Pyridine modified polyethyleneimine and method for removing Cu (II) in industrial wastewater with high selectivity based on pyridine modified polyethyleneimine
The combination of pyridine-modified polyethyleneimine with Cu(II) chelation and power-on ultrafiltration device solves the problem of low Cu(II) removal efficiency in low pH water, achieving high selective removal and heavy metal recovery , improves processing efficiency and cost-effectiveness.
Patent Information
- Application Number
- CN202411323029.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-23
AI Technical Summary
The prior art has low efficiency in removing Cu(II) in water with low pH, and the existing polyelectrolyte materials have poor selectivity for binding to metal ions, making it difficult to achieve efficient heavy metal recovery.
Using pyridine-modified polyethyleneimine (PPEI) to chelate the specific molar ratio with Cu(II), and filter and electrolytic recovery using a power-on ultrafiltration device, achieving high selective removal and reuse of Cu(II) .
The removal rate of Cu(II) is achieved in water at low pH value to reach more than 95%, which improves the selectivity of polyelectrolyte materials, and achieves low-cost heavy metal recovery and treatment through electrolysis recovery of PPEI.
Smart Images

Figure CN118955898A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a pyridine-modified polyethyleneimine and also relates to a method for removing Cu(II) from industrial wastewater with high selectivity based on the modified material. Background Art
[0002] Traditional heavy metal wastewater treatment and copper recovery technologies include chemical precipitation, oxidation-reduction, ion exchange, adsorption, electrochemical, etc. The above treatment methods have their own characteristics but also have certain limitations. Chemical precipitation has the characteristics of fast flocculation speed, low treatment cost, simple operation and certain selectivity, but the removal of Cu(II) is extremely sensitive to pH changes. When the pH value is between 8.5 and 9.5, a higher removal rate (up to more than 90%) can be achieved; however, when the pH value exceeds this range, the removal rate of Cu(II) will drop significantly, below 80%. In the process of treating heavy metal ions, the oxidation-reduction method consumes a large amount of reagents, the catalyst cannot be recovered, and the cost of adjusting the pH value is high. The removal efficiency of Cu(II) is usually no more than 60%. Although the ion exchange method has high removal efficiency and good selectivity, the removal rate can reach more than 95%. However, its treatment cost is high, the resin is easily contaminated by heavy metal ions, and it is difficult to regenerate. Although the adsorption method has low investment and operating costs, does not require the addition of chemicals, and has no secondary pollution, its regeneration efficiency is low, usually not exceeding 70%, making it difficult to recycle heavy metals. The electrochemical method has high removal efficiency and stable treatment effect, with a removal rate of more than 90%, but for electrolyte solutions with lower concentrations, there are problems of high energy consumption and fast consumption of anode materials.
[0003] PEI (polyethyleneimine) is a polyelectrolyte material that can combine with various metal ions in water, thereby removing heavy metals from wastewater through membrane filtration or the addition of surfactants, and then pH adjustment to achieve metal recovery and reuse of PEI. However, PEI has poor selectivity for binding with metal ions, and in low pH water (acidic), PEI has poor binding ability with metal ions. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a pyridine-modified polyethyleneimine that can chelate with Cu(II) in low pH water; another purpose of the present invention is to provide a method for highly selectively removing Cu(II) from industrial wastewater based on the above-mentioned modified material, which method can achieve specific and efficient removal of Cu(II) from industrial wastewater at any pH.
[0005] Technical solution: The pyridine-modified polyethyleneimine of the present invention has the structural formula:
[0006]
[0007] The molecular weight of the pyridine-modified polyethyleneimine is 218,000 or above, and it is easily retained by the ultrafiltration membrane at this molecular weight.
[0008] The pyridine-modified polyethyleneimine is prepared by the following method, and the specific steps are as follows:
[0009] (1) 2-chloromethylpyridine hydrochloride or 4-chloromethylpyridine hydrochloride and NaOH are first mixed, and after the reaction, a PEI aqueous solution is added thereto;
[0010] (2) NaOH is then added to the mixed solution again to neutralize the hydrochloric acid generated by the reaction;
[0011] (3) heating the mixed solution of step (2) in a water bath and stirring, and generating a precipitate;
[0012] (4) adding sulfuric acid solution thereto, the precipitate slowly dissolves under acidic conditions, and the solution is heated in a water bath and stirred for 4 hours until no more precipitate remains in the solution, thereby obtaining a PPEI aqueous solution.
[0013] Wherein, in step (1), the PEI (polyethyleneimine) is a branched chain structure with a molecular weight of 70,000 or above.
[0014] Wherein, in step (1), the molar ratio of 2-chloromethylpyridine hydrochloride or 4-chloromethylpyridine hydrochloride to NaOH is 1:1; the molar ratio of 2-chloromethylpyridine hydrochloride or 4-chloromethylpyridine hydrochloride to PEI (calculated as monomer) is 1:1.
[0015] In step (2), the amount of NaOH added again is consistent with the amount added in step (1).
[0016] Wherein, in step (3), the water bath heating temperature is 60-70° C., and the heating time is 1 hour.
[0017] The method for highly selectively removing Cu(II) from industrial wastewater based on the pyridine-modified polyethyleneimine comprises the following steps:
[0018] (1) PPEI is added to copper-containing industrial wastewater at a molar ratio of PPEI to Cu(II) of 4:1 and stirred, and PPEI selectively chelates Cu(II) in the wastewater;
[0019] (2) filtering the fully reacted solution through an electric ultrafiltration device to obtain a concentrated solution enriched with chelates and wastewater after copper removal;
[0020] (3) placing the concentrated solution filtered in step (2) in an electrolytic cell for electrolysis to recover copper and PPEI solution, and the recovered PPEI solution can be recycled.
[0021] The method of the present invention requires first measuring the concentration of Cu(II) in the wastewater for different industrial wastewaters, and then adding PPEI at a molar ratio of PPEI to Cu(II) of 4:1 based on the amount of Cu(II) to achieve efficient chelation.
[0022] Wherein, in step (2), the powered ultrafiltration device includes a membrane pool; the membrane pool is provided with an inlet electrode plate, an outlet electrode plate and an ultrafiltration membrane attached to the outlet electrode plate; the inlet electrode plate and the outlet electrode plate are arranged opposite to each other and are respectively connected to an external power supply through wires; the inlet electrode plate and the outlet electrode plate are fixed in the membrane pool through a sealing device, and the space between the inlet electrode plate and the outlet electrode plate is enclosed by the sealing device to form a filtration area; the inlet electrode plate and the outlet electrode plate are both metal electrode plates, and the electrode plates are provided with through holes for water to pass through; the reacted solution is pumped into the membrane pool by a pump, and after flowing through the filtration area, the macromolecular substances that have not passed through the ultrafiltration membrane flow out of the membrane pool through the concentrated water outlet on one side of the inlet electrode plate, and the substances that have passed through the ultrafiltration membrane flow out of the membrane pool from the outlet on one side of the outlet electrode plate.
[0023] Among them, the electrode plate at the water outlet and the electrode plate at the water inlet are connected to the positive and negative poles of the power supply respectively, and the working pressure of ultrafiltration is 0.15~0.20MPa
[0024] In step (3), the electrode spacing in the electrolytic cell is 8 cm, the electrolysis current is 0.2 A, and the current density is 44.44 A·m -2 .
[0025] PPEI is a process in which a pyridine group is introduced into the polyethyleneimine (PEI) molecule. The introduction of this group increases the selectivity of PPEI for Cu(II) and enables efficient chelation with Cu(II) at a lower pH. Under the condition of a molar ratio of PPEI:Cu(II)=4:1, combined with the use of a charged ultrafiltration device, the removal rate of Cu(II) in wastewater can reach 95%. Finally, the recovery of Cu(II) and the reuse of PPEI are achieved through the electrolysis of the concentrated solution.
[0026] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The pyridine-modified polyethyleneimine (PPEI) of the present invention can chelate with Cu(II) in low-pH water, thereby overcoming the problem that the existing polyelectrolyte materials have poor binding force with metal ions in low-pH water; (2) The method of the present invention achieves high-selective removal of Cu(II) in industrial wastewater or copper-containing complex water bodies in low-pH water through polyelectrolyte materials with specific structures and polyelectrolyte materials with specific molar ratios to Cu(II), and the removal rate can reach more than 95%; in the ultrafiltration process of the present invention, charging the membrane can increase the anti-pollution ability of the membrane, and the membrane flux decrease rate is nearly 0.5 times that of not charging; the method of the present invention can achieve low-cost treatment of industrial wastewater, remove Cu(II) in the wastewater, meet the wastewater discharge standard, and achieve selective capture and recovery of Cu(II). BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The reaction equation for preparing pyridine-modified polyethyleneimine in Example 1;
[0028] Figure 2 The reaction equation for preparing pyridine-modified polyethyleneimine in Example 2;
[0029] Figure 3 This is the Fourier infrared spectra of PPEI and PEI in Example 1;
[0030] Figure 4 The removal results of Cu(II) at different pH and different polyelectrolyte materials (PPEI and PEI);
[0031] Figure 5 This is a structural principle diagram of the powered ultrafiltration device;
[0032] Figure 6 It is a schematic diagram of the structure of the membrane pool in the powered ultrafiltration device;
[0033] Figure 7 The results of membrane flux decreasing over time under different power conditions. DETAILED DESCRIPTION
[0034] Example 1
[0035] like Figure 1 As shown, the preparation method of pyridine-modified polyethyleneimine of the present invention specifically comprises the following steps:
[0036] (1) Weigh 4.101 g of 2-chloromethylpyridine hydrochloride and add it to a 50 mL centrifuge tube; add one equivalent (relative to 2-chloromethylpyridine hydrochloride) of NaOH to the centrifuge tube to neutralize the hydrochloric acid in the 2-chloromethylpyridine hydrochloride, that is, add 2.5 mL of a 10 mol / L NaOH solution;
[0037] (2) adding 2.15 g of PEI aqueous solution to a centrifuge tube, wherein the mass concentration of PEI in the PEI aqueous solution is 50%, and the molar ratio of 2-chloromethylpyridine hydrochloride to PEI (based on monomer) is 1:1; after the reaction, adding 2.5 mL of 10 mol / L NaOH solution to the centrifuge tube again to neutralize the hydrochloric acid generated by the reaction;
[0038] (3) Place the mixture in a 70°C water bath and stir. After 1 hour, a red precipitate will form in the solution and the rotor will not rotate. At this time, add 2 mL of 5 mol / L H2SO4 solution and shake the centrifuge tube quickly to allow the rotor to continue rotating.
[0039] (4) The solution was heated and stirred at 70° C. for 4 hours until no more precipitation was present in the solution, and then water was added to dilute to the scale to obtain a uniform brown-yellow solution, i.e., 50 mL of a 0.5 mol / L PPEI aqueous solution.
[0040] Figure 3 The Fourier transform infrared (FTIR) spectrum characterization results of branched PEI and PPEI products. The FTIR spectrum of PEI shows typical characteristic peaks, namely, the NH stretching vibration of the primary amine and the secondary amine is about 3300-3500 cm -1 , NH bending is about 1600-1650cm -1 , CN stretching is about 1050cm -1 In contrast, the infrared absorption spectrum of PPEI shows that -C=C- is at 1472 cm -1 and -C=N- at 1570cm -1 There are additional stretching vibration absorption peaks at 1435 and 999 cm -1 Deformation absorption peaks of the ring plane of the 2-substituted pyridine group appeared at all locations. These characteristic peaks confirmed that the 2-methylpyridine group had been successfully grafted onto the main chain of PEI.
[0041] Example 2
[0042] like Figure 2 As shown, the preparation method of pyridine-modified polyethyleneimine of the present invention specifically comprises the following steps:
[0043] (1) Weigh 4.101 g of 4-chloromethylpyridine hydrochloride (amount of substance n = 0.025 mol) and add it to a 50 mL centrifuge tube; add one equivalent (relative to 4-chloromethylpyridine hydrochloride) of NaOH to the centrifuge tube to neutralize the hydrochloric acid in the 4-chloromethylpyridine hydrochloride, that is, add 2.5 mL of a 10 mol / L NaOH solution;
[0044] (2) adding 2.15 g of PEI aqueous solution to a centrifuge tube, wherein the mass concentration of PEI in the PEI aqueous solution is 50%, and the molar ratio of 4-chloromethylpyridine hydrochloride to PEI (based on monomer) is 1:1; after the reaction, adding 2.5 mL of 10 mol / L NaOH solution to the centrifuge tube again to neutralize the hydrochloric acid generated by the reaction;
[0045] (3) Place the mixture in a 70°C water bath and stir. After 1 hour, a red precipitate will form in the solution and the rotor will not rotate. At this time, add 2 mL of 5 mol / L H2SO4 solution and shake the centrifuge tube quickly to allow the rotor to continue rotating.
[0046] (4) The solution was heated and stirred at 70° C. for 4 hours until no more precipitation was present in the solution, and then water was added to dilute to the scale to obtain a uniform brown-yellow solution, i.e., 50 mL of a 0.5 mol / L PPEI aqueous solution.
[0047] Example 3
[0048] Based on the method for highly selectively removing Cu(II) from copper-containing wastewater using pyridine-modified polyethyleneimine prepared in Example 1, the initial Cu(II) concentration in the copper-containing wastewater is 1 mM, and the pH of the copper-containing wastewater is 3. The specific steps are as follows:
[0049] (1) adding 16 mL of the PPEI aqueous solution prepared in Example 1 to 2000 mL of copper-containing wastewater at a molar ratio of PPEI to Cu(II) of 4:1 and stirring, and PPEI selectively chelates Cu(II) in the wastewater;
[0050] (2) Stirring for 10 seconds, filtering the fully reacted solution through a charged ultrafiltration device, with the electrode voltage constant at 0.2 V and the ultrafiltration pressure maintained at 0.15-0.20 MPa, filtering for 8 hours to obtain a 5-fold concentrated solution and wastewater with a Cu(II) removal rate of more than 95%, and the effluent Cu(II) concentration is less than 0.05 mM;
[0051] (3) The concentrated solution filtered in step (2) is placed in an electrolytic cell for electrolysis, wherein the cathode and cathode electrodes are graphite sheets and copper sheets, respectively, the effective size of the electrode plates is 9×5 cm, the electrode spacing is 8 cm, the current during the electrolysis process is constant at 0.2 A, and the copper recovery rates after electrolysis for 1 h, 5 h, and 8 h are 20.3%, 0.666%, and 84.0%, respectively. The PPEI solution after electrolysis can be recycled.
[0052] Figure 5 The schematic diagram of the structure of the powered ultrafiltration device is a tangential flow filtration device. Figures 5-6 It can be seen that the powered ultrafiltration device includes a water inlet, a water outlet and a concentrate outlet; the powered ultrafiltration device also includes a membrane pool; the membrane pool is provided with an inlet electrode plate, an outlet electrode plate and an ultrafiltration membrane attached to the outlet electrode plate; the inlet electrode plate and the outlet electrode plate are arranged opposite to each other and are respectively connected to an external power supply through wires; the inlet electrode plate and the outlet electrode plate are fixed in the membrane pool through a sealing device, and the space between the inlet electrode plate and the outlet electrode plate is enclosed by the sealing device to form a filtration area; the inlet electrode plate and the outlet electrode plate are both metal electrode plates, and the electrode plates are provided with through holes for water to pass through; the reacted solution is pumped into the membrane pool by a pump, and after flowing through the filtration area, the macromolecular substances that have not passed through the ultrafiltration membrane flow out of the membrane pool through the concentrate outlet on one side of the inlet electrode plate, and the substances that have passed through the ultrafiltration membrane flow out of the membrane pool from the outlet on one side of the outlet electrode plate.
[0053] The filtration process of the powered ultrafiltration device is as follows: the feed is pumped into the membrane pool by a pump and the pressure required for ultrafiltration (0.15-0.20Mpa) is provided, the concentrated water outlet (concentrated liquid) flows out of the membrane pool from one side of the electrode plate at the water inlet end, and the filtrate passes through the ultrafiltration membrane to obtain copper-free water. The powered ultrafiltration device also includes a pump group, which is composed of a peristaltic pump and a constant pressure regulating valve; the membrane pool includes two coplanar electrode plates (circular electrode plates), the electrode plates are made of titanium plated with platinum, and the electrode plates are provided with through holes for water to pass through, the diameter of each electrode plate is d=10cm, and the spacing is 5mm; the ultrafiltration membrane is a polyethersulfone ultrafiltration membrane, the effective filtration size is a diameter of d=10cm, and the ultrafiltration membrane is fitted with the electrode plate at the water outlet end; the two coplanar electrode plates are connected to the power supply through wires, wherein the electrode plate at the water outlet end and the electrode plate at the water inlet end are respectively connected to the positive and negative poles of the power supply, and the power supply is a DC power supply.
[0054] Figure 7The figure shows the change of membrane flux under different power supply, where 0.2V means that the electrode plate at the outlet and the electrode plate at the inlet are connected to the positive and negative poles of the power supply respectively, and provide a constant voltage of 0.2V; 0V means that no power supply is provided; -0.2V means that the electrode plate at the outlet and the electrode plate at the inlet are connected to the negative and positive poles of the power supply respectively, and provide a constant voltage of 0.2V. The results show that under the condition of 0.2V, the decrease rate of membrane flux is 0.42 times and 0.30 times of that under the condition of no power and -0.2V respectively, which indicates that under the condition of 0.2V, the anti-pollution performance of the ultrafiltration membrane is better, and more wastewater can be treated under the same filtration time.
[0055] Example 4
[0056] The process of Example 4 is basically the same as that of Example 3, with the only difference being that the initial pH of the copper-containing wastewater is 1; the concentration of Cu(II) in the filtrate effluent is below 0.08 mM; and the copper recovery rate is 82.0% after 8 h of electrolysis.
[0057] Comparative Example 1
[0058] The process of Comparative Example 1 is basically the same as that of Example 3, with the only difference being that in step (1), PEI is added to the copper-containing wastewater at a molar ratio of PEI to Cu(II) of 4:1; and the concentration of Cu(II) in the copper-removing wastewater after filtration is 46%.
[0059] Comparative Example 2
[0060] The process of Comparative Example 2 is basically the same as that of Example 4, with the only difference being that in step (1), PEI is added to the copper-containing wastewater at a molar ratio of PEI to Cu(II) of 4:1; and the concentration of Cu(II) in the copper-removing wastewater after filtration is 28%.
[0061] Under two different pH conditions, the initial Cu(II) concentration was 1 mM. PEI and PPEI solutions with different ratios of Cu(II) were added to the solution. The complexation with Cu(II) was completed within 10 seconds under stirring. The Cu(II) concentration in the effluent was detected by ultrafiltration. The removal rate results are as follows: Figure 4 .pass Figure 4 It can be seen that when the molar ratio of PPEI to Cu(II) is 4:1, the removal rate of copper by PPEI is more than 92%.
Claims
1. A pyridine-modified polyethyleneimine, characterized in that: Its structural formula is:
2. The pyridine-modified polyethyleneimine according to claim 1, characterized in that: The molecular weight of the pyridine-modified polyethyleneimine is 218,000 or above.
3. The method for preparing pyridine-modified polyethyleneimine according to claim 1, characterized in that: The specific steps are as follows: (1) 2-chloromethylpyridine hydrochloride or 4-chloromethylpyridine hydrochloride and NaOH are first mixed, and after the reaction, a PEI aqueous solution is added thereto; (2) NaOH is then added to the mixed solution again to neutralize the hydrochloric acid generated by the reaction; (3) heating the mixed solution of step (2) in a water bath and stirring, and generating a precipitate; (4) adding sulfuric acid solution thereto, the precipitate is slowly dissolved under acidic conditions, and the solution is heated and stirred in a water bath until no more precipitate remains in the solution, thereby obtaining a PPEI aqueous solution.
4. The preparation method according to claim 3, characterized in that: In step (1), the PEI is a branched chain structure with a molecular weight of 70,000 or more.
5. The preparation method according to claim 3, characterized in that: In step (1), the added molar amounts of 2-chloromethylpyridine hydrochloride or 4-chloromethylpyridine hydrochloride and NaOH are the same; based on monomers, the added molar amounts of 2-chloromethylpyridine hydrochloride or 4-chloromethylpyridine hydrochloride and PEI are the same.
6. The preparation method according to claim 3, characterized in that: In step (2), the amount of NaOH added again is the same as that added in step (1).
7. The preparation method according to claim 3, characterized in that: In step (3), the water bath heating temperature is 60-70° C., and the heating time is not less than 1 hour.
8. The method for highly selectively removing Cu(II) from industrial wastewater using pyridine-modified polyethyleneimine according to claim 1, characterized in that: The steps include: (1) PPEI is added to copper-containing industrial wastewater at a molar ratio of PPEI to Cu(II) of 4:1 and stirred, and PPEI selectively chelates Cu(II) in the wastewater; (2) filtering the fully reacted solution through an electric ultrafiltration device to obtain a concentrated solution enriched with chelate and wastewater after copper removal.
9. The method according to claim 8, characterized in that: In step (2), the powered ultrafiltration device includes a membrane pool; the membrane pool is provided with an inlet electrode plate, an outlet electrode plate and an ultrafiltration membrane attached to the outlet electrode plate; the inlet electrode plate and the outlet electrode plate are arranged opposite to each other and are respectively connected to an external power supply through wires; the inlet electrode plate and the outlet electrode plate are fixed in the membrane pool through a sealing device, and the space between the inlet electrode plate and the outlet electrode plate is enclosed by the sealing device to form a filtration area; the inlet electrode plate and the outlet electrode plate are provided with through holes for water to pass through; the reacted solution is pumped into the membrane pool by a pump, and after flowing through the filtration area, the macromolecular substances that have not passed through the ultrafiltration membrane flow out of the membrane pool through the concentrated water outlet on one side of the inlet electrode plate, and the substances that have passed through the ultrafiltration membrane flow out of the membrane pool from the outlet on one side of the outlet electrode plate.
10. The method according to claim 9, characterized in that: The electrode plate at the water outlet and the electrode plate at the water inlet are connected to the positive and negative electrodes of the power supply respectively, and the working pressure of the ultrafiltration is 0.15-0.20MPa.
Citation Information
Patent Citations
Combined process and device for treating slightly polluted water
CN104098209A
Preparation method of pyridine-functionalized chitosan adsorbent
CN110368911A
Pyridylamine chelate resin for removing heavy metal cations in strong acid wastewater and preparation method of pyridylamine chelate resin
CN111068630A
Preparation method of pyridine-functionalized sodium alginate adsorbent
CN112337437A
Preparation method and application of pyridylamino composite hydrogel adsorbent
CN112387256A