obtain a calibration curve. Mw is obtained by the following calculation formula.

[0508] Mw=Σ(Wi×Mi)÷Σ(Wi)

[0509] Wherein, i represents the i-th split point when the molecular weight M is split, Wi represents the i-th weight, and Mi represents the i-th molecular weight. And the molecular weight M refers to the polystyrene molecular weight value at the dissolution time of the calibration curve. As a GPC apparatus, HLC-8320GPC manufactured by Tosoh Corporation was used, as a guard column, one TSK guardcolumn Super MPHZ-M was used, and as an analytical column, a column formed by connecting three TSK gel SuperMultipore HZ-M in series was used. Other conditions are as follows.

[0510] Solvent: HPLC grade tetrahydrofuran

[0511] Injection volume: 10 μL

[0512] Sample concentration: 0.2w / v% HPLC grade chloroform solution

[0513] Solvent flow rate: 0.35ml / min

[0514] Measurement temperature: 40℃

[0515] Detector: RI

[0516] <2. Glass transition temperature (Tg)>

[0517] The measurement was performed using a differential scanning calorimeter (DSC) in accordance with JIS K7121-1987. As the analyzer, Hitachi High-Technologies X-DSC7000 was used.

[0518] <3. Refractive index (nD)>

[0519] The film having a thickness of 0.1 mm and made of the resin produced in the example was measured using an Abbe refractometer in accordance with the method of JIS-K-7142.

[0520] <4. Abbe number (ν)>

[0521] The refractive index of a film having a thickness of 0.1 mm made of the resin produced in Examples at wavelengths of 486 nm, 589 nm and 656 nm was measured at 23° C. using an Abbe refractometer, and the Abbe number was calculated using the following formula.

[0522] ν=(nD-1) / (nF-nC)

[0523] nD: refractive index at a wavelength of 589nm

[0524] nC: refractive index at a wavelength of 656nm

[0525] nF: Refractive index at a wavelength of 486nm<5.b value>

[0526] After the manufactured resin was vacuum dried at 120°C for 4 hours, it was injection molded using an injection molding machine (FANUC ROBOSHOTα-S30iA) at a barrel temperature of 270°C and a mold temperature of Tg-10°C to obtain a disc-shaped test plate with a diameter of 50 mm and a thickness of 3 mm. Using this plate, the b value was measured in accordance with JIS K7105. The smaller the b value, the weaker the yellowish color and the better the hue. The SE2000 spectrophotometer manufactured by Nippon Denshoku Industries Co., Ltd. was used for the measurement of the molded plate.

[0527] <6. Pressure Cooker Test (PCT Test)>

[0528] The produced resin was vacuum dried at 120°C for 4 hours, and then injection molded using an injection molding machine (FANUC ROBOSHOTα-S30iA) at a cylinder temperature of 270°C and a mold temperature set to the resin's Tg-10°C to obtain a disc-shaped test plate with a diameter of 50 mm and a thickness of 3 mm. The plate was placed at 130°C and a relative humidity of 85% rh for 48 hours.

[0529] <7. Total light transmittance>

[0530] The plates before and after the PCT test were measured using a spectrophotometer SE2000 manufactured by Nippon Denshoku Industries, Ltd., in accordance with the method of JIS-K-7361-1.

[0531] <8. Total light transmittance retention rate (%)>

[0532] The total light transmittance was determined according to the following formula using the value of the total light transmittance measured by the above method.

[0533] Total light transmittance retention rate (%) = total light transmittance after PCT test / total light transmittance before PCT test × 100

[0534] <9. Vinyl terminal group content of polycarbonate resin>

[0535] 1 The H-NMR measurement was performed under the following conditions.

[0536] · 1 H-NMR measurement conditions

[0537] Device: Bruker AVANZE III HD 500MHz

[0538] Tipping angle: 30 degrees

[0539] Waiting time: 1 second

[0540] Total times: 500 times

[0541] Measurement temperature: room temperature (298K)

[0542] Concentration: 5wt%

[0543] Solvent: deuterated chloroform

[0544] Internal standard substance: tetramethylsilane (TMS) 0.05wt%

[0545] <10. Determination of the amount of phenol and diphenyl carbonate (DPC) in polycarbonate resin>

[0546] 0.5 g of the sample of Example 1 described in detail later was dissolved in 50 ml of tetrahydrofuran (THF) as a sample solution. A standard curve was prepared using the pure product of each compound as a standard, and 2 μL of the sample solution was quantified using LC-MS under the following measurement conditions. The detection limit under the measurement conditions was 0.01 ppm.

[0547] LC-MS assay conditions:

[0548] Measurement device (LC part): Agilent Infinity 1260LC System

[0549] Chromatographic column: ZORBAX Eclipse XDB-18, and guard column

[0550] Mobile Phase:

[0551] A: 0.01 mol / L ammonium acetate aqueous solution

[0552] B: 0.01mol / L ammonium acetate methanol solution

[0553] C:THF

[0554] Gradient program of mobile phase:

[0555] As shown in Table 1, the mixture of A to C was used as the mobile phase, and the mobile phase was passed through the column for 30 minutes while switching the composition of the mobile phase when the time shown in the time (minutes) column elapsed.

[0556] [Table 1]

[0557]

[0558] Flow rate: 0.3ml / min

[0559] Column temperature: 45°C

[0560] Detector: UV (225nm)

[0561] Measurement device (MS part): Agilent 6120 single quad LCMS System

[0562] Ionization source: ESI

[0563] Polarity: Positive (DPC) & Negative (PhOH)

[0564] Fragmentation voltage: 70V

[0565] Drying gas: 10L / min, 350℃

[0566] Atomizer: 50psi

[0567] Capillary voltage: 3000V (Positive), 2500V (Negqative)

[0568] Measured ions:

[0569] [Table 2]

[0570] monomer Ion type m / z PhOH [MH]_ 93.1 DPC [M+NH4]+ 232.1

[0571] Sample injection volume: 2μL

[0572] Monomer analysis method

[0573] <11. Powder X-ray Diffraction (PXRD)>

[0574] Powder X-ray diffraction (PXRD) patterns were recorded using a D8 Discover X-ray diffractometer from Bruker AXS GmbH, Germany, using a reflection configuration (Bragg Brentano) with Cu Kα1 radiation (40 kV, 40 mA) as the X-ray source. Data were collected at room temperature over the range of 2θ-5.0° to 2θ-80.0° with a resolution of 0.025° and a measurement time of 0.5 sec / step.

[0575] <12.DSC measurement>

[0576] DSC measurement was performed using Linseis Chip-DSC 10. The heating rate was 20°C / min.

[0577] <13. Determination of melting point>

[0578] The melting point was measured by a capillary method using a Büchi Melting Point B-545 apparatus at a heating rate of 1 K / min.

[0579] <14.Near infrared analysis>

[0580] Near infrared analysis was recorded by means of a Bruker FT-NIR spectrometer Matrix Fspectrometer, Bruker Opus 5.5 software and a reflection immersible probe head.

[0581] <15. Determination of Purity>

[0582] Purity was determined by UPLC using the following system and operating conditions.

[0583] Waters Acquity UPLC H-Class System; Columns

[0584] Acquity UPLC BEH C18, 1.7 μm, 2 x 100 mm; Column temperature: 40 °C,

[0585] Gradient: acetonitrile / water (acetonitrile; ACN: 48% at 0 min, 50% at 21 min, 100% at 26 min, 100% at 28 min, 48% at 28.1 min, 48% at 32 min);

[0586] Injection volume: 0.8 μl; flow rate 0.6 ml / min; detection at 210 nm.

[0587] <16. Determination of volatile solvents>

[0588] The amount of volatile solvents was determined by gas chromatography using Shimadzu GC 14B and Class VP 4.3 software, AOC-20i autoinjector, AOC-20s autosampler, and FID detector.

[0589] As a chromatography column, PE 624 20 (Perkin Elmer) having the following dimensions was used. Gas chromatography was performed under the following operating conditions.

[0590] Carrier gas: Hydrogen

[0591] Pressure: 0.3 bar

[0592] Injection temperature: 250℃

[0593] Detection temperature: 300℃

[0594] Column temperature: 40°C (2 minutes), 20°C / min, 200°C (2 minutes)

[0595] Concentration: C = 20 mg / ml

[0596] Injection volume: 0.2~2μl

[0597] As the internal standard, a solution of 100 mg of naphthalene in 10 ml of dimethylformamide was used. The sample was prepared by dissolving 20 mg of the compound in a 0.1 mm internal standard solution and adding 0.9 ml of dimethylformamide. The amount of the medium was calculated by the following formula.

[0598] S Solv *M St *100 / (S St *M Sample *RRF)

[0599] M St : The amount of internal standard in the sample solution

[0600] M Sample : The weight of the sample

[0601] S Solv : The area of ​​the solvent peak

[0602] S St :Standard area

[0603] RRF: Relative sensitivity coefficient of solvent<17. Determination of yellowness>

[0604] The yellowness index YI of 6,6'-DPBHBNA was measured with reference to ASTM E 313 according to the following protocol.

[0605] 1 g of 6,6'-DPBHBNA was dissolved in 19 g of dichloromethane. The solution was transferred to a 50 mm measuring cell and the transmittance in the range of 300 to 800 nm was measured using a Shimadzu UV-Visible spectrophotometer UV-1650PC (spectrophotometer). Dichloromethane was used as a control. From the spectrum, the yellowness index was calculated using the software RCA-softwareUV2DAT according to ASTM E308 (Standard practice for computing the colors of objects by using the CIE System) and ASTM E 313 (Standard practice for calculating yellowness and whiteness indices from instrumentally measured color coordinates).

[0606] <18. Measurement of haze>

[0607] The haze was determined by measuring the transmittance of a 5% dichloromethane solution of 6,6′-DPBHBNA at 860 nm using a standard nephelometer.

[0608] <19. Microscopy>

[0609] The images of the microscopic examination were taken using a Nikon microscope Eclipse TS100 at a magnification of 100 times provided by a Nikon imaging unit Digital Sight DS-U1. The width (W), length (L), and aspect ratio (L / W ratio) were confirmed from these microscopic images.

[0610] [Manufacture of polycarbonate resin]

[0611] (Example 1)

[0612] As raw materials, 31.6 kg (60.0 mol) of 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl (hereinafter sometimes abbreviated as "BINL-2EO"), 13.5 kg (63.0 mol) of diphenyl carbonate (hereinafter sometimes abbreviated as "DPC") and 0.074 g (8.8 × 10 -4mol) was put into a 50L reactor with a stirrer and a distillation device, and heated to 180°C under a nitrogen atmosphere of 760mmHg. After 20 minutes of starting heating, it was confirmed that the raw material was completely dissolved, and then stirred for 120 minutes under this condition. After that, the reduced pressure was adjusted to 200mmHg, and the temperature was raised to 200°C at a rate of 60°C / hr. At this time, it was confirmed that the by-product phenol began to distill. After that, the reaction was maintained at 200°C for 40 minutes. After that, the temperature was raised to 240°C at a rate of 75°C / hr, and after 10 minutes after the temperature was raised, the temperature was maintained while the reduced pressure was reduced to less than 1mmHg for 1 hour. After that, the temperature was raised to 245°C at a rate of 60°C / hr, and stirred for another 30 minutes. After the reaction was completed, nitrogen was introduced into the reactor to restore it to normal pressure, and the generated polycarbonate resin was pelletized and taken out. As a result of measuring the amounts of phenol and diphenyl carbonate (DPC) as impurities in the obtained polycarbonate resin as described above, the amount of phenol in the resin was 100 ppm by mass, and the amount of DPC in the resin was 300 ppm by mass.

[0613] The physical property values ​​of the obtained resin are shown in Table 3 below.

[0614] (Example 2-A)

[0615] The same operation as in Example 1 was carried out except that 7.9 kg (15.0 mol) of BINL-2EO, 24.2 kg (45.0 mol) of BNEF and 13.5 kg (63.0 mol) of DPC were used as raw materials.

[0616] (Example 2-B)

[0617] The same operation as in Example 1 was carried out except that 15.8 kg (30.0 mol) of BINL-2EO, 16.2 kg (30.0 mol) of BNEF and 13.5 kg (63.0 mol) of DPC were used as raw materials.

[0618] (Example 2-C)

[0619] The same operation as in Example 1 was carried out except that 23.7 kg (45.0 mol) of BINL-2EO, 8.1 kg (15.0 mol) of BNEF and 13.5 kg (63.0 mol) of DPC were used as raw materials.

[0620] The physical properties of the obtained resin are shown in Table 3. The NMR spectrum of the resin (BINOL-2EO / BNEF=50 mol / 50 mol) obtained in Example 2-B is shown in Table 3. Figure 1 .

[0621] (Example 3-A)

[0622] The same operation as in Example 1 was performed except that 7.9 kg (15.0 mol) of BINL-2EO, 19.0 kg (45.0 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (hereinafter sometimes abbreviated as "BPEF"), and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0623] (Example 3-B)

[0624] The same operation as in Example 1 was carried out except that 15.8 kg (30.0 mol) of BINL-2EO, 12.7 kg (30.0 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (hereinafter sometimes abbreviated as "BPEF"), and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0625] (Example 3-C)

[0626] The same operation as in Example 1 was carried out except that 23.7 kg (45.0 mol) of BINL-2EO, 6.3 kg (15.0 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (hereinafter sometimes abbreviated as "BPEF"), and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0627] (Example 4-A)

[0628] The same operation as in Example 1 was carried out except that 7.9 kg (15.0 mol) of BINL-2EO, 25.9 kg (45.0 mol) of BPPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials. Table 3 shows the physical properties of the obtained resin.

[0629] (Example 4-B)

[0630] The same operation as in Example 1 was carried out except that 15.8 kg (30.0 mol) of BINL-2EO, 17.2 kg (30.0 mol) of BPPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials. Table 3 shows the physical properties of the obtained resin.

[0631] (Example 4-C)

[0632] The same operation as in Example 1 was carried out except that 23.7 kg (45.0 mol) of BINL-2EO, 8.6 kg (15.0 mol) of BPPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials. Table 3 shows the physical properties of the obtained resin.

[0633] (Example 5)

[0634] The same operation as in Example 1 was performed except that 7.6 kg (18.0 mol) of BPEF, 26.3 kg (42.0 mol) of 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-1-yl)-1,1'-binaphthyl (hereinafter sometimes abbreviated as "DNBINOL-2EO"), and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0635] (Example 6-A)

[0636] The same operation as in Example 1 was performed except that 7.9 kg (15.0 mol) of BINL-2EO, 9.7 kg (18.0 mol) of BNEF, 10.1 kg (27.0 mol) of 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthyl (hereinafter sometimes abbreviated as "BNE"), and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0637] (Example 6-B)

[0638] The same operation as in Example 1 was carried out except that 19.0 kg (36.0 mol) of BINL-2EO, 4.5 kg (12.0 mol) of BNE, 5.1 kg (12.0 mol) of BPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials.

[0639] (Example 6-C)

[0640] The same operation as in Example 1 was carried out except that 19.0 kg (36.0 mol) of BINL-2EO, 4.5 kg (12.0 mol) of BNE, 6.9 kg (12.0 mol) of BPPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0641] The BINL-2EO used in the above-mentioned Example 1, Example 2-A to Example 2-C, Example 3-A to Example 3-C, Example 4-A to Example 3-C, and Example 6-A to Example 3-C is the “Form A” obtained in Example 21 described in detail later.

[0642] (Example 6-D)

[0643] The same operation as in Example 1 was carried out except that 11.3 kg (21.0 mol) of BNEF, 11.2 kg (30.0 mol) of BNE, 5.6 kg (9.0 mol) of DNBINOL-2EO, and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0644] (Example 6-E)

[0645] The same operation as in Example 1 was carried out except that 6.7 kg (18.0 mol) of BNE, 17.2 kg (30.0 mol) of BPPEF, 7.5 kg (12.0 mol) of DNBINOL-2EO, and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0646] (Example 6-F)

[0647] The same operation as in Example 1 was carried out except that 6.7 kg (18.0 mol) of BNE, 10.1 kg (24.0 mol) of BPEF, 11.3 kg (18.0 mol) of DNBINOL-2EO, and 13.5 kg (63.0 mol) of DPC were used as raw materials.

[0648] (Example 7)

[0649] The same operation as in Example 1 was carried out except that 32.0 kg (51.0 mol) of 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-2-yl)-1,1'-binaphthyl (2DNBINOL-2EO), 3.8 kg (9.0 mol) of BPEF and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0650] (Example 7-A)

[0651] The same operation as in Example 1 was carried out except that 18.8 kg (30.0 mol) of 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-2-yl)-1,1'-binaphthyl (2DNBINOL-2EO), 12.7 kg (30.0 mol) of BPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0652] (Example 7-B)

[0653] The same operation as in Example 1 was carried out except that 5.6 kg (9.0 mol) of 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-2-yl)-1,1'-binaphthyl (2DNBINOL-2EO), 21.5 kg (51.0 mol) of BPEF and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0654] (Example 8)

[0655] The same operation as in Example 1 was carried out except that 37.1 kg (51.0 mol) of 2,2'-bis(2-hydroxyethoxy)-6,6'-di(phenanthrene-9-yl)-1,1'-binaphthyl (9DPNBINOL-2EO), 3.8 kg (9.0 mol) of BPEF and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0656] (Example 8-A)

[0657] The same operation as in Example 1 was carried out except that 21.8 kg (30.0 mol) of 2,2'-bis(2-hydroxyethoxy)-6,6'-di(phenanthrene-9-yl)-1,1'-binaphthyl (9DPNBINOL-2EO), 12.7 kg (30.0 mol) of BPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0658] (Example 8-B)

[0659] The same operation as in Example 1 was carried out except that 6.5 kg (9.0 mol) of 2,2'-bis(2-hydroxyethoxy)-6,6'-di(phenanthrene-9-yl)-1,1'-binaphthyl (9DPNBINOL-2EO), 21.5 kg (51.0 mol) of BPEF and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0660] (Example 9)

[0661] The same operation as in Example 1 was carried out except that 10.4 kg (18.0 mol) of 6,6'-bis(3-cyanophenyl)-2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthyl (CN-BNA), 18.4 kg (42.0 mol) of BPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0662] (Example 10)

[0663] The same operation as in Example 1 was carried out except that 12.7 kg (18.0 mol) of 6,6'-di(dibenzo[b,d]furan-4-yl)-2,2'-bis-(2-hydroxyethoxy)-1,1'-binaphthyl (FUR-BNA), 18.4 kg (42.0 mol) of BPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0664] (Example 11)

[0665] The same operation as in Example 1 was carried out except that 13.3 kg (18.0 mol) of 6,6′-di(dibenzo[b,d]thiophen-4-yl)-2,2′-bis-(2-hydroxyethoxy)-1,1′-binaphthyl (THI-BNA), 18.4 kg (42.0 mol) of BPEF, and 13.5 kg (63.0 mol) of DPC were used as raw materials. The physical properties of the obtained resin are shown in Table 3.

[0666] (Comparative Example 1)

[0667] The same operation as in Example 1 was carried out except that 22.5 kg (60.0 mol) of BNE and 13.5 g (63.0 mol) of DPC were used as raw materials. Table 3 shows the physical properties of the obtained resin.

[0668] [Table 3]

[0669]

[0670] Example:

[0671] BINL-2EO 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl

[0672] BNEF 9,9-bis(6-(2-hydroxyethoxy)naphthalene-2-yl)fluorene

[0673] BNE 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthyl

[0674] BPEF 9,9-Bis[4-(2-hydroxyethoxy)phenyl]fluorene

[0675] BPPEF 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene

[0676] DNBINOL-2EO 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-1-yl)-1,1'-binaphthyl

[0677] 2DNBINOL-2EO 2,2'-bis(2-hydroxyethoxy)-6,6'-di(naphthalene-2-yl)-1,1'-binaphthyl

[0678] 9DPNBINOL-2EO 2,2'-bis(2-hydroxyethoxy)-6,6'-di(phenanthrene-9-yl)-1,1'-binaphthyl

[0679] CN-BNA 6,6'-bis(3-cyanophenyl)-2,2'-bis-(2-hydroxyethoxy)-1,1'-binaphthyl

[0680] FUR-BNA 6,6′-di(dibenzo[b,d]furan-4-yl)-2,2′-bis-(2-hydroxyethoxy)-1,1′-binaphthyl

[0681] THI-BNA6,6′-bis(dibenzo[b,d]thiophene-4-yl)-2,2′-bis-(2-hydroxyethoxy)-1,1′-binaphthyl

[0682] Comparative Example:

[0683] BNE 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthyl

[0684] [Moldability]

[0685] A: The molded sheet has no gaps and no undulations on the surface.

[0686] B: There are gaps in the molded sheet.

[0687] C: The surface of the molded piece has undulations.

[0688] D: The molded piece has gaps and the surface is deformed.

[0689]

[0690] [Manufacture of polyester and polyester carbonate resin]

[0691] (Example 12)

[0692] 0.090 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl (BINL-2EO) as a diol compound, 0.010 mol of 9,9-fluorene-dipropionic acid methyl ester (FDPM) as a carboxylic acid dialkyl ester, 0.120 mol of ethylene glycol (EG) and 0.001 mol of tetrabutoxytitanium as an ester exchange catalyst were placed in a reactor equipped with a Nakamura Scientific Instruments Co., Ltd. Sealing mixer UZU with a half-moon-shaped stirring blade and a distillation device, and heated to 180°C under normal pressure in a nitrogen atmosphere and stirred for 30 minutes. After that, the temperature was raised to 250°C over 1 hour, and the pressure was reduced to 0.13 kPa to perform a polymerization reaction. After that, the contents were taken out of the reactor after being maintained at 250°C and 0.13 kPa for 1 hour to obtain a polyester resin. The physical properties of the obtained polyester resin are shown in Table 3.

[0693] (Examples 13 to 18, Comparative Example 2)

[0694] A polyester resin was obtained in the same manner as in Example 12 except that the diol compound listed in Table 3 was used as the diol compound. Table 3 shows the physical properties of the obtained polyester resin.

[0695] (Example 19)

[0696] 0.110 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl (BINL-2EO) as a diol compound, 0.100 mol of 9,9-fluorene-dipropionic acid methyl ester (FDPM) as a carboxylic acid dialkyl ester, 0.010 mol of diphenyl carbonate, and 0.001 mol of tetrabutoxytitanium as an ester exchange catalyst were put into a reactor equipped with a Nakamura Scientific Instruments Co., Ltd. Sealing mixer UZU with a half-moon-shaped stirring blade and a distillation device, and heated to 180°C under normal pressure in a nitrogen atmosphere and stirred for 60 minutes. The distillation of phenol and methanol was confirmed. After that, the temperature was raised to 240°C over 1 hour, and the pressure was reduced to 0.13 kPa to perform a polymerization reaction. After that, the contents were taken out from the reactor after being maintained at 240°C and 0.13 kPa for 1 hour to obtain a polyester carbonate resin. Table 3 shows the physical property values ​​of the obtained polyester carbonate resin.

[0697] (Example 20)

[0698] 0.10 mol of 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl (BINL-2EO) as a diol compound, 0.06 mol of ethylene glycol (EG), 0.12 mol of 2,2'-bis(hydroxycarbonylmethoxy)-1,1'-binaphthyl (BINOL-DC) as a dicarboxylic acid, and 0.001 mol of tetrabutoxytitanium as a catalyst were put into a reactor equipped with a stirrer and a distillation device, heated to 180°C under normal pressure in a nitrogen atmosphere, and stirred for 30 minutes. After that, the temperature was raised to 255°C and the pressure was reduced to less than 0.13 kPa to perform a polymerization reaction. After that, the contents were taken out from the reactor after being maintained at 255°C and 0.13 kPa for 1 hour to obtain a polyester resin. The physical properties of the obtained polyester resin are shown in Table 4.

[0699] [Table 4]

[0700]

[0701]

[0702] Dihydroxy compounds may be further added

[0703]

[0704] [Manufacturing of monomers]

[0705] (Example 21: Preparation of Form A)

[0706] Step 1: Hydroxyethylation of 6,6'-dibromo-1,1'-bis(2-naphthol)

[0707] A nitrogen-purged vessel was charged with 1053 kg of anisole, 157.6 kg of 6,6′-dibromo-1,1′-bis(2-naphthol) (available from commercial sources), 14.6 kg of potassium carbonate, and 97 kg of ethylene carbonate. After the addition of the starting materials was completed, the vessel was heated in such a manner that the internal temperature reached 125-135° C. As indicated by the generation of gas, the reaction started at about 80-90° C. The reaction mixture was maintained at 125-135° C. for 40 hours until TLC showed that the conversion was complete. The reaction mixture was cooled in such a manner that the internal temperature reached 75° C. 145 kg of water was slowly added. The mixture was heated to 80° C. and stirred at this temperature for another 30 minutes. After stopping the stirring, layer separation occurred after 25 minutes. After the layer separation was completed, the lower aqueous layer was removed. 164 kg of sodium hydroxide solution (20% (w / w)) was added to the organic layer remaining in the vessel, and the mixture was stirred at 90° C. for 2 hours (reflux condenser). After 2 hours, the container was cooled to 80°C, stirring was stopped, and layer separation occurred after 25 minutes. The substantially lower aqueous layer was removed. The organic layer was further washed with 160 kg of water and 25 kg of sodium chloride (80°C, 30 minutes), and then the layers were separated for 20 minutes. The aqueous layer was removed.

[0708] The anisole solution of the target 2,2'-bis(2-hydroxyethoxy)-6,6'-dibromo-1,1'-binaphthyl in the organic layer thus obtained was used directly in the next step without isolating the compound.

[0709] Step 2: Preparation of 6,6'-DPBHBNA using Suzuki coupling

[0710] 84 g of tris-(o-tolyl)phosphine and 15 g of palladium (II) acetate were dissolved in 1.5 kg of anisole to prepare a catalyst solution.

[0711] In the first reaction vessel, the anisole solution of 2,2'-bis(2-hydroxyethoxy)-6,6'-dibromo-1,1'-binaphthyl obtained in step 1 was heated to 60°C, and 93.4 kg of phenylboronic acid was added. The mixture was stirred for 15 minutes until the phenylboronic acid was completely dissolved. Thereafter, the mixture was cooled to 40°C to 50°C.

[0712] In the second reaction vessel, 520 kg of a 31% (w / w) aqueous solution of tripotassium phosphate is heated to 50°C. Then, the pre-prepared catalyst solution is slowly added. As a result, a temperature rise of about 15°C occurs as a whole. After the catalyst is added, the mixture is stirred at 60-70°C for 1 hour. Then, the remaining 70% from container 1 is slowly added to the reaction vessel at 55-75°C. After the addition is completed, the mixture is stirred at 60°C for another hour. TLC shows that the conversion is complete. Layer separation occurs after 30 minutes at 50-60°C. Remove the lower water layer. To the organic layer, 186 kg of water and 125 kg of a 20 wt% aqueous solution of sodium hydroxide are added. The mixture is stirred at 55°C for 40 minutes. After that, the mixture is layer separated and the substantial water layer on the lower side is removed.

[0713] Then, 182 kg of 2M hydrochloric acid was added to the organic layer, and the mixture was stirred at 50-60°C for 30 minutes. The layers were separated, and the lower acidic aqueous layer was removed. The organic layer was further washed with 182 kg of 25 wt% brine at 50-60°C. The residual organic layer was stirred at 60-70°C with 10 kg of activated carbon. DX Ultra) and 50 kg of sodium sulfate were stirred for 90 minutes. In addition, the mixture was filtered through a pressure filter at 60 to 70° C. to prevent precipitation of the product (although 6,6'-DPBHBNA can be crystallized from anisole to form polyhedral crystals, the crystals do not have a specific composition and the yield is low).

[0714] After that, the filtrate (about 2500L) was transferred to a distiller. Anisole was distilled off at a temperature of more than 80°C and 90 mbar until about 200L of residue remained. Anisole can be recycled. After the vacuum was released, the residue was cooled to 55°C. At this temperature, 140kg of methanol and 60kg of toluene were added. The mixture was heated to 60-65°C while stirring until the precipitate dissolved and the solution became uniform. After the mixture became completely uniform, the container was cooled to 20°C. When the temperature was about 35-40°C, 40g of 6,6'-DPBHBNA was added to the solution as a seed crystal to start crystallization. The mixture was cooled to 20°C and stirred at 20°C for 4 hours. After that, the precipitate was recovered by centrifugal separation, and the filter cake was washed with two 10kg methanol.

[0715] Thus, 162 kg of 6,6'-DPBHBNA (loss on drying: 15%) was obtained, which was 137 kg of dry 6,6'-DPBHBNA, and the yield through two steps was equivalent to 74%. The chemical purity of the obtained 6,6'-DPBHBNA was 98% as determined by UPLC.

[0716] Step 3: Purification / recrystallization of 6,6'-DPBHBNA

[0717] 6,6'-DPBHBNA (142 kg, 270 mol; purity; 98.0%) obtained by the method of step 2 was dissolved in a mixture of methanol / toluene (7:3 (v / v); 827 kg). The solution was treated with activated carbon (8 kg) at 55°C for 2 hours. The activated carbon was removed by filtration, and the filtrate was cooled to 0°C over 4 hours while stirring, and then stirred at 0°C for 1 hour. Thus, 6,6'-DPBHBNA was crystallized. The crystals of 6,6'-DPBHBNA were collected by filtration and washed with methanol to obtain 154 kg of 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-bisnaphthyl (LOD: 14%; 252 mol; UPLC chemical purity; 98.8%).

[0718] The 6,6'-DPBHBNA thus obtained was dissolved in a mixture of methanol / toluene (7:3 (v / v); 772 kg), and the solution was treated again with activated carbon (7 kg) at 55°C for 2 hours. The activated carbon was removed by filtration, and the filtrate was cooled to 0°C over 5 hours while stirring, and then stirred at 0°C for 1 hour. The solid was collected by filtration and washed with methanol to obtain 131.4 kg of 6,6'-DPBHBNA (LOD: 14%; 220 moles; UPLC chemical purity; 99%). The product was determined to be a methanol solvate by PXRD.

[0719] Step 4: Conversion of the methanol solvate of 6,6'-DPBHBNA to Form A

[0720] The obtained 48 kg of methanol solvate of crystalline 6,6′-DPBHBNA was dried at 40° C. in air for 5 days to obtain 41.3 kg of crystalline 6,6′-DPBHBNA in the form of compact crystals with a size ranging from 5 to 200 μm.

[0721] According to GC measurement, the product obtained in step 4 contains 0.03% bw of methanol and 0.3% bw of toluene as solvent components, that is, based on the weight of 6,6'-DPBHBNA (2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl) (relative to 100% by weight of 6,6'-DPBHBNA), it contains 0.03% by weight of methanol and 0.3% by weight of toluene as solvent components.

[0722] The product of step 4 was analyzed by PXRD. Figure 2 As shown, this clearly shows that the crystalline form is form A. The following reflection peaks were observed.

[0723] [Table 5]

[0724] 2-θ(Theta) %* 6.52 8.07 8.61 22.93 9.42 8.71 10.44 8.04 11.01 24.95 13.19 26.54 14.94 38.29 15.46 16.41 16.19 29.40 17.35 24.87 17.79 25.59 18.43 24.31 18.97 28.39 20.88 100 21.45 45.06 22.50 15.27 22.92 15.41 23.69 20.41 24.49 17.30 25.89 17.46 27.75 15.03 30.82 12.46

[0725] *Indicates relative strength.

[0726] It was confirmed by UPLC that the product of step 4 contained 99.1% bw of 6,6'-DPBHBNA, 0.06% bw (0.06 wt%) of 6,6'-DPMHBNA, and 0.19% bw (0.19 wt%) of 6,6'-DPTHBNA.

[0727] The product of step 4 had a yellowness YI of 3.9 and a haze of 0.5 ntu.

[0728] The product of step 4 was analyzed by IR and NIR. Figure 3 As shown, IR Figure 4 In the NIR, around 7000 and 4500 cm -1 The habit of is characteristic of Form A, showing clear distinction from the solvate.

[0729] The DSC of the product of step 4 showed an endothermic peak with an onset at 113.6°C, a peak maximum at 124.4°C, and a reaction point at 112.9°C. The melting point was immediately determined and the melting points shown were 127.0°C, 126.5°C, and 126.8°C. DSC Figure 5 shown.

[0730] (Example 22: Preparation of methanol solvate of 6,6'-DPBHBNA)

[0731] 20 g of 6,6'-DPBHBNA (UPLC chemical purity; >99%) obtained in step 4 of Example 21 was dissolved in 600 ml of pure methanol and heated under reflux. When the homogeneous solution was slowly cooled to 22°C, 6,6'-DPBHBNA crystallized in a compact crystalline form with a size ranging from 10 to 200 μm. The crystals were collected by filtration, washed with methanol, and air-dried at 25° C. for 2 days to obtain 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl containing 5.98% bw of methanol, which corresponds to a substance having a molar ratio of 6,6′-DPBHBNA:methanol of approximately 1:1 (i.e., 6,6′-DPBHBNA containing 5.98% by weight of methanol based on the weight of 6,6′-DPBHBNA (2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl) (relative to 100% by weight of 6,6′-DPBHBNA)).

[0732] The product thus obtained was analyzed using PXRD. Figure 6 As shown, it was clear that the product was a substance with a crystalline form different from Form A and Form C, and the following reflection peaks were observed. [Table 6]

[0733] 2-θ(Theta) %* 6.23 16.29 8.45 3.99 9.03 50.21 10.59 61.47 11.79 8.13 12.51 11.36 13.00 41.31 14.87 85.66 16.02 8.34 16.93 26.66 17.69 7.31 18.21 22.01 18.45 32.77 19.20 49.49 19.56 53.32 20.86 59.04 21.54 100 22.11 17.86 22.72 20.60 24.29 44.09 24.86 23.58 26.18 22.33 26.65 11.83 27.66 16.59 28.67 12.87 30.48 15.82 31.61 9.93 32.47 8.349

[0734] *Indicates relative strength.

[0735] The product thus obtained was analyzed by IR and NIR. Figure 7 As shown, IR Figure 8 In the NIR, around 4500 and 4300 cm -1 The habit of is characteristic of methanol solvate, showing clear differences from Form A and other solvates.

[0736] The DSC of the product thus obtained showed an endothermic peak with an onset at 100.9°C, a peak maximum at 113.4°C, and a reaction point at 108.3°C. The melting point was immediately determined, and the melting points shown were 107.4°C, 108.7°C, and 107.7°C. DSC was as follows Fig. 9 shown.

[0737] (Example 23: Preparation of a mixture of Form A and methanol solvate)

[0738] Step 1: Hydroxyethylation of 6,6′-dibromo-1,1′-bis(2-naphthol)

[0739] A 2L three-necked flask equipped with a stirrer, a water separator, a reflux condenser, a thermometer and a bubble counter was filled with 89.7 g of 6,6′-dibromo-1,1′-bis(2-naphthol), 573 g of anisole, 8.3 g of K2CO3 and 52.8 g of ethylene carbonate, and the reaction mixture was heated under reflux (internal temperature was 125-135°C) and stirred for 6 hours. Some gas was confirmed to be generated. The progress of the reaction was monitored by TLC. After the reaction was completed, the reaction mixture was cooled to 70-80°C, 75 g of water and 25 g of brine were added, and the mixture was stirred for another 20 minutes at this temperature. After layer separation, 15% bw aqueous solution NaOH (110 g) was added to the organic layer, and the mixture was stirred at 95°C for 3 hours. After layer separation, the organic layer was washed with an aqueous solution prepared from 110 g of water and 25 g of brine. The organic layer obtained after layer separation was used directly in the next step without isolating the compound.

[0740] Step 2: Preparation of 6,6'-DPBHBNA using Suzuki coupling

[0741] In a 2L three-necked flask equipped with a stirrer, a reflux condenser and a thermometer, the organic solution obtained in the previous step 1 was filled, 50.0g of phenylboronic acid, K3PO4 (93.4g) and water (210g) were added, and the mixture was heated until the internal temperature reached 60°C. Then, 49mg of tris-(o-tolyl)phosphine and 9mg of palladium (II) acetate were added under vigorous stirring. The reaction mixture was slowly heated to reflux, and the progress of the reaction was monitored by TLC. After the reaction was completed (after 30 minutes to 1 hour), the mixture was cooled to 70°C and the aqueous layer was separated and removed. The organic layer was continuously washed with 150ml of 10% bw aqueous solution NaOH, 2M HCl aqueous solution (87.5ml), and again with brine (75ml). After that, the organic layer was treated with 2.5g of activated carbon and dried with sodium sulfate (12.5g). After filtration, the solvent was evaporated under vacuum and the residue was crystallized from a mixture of methanol (77 g) and toluene (33 g). In this way, a crystalline product was obtained which was collected by filtration.

[0742] Thus, 110 g of wet 6,6'-DPBHBNA (loss on drying: 15%) was obtained, which was 93.5 g of dry 6,6'-DPBHBNA, and the yield through two steps was equivalent to 89%. The chemical purity of the obtained 6,6'-DPBHBNA was 98% as determined by UPLC.

[0743] Step 3: Purification / recrystallization of 6,6'-DPBHBNA

[0744] 107 g of 6,6'-DPBHBNA (purity; 98.0%) obtained by the method of step 2 was dissolved in a mixture of methanol / toluene (7:3 (v / v); 535 g). The solution was treated with activated carbon (5.4 g) at 55°C for 2 hours. The activated carbon was removed by filtration, and the filtrate was cooled to 0°C while stirring, and stirred at 0°C for 1 hour and 30 minutes. Thus, 6,6'-DPBHBNA was crystallized in a compact crystalline form with a size ranging from 5 to 150 μm. The solid was collected by filtration, washed with methanol, and dried in air at room temperature overnight to obtain 85.0 g of 6,6'-DPBHBNA with a chemical purity of 99.89% (UPLC) and a yellowness YI of 2.1.

[0745] The product obtained in step 3 was determined by GC to contain a solvent component of 2.4% bw of methanol, 0.1% bw of toluene and 0.002% bw of anisole (i.e., it is 6,6'-DPBHBNA containing a solvent component of 2.4% by weight of methanol, 0.1% by weight of toluene and 0.002% by weight of anisole based on the weight of 6,6'-DPBHBNA (2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl) (relative to 100% by weight of 6,6'-DPBHBNA)).

[0746] The product of step 3 is analyzed by PXRD. Fig.10 As shown, the crystalline form of the product was confirmed to be a mixture of form A and methanol solvate. The following reflection peaks were observed.

[0747] [Table 7]

[0748] 2-θ(Theta) %* 6.25 10.87 8.61 58.88 8.98 33.71 9.47 16.41 10.59 41.40 11.82 9.716 12.95 36.20 13.25 22.35 14.82 100 16.02 11.65 16.27 11.10 17.03 26.14 18.43 37.00 19.31 57.83 19.60 48.99 20.83 91.68 21.47 90.71 22.28 23.42 22.62 34.69 24.39 51.81 24.96 27.86 26.13 34.43 27.61 18.75 28.93 14.31 30.28 14.82 30.67 14.72 31.68 11.82 32.47 12.43

[0749] *Indicates relative strength.

[0750] The product of step 3 was analyzed by IR and NIR. Fig.11 As shown, IR Fig.12 In the NIR, around 4500 and 4300 cm -1 The habit is characteristic of methanol solvates.

[0751] The DSC of the product of step 3 showed a first endothermic peak with an onset at 97.3°C, a peak maximum at 109.8°C, and a reaction point at 109.8°C, and a second peak with an onset at 118.9°C, a peak maximum at 124.4°C, and a reaction point at 121.4°C. The melting point was immediately determined, and the melting points shown were 118.6°C, 119.4°C, and 116.7°C. DSC is as follows Fig.13 shown.

[0752] (Example 24: Preparation of toluene solvate of 6,6'-DPBHBNA)

[0753] 20 g of 6,6'-DPBHBNA (UPLC chemical purity; >99.0%) obtained in step 4 of Example 21 was dissolved in 60 ml of pure toluene and heated under reflux. When the uniform solution was slowly cooled to 22°C, 6,6'-DPBHBNA crystallized in a compact crystalline form with a size ranging from 20 to 250 μm. The crystals were collected by filtration, washed with methanol, and air-dried at 25°C for 2 days to obtain 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl containing 5.6% bw of toluene, which was equivalent to a substance with a molar ratio of 6,6'-DPBHBNA:toluene of approximately 2.95:1. A microscopic photograph of the crystals obtained in this way is shown in Fig.14 .

[0754] The product thus obtained was analyzed using PXRD. Fig.15 As shown, it was found that the product had a crystalline form different from that of Form A, and the following reflection peaks were observed.

[0755] [Table 8]

[0756] 2-θ(Theta) %* 5.17 24.19 7.75 78.65 8.24 24.20 9.15 24.11 10.57 30.11 10.84 17.41 11.63 44.87 12.61 36.65 13.59 20.23 14.70 79.90 15.04 37.68 15.65 26.32 16.68 41.77 17.15 27.95 18.03 44.69 18.52 59.36 19.36 77.80 19.95 35.92 20.83 87.49 20.98 91.79 21.59 100 22.23 42.26 22.67 35.50 24.15 85.68 24.96 33.01 25.69 32.43 26.45 25.74 27.14 28.79 27.63 29.19

[0757] *Indicates relative strength.

[0758] The product thus obtained was analyzed by IR and NIR. Fig.16 As shown, IR Fig.17 In the NIR, around 7000 and 4700 cm -1 The habit of α-β-acetyl-1-nitropropene is characteristic of toluene solvate, showing clear differences from Form A, Form B and other solvates.

[0759] The DSC of the product thus obtained showed an endothermic peak with an onset at 106.5°C, a peak maximum at 113.6°C and a reaction point at 110.7°C. The melting point was immediately determined and the melting points shown were 103-107.9°C, 104.0-106.8°C and 104.8-107.6°C. Fig.18 shown.

[0760] (Example 25: Preparation of MEK Solvate of 6,6'-DPBHBNA)

[0761] 100 g of 6,6'-DPBHBNA (UPLC chemical purity; >99.0%) obtained in step 4 of Example 21 was dissolved in 300 ml of pure MEK and heated under reflux. When the uniform solution was slowly cooled to 22°C, 6,6'-DPBHBNA crystallized in a compact crystalline form with a size ranging from 20 to 200 μm. The crystals were collected by filtration, washed with MEK, air-dried at 25°C for 2 days, and then dried at 50°C for 1 hour to obtain 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl containing 8.5% bw of MEK, which was equivalent to a substance with a molar ratio of 6,6'-DPBHBNA:MEK of approximately 1.5:1. A microscopic photograph of the crystals obtained in this way is shown in Fig.19 .

[0762] The product thus obtained was analyzed using NIR. Fig. 20 In the NIR, 4600cm -1 The habit of is characteristic of MEK solvates, showing clear differences from Form A and other solvates.

[0763] The DSC of the product thus obtained showed an endothermic peak with an onset at 89.4°C, a peak maximum at 97.6°C and a reaction point at 95.5°C. The melting point was immediately determined and the melting points shown were 105.9°C and 105.8°C. Fig.21 shown.

[0764] The product of Example 25 thus obtained was analyzed using PXRD. Fig. 22 As shown, it was clear that the product was a substance with a crystalline form different from Form A and Form B, and the following reflection peaks were observed. [Table 9]

[0765] 2-0(Theta) %* 5.0 24.9 7.0 100 7.5 14.4 12.6 200.1 13.4 14.9 14.5 300.4 15.4 27.9 15.7 44.5 16.8 76.6 18.3 33.8 19.4 17.6 20.6 35.7 21.5 59.5 22.7 21.7 23.4 37.5 24.1 s1.9 25.6 24.1 26.2 19.5 26.6 17.0 29.1 13.7 30.8 11.1

[0766] *Indicates relative strength.

[0767] (Example 26: Preparation of Amorphous Form B of 6,6'-DPBHBNA)

[0768] 100 g of 6,6'-DPBHBNA (UPLC chemical purity; >99.0%) obtained in step 4 of Example 21 was heated to 130°C to obtain a clear melt. The melt was immediately cooled to 22°C within 2 minutes to obtain an amorphous (glassy) solid. The amorphous solid was flattened to form small pieces, which were ground in a mortar to obtain a powder.

[0769] The product thus obtained was analyzed using PXRD. Fig.23 As shown, the absence of a crystal layer is clear, as evidenced by the absence of a reflection peak in the range of 5° to 40° at 2θ. On the contrary, a broad halo is observed in the range of 2θ.

[0770] The product thus obtained was analyzed by IR and NIR. Fig.24 As shown, IR Fig.25 shown.

[0771] In DSC (not shown) of the product thus obtained, no endothermic peak was observed in the temperature range of 80 to 200° C. Instead, a step corresponding to the glass transition temperature was observed in the range of 109 to 110° C.

[0772] (Example 27: Preparation of Form C of 6,6'-DPBHBNA)

[0773] Example 27a

[0774] 20 g of 6,6'-DPBHBNA (UPLC chemical purity; >99.0%) obtained in step 4 of Example 21 was dissolved in 300 ml of 96% ethanol and heated under reflux. When the uniform solution was slowly cooled to 22°C, 6,6'-DPBHBNA crystallized in a compact crystalline form with a size ranging from 2 to 150 μm. The crystals were collected by filtration, washed with MEK, and air-dried at 25°C for 2 days and then dried at 50°C for 1 hour to obtain 15.8 g of 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl containing no detectable amount of ethanol.

[0775] Example 27b

[0776] 30 g of 6,6'-DPBHBNA (UPLC chemical purity; >99.0%) obtained in step 4 of Example 21 was dissolved in 250 ml of anisole at 100°C. When the homogeneous solution was cooled very slowly to 22°C, 6,6'-DPBHBNA crystallized in a compact crystalline form with a size ranging from 10 to 300 μm. The crystals were collected by filtration, washed with cooled anisole, and dried in a rotary evaporator at 80°C for 19 hours to obtain 11.4 g of 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl containing a very small amount of anisole (about 0.1% by weight) and no other solvent.

[0777] The product obtained in Example 27a was analyzed using PXRD. Fig.26 As shown, it was found that the crystalline form of the product was the same as the PXRD of the toluene solvate, but different from form A and other solvates, and showed the following reflection peaks. [Table 10]

[0778] 2-θ(Theta) %* 5.1 35.0 7.6 86.3 8.2 26.2 9.2 27.3 10.4 20.7 10.8 31.5 11.4 48.0 1 1.6 43.9 12.8 35.6 13.4 22.8 14.5 53.2 15.2 64.4 15.6 40.6 16.6 41.5 17.4 34.1 17.9 43.3 18.5 58.2 19.2 63.4 19.9 48.2 20.4 44.8 21.0 100.0 21.8 64.7 22.2 82.4 22.6 40.6 23.4 33.7 24.0 71.1 24.9 34.1 25.7 34.2 27.3 26.9 27.9 28.5

[0779] *Indicates relative strength.

[0780] The product obtained in Example 27b was analyzed by PXRD. This PXRD showed the same reflection peaks and habit as those of the product obtained in Example 27a, and it was confirmed that the crystals obtained in Example 27a and Example 27b had the same crystal morphology.

[0781] The product obtained in Example 27a was analyzed by IR and NIR. Fig. 27 As shown, IR Fig.28 In the NIR, around 7000 and 4700 cm -1 The habit of is characteristic of Form C, which shows clear differences from Forms A and B and solvates other than toluene solvate. The product obtained in Example 27b was also analyzed using IR and NIR. These spectra show the same phase as that of the product obtained in Example 27a.

[0782] The DSC of the product obtained in Example 27a showed an endothermic peak having an onset at 116.6°C, a peak maximum at 125.0°C, and a reaction point at 121.0°C. Fig.29 DSC of the product obtained in Example 27b showed an endothermic peak having an onset at 115.4°C, a peak maximum at 124.0°C and a reaction point at 120.0°C.

[0783] [Production of a polycarbonate resin composition using the monomers of the above examples]

[0784] (Example 28)

[0785] As raw materials, BINL-2EO as "Form A" obtained in Example 21, namely 7.9 kg (15.0 mol) of 6,6'-DPBHBNA, 16.8 kg (45.0 mol) of BNE, 21.5 kg (40.0 mol) of BNEF, 22.1 kg (103.0 mol) of DPC and 0.117 g (13.9 × 10 -4 mol), and put it into a 50L reactor with a stirrer and a distillation device through a hopper with a shovel. After that, nitrogen was filled into the reactor, and the reactor was pressurized to 780mmHg. After holding for 3 minutes, nitrogen was discharged from the exhaust port and restored to 760mmHg. Nitrogen was filled into the reactor again, and after holding for 3 minutes, nitrogen was discharged from the exhaust port and restored to 760mmHg. After that, nitrogen was filled into the reactor again, and after holding for 3 minutes, nitrogen was discharged from the exhaust port and restored to 760mmHg. After that, it was heated to 180°C under a nitrogen atmosphere of 760mmHg. After 20 minutes from the start of heating, it was confirmed that the raw material was completely dissolved, and then it was stirred for 120 minutes under this condition. After that, the decompression was adjusted to 200mmHg while the temperature was raised to 200°C at a rate of 60°C / hr. At this time, it was confirmed that the by-product phenol began to distill out. After that, it was kept at 200°C for 40 minutes to react. After that, the temperature was raised to 240°C at a rate of 75°C / hr. Ten minutes after the temperature was raised, the temperature was maintained while the degree of decompression was reduced to less than 1 mmHg over 1 hour. After that, the temperature was raised to 245°C at a rate of 60°C / hr and stirred for another 30 minutes. After the reaction was completed, nitrogen was introduced into the reactor to return to normal pressure, and the generated polycarbonate resin was pelletized and taken out. The Mw of the pellets was 27,500.

[0786] The obtained polycarbonate resin pellets were dried at 100°C for 3 hours, and the moisture content in the pellets was confirmed to be 1% by a Karl Fischer meter. The dried pellets were mixed with 1000 ppm of pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] (AO-60 manufactured by ADEKA: antioxidant), 1500 ppm of stearic acid monoglyceride (S-100A manufactured by Riken Vitamin Co., Ltd.: mold release agent), and 300 ppm of 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (PEP-36 manufactured by ADEKA: antioxidant) as additives, and the additives were added to the dried pellets. Thereafter, the pellets were melt-kneaded and pelletized by a twin-screw extruder while reducing the pressure to 40 mmHg.

[0787] The obtained polycarbonate resin composition had a refractive index of 1.680, an Abbe number of 18.1, a Tg of 147°C, an Mv of 11900, an Mw of 27000, a b value of 3.9, a moldability of A, a total light transmittance of 89%, and a total light transmittance after a PCT test of 89%.

[0788] The physical properties of the polycarbonate resin obtained in Example 28 are shown in Table 11 together with the physical properties of the resins of other Examples and the like.

[0789]

[0790] (BINL-2EO, i.e. 6,6'-DPBHBNA)

[0791] (Example 29)

[0792] As raw materials, 12.6 kg (24.0 mol) of BINL-2EO, 11.1 kg (30.0 mol) of BNE, 17.8 kg (33.0 mol) of BNEF, 8.1 kg (13.0 mol) of 2DNBINOL-2EO, 22.1 kg (103.0 mol) of DPC and 0.117 g (13.9 × 10 -4 mol), a polycarbonate resin and a polycarbonate composition were obtained in the same manner as in Example 28.

[0793] The obtained polycarbonate resin composition had a refractive index of 1.690, an Abbe number of 16.7, a Tg of 155°C, an Mv of 11900, an Mw of 27000, a b value of 3.9, a moldability of A, a total light transmittance of 89%, and a total light transmittance after a PCT test of 89%.

[0794] Table 11 shows the physical properties of the polycarbonate resin obtained in Example 29.

[0795]

[0796] (2DNBINOL-2EO) [Table 11]

[0797]

[0798] (Examples 30 to 36)

[0799] As raw materials, BINL-2EO shown in the table below, namely 6,6'-DPBHBNA 78.99 g (0.15 mol), BNE 168.50 g (0.45 mol), BNEF 215.45 g (0.40 mol), DPC 220.64 g (1.030 mol) and sodium bicarbonate 1.2 mg (1.39 × 10 -5 mol / made into an aqueous solution and added), and added to a 1L reactor with a stirrer and a distillation device through a funnel. After that, nitrogen was filled into the reactor, and the reactor was pressurized to 780 mmHg. After holding for 3 minutes, nitrogen was discharged from the exhaust port and restored to 760 mmHg. Nitrogen was filled into the reactor again, and after holding for 3 minutes, nitrogen was discharged from the exhaust port and restored to 760 mmHg. After that, nitrogen was filled into the reactor again, and after holding for 3 minutes, nitrogen was discharged from the exhaust port and restored to 760 mmHg. After that, it was heated to 180°C under a nitrogen atmosphere of 760 mmHg. After 20 minutes from the start of heating, it was confirmed that the raw material was completely dissolved, and then it was stirred under this condition for 120 minutes. After that, the degree of decompression was adjusted to 200 mmHg, and the temperature was raised to 200°C at a rate of 60°C / hr. At this time, it was confirmed that the by-product phenol began to distill out. After that, the reaction was maintained at 200°C for 40 minutes. After that, the temperature was raised to 240°C at a rate of 75°C / hr. Ten minutes after the temperature was raised, the temperature was maintained while the degree of decompression was reduced to less than 1 mmHg for 1 hour. After that, the temperature was raised to 245°C at a rate of 60°C / hr and stirred for another 30 minutes. After the reaction was completed, nitrogen was introduced into the reactor to return to normal pressure, and the generated polycarbonate resin was taken out. The optical properties of the obtained resin were the same as those of Example 28, but there was a slight difference in the molecular weight.

[0800] [Table 12]

[0801]

[0802] (Reference example)

[0803] In step 3 of Example 23, when "washing with methanol and drying in air at room temperature overnight", the drying time was shortened to obtain BINL-2EO containing 1.3 mol of methanol per 1 mol of 2,2'-bis(2-hydroxyethoxy)-6,6'-diphenyl-1,1'-binaphthyl, that is, 6,6'-DPBHBNA. The reaction was attempted in the same manner as in the additional Example 1 except that the main raw material was replaced with the BINL-2EO (6,6'-DPBHBNA obtained in this way.

[0804] As a result, when the raw material was charged into the reactor through the hopper with a shovel, it was difficult to charge smoothly, and not only the operability was poor, but also the progress of the reaction was slow. Compared with Example 28, the Mw of the obtained pellets was lower than 24,500.

[0805] The properties of the thermoplastic resins obtained in the examples and comparative examples are shown in a graph with the Abbe number (v) as the horizontal axis and the refractive index (nD) as the vertical axis. Fig.30 and 31 .

[0806] These graphs show specific ranges, for example,

[0807] exist Fig.30 The straight line nD=-0.02v+1.96 and the straight line nD=-0.02v+2.04, or

[0808] exist Fig.31 There are points of multiple embodiments marked between the straight line nD = -0.0002ν + 1.6718 and the straight line nD = -0.024ν + 2.124, or between the straight line nD = -0.004v + 1.744 and the straight line y = -0.02x + 2.04, from which it can be confirmed that in each embodiment, the balance between the Abbe number and the refractive index is good, and a thermoplastic resin suitable for optical applications is achieved.

[0809] For example, in Fig.31 The refractive index is higher than 1.660, the Abbe number is lower than 19 or is less than 19, for example, in the range of 13 to 19 or 15 to 19, and

[0810] In the region between the straight line nD=-0.0002ν+1.6718 and the straight line nD=-0.024ν+2.124, the polycarbonate resin satisfying the relationship of -0.0002ν+1.6718<nD<-0.024ν+2.124 has preferred properties.

[0811] In the region between the straight line nD=-0.004v+1.744 and the straight line nD=-0.024v+2.124, the polycarbonate resin satisfying the relationship -0.004v+1.744<nD<-0.024v+2.124 has more preferable properties.

[0812] In the region between the straight line nD=-0.02v+2.04 and the straight line nD=-0.024v+2.124, a polycarbonate resin satisfying the relationship -0.02v+2.04<nD<-0.024v+2.124 has further preferred properties.

Claims

1. A crystalline solvate, which is a crystalline solvate of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, Features: The crystal contains 0.3 to 1.2 mol of an organic solvent per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl. The organic solvent is selected from methanol, toluene and methyl ethyl ketone, The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is: (i) The following three reflection peaks are shown as 2θ values: 13.0±0.2°, 14.9±0.2°, and 21.5±0.2°, At least three of the following reflection peaks are shown as 2θ values: 6.2±0.2°, 9.0±0.2°, 10.6±0.2°, 16.9±0.2°, 18.2±0.2°, 18.5±0.2°, 19.2±0.2°, 19.6±0.2°, 20.9±0.2°, 22.7±0.2°, 24.3±0.2°, 24.9±0.2°, 26.2±0.2°, 28.7±0.2°, and 30.5±0.2°; or (ii) The following three reflection peaks are shown as 2θ values: 5.2±0.2°, 7.7±0.2°, and 21.6±0.2°, As 2θ values, at least three of the following reflection peaks are shown: 8.2±0.2°, 9.1±0.2°, 10.6±0.2°, 10.8±0.2°, 11.6±0.2°, 12.6±0.2°, 13.6±0.2°, 14.7±0.2°, 15.0±0.2°, 15.7±0.2°, 16.7±0.2°, 17.1±0.2°, 18. .0±0.2°, 18.5±0.2°, 19.4±0.2°, 19.9±0.2°, 20.8±0.2°, 21.0±0.2°, 22.2±0.2°, 22.7±0.2°, 24.1±0.2°, 25.0±0.2°, 25.7±0.2°, 26.5±0.2°, 27.1±0.2°, and 27.6±0.2°; or (iii) the following three reflection peaks are shown as 2θ values: 7.0±0.2°, 16.8±0.2°, and 23.4±0.2°, As 2θ values, at least three of the following reflection peaks are shown: 5.0±0.2°, 7.5±0.2°, 12.6±0.2°, 13.4±0.2°, 14.5±0.2°, 15.4±0.2°, 15.7±0.2°, 18.3±0.2°, 19.4±0.2°, 20.6±0.2°, 21.5±0.2°, 22.7±0.2°, 24.1±0.2°, 25.6±0.2°, 26.2±0.2°, 26.6±0.2° and 30.8±0.2°.

2. The morphology of the crystalline solvate according to claim 1, Features: The organic solvent is methanol.

3. The morphology of the crystalline solvate according to claim 2, Features: The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is: (i) The following three reflection peaks are shown as 2θ values: 13.0±0.2°, 14.9±0.2°, and 21.5±0.2°, As 2θ values, at least three of the following reflection peaks are shown: 6.2±0.2°, 9.0±0.2°, 10.6±0.2°, 16.9±0.2°, 18.2±0.2°, 18.5±0.2°, 19.2±0.2°, 19.6±0.2°, 20.9±0.2°, 22.7±0.2°, 24.3±0.2°, 24.9±0.2°, 26.2±0.2°, 28.7±0.2° and 30.5±0.2°.

4. The form of the crystalline solvate according to claim 2 or 3, Features: In differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, an endothermic peak having an onset in the range of 97 to 101°C was shown, and the maximum value of the peak was in the range of 108 to 115°C.

5. The form of the crystalline solvate according to claim 2 or 3, Features: The amount of methanol is 0.3 to 1.0 mol per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl.

6. The morphology of the crystalline solvate according to claim 1, Features: The organic solvent is toluene.

7. The form of the crystalline solvate according to claim 6, Features: The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is: (ii) The following three reflection peaks are shown as 2θ values: 5.2±0.2°, 7.7±0.2°, and 21.6±0.2°, As 2θ values, at least three of the following reflection peaks are shown: 8.2±0.2°, 9.1±0.2°, 10.6±0.2°, 10.8±0.2°, 11.6±0.2°, 12.6±0.2°, 13.6±0.2°, 14.7±0.2°, 15.0±0.2°, 15.7±0.2°, 16.7±0.2°, 17.1±0.2°, 18.4±0.2°, 19.8±0.2°, 20.1±0.2°, 21.3±0.2°, 22.4±0.2°, 23.9±0.2°, 24.8±0.2°, 25.9±0.2°, 26.1±0.2°, 27. 8.0±0.2°, 18.5±0.2°, 19.4±0.2°, 19.9±0.2°, 20.8±0.2°, 21.0±0.2°, 22.2±0.2°, 22.7±0.2°, 24.1±0.2°, 25.0±0.2°, 25.7±0.2°, 26.5±0.2°, 27.1±0.2° and 27.6±0.2°.

8. The form of the crystalline solvate according to claim 6 or 7, Features: In differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, an endothermic peak having an onset point in the range of 105 to 108°C was shown, and the maximum value of the peak was in the range of 112 to 115°C.

9. The form of the crystalline solvate according to claim 6 or 7, Features: The amount of toluene is 0.3 to 0.5 mol per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl.

10. A crystalline form A, which is a crystalline form A of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, Features: The crystal contains less than 0.1 mol of an organic solvent per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl. The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is: The following three reflection peaks were shown as 2θ values: 20.9±0.2°, 21.4±0.2°, and 23.7±0.2°. As 2θ values, at least three of the following reflection peaks are shown: 6.5±0.2°, 8.6±0.2°, 11.0±0.2°, 13.2±0.2°, 14.9±0.2°, 16.2±0.2°, 17.3±0.2°, 17.8±0.2°, 18.4±0.2°, and 19.0±0.2°.

11. The crystalline form according to claim 10, Features: In differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, an endothermic peak having an onset point in the range of 112 to 114°C was shown, and the maximum value of the peak was in the range of 124 to 126°C.

12. A crystalline form C, which is a crystalline form C of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, Features: The crystal contains less than 0.1 mol of an organic solvent per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl. The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is: The following three reflection peaks were shown as 2θ values: 5.1±0.2°, 7.6±0.2°, and 21.0±0.2°. As 2θ values, at least three of the following reflection peaks are shown: 8.2±0.2°, 9.2±0.2°, 10.4±0.2°, 10.8±0.2°, 11.6±0.2°, 12.8±0.2°, 13.4±0.2°, 14.5±0.2°, 15.2±0.2°, 15.6±0.2°, 16.6±0.2°, 17.4±0.2°. .2°, 17.9±0.2°, 18.5±0.2°, 19.2±0.2°, 19.9±0.2°, 20.4±0.2°, 21.8±0.2°, 22.2±0.2°, 22.6±0.2°, 13.4±0.2°, 24.0±0.2°, 25.7±0.2°, 27.3±0.2° and 27.9±0.2°.

13. The crystalline form according to claim 12, Features: In differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, an endothermic peak having an onset point in the range of 112 to 114°C was shown, and the maximum value of the peak was in the range of 124 to 126°C.

14. The crystalline form according to any one of claims 10 and 12, Features: The crystals have an aspect ratio of at most 5:

1.

15. An amorphous form B, which is an amorphous form B of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, Features: The crystal has a purity of at least 99.0% by weight based on organic matter, wherein the crystal contains less than 0.1 mol of an organic solvent per 1 mol of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl. The X-ray powder diffraction pattern obtained by irradiation with Cu Kα1 radiation at 22°C is: No reflection peak as a 2θ value is shown at multiple diffraction angles in the range of 5° to 40°. In differential scanning calorimetry (DSC) recorded in accordance with ISO 11357-3:2018 at a heating rate of 20 K / min, no endothermic peak is shown in the range of 80 to 200°C.

16. A 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl having at least one of the following characteristics: i. The yellowness index (YI) measured by a 5 w / w% dichloromethane solution of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl in accordance with ASTM E 313 is less than 3.0; and ii. The haze measured using a 5 w / w% dichloromethane solution of 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl is less than 1.0 ntu.

17. 2,2′-bis(2-hydroxyethoxy)-6,6′-diphenyl-1,1′-binaphthyl, Features: It exists in the crystalline form as described in claim 1, or in the amorphous form as described in claim 15.

Citation Information

Patent Citations

  • Alcohol having fluorene skeleton

    JP2014028806A

  • Production method of binaphthalene compound

    JP2014227387A

  • Production method of binaphthalene compound

    JP2014227388A

  • Method for producing 2,2'-bis(2-hydroxyethoxy)-1,1'-bi-naphthalene

    JP2015168658A

  • Crystal polymorph of 2,2'-bis(2-hydroxyethoxy)-1,1'-binaphthalene and production method of the same

    JP2015187098A