Preparation method and application of surface western blot polymer relying on enzyme cascade reaction

Through the local radical polymerization method mediated by enzyme cascade reaction, the problem of agglomeration or gelation of traditional surface graft polymerization at high monomer concentration is solved, and the blotting efficiency and adsorption capacity of surface western blot polymers are improved. Suitable for efficient isolation and purification of proteins.

CN118955789AActive Publication Date: 2024-11-15CANGZHOU INSTITUTE OF TIANGONG UNIVERSITY

Patent Information

Application Number
CN202411030051.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Traditional surface graft polymerization methods have problems of agglomeration or gelation at high monomer concentrations when preparing surface western blot polymers with high blotting efficiency, resulting in limited pre-assembly of functional monomers and template molecules, affecting the blotting efficiency.

Method used

The local radical polymerization method mediated by enzyme cascade reaction is used to polymerize on the surface of nanocarriers, and glucose oxidase and horseradish peroxidase are used as initiation systems to avoid random free radical free flow and achieve polymerization at high monomer concentration. No agglomeration occurs, and the pre-assembly and blot efficiency of functional monomers and template proteins is improved.

Benefits of technology

The blotting efficiency is significantly improved. The obtained surface western blot polymer has high adsorption capacity and blotting factor, which can complete the polymerization reaction in a short time, and can control the blotting shell thickness, which is suitable for protein separation and purification of complex biological samples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955789A_ABST
    Figure CN118955789A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of a surface western blot polymer relying on an enzyme cascade reaction. The surface imprinted polymer is prepared under the condition of high monomer concentration by enzyme cascade reaction mediated local free radical polymerization. A local free radical polymerization reaction is started by using an initiating system consisting of GOx / HRP fixed on the surface of the nano-carrier, acetylacetone and glucose, so that the polymerization reaction is carried out around the surface of the nano-carrier. Random dissociation of free radicals in the whole solution is avoided, and even if polymerization is carried out under high monomer concentration, the agglomeration phenomenon cannot occur. Meanwhile, the method is carried out under the condition of high monomer concentration, so that full pre-assembly of the functional monomer and the template protein is facilitated, and the imprinting efficiency can be improved. The imprinting capacity of the synthesized nano imprinting microspheres on lysozyme is 145.3 mg g <-1 >, and the imprinting factor is 14.2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of biological separation and purification, and specifically relates to the preparation and application of a surface protein imprinting polymer, in particular, a preparation method of a surface protein imprinting polymer relying on an enzyme cascade reaction and its application in the separation and purification of proteins in complex biological samples. Background Art

[0002] Molecular imprinting technology (MIPs) is the relationship between antibodies and receptors. It has customized binding sites that complement the template molecule in shape, size, and functional groups. Due to its unique structural predictability, recognition specificity, and versatility, MIPs have been widely used in various fields. Although molecular imprinting technology is widely used, it has been proven to be particularly effective for low molecular weight proteins with a molecular weight of less than 1500, but it still poses great challenges for selective recognition of macromolecules such as proteins and viruses. The main difficulties are the difficulty in template removal and low imprinting factor.

[0003] In order to solve the above problems, researchers have proposed imprinting techniques such as epitope imprinting and surface imprinting. Among them, epitope imprinting uses a peptide segment on the surface of a macromolecule as a template for imprinting. However, it is extremely difficult to find the epitope and difficult to synthesize. The difference is that the surface imprinting technology uses the entire molecule as a template to form a thin imprinted polymer layer on the surface of the nanocarrier, which can reduce the mass transfer resistance of the template molecule and help improve the elution efficiency and accessibility of the imprinted cavity. Therefore, surface imprinting technology has received great attention from researchers.

[0004] Methods for preparing surface imprinted polymers include sol-gel method, self-oxidative polymerization method, surface grafting polymerization method, etc. The first two methods rely on the hydrolysis of silane monomers or the self-oxidative polymerization of dopamine, which have the problem of poor monomer compatibility and are difficult to fully interact with a variety of template molecules. Surface grafting polymerization is to modify vinyl groups on the surface of particles and free radical copolymerize them with various vinyl-containing monomers. It can meet the needs of template molecules with different characteristics and is the most commonly used method for preparing surface imprinted polymers. However, this method requires a low monomer concentration, which will lead to poor imprinting efficiency.

[0005] Fu et al. modified the surface of SiO2 nanoparticles with vinyl groups and carried out surface graft polymerization at a total monomer and crosslinker concentration of about 0.4 wt%. The adsorption capacity of the imprinted polymer obtained was only 11.3 mg g -1 , the imprinting factor is 1.23. Li et al. reported that the adsorption capacity of the surface imprinted polymer prepared by surface graft polymerization was about 78.0 mg g -1) has been improved, but the imprinting factor (1.69) is still low. If the monomer concentration is increased, it will lead to aggregation and even gelation problems. Fu, Jing and others prepared imprinted polymers by traditional surface grafting polymerization under high monomer concentration (about 7wt%) conditions, and they all found particle aggregation and even gelation problems. Therefore, when preparing imprinted polymers with high imprinting efficiency by traditional surface imprinting polymerization, there is a contradiction between the high monomer concentration requirement and the gelation problem. Summary of the invention

[0006] In order to avoid the occurrence of agglomeration, the traditional surface grafting polymerization method requires to be carried out under low monomer concentration conditions when preparing surface imprinted polymers with macromolecules such as proteins as templates. However, low monomer concentration will limit the preassembly of functional monomers and template molecules, thereby affecting the imprinting efficiency of imprinted polymers. Therefore, the present invention uses enzyme cascade reaction to mediate local free radical polymerization to achieve the preparation of surface imprinted polymers under high monomer concentration conditions. Specifically, the present invention uses an initiation system composed of glucose oxidase / horseradish peroxidase, acetylacetone and glucose fixed on the surface of the nanocarrier to start the local free radical polymerization reaction, so that the polymerization reaction is carried out around the surface of the nanocarrier. The present invention avoids the random freedom of free radicals in the entire solution, and even if the polymerization is carried out at a high monomer concentration, there will be no agglomeration phenomenon. At the same time, the method is carried out under high monomer concentration conditions, which is conducive to the full preassembly of functional monomers and template proteins, thereby improving the imprinting efficiency.

[0007] The technical solution of the present invention is as follows:

[0008] A method for preparing a surface protein imprinting polymer by enzyme cascade reaction comprises the following steps:

[0009] (1) Carboxyl modification of the surface of the nanoparticles: 3-aminopropyltriethoxysilane is used to hydrolyze the surface of the nanoparticles, and then the aminated nanoparticles are obtained after washing;

[0010] (2) dispersing the aminated nanoparticles in a tetrahydrofuran solution, adding succinic anhydride, stirring at room temperature for 1-8 hours, and then washing to obtain surface carboxylated nanoparticles;

[0011] (3) The washed carboxylated nanoparticles were dispersed in phosphate buffer, and glucose oxidase (GOx) and horseradish peroxidase (HRP) were added at a molar ratio of 1.5:1. Subsequently, GOx and HRP were covalently coupled to the surface of the nanoparticles under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide;

[0012] (4) washing the product of step (3) with deionized water to obtain a nano-ionic dispersion of immobilized enzyme;

[0013] (5) adding the template protein, main monomer, functional monomer, and cross-linking agent to a pH 5.0 phosphate buffer and pre-assembling for 10-60 minutes to obtain a pre-assembly solution;

[0014] (6) adding the nanoparticle dispersion of the immobilized enzyme, acetylacetone and glucose to the pre-assembled solution of step (5) to initiate a polymerization reaction; after polymerizing for 4-8 hours at room temperature, the reaction is stopped to obtain a polymerization solution;

[0015] (7) Centrifuge the polymer solution in step (6) and wash 3-6 times to obtain a surface protein imprinted polymer.

[0016] The nanoparticles include SiO2, Fe3O4, Fe3O4-Cu, MOF, COF, Au, CeO2 or Ag.

[0017] The concentration of 3-aminopropyltriethoxysilane in step (1) is 0.01-0.20M.

[0018] In step (2), the amination nanoparticles are dispersed in the tetrahydrofuran solution at a particle concentration of 0.01-0.10 mg mL -1 , the concentration of added succinic anhydride is 0.01-0.20M.

[0019] In step (3), the washed carboxylated nanoparticles are dispersed in phosphate buffer at a particle concentration of 0.01-0.10 mg mL -1 , glucose oxidase (GOx) and horseradish peroxidase (HRP) were added at a molar ratio of 1.5:1, and the concentration of 1-ethyl-(3-dimethylaminopropyl)carbodiimide was 0.05-1.0M.

[0020] The nano-ion dispersion of immobilized enzyme obtained in step (4) has a particle concentration of 0.01-0.10 mg mL -1 .

[0021] In the step (5), the concentration of the template protein is 0.01-0.10 mM, the concentration of the main monomer is 0.05-1.00 M, the concentration of the functional monomer is 1.74-34.80 mM, the concentration of methacrylic acid is 1.74-34.80 mM, and the concentration of the cross-linking agent is 0.67-13.35 mM; the template protein in the pre-assembly solution is lysozyme, bovine serum albumin, cytochrome C, bovine hemoglobin, human immunoglobulin, amyloid protein and other acidic, neutral and basic proteins; the main monomer includes N-isopropyl acrylamide and acrylamide; the functional monomer includes methacrylic acid, acrylamide, styrene, N-tert-butyl acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and dimethylaminoethyl methacrylate; and the cross-linking agent is N,N-methylenebisacrylamide, polyethylene glycol diacrylate, and polyglutamic acid polypeptide cross-linking agent.

[0022] In the step (6), 4.0 mL of the nanoparticle dispersion of the immobilized enzyme is added to the pre-assembly solution, 0.01-0.10 mg mL -1 , acetylacetone concentration 0.05-0.20M, glucose concentration 0.05-0.20M.

[0023] The surface protein imprinting polymer relying on enzyme cascade reaction prepared by the method of the invention is applied to the extraction and purification of proteins in complex biological samples.

[0024] The complex biological samples include egg white and the like.

[0025] The imprinting efficiency test of the surface protein imprinting polymer in the present invention is carried out using a common method reported in the literature, specifically as follows:

[0026] (1) vacuum drying the surface protein imprinted polymer (MIP) and the corresponding non-imprinted polymer (NIP) prepared by the synthesis method of the present invention.

[0027] (2) Weigh about 10 mg of the dried MIP and corresponding NIP in step (1) into centrifuge tubes (6 each), add pH 5.0 phosphate buffer (8 mL) to fully swell, and remove the solution after the swelling reaches equilibrium.

[0028] (3) Prepare 1.0 mg mL -1 The lysozyme stock solution was diluted to a gradient with initial concentrations (C0) of 0.1, 0.2, 0.4,

[0029] 0.6, 0.8 and 1.0 lysozyme solutions.

[0030] (4) Add the lysozyme solutions of different concentrations prepared in step (3) to the centrifuge tubes containing MIP or NIP in step (2) in sequence, adding 8 mL to each centrifuge tube, and incubate at room temperature for 1 h.

[0031] (5) Determine the concentration of the remaining lysozyme in each centrifuge tube after incubation in step (4) by UV-visible spectrophotometer

[0032] (C).

[0033] (6) Calculate the equilibrium adsorption capacity (Q), Q = 0.8*(C0-C).

[0034] (7) The maximum saturated adsorption capacity of MIP and NIP was calculated according to the Langmuir adsorption model. The imprinting factor (IF) is the ratio of the maximum saturated adsorption capacity of MIP to the maximum saturated adsorption capacity of NIP.

[0035] (8) According to the calculation formula and method in step (6) and step (7), the maximum saturated adsorption capacity is 145.3 mg g -1 , the imprinting factor is 14.3.

[0036] Advantages and excellent effects

[0037] The local free radical polymerization mediated by enzyme cascade reaction solves the aggregation and even gelation problems that occur when preparing surface protein imprinted polymers by traditional surface grafting polymerization under high monomer concentration conditions. In addition, high-concentration monomers can be fully preassembled with template proteins, increasing the number of imprinting sites, thereby greatly improving the imprinting efficiency.

[0038] The present invention uses nanoparticles as carriers, and the carriers for enzymatic reactions are also more selective, and can be applied to nanoparticles such as SiO2, Fe3O4, Fe3O4-Cu, MOF, COF, Au, CeO2, and Ag. The present invention modifies horseradish peroxidase and glucose oxidase on the surface of nanoparticles as active cores, so that polymerization reaction is carried out around the nanoparticles, thereby avoiding the occurrence of agglomeration or even gelation under high monomer concentration conditions. At the same time, due to the immobilization of the enzyme, the enzyme reaction activity is increased, the polymerization rate is accelerated, and the polymerization reaction can be completed rapidly in a short time (4-8h). In addition, the thickness of the imprinted shell can be controllably adjusted by polymerization time and monomer concentration to meet the needs of practical applications.

[0039] In terms of monomer selection, vinyl monomers containing various functional groups can be selected to tailor corresponding artificial receptors for different proteins to meet the needs of protein purification in the biomedical field. In the present invention, the main monomers are selected from N-isopropylacrylamide and acrylamide. In the present invention, the functional monomers are selected from methacrylic acid, acrylamide, styrene, N-tert-butylacrylamide, 2-acrylamido-2-methylpropanesulfonic acid, dimethylaminoethyl methacrylate, etc.

[0040] In terms of cross-linking agent selection, N,N-methylenebisacrylamide, polyethylene glycol diacrylate, and polyglutamic acid polypeptide cross-linking agents can be selected for use in the present invention.

[0041] The results of protein re-adsorption experiments showed that the imprinting capacity of the synthesized nanoimprinted microspheres for lysozyme was 145.3 mg g -1 , the imprinting factor is 14.2. The results of protein adsorption kinetics experiments show that nano-imprinted microspheres can reach adsorption equilibrium in a relatively short time (30-45min). Compared with the results of other literatures, the peptide cross-linked surface protein imprinted polymer obtained by local free radical polymerization mediated by horseradish peroxidase and glucose oxidase cascade reaction has greatly improved in polymerization reaction time, specific selectivity, adsorption capacity and elution efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 :TEM image of enzyme coated on the surface of prepared SiO2 nanoparticles

[0043] Figure 2 :TEM images of surface protein-imprinted polymers prepared by local free radical polymerization mediated by enzyme cascade reaction on SiO2 nanoparticles

[0044] Figure 3 :TEM images of surface protein-imprinted polymers prepared by local free radical polymerization mediated by enzyme cascade reaction on Fe3O4 nanoparticles

[0045] Figure 4 :Preparation of Fe3O4 by localized free radical polymerization mediated by enzyme cascade reaction 4- TEM image of surface protein imprinted polymer with Cu nanoparticles as carrier

[0046] Figure 5 :SDS-PAGE analysis of lysozyme extracted from egg white, the leftmost lane is the Mark lane, the first lane is the lysozyme standard sample lane, the second lane is the untreated egg white sample supernatant, the third lane is the egg white supernatant treated with surface protein imprinting polymer, and the fourth lane is the sample supernatant after elution. DETAILED DESCRIPTION

[0047] The present invention provides a new method for preparing surface protein imprinted polymers, which adopts local free radical polymerization mediated by enzyme cascade reaction to prepare surface protein imprinted polymers with high imprinting efficiency, and specifically comprises the following steps:

[0048] (1) dispersing the nanoparticles in a mixture of anhydrous ethanol and deionized water, adding 3-aminopropyltriethoxysilane (0.01-0.20 M) and aqueous ammonia (28 wt%, 0.001-0.02 M), reacting at room temperature for 10-24 h, and washing with anhydrous ethanol and water in turn to obtain amino nanoparticles;

[0049] (2) Disperse the aminated nanoparticles obtained in step (1) into tetrahydrofuran (particle concentration 0.01-0.10 mg mL -1 ), adding succinic anhydride (0.01-0.20 M), reacting at room temperature for 1-8 h, and washing with ethanol and water in sequence to obtain surface carboxyl-modified nanoparticles;

[0050] (3) Dispersing the carboxylated nanoparticles in step (2) in phosphate buffer (particle concentration 0.01-0.10 mg / mL) -1), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added at a molar ratio of 1.5:1, and stirred at room temperature for 1-8 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (0.05-1.0 M);

[0051] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration 0.01-0.10 mg / mL). -1 The microscopic morphology of the particles after covalent coupling is shown in the attached manual. Figure 1 As shown, it can be clearly seen that the enzyme is successfully immobilized on the particle surface;

[0052] (5) adding a certain volume of pH 5.0 phosphate buffer, pre-assembling for 10-60 min, and obtaining a pre-assembly solution for use;

[0053] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL,

[0054] 0.01-0.10mg mL -1 ), acetylacetone (0.05-0.20M) and glucose (0.05-0.20M) to initiate the polymerization reaction. After 4-8 hours of polymerization at room temperature, the reaction was stopped to obtain a polymerization solution;

[0055] (7) The polymer solution in step (6) is centrifuged and washed 3-6 times to obtain a surface protein imprinted polymer, the microscopic morphology of which is as shown in the attached manual. Figure 2 , 3 , as shown in Figure 4.

[0056] There are no special requirements for the selection of nanoparticles in the present invention, including but not limited to SiO2, Ag, Au, Fe3O4, MOF, COF and other nanoparticles.

[0057] There is no special requirement for the selection of enzymes in the present invention, including but not limited to glucose oxidase and horseradish peroxidase.

[0058] There are no specific requirements for the template protein, main monomer and functional monomer used in the polymerization of the present invention. All of them are proteins and monomers commonly used in this research field. The water-soluble solution used in this experiment is generally based on phosphate buffer, which is configured according to the pH value required by the cross-linking agent, and the ion concentration is 10mM.

[0059] The specific implementation case uses different nanoparticles, different template proteins, different types and amounts of monomers and cross-linking agents as variables, and relies on the local free radical polymerization method mediated by the enzyme cascade reaction in the present invention to prepare protein surface imprinted polymers. The research results show that with the increase of the total mass concentration of monomers and cross-linking agents in the present invention, the surface protein imprinted polymer obtained not only maintains the monodisperse characteristics, but also greatly improves its adsorption efficiency.

[0060] Implementation 1

[0061] Preparation of surface protein-imprinted polymers by localized free radical polymerization mediated by enzyme cascade reaction:

[0062] (1) dispersing SiO2 nanoparticles in a mixture of anhydrous ethanol and deionized water, adding 3-aminopropyltriethoxysilane (0.01 M) and ammonia water (28 wt%, 0.001 M), reacting at room temperature for 10 h, and washing with anhydrous ethanol and water in turn to obtain amino SiO2 nanoparticles;

[0063] (2) Disperse the aminated SiO2 nanoparticles obtained in step (1) into tetrahydrofuran (particle concentration 0.01 mg / mL) -1 ), adding succinic anhydride (0.01 M), reacting at room temperature for 1 h, washing with ethanol and water in sequence to obtain SiO2 nanoparticles with surface carboxylation modification;

[0064] (3) Disperse the carboxylated SiO2 nanoparticles in step (2) in phosphate buffer (particle concentration 0.01 mg / mL) -1 ), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added in a molar ratio of 1.5:1, and stirred at room temperature for 1 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (0.05 M).

[0065] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration 0.01 mg / mL). -1 ).

[0066] (5) Lysozyme (0.01 mM), N-isopropylacrylamide (0.05 M), acrylamide (1.74 mM), methacrylic acid (1.74 mM), and polyglutamic acid polypeptide cross-linker (0.67 mM) were added to pH 5.0 phosphate buffer and preassembled for 10 minutes to obtain a preassembly solution for use.

[0067] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL, 0.01 mg mL -1), acetylacetone (0.05M) and glucose (0.05M) were added to initiate the polymerization reaction. The polymerization was stopped after 4 hours at room temperature to obtain a polymerization solution.

[0068] (7) The polymer solution in step (6) was centrifuged and washed three times to obtain a surface protein imprinted polymer.

[0069] Implementation 2

[0070] Preparation of surface protein-imprinted polymers by localized free radical polymerization mediated by enzyme cascade reaction:

[0071] (1) dispersing SiO2 nanoparticles in a mixture of anhydrous ethanol and deionized water, adding 3-aminopropyltriethoxysilane (0.10 M) and ammonia water (28 wt%, 0.01 M), reacting at room temperature for 15 h, and washing with anhydrous ethanol and water in turn to obtain amino SiO2 nanoparticles;

[0072] (2) Disperse the aminated SiO2 nanoparticles obtained in step (1) into tetrahydrofuran (particle concentration 0.05 mg / mL) -1 ), adding succinic anhydride (0.10 M), reacting at room temperature for 4 h, and washing with ethanol and water in sequence to obtain surface carboxyl-modified SiO2 nanoparticles;

[0073] (3) Disperse the carboxylated SiO2 nanoparticles in step (2) in phosphate buffer (particle concentration 0.05 mg / mL) -1 ), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added in a molar ratio of 1.5:1, and stirred at room temperature for 4 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (0.50 M).

[0074] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration 0.05 mg / mL). -1 ).

[0075] (5) Lysozyme (0.05 mM), N-isopropylacrylamide (0.50 M), acrylamide (17.40 mM), methacrylic acid (17.40 mM), and polyglutamic acid polypeptide cross-linker (6.70 mM) were added to pH 5.0 phosphate buffer and preassembled for 30 minutes to obtain a preassembly solution for use.

[0076] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL, 0.10 mg mL -1 ), acetylacetone (0.05M) and glucose (0.05M) were added to initiate the polymerization reaction. The polymerization was stopped after 6 hours at room temperature to obtain a polymerization solution.

[0077] (7) The polymer solution in step (6) was centrifuged and washed 4 times to obtain a surface protein imprinted polymer.

[0078] Implementation 3

[0079] Preparation of surface protein-imprinted polymers by localized free radical polymerization mediated by enzyme cascade reaction:

[0080] (1) dispersing SiO2 nanoparticles in a mixture of anhydrous ethanol and deionized water, adding 3-aminopropyltriethoxysilane (0.20 M) and ammonia water (28 wt%, 0.02 M), reacting at room temperature for 24 h, and washing with anhydrous ethanol and water in turn to obtain amino SiO2 nanoparticles;

[0081] (2) Disperse the aminated SiO2 nanoparticles obtained in step (1) into tetrahydrofuran (particle concentration of about 0.10 mg / mL) -1 ), adding succinic anhydride (0.20 M), reacting at room temperature for 8 h, and washing with ethanol and water in sequence to obtain SiO2 nanoparticles with surface carboxylation modification;

[0082] (3) Dispersing the carboxylated SiO2 nanoparticles in step (2) in phosphate buffer (particle concentration of about 0.10

[0083] mg mL -1 ), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added in a molar ratio of 1.5:1, and stirred at room temperature for 8 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (1.0 M).

[0084] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration of about 0.10 mg / mL). -1 ).

[0085] (5) Lysozyme (0.10 mM), N-isopropylacrylamide (1.00 M), acrylamide (34.80 mM), methacrylic acid (34.80 mM), and polyglutamic acid polypeptide cross-linker (13.40 mM) were added to pH 5.0 phosphate buffer and preassembled for 60 minutes to obtain a preassembly solution for use.

[0086] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL, 0.10 mg mL -1 ), acetylacetone (0.05M) and glucose (0.05M) were added to initiate the polymerization reaction. The polymerization was stopped after 8 hours at room temperature to obtain a polymerization solution.

[0087] (7) The polymer solution in step (6) was centrifuged and washed 6 times to obtain a surface protein imprinted polymer.

[0088] Implementation 4

[0089] Preparation of surface protein-imprinted polymers by localized free radical polymerization mediated by enzyme cascade reaction:

[0090] (1) Ag nanoparticles were dispersed in a mixture of anhydrous ethanol and deionized water, 3-aminopropyltriethoxysilane (0.10 M) and ammonia water (28 wt%, 0.01 M) were added, and the mixture was reacted at room temperature for 15 h. The Ag nanoparticles were then washed with anhydrous ethanol and water in turn to obtain amino Ag nanoparticles;

[0091] (2) The aminated Ag nanoparticles obtained in step (1) were dispersed in tetrahydrofuran (particle concentration: 0.05 mg / mL) -1 ), adding succinic anhydride (0.10 M), reacting at room temperature for 4 h, and washing with ethanol and water in sequence to obtain surface carboxyl-modified Ag nanoparticles;

[0092] (3) Disperse the carboxylated Ag nanoparticles in step (2) in phosphate buffer (particle concentration 0.05 mg / mL) -1 ), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added in a molar ratio of 1.5:1, and stirred at room temperature for 4 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (0.50 M).

[0093] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration 0.05 mg / mL). -1 ).

[0094] (5) Add bovine serum albumin (0.05 mM), N-isopropylacrylamide (0.50 M), acrylamide (17.40 mM), methacrylic acid (17.40 mM), and polyethylene glycol diacrylamide (6.70 mM) to pH 5.0 phosphate buffer and preassemble for 30 minutes to obtain a preassembly solution for use.

[0095] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL, 0.10 mg mL -1 ), acetylacetone (0.05M) and glucose (0.05M) were added to initiate the polymerization reaction. The polymerization was stopped after 6 hours at room temperature to obtain a polymerization solution.

[0096] (7) The polymer solution in step (6) was centrifuged and washed 4 times to obtain a surface protein imprinted polymer.

[0097] Implementation 5

[0098] Preparation of surface protein-imprinted polymers by localized free radical polymerization mediated by enzyme cascade reaction:

[0099] (1) CeO2 nanoparticles were dispersed in a mixture of anhydrous ethanol and deionized water, 3-aminopropyltriethoxysilane (0.10 M) and ammonia water (28 wt%, 0.01 M) were added, and the mixture was reacted at room temperature for 15 h. The amination Ag nanoparticles were obtained after washing with anhydrous ethanol and water in turn;

[0100] (2) Disperse the aminated CeO2 nanoparticles obtained in step (1) into tetrahydrofuran (particle concentration 0.05 mg / mL) -1 ), adding succinic anhydride (0.10 M), reacting at room temperature for 4 h, and washing with ethanol and water in sequence to obtain surface carboxyl-modified Ag nanoparticles;

[0101] (3) Disperse the carboxylated CeO2 nanoparticles in step (2) in phosphate buffer (particle concentration 0.05 mg / mL) -1 ), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added in a molar ratio of 1.5:1, and stirred at room temperature for 4 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (0.50 M).

[0102] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration 0.05 mg / mL). -1 ).

[0103] (5) Human immunoglobulin (0.05 mM), N-isopropylacrylamide (0.50 M), acrylamide (17.40 mM), methacrylic acid (17.40 mM), and N,N-methylenebisacrylamide (6.70 mM) were added to pH 5.0 phosphate buffer and preassembled for 30 minutes to obtain a preassembly solution for use.

[0104] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL, 0.10 mg mL -1 ), acetylacetone (0.05M) and glucose (0.05M) were added to initiate the polymerization reaction. The polymerization was stopped after 6 hours at room temperature to obtain a polymerization solution.

[0105] (7) The polymer solution in step (6) was centrifuged and washed 4 times to obtain a surface protein imprinted polymer.

[0106] Implementation 6

[0107] Preparation of surface protein-imprinted polymers by localized free radical polymerization mediated by enzyme cascade reaction:

[0108] (1) Au nanoparticles were dispersed in a mixture of anhydrous ethanol and deionized water, 3-aminopropyltriethoxysilane (0.10 M) and ammonia water (28 wt%, 0.01 M) were added, and the mixture was reacted at room temperature for 15 h. The mixture was washed with anhydrous ethanol and water in turn to obtain amino Ag nanoparticles;

[0109] (2) The amine Au nanoparticles obtained in step (1) were dispersed in tetrahydrofuran (particle concentration: 0.05 mg / mL) -1 ), adding succinic anhydride (0.10 M), reacting at room temperature for 4 h, and washing with ethanol and water in sequence to obtain surface carboxyl-modified Ag nanoparticles;

[0110] (3) Disperse the carboxylated Au nanoparticles in step (2) in phosphate buffer (particle concentration 0.05 mg / mL) -1 ), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added in a molar ratio of 1.5:1, and stirred at room temperature for 4 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (0.50 M).

[0111] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration 0.05 mg / mL). -1 ).

[0112] (5) Human immunoglobulin (0.05 mM), N-isopropylacrylamide (0.50 M), N-tert-butylacrylamide (17.40

[0113] mM), 2-acrylamido-2-methylpropanesulfonic acid (17.40 mM), N,N-methylenebisacrylamide (6.70 mM)

[0114] A pH 5.0 phosphate buffer was added and pre-assembled for 30 minutes to obtain a pre-assembly solution for use.

[0115] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL, 0.10 mg mL -1 ), acetylacetone (0.05M) and glucose (0.05M) were added to initiate the polymerization reaction. The polymerization was stopped after 6 hours at room temperature to obtain a polymerization solution.

[0116] (7) The polymer solution in step (6) was centrifuged and washed 4 times to obtain a surface protein imprinted polymer.

[0117] Implementation Plan 7

[0118] Preparation of surface protein-imprinted polymers by localized free radical polymerization mediated by enzyme cascade reaction:

[0119] (1) dispersing MOF nanoparticles in a mixture of anhydrous ethanol and deionized water, adding 3-aminopropyltriethoxysilane (0.10 M) and ammonia water (28 wt%, 0.01 M), reacting at room temperature for 15 h, and washing with anhydrous ethanol and water in turn to obtain amino MOF nanoparticles;

[0120] (2) Disperse the aminated MOF nanoparticles obtained in step (1) into tetrahydrofuran (particle concentration 0.05 mg / mL) -1 ), adding succinic anhydride (0.10 M), reacting at room temperature for 4 h, and washing with ethanol and water in sequence to obtain surface carboxyl-modified MOF nanoparticles;

[0121] (3) Dispersing the carboxyl-modified MOF nanoparticles in step (2) in phosphate buffer (particle concentration 0.05

[0122] mg mL -1 ), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added in a molar ratio of 1.5:1, and stirred at room temperature for 4 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (0.50 M).

[0123] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration 0.05 mg / mL). -1 ).

[0124] (5) Cytochrome C (0.05 mM), N-isopropylacrylamide (0.50 M), styrene (17.40 mM), dimethylaminoethyl methacrylate (17.40 mM), and N,N-methylenebisacrylamide (6.70 mM) were added to pH 5.0 phosphate buffer and preassembled for 30 minutes to obtain a preassembly solution for use.

[0125] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL, 0.10 mg mL -1 ), acetylacetone (0.05M) and glucose (0.05M) were added to initiate the polymerization reaction. The polymerization was stopped after 6 hours at room temperature to obtain a polymerization solution.

[0126] (7) The polymer solution in step (6) was centrifuged and washed 4 times to obtain a surface protein imprinted polymer.

[0127] Implementation 8

[0128] Preparation of surface protein-imprinted polymers by localized free radical polymerization mediated by enzyme cascade reaction:

[0129] (1) Dispersing COF nanoparticles in a mixture of anhydrous ethanol and deionized water, adding 3-aminopropyltriethoxysilane (0.10 M) and ammonia water (28 wt%, 0.01 M), reacting at room temperature for 15 h, and washing with anhydrous ethanol and water in turn to obtain amino MOF nanoparticles;

[0130] (2) The aminated COF nanoparticles obtained in step (1) were dispersed in tetrahydrofuran (particle concentration 0.05 mg / mL) -1 ), succinic anhydride (0.10 M) was added, reacted at room temperature for 4 h, and washed with ethanol and water in sequence to obtain surface carboxyl-modified COF nanoparticles;

[0131] (3) Disperse the carboxyl modified COF nanoparticles in step (2) in phosphate buffer (particle concentration 0.05 mg / mL) -1 ), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added in a molar ratio of 1.5:1, and stirred at room temperature for 4 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (0.50 M).

[0132] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration 0.05 mg / mL). -1 ).

[0133] (5) Bovine hemoglobin (0.05 mM), N-isopropylacrylamide (0.50 M), acrylamide (17.40 mM), dimethylaminoethyl methacrylate (17.40 mM), and N,N-methylenebisacrylamide (6.70 mM) were added to pH

[0134] 5.0 phosphate buffer, pre-assemble for 30 min, and obtain the pre-assembly solution for use.

[0135] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL, 0.10 mg mL -1 ), acetylacetone (0.05M) and glucose (0.05M) were added to initiate the polymerization reaction. The polymerization was stopped after 6 hours at room temperature to obtain a polymerization solution.

[0136] (7) The polymer solution in step (6) was centrifuged and washed 4 times to obtain a surface protein imprinted polymer.

[0137] Implementation Plan 9

[0138] Preparation of surface protein-imprinted polymers by localized free radical polymerization mediated by enzyme cascade reaction:

[0139] (1) dispersing Fe3O4 nanoparticles in a mixture of anhydrous ethanol and deionized water, adding 3-aminopropyltriethoxysilane (0.10 M) and ammonia water (28 wt%, 0.01 M), reacting at room temperature for 15 h, and washing with anhydrous ethanol and water in turn to obtain amination Fe3O4 nanoparticles;

[0140] (2) Disperse the amination-containing Fe3O4 nanoparticles obtained in step (1) into tetrahydrofuran (particle concentration 0.05 mg / mL) -1 ), succinic anhydride (0.10 M) was added, reacted at room temperature for 4 h, and washed with ethanol and water in sequence to obtain surface carboxyl-modified Fe3O4 nanoparticles;

[0141] (3) Disperse the carboxylated Fe3O4 nanoparticles in step (2) in phosphate buffer (particle concentration 0.05

[0142] mg mL -1 ), glucose oxidase (GOx) and horseradish peroxidase (HRP) were added in a molar ratio of 1.5:1, and stirred at room temperature for 4 h under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (0.50 M).

[0143] (4) The reaction product was washed with deionized water and dispersed in a phosphate buffer solution at pH 5.0 (ion concentration 0.05 mg / mL). -1 ).

[0144] (5) Add amyloid protein (0.05 mM), N-isopropylacrylamide (0.50 M), styrene (17.40 mM), dimethylaminoethyl methacrylate (17.40 mM), and polyglutamic acid polypeptide cross-linker (6.70 mM) into pH 5.0 phosphate buffer and pre-assemble for 30 minutes to obtain a pre-assembly solution for use.

[0145] (6) Add the nanoparticle dispersion of immobilized enzyme obtained in step (4) (4.0 mL, 0.10 mg mL -1 ), acetylacetone (0.05M) and glucose (0.05M) were added to initiate the polymerization reaction. The polymerization was stopped after 6 hours at room temperature to obtain a polymerization solution.

[0146] (7) The polymer solution in step (6) was centrifuged and washed 4 times to obtain a surface protein imprinted polymer.

[0147] Implementation 10

[0148] The surface protein imprinted polymer prepared by the synthesis method of the present invention is applied to the separation and purification of lysozyme in egg white:

[0149] (1) vacuum drying the surface protein imprinted polymer (MIP) prepared by the synthesis method of the present invention;

[0150] (2) Weigh about 10 mg of the dried MIP in step (2) into a centrifuge tube and add pH 5.0 phosphate buffer (8 mL)

[0151] Allow it to swell fully and then remove the solution after reaching swelling equilibrium;

[0152] (3) Dilute the egg white of fresh eggs 50 times with pH 5.0 phosphate buffer;

[0153] (4) Take 5 mL of the egg white solution diluted 50% in step (3) and add it to the centrifuge tube containing MIP in step (2) and incubate at room temperature for 1 hour to extract lysozyme in the egg white.

[0154] (5) The solution in step (4) was completely removed, and 5 mL of pH 7.4 phosphate buffer was added to elute the lysozyme adsorbed by MIP.

[0155] (6) Detect the extraction effect by gel electrophoresis. The lysozyme standard solution, the egg white solution diluted 50 times, the remaining solution after MIP adsorbed lysozyme, and the eluate were used as four sample solutions for gel electrophoresis. Figure 5 ), the lysozyme in the egg white was almost completely adsorbed by the MIP, while other proteins were well retained (lane 3). After the MIP was eluted, the lysozyme was well eluted and contained almost no other proteins (lane 4).

[0156] The technical solutions disclosed and proposed by the present invention can be realized by those skilled in the art by referring to the contents of this article and appropriately changing the conditions, routes and other links. Although the methods and preparation techniques of the present invention have been described through preferred embodiments, relevant technicians can obviously modify or re-combine the methods and technical routes described herein without departing from the content, spirit and scope of the present invention to realize the final preparation technology. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the spirit, scope and content of the present invention.

Claims

1. A method for preparing a surface protein imprinted polymer by enzyme cascade reaction, characterized in that: The steps include: (1) Carboxyl modification of the surface of the nanoparticles: 3-aminopropyltriethoxysilane is used to hydrolyze the surface of the nanoparticles, and then the aminated nanoparticles are obtained after washing; (2) dispersing the aminated nanoparticles in a tetrahydrofuran solution, adding succinic anhydride, stirring at room temperature for 1-8 hours, and then washing to obtain surface carboxylated nanoparticles; (3) The washed carboxylated nanoparticles were dispersed in phosphate buffer, and glucose oxidase (GOx) and horseradish peroxidase (HRP) were added at a molar ratio of 1.5:

1. Subsequently, GOx and HRP were covalently coupled to the surface of the nanoparticles under the catalysis of 1-ethyl-(3-dimethylaminopropyl)carbodiimide; (4) washing the product of step (3) with deionized water to obtain a nano-ionic dispersion of immobilized enzyme; (5) adding the template protein, main monomer, functional monomer, and cross-linking agent to a pH 5.0 phosphate buffer and pre-assembling for 10-60 minutes to obtain a pre-assembly solution; (6) adding the nanoparticle dispersion of the immobilized enzyme, acetylacetone and glucose to the pre-assembled solution of step (5) to initiate a polymerization reaction; after polymerizing for 4-8 hours at room temperature, the reaction is stopped to obtain a polymerization solution; (7) Centrifuge the polymer solution in step (6) and wash 3-6 times to obtain a surface protein imprinted polymer.

2. The method for preparing a surface protein imprinted polymer by enzyme cascade reaction according to claim 1, characterized in that: Nanoparticles include SiO2, Fe3O4, Fe3O4-Cu, MOF, COF, Au, CeO2 or Ag.

3. The method for preparing a surface protein imprinted polymer by enzyme cascade reaction according to claim 1, characterized in that: In step (1), the concentration of 3-aminopropyltriethoxysilane is 0.01-0.20M.

4. The method for preparing a surface protein imprinted polymer by enzyme cascade reaction according to claim 1, characterized in that: In step (2), the amination nanoparticles are dispersed in tetrahydrofuran solution at a particle concentration of 0.01-0.10 mg mL -1 , the concentration of added succinic anhydride is 0.01-0.20M.

5. The method for preparing a surface protein imprinted polymer by enzyme cascade reaction according to claim 1, characterized in that: In step (3), the washed carboxylated nanoparticles are dispersed in phosphate buffer at a particle concentration of 0.01-0.10 mg / mL. -1 , glucose oxidase (GOx) and horseradish peroxidase (HRP) were added at a molar ratio of 1.5:1, and the concentration of 1-ethyl-(3-dimethylaminopropyl)carbodiimide was 0.05-1.0M.

6. The method for preparing a surface protein imprinted polymer by enzyme cascade reaction according to claim 1, characterized in that: The nano-ion dispersion particle concentration of the immobilized enzyme obtained in step (4) is 0.01-0.10 mg mL -1 .

7. The method for preparing a surface protein imprinted polymer by enzyme cascade reaction according to claim 1, characterized in that: In step (5), the concentration of template protein is 0.01-0.10 mM, the concentration of main monomer is 0.05-1.00 M, the concentration of functional monomer is 1.74-34.80 mM, the concentration of methacrylic acid is 1.74-34.80 mM, and the concentration of cross-linking agent is 0.67-13.35 mM; the template protein in the pre-assembly solution is lysozyme, bovine serum albumin, cytochrome C, bovine hemoglobin, human immunoglobulin, amyloid protein and other acidic, neutral and basic proteins; the main monomer includes N-isopropyl acrylamide and acrylamide; the functional monomer includes methacrylic acid, acrylamide, styrene, N-tert-butyl acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, dimethylaminoethyl methacrylate; the cross-linking agent is N,N-methylenebisacrylamide, polyethylene glycol diacrylate, polyglutamic acid polypeptide cross-linking agent.

8. The method for preparing a surface protein imprinted polymer by enzyme cascade reaction according to claim 1, characterized in that: Step (6) Add 4.0 mL of the nanoparticle dispersion of immobilized enzyme to the pre-assembly solution, 0.01-0.10 mg mL -1 , acetylacetone concentration 0.05-0.20M, glucose concentration 0.05-0.20M.

9. The surface protein imprinted polymer prepared by the method of claim 1 and relying on enzyme cascade reaction is applied to the extraction and purification of proteins in complex biological samples.

Citation Information

Patent Citations

  • Method for preparing lysozyme molecular imprinting nano particles with magnetic responsiveness and extremely high adsorption capacity

    CN102145279A

  • Protein surface molecular imprinting material based on RAFT (Reversible Addition-Fragmentation Chain Transfer) strategy as well as preparation method and application thereof

    CN104231143A

  • Polyeptide crosslinked protein molecularly imprinted polymer, and preparation method and application thereof

    CN109897144A

Cited By

  • Western blot polymer based on organic framework nano-enzyme, preparation method and application

    CN122037060A

  • Protein imprinting polymer based on organic framework nanoszyme, preparation method and application

    CN122037060B