Super constant-viscosity natural rubber and preparation method thereof
By adding constant viscosity agent in two stages during the preparation of natural rubber, the surface and internal molecular chain reaction of rubber particles is ensured, and the problem of increasing viscosity of natural rubber in storage is solved, and super constant viscosity with high constant viscosity and good mechanical properties is achieved Natural rubber.
Patent Information
- Application Number
- CN202411316999.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During processing and storage of natural rubber, the Mooney viscosity will increase, resulting in extended mixing time, poor rubber fluidity and unstable product quality. The existing constant viscosity natural rubber still has the problem of increasing viscosity during long-term storage, which is difficult to effectively solve.
The method of adding a constant adhesive in two stages is adopted. The first constant adhesive is mixed with fresh latex and solidified, pressed, creped, granulated and dried to form a granulated glue, and then the second constant adhesive is mixed in dry agitated treatment. Mixing ensures that the end groups of the rubber particles' surface and internal molecular chains react with the side groups, completely block the abnormal groups, and improve the constant viscosity of natural rubber.
After 18 months of accelerated or natural storage of the super constant viscosity natural rubber prepared by this method, the Mooney's viscosity increase value is ≤2, and the tensile strength of the ACS1 test formula is ≥21MPa, which significantly improves the constant viscosity and mechanical properties.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of natural rubber, and in particular relates to a super constant viscosity natural rubber and a preparation method thereof. Background Art
[0002] During the processing, maturation and storage of natural rubber, the gel content will increase, causing the Mooney viscosity to rise, resulting in problems such as extended mixing time, poor fluidity of the mixed rubber, unstable extrusion process and product quality during subsequent product processing. Constant viscosity natural rubber has overcome the above problems and is popular in vibration reduction products such as automobiles and high-speed railways.
[0003] At present, constant viscosity agents are added before the fresh latex solidifies, which is theoretically conducive to the dispersion of constant viscosity agents. However, in actual application, product companies have reported that the Mooney viscosity of the prepared constant viscosity natural rubber will still increase significantly after long-term storage. Therefore, how to improve the constant viscosity performance of natural rubber has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0004] The object of the present invention is to provide a super constant viscosity natural rubber and a preparation method thereof. The super constant viscosity natural rubber prepared by the preparation method provided by the present invention has excellent constant viscosity performance.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing super constant viscosity natural rubber, comprising the following steps:
[0007] (1) mixing fresh latex and a first constant viscosity agent to obtain a mixed latex;
[0008] (2) coagulating, thinning, sheeting, granulating and drying the mixed latex obtained in step (1) to obtain granular rubber;
[0009] (3) Mixing the granular rubber obtained in step (2) with a second constant viscosity agent, and performing dry stirring to obtain super constant viscosity natural rubber.
[0010] Preferably, the first constant viscosity agent in step (1) comprises at least one of hydroxylamine sulfate, hydroxylamine hydrochloride, hydrazine hydrochloride, hydrazine sulfate, hydrazine hydrate, semicarbazide hydrochloride, aniline and hydrazide compounds. Preferably, the hydrazide compound comprises propionyl hydrazide, lauryl hydrazide or stearyl hydrazide.
[0011] Preferably, the moisture content of the granular glue in step (2) is 0.2-5%.
[0012] Preferably, the moisture content of the granular glue is 3-4%.
[0013] Preferably, the second constant viscosity agent in step (3) comprises at least one of hydroxylamine sulfate, hydroxylamine sulfate solution, hydroxylamine hydrochloride, hydroxylamine hydrochloride solution, hydrazine hydrochloride, hydrazine hydrochloride solution, hydrazine sulfate, hydrazine sulfate solution, hydrazine hydrate, hydrazine hydrate solution, semicarbazide hydrochloride, semicarbazide hydrochloride solution, aniline and hydrazide compounds.
[0014] Preferably, based on the dry rubber mass of the fresh latex, the mass content of the first constant viscosity agent in step (1) and the second constant viscosity agent in step (3) are independently 0.03-0.3%.
[0015] Preferably, the temperature of the dry stirring treatment in step (3) is 100-135°C.
[0016] Preferably, the temperature of the dry stirring treatment is 110-125°C.
[0017] The present invention also provides a super constant viscosity natural rubber prepared by the preparation method described in the above technical solution.
[0018] The present invention provides a method for preparing super constant viscosity natural rubber, comprising the following steps: mixing fresh latex and a first constant viscosity agent to obtain a mixed latex; sequentially coagulating, thinning, creping, granulating and drying the mixed latex to obtain granular rubber; mixing the granular rubber with a second constant viscosity agent, and performing dry stirring to obtain super constant viscosity natural rubber. The present invention adds the constant viscosity agent in two stages, in the fresh latex stage and the dry stirring stage, respectively reacting with the molecular chain end groups on the surface of the rubber particles and the molecular chain side groups inside the rubber particles, completely sealing the abnormal groups that cause gel formation, thereby improving the constant viscosity performance of the natural rubber. Experimental results show that the Mooney viscosity increase value of the super constant viscosity natural rubber prepared by the preparation method provided by the present invention is ≤2 after an accelerated storage test or natural storage for 18 months, and the tensile strength of the formula tested by ACS1 is ≥21MPa. DETAILED DESCRIPTION
[0019] The present invention provides a method for preparing super constant viscosity natural rubber, comprising the following steps:
[0020] (1) mixing fresh latex and a first constant viscosity agent to obtain a mixed latex;
[0021] (2) coagulating, thinning, sheeting, granulating and drying the mixed latex obtained in step (1) to obtain granular rubber;
[0022] (3) Mixing the granular rubber obtained in step (2) with a second constant viscosity agent, and performing dry stirring to obtain super constant viscosity natural rubber.
[0023] The present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.
[0024] In the present invention, the first and the second have no special meanings and are only used to distinguish the raw materials.
[0025] The invention mixes fresh latex and a first constant viscosity agent to obtain a mixed latex. The invention mixes fresh latex and a constant viscosity agent, and the constant viscosity agent reacts with the molecular chain end groups on the surface of rubber ions, thereby improving the constant viscosity performance of natural rubber.
[0026] In the present invention, the fresh latex is preferably filtered and diluted in sequence before use.
[0027] The present invention has no particular limitation on the filtering operation, and any operation well known to those skilled in the art may be used.
[0028] In the present invention, the diluent used for the dilution is preferably water. The present invention has no particular limitation on the amount of water used, as long as the dilution is performed to a dry glue content of 20%.
[0029] In the present invention, the first constant viscosity agent preferably includes at least one of hydroxylamine sulfate, hydroxylamine hydrochloride, hydrazine hydrochloride, hydrazine sulfate, hydrazine hydrate, semicarbazide hydrochloride, aniline and hydrazide compounds; the hydrazide compounds preferably include propionyl hydrazide, lauryl hydrazide or stearyl hydrazide. The first constant viscosity agent used in the present invention can improve the constant viscosity performance of natural rubber.
[0030] In the present invention, based on the dry rubber mass of the fresh latex, the mass content of the first constant viscosity agent is preferably 0.03-0.3%. As an embodiment, the mass content of the first constant viscosity agent can be 0.05-0.15%. The present invention limits the mass content of the first constant viscosity agent to the above range to further improve the constant viscosity performance of natural rubber.
[0031] The present invention has no special limitation on the operation of mixing the fresh latex and the first constant viscosity agent, and the technical scheme for preparing the mixed material well known to those skilled in the art can be adopted.
[0032] After obtaining the mixed latex, the present invention sequentially coagulates, thins, crepes, granulates and dries the mixed latex to obtain granular rubber.
[0033] The present invention has no particular limitation on the solidification operation, and any operation well known to those skilled in the art may be used.
[0034] As an implementation mode, the coagulation may be performed using formic acid coagulation.
[0035] After the solidification is completed, the present invention preferably performs ripening on the product obtained by the solidification. The present invention has no special limitation on the ripening operation, and the operation well known to those skilled in the art can be adopted.
[0036] As an implementation mode, the aging time may be 16 hours.
[0037] The present invention has no particular limitation on the operations of pressing, sheeting, granulating and drying, and operations well known to those skilled in the art may be used.
[0038] In the present invention, the water content of the granular glue is preferably 0.2-5%. As an embodiment, the water content of the granular glue can be 3-4%.
[0039] After obtaining the granular rubber, the present invention mixes the granular rubber with a second constant viscosity agent and performs dry stirring to obtain super constant viscosity natural rubber. The present invention adds the constant viscosity agent during the dry stirring stage, and the constant viscosity agent can react with the molecular chain side groups inside the rubber particles, thereby improving the constant viscosity performance of the natural rubber.
[0040] In the present invention, the second constant viscosity agent preferably includes at least one of hydroxylamine sulfate, hydroxylamine sulfate solution, hydroxylamine hydrochloride, hydroxylamine hydrochloride solution, hydrazine hydrochloride, hydrazine hydrochloride solution, hydrazine sulfate, hydrazine sulfate solution, hydrated hydrazine, hydrated hydrazine solution, semicarbazide hydrochloride, semicarbazide hydrochloride solution, aniline and hydrazide compounds; the hydrazide compound preferably includes propionyl hydrazide, lauryl hydrazide or stearyl hydrazide. The present invention uses the second constant viscosity agent to improve the constant viscosity of natural rubber.
[0041] In the present invention, the solvent of the hydroxylamine sulfate solution, hydroxylamine hydrochloride solution, hydrazine hydrochloride solution, hydrazine sulfate solution, hydrazine hydrate solution and semicarbazide hydrochloride solution is independently preferably water; the mass concentration of the hydroxylamine sulfate solution, hydroxylamine hydrochloride solution, hydrazine hydrochloride solution, hydrazine sulfate solution, hydrazine hydrate solution and semicarbazide hydrochloride solution is independently preferably 5-40%, more preferably 20-30%.
[0042] In the present invention, based on the dry rubber mass of the fresh latex, the mass content of the second constant viscosity agent is preferably 0.03-0.3%. As an embodiment, the mass content of the second constant viscosity agent can be 0.05-0.15%. The present invention limits the mass content of the second constant viscosity agent to the above range to further improve the constant viscosity performance of natural rubber.
[0043] The present invention has no special limitation on the operation of mixing the granular glue and the second constant viscosity agent, and the technical scheme for preparing the mixed material well known to those skilled in the art can be adopted.
[0044] In the present invention, the temperature of the dry stirring treatment is preferably 100-135° C. The present invention limits the temperature of the dry stirring treatment to the above range to control the temperature of the rubber material, make the second constant viscosity agent dispersed evenly, and prevent the rubber molecular chain from excessive oxidation and chain breaking, which is beneficial to improving the mechanical properties of the rubber.
[0045] As an embodiment, the temperature of the dry stirring treatment may be 110-125°C, and may also be 115°C.
[0046] After the dry mixing process is completed, the present invention preferably cools and packages the product obtained by the dry mixing process in sequence to obtain super constant viscosity natural rubber.
[0047] In the present invention, the temperature of the cooled rubber material is preferably 25-75° C. As an embodiment, the temperature of the cooled rubber material can be 40-60° C., or 45° C.
[0048] The present invention has no special limitation on the packaging operation, and operations well known to those skilled in the art may be used.
[0049] The present invention adds the constant viscosity agent in two stages, namely, the fresh latex stage and the dry stirring stage, and reacts with the molecular chain end groups on the surface of the rubber particles and the molecular chain side groups inside the rubber particles respectively, completely sealing the abnormal groups that cause gel formation, and the constant viscosity performance is superior to the traditional process method that can only seal part of the abnormal groups; by reasonably controlling the water content of the particle rubber and the temperature of the dry stirring treatment, the constant viscosity agent is evenly dispersed, and at the same time, the rubber molecular chain is prevented from excessive oxidation and chain breaking, which is beneficial to improving the mechanical properties of the rubber.
[0050] The super constant viscosity natural rubber prepared by the present invention has excellent constant viscosity performance and good mechanical properties. The Mooney viscosity increase value after accelerated storage test or natural storage for 18 months is ≤2, and the tensile strength of the formula tested by ACS1 is ≥21MPa.
[0051] The present invention also provides a super constant viscosity natural rubber prepared by the preparation method described in the above technical solution.
[0052] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] The fresh latex adopted in the embodiments and comparative examples was produced by Maoming Branch of Guangdong Guangken Rubber Group Co., Ltd.
[0054] Example 1
[0055] The preparation method of super constant viscosity natural rubber is as follows:
[0056] (1) taking the filtered fresh latex, diluting it with water to a dry rubber content of 20%, then adding 0.1% of the mass of the dry rubber of the fresh latex with hydroxylamine sulfate to mix, and obtaining a mixed latex;
[0057] (2) the mixed latex obtained in step (1) is coagulated with formic acid and then matured for 16 hours, and then thinned, creped and granulated, and then dried in an oven at 83° C. to a moisture content of 3%, to obtain granular rubber;
[0058] (3) putting the granular rubber obtained in step (2) into the feed port of the dry mixing machine, and adding 0.05% of the mass of the fresh latex dry rubber and a 20% hydroxylamine sulfate solution, controlling the dry mixing temperature to 120° C. for dry mixing. After the dry mixing is completed, the rubber is cooled to 50° C. and then packaged to obtain super constant viscosity natural rubber.
[0059] 400 g of the super constant viscosity natural rubber prepared in Example 1 was used to prepare a vulcanized rubber according to the ACS1 formula (100 parts of natural rubber, 6 parts of zinc oxide, 3.5 parts of sulfur, 0.5 parts of stearic acid, and 0.5 parts of accelerator M). The Mooney viscosity was measured according to the national standard GB / T 1232.1-2016, the accelerated storage hardening value was measured according to the national standard GB / T 18013-2008 Mooney viscometer method, and the mechanical properties were measured according to the national standard GB / T 528-2009. The results are shown in Table 1.
[0060] Example 2
[0061] The preparation method of super constant viscosity natural rubber is as follows:
[0062] (1) taking the filtered fresh latex, adding water to dilute it to a dry rubber content of 20%, and then adding 0.1% of the mass of the fresh latex dry rubber hydroxylamine hydrochloride to mix, to obtain a mixed latex;
[0063] (2) the mixed latex obtained in step (1) is coagulated with formic acid and then matured for 16 hours, and then thinned, creped and granulated, and then dried in an oven at 83° C. to a moisture content of 2%, thereby obtaining granular rubber;
[0064] (3) putting the granular rubber obtained in step (2) into the feed port of the dry mixer, and adding 0.08% of the mass of the fresh latex dry rubber and a 20% hydroxylamine sulfate solution, controlling the dry mixing temperature to 115° C. for dry mixing. After the dry mixing is completed, the rubber is cooled to 45° C. and then packaged to obtain super constant viscosity natural rubber.
[0065] 400 g of the super constant viscosity natural rubber prepared in Example 2 was used to prepare a vulcanized rubber according to the ACS1 formula (100 parts of natural rubber, 6 parts of zinc oxide, 3.5 parts of sulfur, 0.5 parts of stearic acid, and 0.5 parts of accelerator M). The Mooney viscosity was measured according to the national standard GB / T 1232.1-2016, the accelerated storage hardening value was measured according to the national standard GB / T 18013-2008 Mooney viscometer method, and the mechanical properties were measured according to the national standard GB / T 528-2009. The results are shown in Table 1.
[0066] Example 3
[0067] The preparation method of super constant viscosity natural rubber is as follows:
[0068] (1) taking the filtered fresh latex, diluting it with water until the dry rubber content is 20%, then adding 0.12% of the mass of the dry rubber of the fresh latex to hydroxylamine sulfate to mix, and obtaining a mixed latex;
[0069] (2) the mixed latex obtained in step (1) is coagulated with formic acid and then matured for 16 hours, and then thinned, creped and granulated, and then dried in an oven at 83° C. to a moisture content of 3%, to obtain granular rubber;
[0070] (3) putting the granular rubber obtained in step (2) into the feed port of the dry mixing machine, and adding 0.05% of the mass of the fresh latex dry rubber and a 20% hydroxylamine sulfate solution, controlling the dry mixing temperature to 125° C. for dry mixing. After the dry mixing is completed, the rubber is cooled to 45° C. and then packaged to obtain super constant viscosity natural rubber.
[0071] 400 g of the super constant viscosity natural rubber prepared in Example 3 was taken to prepare a vulcanized rubber according to the ACS1 formula (100 parts of natural rubber, 6 parts of zinc oxide, 3.5 parts of sulfur, 0.5 parts of stearic acid, and 0.5 parts of accelerator M). The Mooney viscosity was measured according to the national standard GB / T 1232.1-2016, the accelerated storage hardening value was measured according to the national standard GB / T 18013-2008 Mooney viscometer method, and the mechanical properties were measured according to the national standard GB / T 528-2009. The results are shown in Table 1.
[0072] Table 1 Intrinsic properties of super constant viscosity natural rubber prepared in Examples 1 to 3 and mechanical properties data of ACS1 formula
[0073] Test items Example 1 Example 2 Example 3 <![CDATA[ML (1+4) 100℃]]> 57 60 58 Accelerated storage ΔMv 1.6 2.0 1.8 Tensile strength, MPa 21 21 22 500% tensile stress, MPa 2.7 2.3 2.5 Elongation at break, % 807 811 815
[0074] It can be seen from Table 1 that the super constant viscosity natural rubber prepared by the present invention has excellent constant viscosity and mechanical properties.
[0075] Comparative Example 1
[0076] The preparation method of natural rubber is:
[0077] Take the filtered fresh latex, add water to dilute it to a dry rubber content of 20%, use formic acid to coagulate it and continue to mature it for 16 hours, then press it into thin sheets, crepe it and granulate it, and then dry it in an oven at a constant temperature of 83°C until the granular rubber has a constant weight to obtain natural rubber.
[0078] 400 g of the natural rubber prepared in Comparative Example 1 was used to prepare a vulcanized rubber according to the ACS1 formula (100 parts of natural rubber, 6 parts of zinc oxide, 3.5 parts of sulfur, 0.5 parts of stearic acid, and 0.5 parts of accelerator M). The Mooney viscosity was measured according to the national standard GB / T 1232.1-2016, the accelerated storage hardening value was measured according to the Mooney viscometer method of the national standard GB / T 18013-2008, and the mechanical properties were measured according to the national standard GB / T528-2009. The results are shown in Table 2.
[0079] Table 2 Intrinsic properties of natural rubber prepared in Comparative Example 1 and mechanical properties of ACS1 formula
[0080] Test items Comparative Example 1 <![CDATA[ML (1+4) 100℃]]> 60 Accelerated storage ΔMv 6.5 Tensile strength, MPa 17 500% tensile stress, MPa 2.5 Elongation at break, % 810
[0081] By comparing Tables 1 and 2, it can be seen that the technical solution of the present invention has excellent constant viscosity and mechanical properties compared with the comparative example.
[0082] It can be seen from the above embodiments and comparative examples that the super constant viscosity natural rubber prepared by the preparation method provided by the present invention has excellent constant viscosity and mechanical properties.
[0083] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing super constant viscosity natural rubber, comprising the following steps: (1) mixing fresh latex and a first constant viscosity agent to obtain a mixed latex; (2) coagulating, thinning, sheeting, granulating and drying the mixed latex obtained in step (1) to obtain granular rubber; (3) Mixing the granular rubber obtained in step (2) with a second constant viscosity agent, and performing dry stirring to obtain super constant viscosity natural rubber.
2. The preparation method according to claim 1, characterized in that: The first constant viscosity agent in step (1) comprises at least one of hydroxylamine sulfate, hydroxylamine hydrochloride, hydrazine hydrochloride, hydrazine sulfate, hydrazine hydrate, semicarbazide hydrochloride, aniline and hydrazide compounds.
3. The preparation method according to claim 2, characterized in that: The hydrazide compound includes propionyl hydrazide, lauryl hydrazide or stearyl hydrazide.
4. The preparation method according to claim 1, characterized in that: The moisture content of the granular glue in the step (2) is 0.2-5%.
5. The preparation method according to claim 4, characterized in that: The moisture content of the granular glue is 3-4%.
6. The preparation method according to claim 1, characterized in that: The second constant viscosity agent in step (3) includes at least one of hydroxylamine sulfate, hydroxylamine sulfate solution, hydroxylamine hydrochloride, hydroxylamine hydrochloride solution, hydrazine hydrochloride, hydrazine hydrochloride solution, hydrazine sulfate, hydrazine sulfate solution, hydrazine hydrate, hydrazine hydrate solution, semicarbazide hydrochloride, semicarbazide hydrochloride solution, aniline and hydrazide compounds.
7. The preparation method according to claim 1, characterized in that: Based on the dry rubber mass of the fresh latex, the mass content of the first constant viscosity agent in step (1) and the second constant viscosity agent in step (3) are independently 0.03-0.3%.
8. The preparation method according to claim 1, characterized in that: The temperature of the dry stirring treatment in step (3) is 100-135°C.
9. The preparation method according to claim 8, characterized in that: The temperature of the dry stirring treatment is 110-125°C.
10. The super constant viscosity natural rubber prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Constant viscosity natural rubber and preparation method thereof
CN103627044A
Environment-friendly constant-viscosity natural rubber and preparation method thereof
CN108570167A
Constant viscosity natural rubber and preparation method thereof
CN109109203A
High-PRI constant-Mooney-viscosity natural rubber and preparation method thereof
CN112898645A