Modified polyfunctional epoxy resin as well as preparation method and application thereof

Through the preparation method of modified multifunctional epoxy resin, the problem of insufficient modulus of existing epoxy resin cured products is solved, and a high modulus and dense structure is achieved, which meets the mechanical properties requirements of semiconductor packaging.

CN118955434AActive Publication Date: 2024-11-15XIAMEN WELDTONE TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411022733.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The modulus of existing epoxy resin cured products is low and cannot meet the mechanical properties requirements of semiconductor packaging.

Method used

By using the preparation method of a modified multifunctional epoxy resin, a cured product with a dense three-dimensional network structure with a high modulus is formed by substitution reaction between intermediate compounds and halogenated epoxy compounds under an alkaline medium.

Benefits of technology

It improves the modulus and reliability of the cured substance, can effectively protect the packaging materials, and meet the application requirements of semiconductor packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955434A_ABST
    Figure CN118955434A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of organic adhesives, and particularly relates to modified polyfunctional epoxy resin as well as a preparation method and application thereof. The modified polyfunctional epoxy resin provided by the invention has a structure as shown in a formula (1). The key point of the invention is to provide the modified polyfunctional epoxy resin with the structure as shown in the formula (1), and the specific structure enables a cured product formed after the modified polyfunctional epoxy resin is cured to form a compact three-dimensional network structure, so that the modified polyfunctional epoxy resin has high modulus, the reliability of the cured product is improved, and the service life of the cured product is prolonged. Effective protection of a base material attached to a cured product is achieved, various packaging application requirements can be met, and the method has a good application prospect. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic adhesives, and specifically relates to a modified multifunctional epoxy resin and a preparation method and application thereof. Background Art

[0002] Since the material structure formed by epoxy resin after curing has obvious reliability advantages compared with other resins, it is often the first choice among many resin materials and is widely used in semiconductor packaging, adhesives, coatings, advanced composite materials and other fields. Among them, when epoxy resin is used in semiconductor packaging, the epoxy resin cured material is required to have good mechanical properties and can effectively protect semiconductor materials with packaging requirements, and the mechanical properties of epoxy resin cured material are mainly affected by modulus. However, most of the epoxy resins currently used in the packaging field are imported. Compared with domestic epoxy resins, their structures and functionality are richer and the halogen content is more accurately controlled. However, due to the limitations of their own structure, the existing epoxy resins have a low material modulus after curing and cannot meet the packaging requirements well. Summary of the invention

[0003] The first purpose of the present invention is to provide a modified multifunctional epoxy resin in view of the problem that the cured product formed by the existing epoxy resin has a low modulus and is difficult to meet the packaging requirements.

[0004] The second object of the present invention is to provide a method for preparing the modified multifunctional epoxy resin.

[0005] The third object of the present invention is to provide a modified multifunctional epoxy resin prepared by the above preparation method.

[0006] The fourth object of the present invention is to provide application of the modified multifunctional epoxy resin in semiconductor packaging.

[0007] Specifically, the modified multifunctional epoxy resin has a structure shown in formula (1);

[0008]

[0009] In formula (1), R1 and R2 are each independently a C1-C2 alkylene group, R3 and R4 are each independently a C1-C4 alkyl group, and R5 and R6 are each independently a hydrogen atom, a hydroxyl group, a C1-C4 alkyl group, or R7`` and R8`` are each independently C1-C4 alkylene, R9`` and R 10 `Each independently is hydrogen, hydroxyl, C1-C4 alkyl or R5' and R6' are each independently a C1-C4 alkylene group.

[0010] In a preferred embodiment, the modified multifunctional epoxy resin has a structure shown in formula (2) and / or formula (3):

[0011]

[0012] In formula (2) and formula (3), R1, R1', R2 and R2' are each independently a C1-C2 alkylene group, R3, R3', R4 and R4' are each independently a C1-C4 alkyl group, and R5 and R6 are each independently hydrogen, hydroxyl, C1-C4 alkyl or R7, R7', R8 and R8' are each independently C1-C4 alkylene, R9 and R 10 are independently hydrogen, hydroxy, C1-C4 alkyl or R5' and R6' are each independently a C1-C4 alkylene group.

[0013] The preparation method of the modified multifunctional epoxy resin comprises subjecting an intermediate compound having a structure represented by formula (4) to a substitution reaction with a halogenated epoxy alkane compound having a structure represented by formula (5) in the presence of an alkaline medium, and obtaining the modified multifunctional epoxy resin after purification;

[0014]

[0015] In formula (4) and formula (5), R1`` and R2`` are each independently a C1-C2 alkylene group, R3`` and R4`` are each independently a C1-C4 alkyl group, Q1` and Q2` are each independently a hydrogen group, a C1-C4 alkyl group or a hydroxyl group, Q3` and Q4` are each independently a hydrogen group, a C1-C4 alkyl group or a hydroxyl group, R is a C1-C4 alkylene group, and X is a halogen.

[0016] In a preferred embodiment, the intermediate compound has a structure shown in formula (6) and / or formula (7);

[0017]

[0018] In formula (6) and formula (7), R1, R1', R2 and R2' are each independently a C1-C2 alkylene group, R3, R3', R4 and R4' are each independently a C1-C4 alkyl group, Q1 and Q2 are each independently a hydrogen group, a C1-C4 alkyl group or a hydroxyl group, and Q3 and Q4 are each independently a hydrogen group, a C1-C4 alkyl group or a hydroxyl group.

[0019] In a preferred embodiment, the molar ratio of the intermediate compound to the halogenated epoxyalkylene compound is 1:(2.2-6.2).

[0020] In a preferred embodiment, the temperature of the substitution reaction is 50-70° C., and the time is 1-3 h.

[0021] In a preferred embodiment, the halogenated epoxyalkylene compound is selected from epichlorohydrin and / or epichlorohydrin.

[0022] In a preferred embodiment, the alkaline medium is selected from at least one of sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, ammonia water, sodium carbonate and potassium carbonate.

[0023] In a preferred embodiment, the intermediate compound is prepared by a method comprising the following steps:

[0024] S1. The alkoxy-formaldehyde benzene having the structure shown in formula (8) is subjected to a condensation reaction in the presence of a catalyst and then purified to obtain a first reaction product;

[0025] S2. The first reaction product is subjected to a reduction reaction in the presence of a reducing agent and then purified to obtain an intermediate compound;

[0026]

[0027] In formula (8), R1`` is a C1-C2 alkylene group, R3`` is a C1-C4 alkyl group, Q1` is a hydrogen atom, a C1-C4 alkyl group or a hydroxyl group, and Q3` is a hydrogen atom, a C1-C4 alkyl group or a hydroxyl group.

[0028] In a preferred embodiment, the alkoxy-aldehyde benzene has a structure shown in formula (9) and / or formula (10);

[0029]

[0030] In formula (9) and formula (10), R1 and R1' are each independently a C1-C2 alkylene group, R3 and R3' are each independently a C1-C4 alkyl group, Q1 is hydrogen, a C1-C4 alkyl group or a hydroxyl group, and Q3 is hydrogen, a C1-C4 alkyl group or a hydroxyl group.

[0031] In a preferred embodiment, in step S1, the alkoxy-formaldehyde benzene is selected from at least one of 3-methoxybenzaldehyde, 2-methyl-3-methoxybenzaldehyde, 2-ethyl-3-methoxybenzaldehyde, 2-hydroxy-3-methoxybenzaldehyde, 4-hydroxy-3-methoxybenzaldehyde and 2-methoxybenzaldehyde.

[0032] In a preferred embodiment, in step S1, the catalyst is Laccase enzyme.

[0033] In a preferred embodiment, in step S1, the condensation reaction temperature is 20-30° C. and the time is 1-3 hours.

[0034] In a preferred embodiment, in step S2, the reducing agent is selected from NaBH4 and / or LiAlH4.

[0035] In a preferred embodiment, in step S2, the reduction reaction is carried out at a temperature of 20 to 30° C. and for a time of 1 to 5 hours.

[0036] The key of the present invention is to provide a modified multifunctional epoxy resin having a structure shown in formula (1). This specific structure enables the cured product formed by the modified multifunctional epoxy resin after curing to form a dense three-dimensional network structure, thereby having a high modulus, improving the reliability of the cured product, and achieving effective protection of the substrate to which the cured product is attached, which can meet the requirements of various packaging applications and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 to Figure 6 They are respectively the nuclear magnetic resonance test result diagrams of the modified multifunctional epoxy resins prepared in Preparation Examples 1 to 6. DETAILED DESCRIPTION

[0038] The modified multifunctional epoxy resin provided by the present invention has a structure shown in formula (1). In formula (1), R1 and R2 are each independently a C1-C2 alkylene group, R3 and R4 are each independently a C1-C4 alkyl group, and R5 and R6 are each independently a hydrogen atom, a hydroxyl group, a C1-C4 alkyl group, or R7`` and R8`` are each independently C1-C4 alkylene, R9`` and R 10 `Each independently is hydrogen, hydroxyl, C1-C4 alkyl or R5' and R6' are each independently a C1-C4 alkylene group. The C1-C2 alkylene group may be a methylene group or an ethylene group. The C1-C4 alkyl group may be a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group or a tert-butyl group. The C1-C4 alkylene group may be a methylene group, an ethylene group, a n-propylene group, an isopropylene group, a n-butyl group, a sec-butyl group, an isobutyl group or a tert-butyl group.

[0039]

[0040] In the present invention, the modified multifunctional epoxy resin preferably has a structure as shown in formula (2) and / or formula (3). In formula (2) and formula (3), R1, R1', R2 and R2' are each independently preferably a C1-C2 alkylene group, R3, R3', R4 and R4' are each independently preferably a C1-C4 alkyl group, and R5 and R6 are each independently preferably hydrogen, hydroxyl, C1-C4 alkyl or R7, R7', R8 and R8' are each independently preferably a C1-C4 alkylene group, and R9 and R 10 Each is independently preferably hydrogen, hydroxy, C1-C4 alkyl or R5' and R9' are each independently preferably C1-C4 alkylene groups, wherein specific examples of C1-C2 alkylene groups, C1-C4 alkyl groups and C1-C4 alkylene groups are as described above and are not described in detail here.

[0041]

[0042] The preparation method of the modified multifunctional epoxy resin provided by the present invention comprises the steps of subjecting an intermediate compound having a structure shown in formula (4) to a substitution reaction with a halogenated epoxy alkane compound having a structure shown in formula (5) in the presence of an alkaline medium, and obtaining the modified multifunctional epoxy resin after purification;

[0043]

[0044] In formula (4) and formula (5), R1`` and R2`` are each independently a C1-C2 alkylene group, R3`` and R4`` are each independently a C1-C4 alkyl group, Q1` and Q2` are each independently a hydrogen, a C1-C4 alkyl group or a hydroxyl group, Q3` and Q4` are each independently a hydrogen, a C1-C4 alkyl group or a hydroxyl group, R is a C1-C4 alkylene group, and X is a halogen. Among them, the C1-C2 alkylene group may be a methylene group or an ethylene group. The C1-C4 alkyl group may be: a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group or a tert-butyl group. The C1-C4 alkylene group may be: a methylene group, an ethylene group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group or a tert-butyl group. The X may be a fluorine group, a chlorine group, a bromine group or an iodine group.

[0045] In the present invention, the intermediate compound preferably has a structure represented by formula (6) and / or formula (7);

[0046]

[0047] In formula (6) and formula (7), R1, R1', R2 and R2' are each independently preferably C1-C2 alkylene, R3, R3', R4 and R4' are each independently preferably C1-C4 alkyl, Q1 and Q2 are each independently preferably hydrogen, C1-C4 alkyl or hydroxyl, Q3 and Q4 are each independently hydrogen, C1-C4 alkyl or hydroxyl, R is C1-C4 alkylene, and X is halogen. Specific examples of C1-C2 alkylene, C1-C4 alkyl and C1-C4 alkylene are as described above and are not described one by one here.

[0048] The present invention does not particularly limit the input amount ratio of the intermediate compound and the halogenated epoxy alkylene compound during the substitution reaction, as long as the generated product can be mainly a modified multifunctional epoxy resin. In some specific embodiments, the molar ratio of the intermediate compound to the halogenated epoxy alkylene compound is preferably 1:(2.2-6.2), such as 1:2.2, 1:2.5, 1:2.8, 1:3, 1:4, 1:5, 1:6 or any value therebetween.

[0049] The present invention does not particularly limit the conditions of the substitution reaction, as long as the epoxy group can be modified to the intermediate compound to obtain a modified multifunctional epoxy resin. In some specific embodiments, the temperature of the substitution reaction is preferably 50 to 70°C, such as 50°C, 55°C, 60°C, 65°C, 70°C or any value therebetween; the time is preferably 1 to 3 hours, such as 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours or any value therebetween.

[0050] In the present invention, the halogenated epoxyalkylene compound may have a structure represented by formula (5). In view of the availability of raw materials, the halogenated epoxyalkylene compound is particularly preferably epichlorohydrin and / or epichlorohydrin.

[0051] In the present invention, the alkaline medium can be any compound that can make the pH value of the reaction system alkaline, and specific examples thereof can be at least one of sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, ammonia water, sodium carbonate and potassium carbonate, and more preferably sodium hydroxide and / or potassium hydroxide. The present invention has no specific limitation on the amount of the alkaline medium, and the amount thereof can be any amount that can provide a suitable alkaline environment for the substitution reaction.

[0052] In the preparation process of the modified multifunctional epoxy resin, the substitution reaction is preferably carried out in the following manner: the intermediate compound having the structure shown in formula (6) and / or formula (7) is mixed and stirred with the halogenated epoxy alkylene compound having the structure shown in formula (5), and heated to 50-70°C at the same time, and then the alkaline medium is added dropwise to the above mixture, and the reaction is continued at 50-70°C for 1-3 hours, and then purified to obtain the modified multifunctional epoxy resin. The purification method can be to extract the obtained product with dichloromethane as an extractant, and the obtained extract phase is washed with water 1-3 times and then treated with reduced pressure distillation.

[0053] In the present invention, the intermediate compound can be obtained by commercial purchase or by various methods known in the prior art. In a specific embodiment, the intermediate compound is preferably prepared by a method comprising the following steps: S1. condensing an alkoxy-formylbenzene having a structure shown in formula (8) in the presence of a catalyst and then purifying it to obtain a first reaction product; S2. reducing the first reaction product in the presence of a reducing agent and then purifying it to obtain an intermediate compound;

[0054]

[0055] In formula (8), R1`` is preferably a C1-C2 alkylene group, R3`` is preferably a C1-C4 alkyl group, Q1` is preferably hydrogen, a C1-C4 alkyl group or a hydroxyl group, and Q3` is hydrogen, a C1-C4 alkyl group or a hydroxyl group. Specific examples of the C1-C2 alkylene group and the C1-C4 alkyl group are as described above and are not described one by one here.

[0056] In the preparation process of the intermediate compound, the alkoxy-formaldehyde benzene can be any one of the structures shown in formula (8), more preferably the structures shown in formula (9) and / or formula (10). From the perspective of the availability of raw materials, the alkoxy-formaldehyde benzene is particularly preferably at least one selected from 3-methoxybenzaldehyde, 2-methyl-3-methoxybenzaldehyde, 2-ethyl-3-methoxybenzaldehyde, 2-hydroxy-3-methoxybenzaldehyde, 4-hydroxy-3-methoxybenzaldehyde and 2-methoxybenzaldehyde.

[0057]

[0058] In formula (6) and formula (7), R1 and R1' are each independently a C1-C2 alkylene group, R3 and R3' are each independently a C1-C4 alkyl group, Q1 is hydrogen, a C1-C4 alkyl group or a hydroxyl group, and Q3 is hydrogen, a C1-C4 alkyl group or a hydroxyl group. Specific examples of the C1-C2 alkylene group and the C1-C4 alkyl group are as described above and are not described one by one here.

[0059] In the preparation process of the above intermediate compound, the catalyst can be any existing compound that can catalyze the condensation reaction of the benzene ring in the alkoxy-aldehyde benzene to obtain a biphenyl structure, preferably a laccase enzyme. When the catalyst is laccase, the ratio of the added enzyme activity to the molar amount of the alkoxy-aldehyde benzene is preferably (10-15) U:1 mmol, such as 10 U:1 mmol, 11 U:1 mmol, 12 U:1 mmol, 13 U:1 mmol, 14 U:1 mmol, 15 U:1 mmol or any value therebetween.

[0060] The present invention does not particularly limit the conditions of the condensation reaction, as long as the benzene ring in the alkoxy-aldehyde benzene can be subjected to a condensation reaction to obtain a first reaction product having a biphenyl structure. In some specific embodiments, the temperature of the condensation reaction is preferably 20 to 30°C, such as 20°C, 22°C, 25°C, 28°C, 30°C or any value therebetween; the time is preferably 1 to 3h, such as 1h, 1.5h, 2h, 2.5h, 3h or any value therebetween.

[0061] In the preparation process of the above intermediate compound, in step S1, the condensation reaction is preferably carried out in the following manner: dissolving the alkoxy-formylbenzene having the structure shown in formula (9) and / or formula (10) in a first organic solvent and an optional sodium acetate buffer solution, adding a catalyst, reacting at 20-30° C. for 1-3 hours, acidifying the reactant after the reaction, and then purifying to obtain a first reaction product. The purification method can be to extract the obtained product with dichloromethane as an extractant, washing the obtained extract phase with water for 1-3 times and then distilling under reduced pressure.

[0062] In the preparation process of the above intermediate compound, in step S1, the first reaction product may have a structure as shown in formula (11), and more preferably has a structure as shown in formula (12) and / or formula (13);

[0063]

[0064] In formula (11), R1`` and R2`` are each independently preferably C1~C2 alkylene, R3`` and R4`` are each independently preferably C1~C4 alkyl, Q1` and Q2` are each independently preferably hydrogen, C1~C4 alkyl or hydroxyl, Q3` and Q4` are each independently preferably hydrogen, C1~C4 alkyl or hydroxyl. In formula (12) and formula (13), R1 and R1` are each independently C1~C2 alkylene, R3 and R3` are each independently C1~C4 alkyl, Q1 is hydrogen, C1~C4 alkyl or hydroxyl, and Q3 is hydrogen, C1~C4 alkyl or hydroxyl. Among them, specific examples of C1~C2 alkylene and C1~C4 alkyl are as described above and will not be repeated here.

[0065] In the preparation process of the above intermediate compound, the reducing agent can be any existing compound capable of reducing the aldehyde group in the first reaction product to a hydroxyl group, and a specific example thereof can be NaBH4 and / or LiAlH4. The present invention does not specifically limit the amount of the reducing agent, as long as the aldehyde group in the first reaction product can be substantially reduced to a hydroxyl group. In a preferred embodiment, the molar ratio of the reducing agent to the first reaction product is (2 to 5):1, such as 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1 or any value therebetween.

[0066] The present invention does not particularly limit the conditions of the reduction reaction, as long as the first reaction product can be reduced to obtain an intermediate compound having a structure shown in formula (4). In some specific embodiments, the temperature of the reduction reaction is preferably 20 to 30°C, such as 20°C, 22°C, 25°C, 28°C, 30°C or any value therebetween; the time is preferably 1 to 5h, such as 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h or any value therebetween.

[0067] In the preparation process of the above intermediate compound, in step S2, the reduction reaction is preferably carried out in the following manner: the first reaction product prepared in step S1 is dissolved in a second organic solvent, a reducing agent is added, and the reaction is carried out at 20 to 30° C. for 1 to 5 hours, and then the second organic solvent is added to stop the reaction, the reaction solution is subjected to rotary evaporation, and then extracted with dichloromethane as an extractant, and the obtained extract phase is washed with water for 1 to 3 times and then subjected to reduced pressure distillation to obtain the intermediate compound.

[0068] In the preparation process of the intermediate compound, the first organic solvent and the second organic solvent are each independently selected from at least one of methanol, acetone, ethanol, benzene, toluene and N,N-dimethylformamide.

[0069] In addition, the terms "first" and "second" are only for the convenience of distinction and description and have no other special meanings.

[0070] The present invention will be described in detail below through specific embodiments.

[0071] The raw materials and their sources used in the following preparation examples and embodiments are as follows: bisphenol A epoxy resin, purchased from Mitsubishi Chemical, brand 828; Laccase enzyme, purchased from Sigma-Aldrich, brand 38429.

[0072] Preparation Example 1 Preparation of modified multifunctional epoxy resin

[0073] The preparation method of the modified multifunctional epoxy resin provided by the present invention has the following specific steps and reaction process:

[0074] S1. 3-methoxybenzaldehyde (353.7 mg, 2.6 mmol) was dissolved in 9 mL of acetone solvent, and then 430 mL of sodium acetate buffer solution and Laccase enzyme (2.5 mg, 27 U) were added, and the reaction was carried out at room temperature for 2 h, and then the reaction mixture was acidified with HCl (5 M, 25 mL), stirred at room temperature for 5 min, and then extracted with dichloromethane, washed with water, and dried by reduced pressure distillation to obtain a first reaction product;

[0075] S2. The first reaction product of step S1 (270 mg, 1 mmol) was dissolved in 20 mL of methanol solution, and NaBH4 (95 mg, 2.5 mmol) was added to react at room temperature for 3 h. When the reaction time was reached, a large amount of methanol was added to stop the reaction, and the reaction mixture was subjected to rotary evaporation, and then extracted with dichloromethane, washed with water, and dried by vacuum distillation to obtain an intermediate compound;

[0076] S3. The intermediate compound (274 mg, 1 mmol) of step S1 and epichlorohydrin (230 mg, 2.5 mmol) were mixed and heated. When the temperature reached 50°C, 35 mL of 30% NaOH solution was added dropwise to the mixture. After the addition, the temperature was raised to 70°C and the reaction was continued for 1 hour. Then, the mixture was extracted with dichloromethane, washed with water and dried by vacuum distillation to obtain a modified multifunctional epoxy resin. The synthesis process and structure are shown below.

[0077] Depend on Figure 1 It can be seen that the successful synthesis of the modified multifunctional epoxy resin having the structure shown below was proved by nuclear magnetic resonance testing.

[0078]

[0079] Preparation Example 2 Preparation of modified multifunctional epoxy resin

[0080] S1. 2-methyl-3-methoxybenzaldehyde (390.4 mg, 2.6 mmol) was dissolved in 9 mL of acetone solvent, and then 430 mL of sodium acetate buffer solution and Laccase enzyme (2.5 mg, 27 U) were added, and the reaction was carried out at room temperature for 2 h, and the reaction mixture was acidified with HCl (5 M, 25 mL), stirred at room temperature for 5 min, and then extracted with dichloromethane, washed with water, and dried by reduced pressure distillation to obtain a first reaction product;

[0081] S2. The first reaction product of step S1 (298 mg, 1 mmol) was dissolved in 20 mL of methanol solution, and NaBH4 (95 mg, 2.5 mmol) was added to react at room temperature for 3 h. When the reaction time was reached, a large amount of methanol was added to stop the reaction, and the reaction mixture was subjected to rotary evaporation, and then extracted with dichloromethane, washed with water, and dried by vacuum distillation to obtain an intermediate compound;

[0082] S3. The intermediate compound (302 mg, 1 mmol) of step S1 and epichlorohydrin (230 mg, 2.5 mmol) are mixed and heated. When the temperature rises to 50°C, 35 mL of 30% NaOH solution is added dropwise to the mixture. After the addition, the temperature is raised to 70°C and the reaction is continued for 1 hour. Then, extraction is carried out with dichloromethane, washing with water and drying by reduced pressure distillation to obtain a modified multifunctional epoxy resin.

[0083] Depend on Figure 2 It can be seen that the successful synthesis of the modified multifunctional epoxy resin having the structure shown below was proved by nuclear magnetic resonance testing.

[0084]

[0085] Preparation Example 3 Preparation of modified multifunctional epoxy resin

[0086] S1. 2-ethyl-3-methoxybenzaldehyde (426.9 mg, 2.6 mmol) was dissolved in 9 mL of acetone solvent, and then 430 mL of sodium acetate buffer solution and Laccase enzyme (2.5 mg, 27 U) were added, and the reaction was carried out at room temperature for 2 h, and then the reaction mixture was acidified with HCl (5 M, 25 mL), stirred at room temperature for 5 min, and then extracted with dichloromethane, washed with water, and dried by reduced pressure distillation to obtain a first reaction product;

[0087] S2. The first reaction product of step S1 (326 mg, 1 mmol) was dissolved in 20 mL of methanol solution, and NaBH4 (95 mg, 2.5 mmol) was added to react at room temperature for 3 h. When the reaction time was reached, a large amount of methanol was added to stop the reaction, and the reaction mixture was subjected to rotary evaporation, and then extracted with dichloromethane, washed with water, and dried by vacuum distillation to obtain an intermediate compound;

[0088] S3. The intermediate compound (330 mg, 1 mmol) of step S1 and epichlorohydrin (230 mg, 2.5 mmol) are mixed and heated. When the temperature rises to 50°C, 35 mL of 30% NaOH solution is added dropwise to the mixture. After the addition, the temperature is raised to 70°C and the reaction is continued for 1 hour. Then, extraction is carried out with dichloromethane, washing with water and drying by reduced pressure distillation to obtain a modified multifunctional epoxy resin.

[0089] Depend on Figure 3 It can be seen that the successful synthesis of the modified multifunctional epoxy resin having the structure shown below was proved by nuclear magnetic resonance testing.

[0090]

[0091] Preparation Example 4 Preparation of modified multifunctional epoxy resin

[0092] S1. 2-Hydroxy-3-methoxybenzaldehyde (395.6 mg, 2.6 mmol) was dissolved in 9 mL of acetone solvent, and then 430 mL of sodium acetate buffer solution and Laccase enzyme (2.5 mg, 27 U) were added, and the reaction was carried out at room temperature for 2 h, and then the reaction mixture was acidified with HCl (5 M, 25 mL), stirred at room temperature for 5 min, and then extracted with dichloromethane, washed with water, and dried by reduced pressure distillation to obtain a first reaction product;

[0093] S2. The first reaction product of step S1 (302 mg, 1 mmol) was dissolved in 20 mL of methanol solution, and NaBH4 (95 mg, 2.5 mmol) was added to react at room temperature for 3 h. When the reaction time was reached, a large amount of methanol was added to stop the reaction, and the reaction mixture was subjected to rotary evaporation, and then extracted with dichloromethane, washed with water, and dried by vacuum distillation to obtain an intermediate compound;

[0094] S3. The intermediate compound (306 mg, 1 mmol) of step S1 and epichlorohydrin (462.5 mg, 5 mmol) are mixed and heated. When the temperature rises to 50°C, 35 mL of 30% NaOH solution is added dropwise to the mixture. After the addition, the temperature is raised to 70°C and the reaction is continued for 1 hour. Then, extraction is carried out with dichloromethane, washing with water and drying by reduced pressure distillation to obtain a modified multifunctional epoxy resin.

[0095] Depend on Figure 4 It can be seen that the successful synthesis of the modified multifunctional epoxy resin having the structure shown below was proved by nuclear magnetic resonance testing.

[0096]

[0097] Preparation Example 5 Preparation of modified multifunctional epoxy resin

[0098] A modified multifunctional epoxy resin was prepared according to the method of Preparation Example 4, except that the same molar amount of 3-methoxy-4-hydroxybenzaldehyde was used instead of 2-hydroxy-3-methoxybenzaldehyde, and the other conditions were the same as those of Preparation Example 4 to obtain a modified multifunctional epoxy resin.

[0099] Depend on Figure 5 It can be seen that the successful synthesis of the modified multifunctional epoxy resin having the structure shown below was proved by nuclear magnetic resonance testing.

[0100]

[0101] Preparation Example 6 Preparation of modified multifunctional epoxy resin

[0102] The modified multifunctional epoxy resin was prepared according to the method of Preparation Example 1, except that the same molar amount of 2-methoxybenzaldehyde was used instead of 3-methoxybenzaldehyde, and the other conditions were the same as those of Preparation Example 1 to obtain the modified multifunctional epoxy resin.

[0103] Depend on Figure 6 It can be seen that the successful synthesis of the modified multifunctional epoxy resin having the structure shown below was proved by nuclear magnetic resonance testing.

[0104]

[0105] Example 1 Preparation of epoxy resin adhesive

[0106] The components of the epoxy resin adhesive and their weight proportions are as follows: 15 parts of the modified multifunctional epoxy resin provided in Preparation Example 1, 25 parts of bisphenol A epoxy resin, 10 parts of meta-phenylenediamine, and 50 parts of silica powder.

[0107] The preparation method of the epoxy resin adhesive is specifically as follows: a modified multifunctional epoxy resin, a bisphenol A epoxy resin and m-phenylenediamine are mixed uniformly in a container to obtain a premix, silicon dioxide powder is added to the premix and mixed uniformly, and then the obtained mixture is passed through three rollers twice, and then transferred to a double planetary hybrid stirring kettle and stirred for 30 minutes, and the wall is scraped when the stirring time is 15 minutes. After the mixing is completed, the mixture is vacuumed and degassed, and then discharged to obtain the epoxy resin adhesive.

[0108] Example 2 Preparation of epoxy resin adhesive

[0109] The components of the epoxy resin adhesive and their weight proportions are as follows: 35 parts of the modified multifunctional epoxy resin provided in Preparation Example 1, 5 parts of bisphenol A epoxy resin, 10 parts of m-phenylenediamine, and 50 parts of silica powder.

[0110] The preparation method of the epoxy resin adhesive is specifically as follows: a modified multifunctional epoxy resin, a bisphenol A epoxy resin and m-phenylenediamine are mixed uniformly in a container to obtain a premix, silicon dioxide powder is added to the premix and mixed uniformly, and then the obtained mixture is passed through three rollers twice, and then transferred to a double planetary hybrid stirring kettle and stirred for 30 minutes, and the wall is scraped when the stirring time is 15 minutes. After the mixing is completed, the mixture is vacuumed and degassed, and then discharged to obtain the epoxy resin adhesive.

[0111] Example 3 Preparation of epoxy resin adhesive

[0112] The components of the epoxy resin adhesive and their weight proportions are as follows: 5 parts of the modified multifunctional epoxy resin provided in Preparation Example 1, 35 parts of bisphenol A epoxy resin, 10 parts of m-phenylenediamine, and 50 parts of silicon dioxide powder.

[0113] The preparation method of the epoxy resin adhesive is specifically as follows: a modified multifunctional epoxy resin, a bisphenol A epoxy resin and m-phenylenediamine are mixed uniformly in a container to obtain a premix, silicon dioxide powder is added to the premix and mixed uniformly, and then the obtained mixture is passed through three rollers twice, and then transferred to a double planetary hybrid stirring kettle and stirred for 30 minutes, and the wall is scraped when the stirring time is 15 minutes. After the mixing is completed, the mixture is vacuumed and degassed, and then discharged to obtain the epoxy resin adhesive.

[0114] Example 4 Preparation of epoxy resin adhesive

[0115] An epoxy resin adhesive was prepared according to the method of Example 1, except that the modified multifunctional epoxy resin provided in Preparation Example 2 was used in the same weight portion instead of the modified multifunctional epoxy resin provided in Preparation Example 1, and the other conditions were the same to obtain an epoxy resin adhesive.

[0116] Example 5 Preparation of epoxy resin adhesive

[0117] An epoxy resin adhesive was prepared according to the method of Example 1, except that the modified multifunctional epoxy resin provided in Preparation Example 3 was used in the same weight portion instead of the modified multifunctional epoxy resin provided in Preparation Example 1, and the other conditions were the same to obtain an epoxy resin adhesive.

[0118] Example 6 Preparation of epoxy resin adhesive

[0119] An epoxy resin adhesive was prepared according to the method of Example 1, except that the modified multifunctional epoxy resin provided in Preparation Example 4 was used in the same weight portion instead of the modified multifunctional epoxy resin provided in Preparation Example 1, and the other conditions were the same to obtain an epoxy resin adhesive.

[0120] Example 7 Preparation of epoxy resin adhesive

[0121] An epoxy resin adhesive was prepared according to the method of Example 1, except that the modified multifunctional epoxy resin provided in Preparation Example 5 was used in the same weight portion instead of the modified multifunctional epoxy resin provided in Preparation Example 1, and the other conditions were the same to obtain an epoxy resin adhesive.

[0122] Example 8 Preparation of epoxy resin adhesive

[0123] An epoxy resin adhesive was prepared according to the method of Example 1, except that the modified multifunctional epoxy resin provided in Preparation Example 6 was used in the same weight portion instead of the modified multifunctional epoxy resin provided in Preparation Example 1, and the other conditions were the same to obtain an epoxy resin adhesive.

[0124] Comparative Example 1 Preparation of Reference Epoxy Resin Adhesive

[0125] A reference epoxy resin adhesive was prepared according to the method of the example, except that the same weight portion of bisphenol A epoxy resin was used instead of the modified multifunctional epoxy resin provided in Preparation Example 1, and the other conditions were the same to obtain a reference epoxy resin adhesive.

[0126] Test Case

[0127] The epoxy resin adhesives prepared in the above examples and comparative examples were tested for viscosity, glass transition temperature and modulus according to the following methods. The results are shown in Table 1.

[0128] (1) Viscosity: The initial viscosity of the epoxy resin adhesive just prepared and the viscosity after standing for 24 hours were tested using a Brookfield viscometer. Specifically, at room temperature, the epoxy adhesive was rotated and stirred for 30 minutes using a 29# rotor, and then the viscosity data was measured at a rotation speed of 5 rpm.

[0129] (2) Glass transition temperature (Tg): The epoxy resin adhesive was cured at 150°C / 120 min and the glass transition temperature was measured using a differential calorimeter. The heating rate during the test was 10°C / min.

[0130] (3) Modulus: The epoxy resin adhesive was cured at 150°C / 120 min and made into a specimen with a size of 55 mm*5 mm*2 mm. The specimen was tested on the DMA in the measurement mode of dual cantilever mode, with a vibration frequency of 1 Hz, an amplitude of 10 μm, a heating rate of 10°C / min, and a test temperature range of -65°C to 300°C. The modulus data at 200°C were selected for comparison.

[0131] Table 1

[0132]

[0133] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention.

Claims

1. A modified multifunctional epoxy resin, characterized in that: The modified multifunctional epoxy resin has a structure shown in formula (1); In formula (1), R1 and R2 are each independently a C1-C2 alkylene group, R3 and R4 are each independently a C1-C4 alkyl group, and R5 and R6 are each independently a hydrogen atom, a hydroxyl group, a C1-C4 alkyl group, or R7`` and R8`` are each independently C1-C4 alkylene, R9`` and R 10 `Each independently is hydrogen, hydroxyl, C1-C4 alkyl or R5' and R6' are each independently a C1-C4 alkylene group.

2. The modified multifunctional epoxy resin according to claim 1, characterized in that: The modified multifunctional epoxy resin has a structure shown in formula (2) and / or formula (3): In formula (2) and formula (3), R1, R1', R2 and R2' are each independently a C1-C2 alkylene group, R3, R3', R4 and R4' are each independently a C1-C4 alkyl group, and R5 and R6 are each independently hydrogen, hydroxyl, C1-C4 alkyl or R7, R7', R8 and R8' are each independently C1-C4 alkylene, R9 and R 10 are independently hydrogen, hydroxy, C1-C4 alkyl or R5' and R6' are each independently a C1-C4 alkylene group.

3. A method for preparing a modified multifunctional epoxy resin, characterized in that: The method comprises subjecting an intermediate compound having a structure shown in formula (4) to a substitution reaction with a halogenated epoxy alkane compound having a structure shown in formula (5) in the presence of an alkaline medium, and obtaining a modified multifunctional epoxy resin after purification; In formula (4) and formula (5), R1`` and R2`` are each independently a C1-C2 alkylene group, R3`` and R4`` are each independently a C1-C4 alkyl group, Q1` and Q2` are each independently a hydrogen group, a C1-C4 alkyl group or a hydroxyl group, Q3` and Q4` are each independently a hydrogen group, a C1-C4 alkyl group or a hydroxyl group, R is a C1-C4 alkylene group, and X is a halogen.

4. The method for preparing a modified multifunctional epoxy resin according to claim 3, characterized in that: The intermediate compound has a structure shown in formula (6) and / or formula (7); In formula (6) and formula (7), R1, R1', R2 and R2' are each independently a C1-C2 alkylene group, R3, R3', R4 and R4' are each independently a C1-C4 alkyl group, Q1 and Q2 are each independently a hydrogen group, a C1-C4 alkyl group or a hydroxyl group, and Q3 and Q4 are each independently a hydrogen group, a C1-C4 alkyl group or a hydroxyl group.

5. The method for preparing a modified multifunctional epoxy resin according to claim 3, characterized in that: The molar ratio of the intermediate compound to the halogenated epoxyalkane compound is 1:(2.2-6.2); Preferably, the temperature of the substitution reaction is 50-70°C and the time is 1-3h; Preferably, the halogenated epoxyalkane compound is selected from epichlorohydrin and / or epichlorohydrin; Preferably, the alkaline medium is selected from at least one of sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, ammonia water, sodium carbonate and potassium carbonate.

6. The method for preparing a modified multifunctional epoxy resin according to claim 3, characterized in that: The intermediate compound is prepared by a method comprising the following steps: S1. The alkoxy-formaldehyde benzene having the structure shown in formula (8) is subjected to a condensation reaction in the presence of a catalyst and then purified to obtain a first reaction product; S2. The first reaction product is subjected to a reduction reaction in the presence of a reducing agent and then purified to obtain an intermediate compound; In formula (8), R1`` is a C1-C2 alkylene group, R3`` is a C1-C4 alkyl group, Q1` is a hydrogen atom, a C1-C4 alkyl group or a hydroxyl group, and Q3` is a hydrogen atom, a C1-C4 alkyl group or a hydroxyl group.

7. The method for preparing a modified multifunctional epoxy resin according to claim 6, characterized in that: The alkoxy-formaldehyde benzene has a structure shown in formula (9) and / or formula (10); In formula (9) and formula (10), R1 and R1' are each independently a C1-C2 alkylene group, R3 and R3' are each independently a C1-C4 alkyl group, Q1 is hydrogen, a C1-C4 alkyl group or a hydroxyl group, and Q3 is hydrogen, a C1-C4 alkyl group or a hydroxyl group.

8. The method for preparing a modified multifunctional epoxy resin according to claim 6, characterized in that: In step S1, the alkoxy-formaldehyde benzene is selected from at least one of 3-methoxybenzaldehyde, 2-methyl-3-methoxybenzaldehyde, 2-ethyl-3-methoxybenzaldehyde, 2-hydroxy-3-methoxybenzaldehyde, 4-hydroxy-3-methoxybenzaldehyde and 2-methoxybenzaldehyde; Preferably, in step S1, the catalyst is Laccase enzyme; Preferably, in step S1, the condensation reaction temperature is 20-30°C and the time is 1-3h; Preferably, in step S2, the reducing agent is selected from NaBH4 and / or LiAlH4; Preferably, in step S2, the reduction reaction is carried out at a temperature of 20 to 30° C. and for a time of 1 to 5 hours.

9. The modified multifunctional epoxy resin prepared by the preparation method according to any one of claims 3 to 8.

10. Use of the modified multifunctional epoxy resin according to claim 1, 2 or 9 in semiconductor packaging.

Citation Information

Patent Citations

  • Bio-based resin matrix material, carbon fiber bio-based resin composite material and preparation method thereof

    CN113897026A