Preparation method and application of waterborne polyurethane slurry
By modifying the reaction of silica and vinyl monomer γ, the adhesion of water-based polyurethane slurry is improved, the problem of short adhesion time of water-based polyurethane is solved, and the green environmental protection and mechanical strength are achieved. It is suitable for shoe materials and separators. Stainless pads, gloves and car interiors.
Patent Information
- Application Number
- CN202411014625.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The short adhesion time of water-based polyurethane in synthetic leather makes it difficult to effectively extend the service life of the leather, and traditional solvent-based ultra-fiber synthetic leather has problems in environmental pollution and energy consumption.
Using an aqueous polyurethane slurry preparation method, the modified silica is mixed with ethylene glycol ether, aromatic polyester polyol, polyether triol and chain extension by mixing vinyl monomer gamma with modified silica. The agent reacts, controls the reaction conditions to improve the adhesion of the slurry.
It significantly improves the adhesion and mechanical strength of water-based polyurethane slurry, extends the service life of the product, and achieves a green and environmentally friendly effect, reduces production costs, and expands application scenarios.
Smart Images

Figure BDA0004965344190000021 
Figure BDA0004965344190000022 
Figure BDA0004965344190000041
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polyurethane, and in particular to a method for preparing a waterborne polyurethane slurry and its application. Background Art
[0002] The traditional microfiber leather process generally adopts the release paper transfer method, which is to first apply the coating chemical material on the textured release paper by roller coating or scraping. There are three layers, namely the surface layer, the middle layer and the adhesive layer. After applying these three layers, the microfiber and the chemical material are bonded by adhesion and with a certain pressure, and then dried at high temperature. Finally, the release paper is peeled off, rolled up, and the finished product is obtained.
[0003] At present, microfiber synthetic leather can be divided into water-based microfiber leather and solvent-based microfiber leather according to the different polyurethane slurries impregnated. Most of the domestic microfiber synthetic leather is solvent-based microfiber leather. This is because compared with water-based microfiber leather, the advantage of solvent-based microfiber leather is that the polyurethane component has a large number of microporous structures, and the synthetic leather made from it feels plump, soft, and has a strong leather feel; the disadvantage is that a large amount of solvent DMF is used in the preparation process, which will cause certain pollution to the environment, and a large amount of energy is required when recycling DMF. Water-based polyurethane uses water as a dispersion medium, does not pollute the environment, and water is cheap and safe to use. Its application in synthetic leather has become a development trend and industry consensus. However, water-based polyurethane has a short adhesion time in synthetic leather, which makes it difficult to effectively extend the service life of the leather material, which needs to be improved. Summary of the invention
[0004] In view of this, the first purpose of the present application is to provide a method for preparing waterborne polyurethane slurry, so as to achieve the purpose of green environmental protection and improve the adhesion of waterborne polyurethane slurry. The specific scheme is as follows:
[0005] A method for preparing an aqueous polyurethane slurry comprises the following steps:
[0006] Step 1, raw material composition: select 30-50 parts of ethylene glycol ether, 5-15 parts of aromatic polyester polyol, 2-8 parts of polyether triol, 2-3 parts of chain extender, 0.3-0.6 parts of fumed silica, 0.1-3 parts of ethyl acetate and 0.01-1 parts of vinyl monomer gamma respectively by weight;
[0007] Step 2, combination optimization: 0.3-0.6 parts by weight of meteorological silica and 60-80% by mass of sulfuric acid solution are mixed, stirred evenly, and 0.01-1 parts by weight of vinyl monomer γ are added dropwise while stirring, and after the addition is completed, stirring is continued for 1-6 hours to obtain modified silica;
[0008] Step 3, chain extension treatment: the modified silica is mixed with 30-50 parts by weight of ethylene glycol ether, 5-15 parts of aromatic polyester polyol, 2-8 parts of polyether triol and 0.1-3 parts of ethyl acetate, and then 2-3 parts by weight of chain extender is added, the chain extension reaction temperature is controlled to be greater than 80°C, and stirred for 5-10 hours;
[0009] Step 4, standing and packaging: lower the temperature to 25°C, stand for 4-24 hours, filter and obtain the finished slurry, and then can it.
[0010] Preferably: the number average molecular weight of the aromatic polyester polyol is 2800-3800; the number average molecular weight of the polyether triol is 3500-4200.
[0011] Preferably: the chain extender is diethylene glycol, sorbitol or diethylaminoethanol.
[0012] Preferably: the vinyl monomer γ is:
[0013]
[0014] Wherein, n is 0, 1, 2 or 3; R1 is a C2-C10 alkyl group or an alkyl group substituted by a chloride ion; R2 is
[0015] Preferably: in step 2, the reaction temperature is controlled to be 40-50°C, and the reaction pressure is controlled to be 10-20 atmospheres.
[0016] Preferably: the specific surface area of the gaseous silica is 60-200m 2 / g, particle size is 10-30nm.
[0017] The second object of the present application is to provide an application of an aqueous polyurethane slurry, including an aqueous polyurethane slurry prepared by the aqueous polyurethane slurry preparation method as described above, and applied to the preparation of shoe materials, dirt-isolating pads, gloves and automobile interiors.
[0018] Preferably, the method comprises coating the aqueous polyurethane slurry on one side of the release paper and then attaching a base cloth thereto to obtain the corresponding shoe material, dirt-isolating pad, glove or automobile interior.
[0019] Preferably, the method further comprises drying, and the drying temperature is controlled to be 70-100°C.
[0020] Preferably: the aqueous polyurethane slurry is cured and printed multiple times until the thickness reaches a preset thickness, and then treated at 80-95% RH and 90-100°C for 2h to obtain a corresponding aqueous polyurethane coating, and then the aqueous polyurethane coating is composited with a corresponding substrate, or the aqueous polyurethane slurry is cured and fixed on a corresponding substrate.
[0021] It can be seen from the above scheme that the present application provides a method for preparing a water-based polyurethane slurry and its application. The method for preparing a water-based polyurethane slurry is achieved by mixing and modifying a vinyl monomer γ with weathered silica, so that the weathered silica plays a role in significantly improving the surface adhesion of the water-based polyurethane slurry. At the same time, the free hydroxyl groups of the active functional groups on the surface of the weathered silica are modified by combining with the vinyl groups in the vinyl monomer γ, thereby significantly improving the adhesion of the modified silica in the obtained water-based polyurethane slurry and having a green and environmentally friendly effect. DETAILED DESCRIPTION
[0022] The following will be clearly and completely described in conjunction with the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0023] The following is a detailed description of a method for preparing a waterborne polyurethane slurry and its application in the present application.
[0024] A method for preparing an aqueous polyurethane slurry comprises the following steps:
[0025] Step 1, raw material composition: select 30-50 parts of ethylene glycol ether, 5-15 parts of aromatic polyester polyol, 2-8 parts of polyether triol, 2-3 parts of chain extender, 0.3-0.6 parts of fumed silica, 0.1-3 parts of ethyl acetate and 0.01-1 parts of vinyl monomer gamma respectively by weight;
[0026] Step 2, combination optimization: 0.3-0.6 parts by weight of meteorological silica and 60-80% by mass of sulfuric acid solution are mixed, stirred evenly, and then stirred and 0.01-1 parts by weight of vinyl monomer γ are added dropwise, the reaction temperature is controlled to be 40-50° C., the reaction pressure is controlled to be 10-20 atmospheres, and after the addition of vinyl monomer γ is completed, stirring is continued for 1-6 hours to obtain modified silica;
[0027] Step 3, chain extension treatment: the modified silica is mixed with 30-50 parts by weight of ethylene glycol ether, 5-15 parts of aromatic polyester polyol, 2-8 parts of polyether triol and 0.1-3 parts of ethyl acetate, and then 2-3 parts by weight of chain extender is added, the chain extension reaction temperature is controlled to be greater than 80°C, and stirred for 5-10 hours;
[0028] Step 4, standing and packaging: lower the temperature to 25°C, stand for 4-24 hours, filter and obtain the finished slurry, and then can it.
[0029] Among them, the number average molecular weight of aromatic polyester polyol is 2800-3800, the number average molecular weight of polyether triol is 3500-4200, and the specific surface area of the meteorological silica is 60-200m 2 / g, particle size is 10-30nm.
[0030] The chain extender is a conventional chain extender material. The chain extenders in the embodiments of the present application are diethylene glycol and sorbitol purchased from Hubei Jusheng Technology Co., Ltd. and diethylaminoethanol purchased from Shanghai Dingmiao Chemical Technology Co., Ltd.
[0031] Meanwhile, the vinyl monomer γ is:
[0032]
[0033] Wherein, n is 0, 1, 2 or 3; R1 is a C2-C10 alkyl group or an alkyl group substituted by a chloride ion; R2 is
[0034] An application of waterborne polyurethane slurry includes waterborne polyurethane slurry prepared by the waterborne polyurethane slurry preparation method as described above, and is used in preparing shoe materials, dirt-isolating pads, gloves and automobile interiors.
[0035] In the application process, the water-based polyurethane slurry is coated on one side of the release paper and then attached to the base cloth, and the drying temperature is controlled to be 70-100°C, and then the corresponding shoe material, dirt isolation pad, gloves or car interior is obtained. Alternatively, the water-based polyurethane slurry is cured and printed multiple times until the thickness reaches the preset thickness, and then treated at 80-95% RH and 90-100°C for 2h to obtain the corresponding water-based polyurethane coating, and then the water-based polyurethane coating is composited with the corresponding substrate, or the water-based polyurethane slurry is cured and fixed on the corresponding substrate.
[0036] Embodiment 1
[0037] A method for preparing an aqueous polyurethane slurry comprises the following steps:
[0038] Step 1, raw material composition: select 30 parts of ethylene glycol ether, 5 parts of aromatic polyester polyol, 2 parts of polyether triol, 2 parts of chain extender, 0.3 parts of fumed silica, 0.1 parts of ethyl acetate and 0.01 parts of vinyl monomer γ respectively by weight;
[0039] Step 2, combination optimization: 0.3 parts by weight of meteorological silica and 60% by mass of sulfuric acid solution are mixed, stirred evenly, and then 0.01 parts by weight of vinyl monomer γ are added dropwise while stirring, the reaction temperature is controlled to be 40° C., the reaction pressure is controlled to be 10 atmospheres, and after the addition of vinyl monomer γ is completed, stirring is continued for 1 hour to obtain modified silica;
[0040] Step 3, chain extension treatment: the modified silica is mixed with 30 parts by weight of ethylene glycol ether, 5 parts of aromatic polyester polyol, 2 parts of polyether triol and 0.1 parts of ethyl acetate, and then 2 parts by weight of chain extender are added, the chain extension reaction temperature is controlled to 82° C., and stirred for 10 hours;
[0041] Step 4, standing and packaging: lower the temperature to 25°C, stand for 4 hours, filter and obtain the finished slurry, and then can it.
[0042] Among them, the number average molecular weight of aromatic polyester polyol is 2800-3800, the number average molecular weight of polyether triol is 3500-4200, and the specific surface area of the meteorological silica is 60-200m 2 / g, particle size is 10-30nm.
[0043] The chain extender is a conventional chain extender material. The chain extender in the embodiment of the present application is sorbitol purchased from Hubei Jusheng Technology Co., Ltd.
[0044] Meanwhile, the vinyl monomer γ is:
[0045]
[0046] Where n is 0; R2 is
[0047] An application of waterborne polyurethane slurry includes waterborne polyurethane slurry prepared by the waterborne polyurethane slurry preparation method as described above, and is used in preparing shoe materials, dirt-isolating pads, gloves and automobile interiors.
[0048] During the application process, the water-based polyurethane slurry is coated on one side of the release paper and then attached to the base cloth, and the drying temperature is controlled to be 70°C, thereby obtaining the corresponding shoe materials, dirt isolation pads, gloves or car interiors.
[0049] Embodiment 2
[0050] A method for preparing an aqueous polyurethane slurry comprises the following steps:
[0051] Step 1, raw material composition: select 40 parts of ethylene glycol ether, 10 parts of aromatic polyester polyol, 5 parts of polyether triol, 2 parts of chain extender, 0.4 parts of fumed silica, 1 part of ethyl acetate and 0.5 parts of vinyl monomer γ respectively by weight;
[0052] Step 2, combination optimization: 0.4 parts by weight of meteorological silica and 72% by mass of sulfuric acid solution are mixed, stirred evenly, and 0.5 parts by weight of vinyl monomer γ is added dropwise while stirring, the reaction temperature is controlled to be 45° C., the reaction pressure is controlled to be 15 atmospheres, and after the addition of vinyl monomer γ is completed, stirring is continued for 3 hours to obtain modified silica;
[0053] Step 3, chain extension treatment: the modified silica is mixed with 40 parts by weight of ethylene glycol ether, 10 parts of aromatic polyester polyol, 5 parts of polyether triol and 1 part of ethyl acetate, and then 2 parts by weight of chain extender are added, the chain extension reaction temperature is controlled at 90° C., and stirred for 7 hours;
[0054] Step 4: Stand and package: Lower the temperature to 25°C, stand for 12 hours, filter and obtain the finished slurry, and then can it.
[0055] Among them, the number average molecular weight of aromatic polyester polyol is 2800-3800, the number average molecular weight of polyether triol is 3500-4200, and the specific surface area of the meteorological silica is 60-200m 2 / g, particle size is 10-30nm.
[0056] The chain extender is a conventional chain extender material. The chain extender in the embodiment of the present application is diethylene glycol purchased from Hubei Jusheng Technology Co., Ltd.
[0057] Meanwhile, the vinyl monomer γ is:
[0058]
[0059] Wherein, n is 3; R1 is a C2 alkyl group substituted by a chloride ion.
[0060] An application of waterborne polyurethane slurry includes waterborne polyurethane slurry prepared by the waterborne polyurethane slurry preparation method as described above, and is used in preparing shoe materials, dirt-isolating pads, gloves and automobile interiors.
[0061] During the application process, the water-based polyurethane slurry is cured and printed multiple times until the thickness reaches a preset thickness, and then treated at 80% RH and 90°C for 2 hours to obtain the corresponding water-based polyurethane coating. The water-based polyurethane coating is then composited with the corresponding substrate, or the water-based polyurethane slurry is cured and fixed on the corresponding substrate.
[0062] Embodiment 3
[0063] A method for preparing an aqueous polyurethane slurry comprises the following steps:
[0064] Step 1, raw material composition: select 50 parts of ethylene glycol ether, 15 parts of aromatic polyester polyol, 8 parts of polyether triol, 3 parts of chain extender, 0.6 parts of fumed silica, 3 parts of ethyl acetate and 1 part of vinyl monomer gamma respectively by weight;
[0065] Step 2, combination optimization: 0.6 parts by weight of meteorological silica and 80% by mass of sulfuric acid solution are mixed, stirred evenly, and then 1 part by weight of vinyl monomer γ is added dropwise while stirring, the reaction temperature is controlled to be 50° C., the reaction pressure is controlled to be 20 atmospheres, and after the addition of vinyl monomer γ is completed, stirring is continued for 6 hours to obtain modified silica;
[0066] Step 3, chain extension treatment: the modified silica is mixed with 50 parts by weight of ethylene glycol ether, 15 parts of aromatic polyester polyol, 8 parts of polyether triol and 3 parts of ethyl acetate, and then 3 parts by weight of chain extender are added, the chain extension reaction temperature is controlled at 98°C, and stirred for 5 hours;
[0067] Step 4: Stand and package: Lower the temperature to 25°C, stand for 24 hours, filter and obtain the finished slurry, and then can it.
[0068] Among them, the number average molecular weight of aromatic polyester polyol is 2800-3800, the number average molecular weight of polyether triol is 3500-4200, and the specific surface area of the meteorological silica is 60-200m 2 / g, particle size is 10-30nm.
[0069] The chain extender is a conventional chain extender material. The chain extender in the embodiment of the present application is diethylaminoethanol purchased from Shanghai Dingmiao Chemical Technology Co., Ltd.
[0070] Meanwhile, the vinyl monomer γ is:
[0071]
[0072] Wherein, n is 2; R1 is a C2 alkyl group; R2 is
[0073] An application of waterborne polyurethane slurry includes waterborne polyurethane slurry prepared by the waterborne polyurethane slurry preparation method as described above, and is used in preparing shoe materials, dirt-isolating pads, gloves and automobile interiors.
[0074] During the application process, the water-based polyurethane slurry is cured and printed multiple times until the thickness reaches a preset thickness, and then treated at 95% RH and 100°C for 2 hours to obtain the corresponding water-based polyurethane coating. The water-based polyurethane coating is then compounded with the corresponding substrate, or the water-based polyurethane slurry is cured and fixed on the corresponding substrate.
[0075] Embodiment 4
[0076] The difference between Example 4 and Example 3 is that n is 1; R1 is a C6 alkyl group substituted by chloride ion; R2 is
[0077] Comparative Example 1
[0078] The difference between Comparative Example 1 and Example 2 is that the vinyl monomer γ in Comparative Example 1 is trimethylchlorosilane.
[0079] Comparative Example 2
[0080] The difference between Comparative Example 2 and Example 3 is that in Comparative Example 2, fumed silica is used instead of modified silica.
[0081] Comparative Example 3
[0082] The difference between Comparative Example 3 and Example 3 is that R2 in Comparative Example 3 is tolyl.
[0083] Performance tests were performed on the above-mentioned embodiments 1 to 4 and comparative examples 1 to 3.
[0084] The test contents include abrasion resistance test according to GB / T 3903.16-2008 and folding resistance test according to GB / T3903.41-2009, as well as one-day compressive strength and tensile strength. The thickness of the above coatings is controlled to be consistent. The test results are shown in Table 1 below:
[0085] Table 1 Performance test results
[0086]
[0087] As can be seen from Table 1 above, the method for preparing water-based polyurethane slurry of the present application adopts vinyl monomer γ as a modifying material and obtains a modified silica material after mixing and reacting with meteoric silica, and then obtains a water-based polyurethane slurry with significantly improved surface adhesion and mechanical strength by reacting the modified silica with ethylene glycol ether, aromatic polyester polyol, polyether triol, chain extender and ethyl acetate. The wear resistance, folding resistance, compressive strength and tensile strength are significantly improved, and the method is suitable for surface coating treatment in various fields, thereby significantly expanding the application scenarios while reducing the production and preparation cost of the water-based polyurethane slurry, and has huge economic benefits and market prospects.
[0088] In summary, the present application provides a method for preparing a waterborne polyurethane slurry and its application. The method for preparing a waterborne polyurethane slurry is to modify the vinyl monomer γ by mixing and modifying the weathered silica so that the weathered silica can significantly improve the surface adhesion in the waterborne polyurethane slurry. The free hydroxyl groups on the surface of the weathered silica are modified by combining with the vinyl groups in the vinyl monomer γ, thereby significantly improving the adhesion of the modified silica in the obtained waterborne polyurethane slurry and having a green and environmentally friendly effect. The application of the waterborne polyurethane slurry has the effects of wide applicability and strong adhesion, thereby effectively reducing the production and manufacturing cost of the waterborne polyurethane slurry while extending the service life of the applied product, thereby expanding the market prospects.
[0089] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods or devices.
[0090] It should be noted that the descriptions involving "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.
[0091] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A method for preparing an aqueous polyurethane slurry, characterized in that: The steps include: Step 1, raw material composition: select 30-50 parts of ethylene glycol ether, 5-15 parts of aromatic polyester polyol, 2-8 parts of polyether triol, 2-3 parts of chain extender, 0.3-0.6 parts of fumed silica, 0.1-3 parts of ethyl acetate and 0.01-1 parts of vinyl monomer gamma respectively by weight; Step 2, combination optimization: 0.3-0.6 parts by weight of meteorological silica and 60-80% by mass of sulfuric acid solution are mixed, stirred evenly, and 0.01-1 parts by weight of vinyl monomer γ are added dropwise while stirring, and after the addition is completed, stirring is continued for 1-6 hours to obtain modified silica; Step 3, chain extension treatment: the modified silica is mixed with 30-50 parts by weight of ethylene glycol ether, 5-15 parts of aromatic polyester polyol, 2-8 parts of polyether triol and 0.1-3 parts of ethyl acetate, and then 2-3 parts by weight of chain extender is added, the chain extension reaction temperature is controlled to be greater than 80°C, and stirred for 5-10 hours; Step 4, standing and packaging: lower the temperature to 25°C, stand for 4-24 hours, filter and obtain the finished slurry, and then can it.
2. The method for preparing an aqueous polyurethane slurry according to claim 1, characterized in that: The number average molecular weight of the aromatic polyester polyol is 2800-3800; the number average molecular weight of the polyether triol is 3500-4200.
3. The method for preparing an aqueous polyurethane slurry according to claim 1, characterized in that: The chain extender is diethylene glycol, sorbitol or diethylaminoethanol.
4. The method for preparing an aqueous polyurethane slurry according to claim 1, characterized in that: The vinyl monomer γ is: Wherein, n is 0, 1, 2 or 3; R1 is a C2-C10 alkyl group or an alkyl group substituted with a chloride ion; R2 is 5. The method for preparing an aqueous polyurethane slurry according to claim 1, characterized in that: In step 2, the reaction temperature is controlled to be 40-50° C. and the reaction pressure is controlled to be 10-20 atmospheres.
6. The method for preparing an aqueous polyurethane slurry according to claim 1, characterized in that: The specific surface area of the gaseous silica is 60-200m 2 / g, particle size is 10-30nm.
7. An application of an aqueous polyurethane slurry, characterized in that: The invention comprises an aqueous polyurethane slurry prepared by the aqueous polyurethane slurry preparation method according to any one of claims 1 to 6, and is used for preparing shoe materials, dirt-isolating pads, gloves and automobile interiors.
8. The use of an aqueous polyurethane slurry according to claim 7, characterized in that: The method comprises coating water-based polyurethane slurry on one side of release paper and then laminating base cloth to obtain the corresponding shoe material, dirt-isolating pad, glove or automobile interior.
9. The use of an aqueous polyurethane slurry according to claim 8, characterized in that: The method also includes drying, and the drying temperature is controlled to be 70-100°C.
10. The use of an aqueous polyurethane slurry according to claim 7, characterized in that: The method comprises curing the waterborne polyurethane slurry, printing it multiple times until the thickness reaches a preset thickness, treating it at 80-95% RH and 90-100°C for 2h to obtain a corresponding waterborne polyurethane coating, and then compounding the waterborne polyurethane coating with a corresponding substrate, or curing the waterborne polyurethane slurry and fixing it on a corresponding substrate.