Preparation method of vinyl-terminated polydimethylsiloxane with medium and high viscosity
By using low viscosity vinyl ended polysiloxane and linear phosphazene catalyst under low temperature vacuum conditions, medium and high viscosity vinyl ended polydimethylsiloxane was prepared, solving the difficulty of viscosity measurement and production in the prior art. The high cost problem achieves efficient vinyl retention and hardness improvement.
Patent Information
- Application Number
- CN202411300145.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-18
AI Technical Summary
The prior art is difficult to effectively prepare medium and high viscosity vinyl end-ended polydimethylsiloxane, especially in the reactor bubble accumulation and stability problems of linear phosphazene catalysts under high viscosity, resulting in difficulty in measuring viscosity and increased production costs.
Low viscosity vinyl end capped polysiloxane is used as the header, combined with linear phosphazene catalyst and terminator, and reacted under low temperature vacuum conditions. The viscosity is prepared by siloxane hydroxyl condensation and polysiloxane segment rearrangement. Medium- and high viscosity vinyl end-capped polydimethylsiloxane of 500mPa·s or above reduces volatile components and simplifies the process flow.
The preparation of medium and high viscosity vinyl end-capped polydimethylsiloxane is realized, reducing volatile content and vinyl loss, improving vinyl retention and hardness, simplifying the production process, and avoiding additional vacuum removal rings body operation.
Smart Images

Figure CN118955911A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of vinyl-terminated polysiloxane preparation, and in particular relates to a method for preparing medium- and high-viscosity vinyl-terminated polydimethylsiloxane. Background Art
[0002] Vinyl-terminated polysiloxane can be used as a key raw material to prepare a variety of downstream products such as silicone rubber, silicone emulsion and silicone release products. For example, high-temperature silicone rubber (HTV) and liquid silicone rubber (RTV) are made by mixing polysiloxane and white carbon black at high temperature, and can obtain corresponding functions after vulcanization. Silicone rubber maintains good mechanical properties in a wide temperature range (-50℃~200℃) and can be used at high temperatures for a long time. Compared with other materials, it has an irreplaceable role.
[0003] At present, the preparation of vinyl-terminated polysiloxane used in industry mostly uses cyclosiloxane monomer (DMC) as raw material, divinyltetramethyldisiloxane as vinyl double-capping agent, and obtains vinyl-terminated polydimethylsiloxane polymer (85-87%) and DMC (13-15%) mixture by base catalysis, and then removes DMC by vacuum distillation to obtain polysiloxanes with different molecular weights. However, vacuum distillation is an energy-consuming process, especially when a large amount of DMC needs to be separated, the energy consumption increases significantly.
[0004] In order to reduce the generation of cyclosiloxane monomers, researchers have explored a new preparation method. This method uses linear monomers as raw materials and linear chlorophosphazene as catalysts to prepare polysiloxanes through the polycondensation reaction of silanol groups. No obvious cyclosiloxane is generated during the reaction process. This is one of the main ways to synthesize low-volatility polysiloxanes. For example, Chinese patent CN 117777452A discloses a method for preparing medium-low viscosity (1-10000mm) polysiloxanes using linear phosphazene as catalyst, linear monomers as raw materials, vinyl double caps as molecular weight regulators, and continuous nitrogen dehydration. 2 / s) of vinyl silicone oil. It should be pointed out that for vinyl silicone oils that are usually used in liquid silicone rubber or need to be used at high temperatures, their viscosity is usually more than 10,000 mPa·s, and the raw rubber molecular weight can even reach 600,000 to 800,000 Daltons. Such high viscosity makes them difficult to measure with conventional viscometers. However, the preparation method disclosed in CN 117777452 A is not suitable for preparing such high-viscosity vinyl silicone oils, because continuous nitrogen gas dehydration will cause a large number of bubbles to accumulate in the reactor, and at high viscosity, it will become extremely difficult to eliminate foam, resulting in low utilization; secondly, based on the relationship between viscosity and vinyl content in CN 117777452A, it is found that there is a certain loss of vinyl, which undoubtedly increases the production cost. Furthermore, linear phosphazenes are easily hydrolyzed and inactivated in the presence of trace water and at high temperatures (80°C and above), and their stability is not ideal.
[0005] Therefore, there is an urgent need for a method for preparing medium-to-high viscosity vinyl-terminated polydimethylsiloxane to solve the shortcomings of the prior art. Summary of the invention
[0006] In view of the above problems, the object of the present invention is to provide a method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane, which can produce medium-high viscosity vinyl-terminated polydimethylsiloxane with a viscosity of 500 mPa·s and above, and the medium-high viscosity vinyl-terminated polydimethylsiloxane has a low volatile content, a high vinyl retention rate, and a hardness reaching a normal level.
[0007] To achieve the above objectives, the first aspect of the present invention provides a method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane, comprising the steps of:
[0008] (1) heating the linear body to 35-60° C. and then performing a dehydration treatment;
[0009] (2) adding a capping agent, a linear phosphazene catalyst, and a vinyl-terminated side-chain vinyl polysiloxane to the linear product after step (1), and then reacting under vacuum conditions;
[0010] (3) adding a terminator to the product after the reaction in step (2) to react to obtain a medium-high viscosity vinyl-terminated polydimethylsiloxane with a viscosity of 500 mPa·s or more;
[0011] The linear body is a straight-chain hydroxyl-terminated polydimethylsiloxane with a viscosity of 40 to 200 mPa·s;
[0012] The capping agent is a vinyl-terminated polysiloxane with a viscosity of 2 to 50 mPa·s;
[0013] The structure of the terminator is shown in Formula 1:
[0014]
[0015] Where n 1 The value ranges from 30 to 150.
[0016] Compared with the prior art, the present invention adopts a linear phosphazene (LPNC) that can catalyze both silanol condensation and rearrangement of polysiloxane segments as a catalyst, so that a linear body, a capping agent and a vinyl-terminated side-chain vinyl polysiloxane react under low-temperature vacuum conditions, and finally obtains a medium-high viscosity vinyl-terminated polydimethylsiloxane with a viscosity of 500mPa·s and above. Wherein, a low-viscosity vinyl-terminated polysiloxane is used as a capping agent, which greatly improves the boiling point of the capping agent, is not easy to volatilize under vacuum and heating conditions, thereby reducing the loss of the capping agent and improving the vinyl retention rate. At the same time, the reaction mode of low-temperature vacuum makes the linear phosphazene catalyst have a good catalytic activity, thereby effectively reducing the amount of volatile ring body generated, so that there is no need to perform an additional vacuum removal ring body operation after the termination reaction is completed, simplifying the entire production process. In addition, the terminator shown in Formula 1 can not only neutralize the linear phosphazene catalyst to stop the reaction, but also vinyl-cap a small amount of the reaction ends to make the hardness reach a normal level, which effectively reduces the hydroxyl value of the system and avoids the structuring problem when preparing liquid rubber base or high-temperature mixed rubber.
[0017] Furthermore, the dehydration treatment of the present invention comprises: vacuum stirring and dehydrating the linear body so that the linear body loses less than 0.2% of its weight after being dried in an oven at 100° C. for 1 hour.
[0018] Further, the preparation raw materials of the present invention include 100 parts by mass of linear body, 0.1-10 parts by mass of capping agent, 0-10 parts by mass of vinyl-terminated side-chain vinyl polysiloxane, 0.05-2 parts by mass of terminator, and 10-80 ppm of linear phosphazene catalyst. Specifically, the content of capping agent can be but not limited to 0.1 parts, 1 parts, 3 parts, 4 parts, 6 parts, 8 parts, 10 parts; the content of vinyl-terminated side-chain vinyl polysiloxane can be but not limited to 0 parts, 1 parts, 3 parts, 4 parts, 6 parts, 8 parts, 10 parts; the content of terminator can be but not limited to 0.05 parts, 1 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2.0 parts; the content of linear phosphazene catalyst can be but not limited to 10ppm, 20ppm, 40ppm, 60ppm, 70ppm, 80ppm.
[0019] Furthermore, when the amount of the added vinyl-terminated side-chain vinyl polysiloxane is 0 parts, the reaction equation of step (2) of the present invention is as follows:
[0020]
[0021] Among them, n2 The value of n is 10~100, 3 The value ranges from 170 to 8500.
[0022] Furthermore, when the amount of the vinyl-terminated side chain vinyl polysiloxane added is greater than 0 parts, vinyl groups can be provided for the side chains of the polysiloxane. The reaction equation of step (2) of the present invention is as follows:
[0023]
[0024] Where n 2 =10~100, m+n=10~1200, p+q=170~8500.
[0025] Furthermore, in step (2) of the present invention, the vacuum degree under vacuum conditions is greater than 0.08 MPa, and the reaction time is 2 to 10 hours. The vacuum conditions allow the water generated in the system to be discharged, maintain the stability of the linear phosphazene catalyst, and accelerate the reaction process. Under the catalytic action of the linear phosphazene catalyst, rearrangement is achieved between molecular chains, and equilibrium is finally reached after 2 to 10 hours of reaction.
[0026] Furthermore, the structural formula of the linear phosphazene catalyst (LPNC) of the present invention is as follows:
[0027]
[0028] Further, the preparation of the capping agent of the present invention comprises: mixing vinyl double capping (cas: 2627-95-4), vinyl terminated dimethyl silicone oil, and linear phosphazene catalyst and reacting at 50-80°C for 2-10h. The inventors of the present application found in the research process that a reaction temperature lower than 50°C will result in a longer reaction time, while a reaction temperature higher than 80°C will increase the amount of volatile ring bodies generated in the system, so the reaction temperature is preferably 50-80°C, such as the reaction temperature can be but not limited to 50°C, 60°C, 70°C, 80°C.
[0029] Furthermore, the reaction formula for preparing the capping agent of the present invention is as follows:
[0030]
[0031] Among them, n 4 =170~1200,n 5 =1~50.
[0032] Furthermore, the raw materials for preparing the capping agent of the present invention include 100 parts by mass of vinyl double capping, 120 to 2000 parts by mass of vinyl-terminated dimethyl silicone oil, and 40 to 120 ppm of linear phosphazene catalyst. Specifically, the content of vinyl-terminated dimethyl silicone oil can be but not limited to 120 parts, 250 parts, 380 parts, 500 parts, 720 parts, 950 parts, 1080 parts, 1400 parts, 1600 parts, 1800 parts, and 2000 parts; the content of linear phosphazene catalyst can be but not limited to 40ppm, 60ppm, 80ppm, 100ppm, and 120ppm. Compared with the traditional alkaline method for preparing capping agents, the advantages of using linear phosphazene catalysts are: 1) No neutralization is required, and it can be directly used in the next step; 2) The ring body content is low, and no de-lowening treatment is required, and it can be directly used in the next step.
[0033] Further, the preparation of the terminator of the present invention comprises: putting cyclic siloxane and potassium hydroxide into a reactor, introducing nitrogen, evacuating, introducing nitrogen and heating, stopping introducing nitrogen after the potassium hydroxide is completely dissolved, adding a vinyl double end cap to react, and continuing to introduce nitrogen after the reaction is completed. Specifically, the cyclic siloxane can be octamethylcyclotetrasiloxane (D4). Specifically, the reaction formula for preparing the terminator of the present invention is as follows:
[0034]
[0035] Where z is the molar amount of octamethylcyclotetrasiloxane, n 1 The value ranges from 30 to 150.
[0036] Furthermore, the preparation of the terminator of the present invention comprises: putting cyclic siloxane and potassium hydroxide into a reactor, bubbling nitrogen, then vacuuming at below 60°C for 10 minutes to remove carbon dioxide in the air of the reactor, then passing nitrogen to eliminate vacuum and heating to 140-150°C; stopping passing nitrogen after KOH is completely dissolved, then adding a vinyl double-capping agent to react for 15 minutes, and continuing to bubbling nitrogen for 3 hours after the reaction is completed. In addition, the inventor of the present invention found in the process of invention that if organic amines (such as triethylamine) are simply used as terminators, the hardness of the vinyl-terminated polysiloxane obtained in step (3) does not reach the normal level.
[0037] Further, the raw materials for preparing the terminator of the present invention include 100 parts by mass of cyclic siloxane, 1.5 to 3.5 parts by mass of potassium hydroxide, and 2.5 to 5.83 parts by mass of vinyl double-end caps. Specifically, the content of potassium hydroxide (KOH) can be but not limited to 1.5 parts, 2 parts, 2.5 parts, 3 parts, and 3.5 parts; the content of vinyl double-end caps can be but not limited to 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5.0 parts, 5.5 parts, and 5.83 parts.
[0038] Further, the molar ratio of potassium hydroxide to the vinyl double end cap of the present invention is 1.9 to 2.1: 1. Specifically, the molar ratio of potassium hydroxide to the vinyl double end cap may be, but is not limited to, 1.9: 1, 2.0: 1, or 2.1: 1.
[0039] Furthermore, the reaction time in step (3) of the present invention is 2 to 5 hours. Specifically, the reaction time in step (3) can be, but is not limited to, 2 hours, 3 hours, 4 hours, or 5 hours.
[0040] Furthermore, the reaction formula of step (3) of the present invention is as follows:
[0041]
[0042] n 1 The value ranges from 30 to 150. DETAILED DESCRIPTION
[0043] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.
[0044] The capping agent, linear phosphazene catalyst and terminator used in the examples and comparative examples can be prepared by referring to the following preparation method:
[0045] The preparation of the capping agent includes: mixing 100 parts by mass of a vinyl double capping agent, 240 parts by mass of a vinyl-terminated dimethyl silicone oil having a viscosity of 2000 mPa·s, and 120 ppm of a linear phosphazene catalyst, and reacting the mixture at 80°C for 2 hours. After testing, a vinyl-terminated polysiloxane capping agent having a viscosity of 4 mPa·s is obtained, wherein the vinyl content is 8.54 wt%.
[0046] The preparation of the linear phosphazene catalyst comprises: 22.69 g PCl 5 、2.912g NH 4 Cl, 73.42gC 2 H 2 Cl 4 Mix, heat to reflux temperature and react for 12 hours to obtain a transparent liquid. After testing, the effective content of the catalyst is 30%. Since the linear phosphazene catalyst is easy to absorb moisture, N 2 Atmosphere preservation.
[0047] The preparation of the terminator includes: putting 100g of octamethylcyclotetrasiloxane and 2.1g of KOH into a reactor, bubbling with nitrogen, vacuuming for 10 minutes at a material temperature below 60°C to remove carbon dioxide in the air of the reactor, and then heating to 145°C by nitrogen de-vacuuming; stopping nitrogen bubbling after KOH is completely dissolved, adding 3.5g of vinyl double head (the molar ratio of potassium hydroxide to vinyl double head is 2:1) to react for 15min, and continuing to bubble nitrogen for 3 hours after the reaction to obtain a terminator, and the alkali content in the terminator is detected to be 0.3743mmol / g.
[0048] Example 1
[0049] This embodiment provides a method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane, the steps comprising:
[0050] (1) 100 parts by weight of a linear body having a viscosity of 100 mPa·s is heated to 40° C., and then subjected to vacuum stirring and dehydration so that the linear body loses less than 0.2% in weight after being dried in an oven at 100° C. for 1 hour;
[0051] (2) adding 1.54 parts by mass of a capping agent and 40 ppm of a linear phosphazene catalyst to the linear product after step (1), and then reacting under a vacuum condition of 0.09 MPa for 5 hours;
[0052] (3) 0.23 parts by weight of the terminator was added to the product after the reaction in step (2) and reacted for 3 hours. The product having a viscosity of 1×10 4 mPa·s of vinyl-terminated polydimethylsiloxane, wherein the terminal vinyl content is 0.13 wt%.
[0053] Example 2
[0054] This embodiment provides a method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane, the steps comprising:
[0055] (1) 100 parts by weight of a linear body having a viscosity of 100 mPa·s is heated to 60° C., and then subjected to vacuum stirring and dehydration so that the linear body loses less than 0.2% in weight after being dried in an oven at 100° C. for 1 hour;
[0056] (2) Add 1.5 parts by mass of a capping agent, 40 ppm of a linear phosphazene catalyst, and 1 part by mass of a vinyl-terminated side-chain vinyl polysiloxane (viscosity 3×10 4 mPa·s, vinyl content of 4 wt%), and then reacted under 0.09 MPa vacuum conditions for 8 h;
[0057] (3) 0.23 parts by weight of the terminator was added to the product after the reaction in step (2) and reacted for 3 hours. The product having a viscosity of 1×104 mPa·s of vinyl-terminated and vinyl-side polydimethylsiloxane, wherein the vinyl-terminated content is 0.13wt%, the vinyl-side content is 0.04wt%, and the total vinyl content is 0.17wt%.
[0058] Example 3
[0059] This embodiment provides a method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane, the steps comprising:
[0060] (1) 100 parts by weight of a linear body having a viscosity of 100 mPa·s is heated to 40° C., and then subjected to vacuum stirring and dehydration so that the linear body loses less than 0.2% in weight after being dried in an oven at 100° C. for 1 hour;
[0061] (2) adding 0.7 parts by weight of a capping agent and 40 ppm of a linear phosphazene catalyst to the linear product after step (1), and then reacting under a vacuum condition of 0.095 MPa for 5 hours;
[0062] (3) 0.23 parts by weight of the terminator was added to the product after the reaction in step (2) and reacted for 3 hours. The product having a viscosity of 1×10 5 mPa·s of vinyl-terminated polydimethylsiloxane, wherein the terminal vinyl content is 0.06 wt%.
[0063] Example 4
[0064] This embodiment provides a method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane, the steps comprising:
[0065] (1) 100 parts by weight of a linear body having a viscosity of 100 mPa·s is heated to 60° C., and then subjected to vacuum stirring and dehydration so that the linear body loses less than 0.2% in weight after being dried in an oven at 100° C. for 1 hour;
[0066] (2) Add 0.7 parts by mass of a capping agent, 40 ppm of a linear phosphazene catalyst, and 0.5 parts by mass of a vinyl-terminated side-chain vinyl polysiloxane (viscosity 3×10 4 mPa·s, vinyl content of 4 wt%), and then reacted under 0.095 MPa vacuum conditions for 8 h;
[0067] (3) 0.23 parts by weight of the terminator was added to the product after the reaction in step (2) and reacted for 3 hours. The product having a viscosity of 1×10 5 mPa·s of vinyl-terminated and vinyl-side polydimethylsiloxane, wherein the vinyl-terminated content is 0.06wt%, the vinyl-side content is 0.02wt%, and the total vinyl content is 0.08wt%.
[0068] Example 5
[0069] This embodiment provides a method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane, the steps comprising:
[0070] (1) 100 parts by weight of a linear body having a viscosity of 200 mPa·s is heated to 40° C., and then subjected to vacuum stirring and dehydration so that the linear body loses less than 0.2% in weight after being dried in an oven at 100° C. for 1 hour;
[0071] (2) adding 0.17 parts by mass of a capping agent and 10 ppm of a linear phosphazene catalyst to the linear product after step (1), and then reacting under a vacuum condition of 0.095 MPa for 10 hours;
[0072] (3) adding 0.05 parts by weight of a terminator to the product of step (2) for 3 hours, and filtering to obtain a semi-fluid vinyl-terminated polydimethylsiloxane (i.e., raw rubber with a trade name of 110-0) having a vinyl mass fraction of 0.015%.
[0073] Example 6
[0074] This embodiment provides a method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane, the steps comprising:
[0075] (1) 100 parts by weight of a linear body having a viscosity of 200 mPa·s is heated to 40° C., and then subjected to vacuum stirring and dehydration so that the linear body loses less than 0.2% in weight after being dried in an oven at 100° C. for 1 hour;
[0076] (2) Add 0.17 parts by mass of a capping agent, 10 ppm of a linear phosphazene catalyst, and 0.7 parts by mass of a vinyl-terminated side-chain vinyl polysiloxane (viscosity 1×10 5 mPa·s, vinyl content of 10 wt%), and then reacted under 0.095 MPa vacuum conditions for 8 h;
[0077] (3) 0.05 parts by weight of a terminator is added to the product of step (2) and reacted for 3 hours. A semi-fluid vinyl-terminated polydimethylsiloxane (i.e., raw rubber with the trade name 110-3) is obtained by filtration. The mass fraction of terminal vinyl groups is 0.014%, the mass fraction of side vinyl groups is 0.069%, and the mass fraction of total vinyl groups is 0.083%.
[0078] Comparative Example 1
[0079] This comparative example provides a method for preparing vinyl-terminated polydimethylsiloxane, the steps comprising:
[0080] (1) heating 100 parts by mass of octamethylcyclotetrasiloxane to 100° C.;
[0081] (2) adding 1.54 parts by mass of a capping agent and 100 ppm of a tetramethylammonium hydroxide catalyst to the octamethylcyclotetrasiloxane after step (1), and then reacting for 5 hours;
[0082] (3) After step (2), the temperature was raised to 140° C. to degrade the tetramethylammonium hydroxide catalyst to obtain a solution with a viscosity of 7.0×10 3 mPa·s of vinyl terminated polydimethylsiloxane.
[0083] Comparative Example 2
[0084] This comparative example provides a method for preparing vinyl-terminated polydimethylsiloxane, the steps comprising: (1) heating 100 parts by mass of a 100 mPa·s linear solid to 100° C.;
[0085] (2) adding 1.54 parts by mass of a capping agent and 100 ppm of tetramethylammonium hydroxide to the linear body after step (1), reacting for 5 hours, and then dehydrating under a vacuum condition of 0.05 MPa;
[0086] (3) after step (2), the temperature was raised to 140° C. to degrade the tetramethylammonium hydroxide catalyst, and a viscosity of 6.5*10 3 mPa·s of vinyl terminated polydimethylsiloxane.
[0087] Comparative Example 3
[0088] This comparative example provides a method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane, the steps comprising:
[0089] (1) 100 parts by weight of a linear body having a viscosity of 100 mPa·s is heated to 40° C., and then subjected to vacuum stirring and dehydration so that the linear body loses less than 0.2% in weight after being dried in an oven at 100° C. for 1 hour;
[0090] (2) adding 1.54 parts by mass of a capping agent and 40 ppm of a linear phosphazene catalyst to the linear product after step (1), and then reacting under a vacuum condition of 0.09 MPa for 5 hours;
[0091] (3) Add 50 ppm KOH (50% aqueous solution) to the product after the reaction in step (2) and react for 3 hours. After filtration, a solution with a viscosity of 1×10 4 mPa·s of vinyl-terminated polydimethylsiloxane, wherein the terminal vinyl content is 0.13 wt%.
[0092] Comparative Example 4
[0093] This comparative example provides a method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane, the steps comprising:
[0094] (1) 100 parts by weight of a linear body having a viscosity of 100 mPa·s is heated to 40° C., and then subjected to vacuum stirring and dehydration so that the linear body loses less than 0.2% in weight after being dried in an oven at 100° C. for 1 hour;
[0095] (2) adding 0.45 parts by mass of vinyl double-capped (cas: 2627-95-4) and 40 ppm of linear phosphazene catalyst to the linear product after step (1), and then reacting under a vacuum condition of 0.09 MPa for 5 hours;
[0096] (3) 0.073 parts by mass of the terminator was added to the product after the reaction in step (2) and reacted for 3 hours. The obtained product had a viscosity of 2.5×10 4 mPa·s vinyl-terminated polydimethylsiloxane, wherein the terminal vinyl content is 0.09 wt%.
[0097] It is necessary to explain that: in Examples 1 to 6, only a small portion of the terminator is used to end-cap the polysiloxane main chain, and the remaining majority serves to neutralize the catalyst and render it ineffective, so the amount of vinyl introduced by the terminator is very small, so when calculating the terminal vinyl content of the finished silicone oil, the terminal vinyl introduced by the terminator can be ignored. In addition, since the amount of terminal vinyl in the vinyl-terminated side-chain vinyl polysiloxane is relatively small, the terminal vinyl introduced by the vinyl-terminated side-chain vinyl polysiloxane can be ignored when calculating the terminal vinyl content of the finished silicone oil in Examples 2, 4, and 6.
[0098] The vinyl-terminated polydimethylsiloxanes prepared in Examples 1 to 6 and Comparative Examples 1 to 4 were tested for hardness, volatile matter, and vinyl retention rate according to the following testing methods. The test results are shown in Table 1.
[0099] Hardness test: take the silicone oil after the reaction is completed, determine the vinyl content through a hydrogen spectrum, use Si-H / Si-Vi=2 times hydrogen-containing silicone oil for vulcanization, the hydrogen content in the hydrogen-containing silicone oil is 0.75%, and the platinum catalyst usage is 3ppm.
[0100] Volatile content detection: Accurately weigh about 5g of polysiloxane 1 , placed in an aluminum box, baked at 200℃ for 4h, residual mass m 2 , volatile matter = (m 1 -m 2 ) / m 1 , measure 3 times and take the average value.
[0101] Vinyl retention rate: The ratio of actual content to vinyl addition amount was determined by H NMR spectrum.
[0102] Table 1 Performance test results
[0103]
[0104] As shown in Example 1 to Example 6, the preparation method of the medium and high viscosity vinyl-terminated polydimethylsiloxane of the present invention can be used to obtain a medium and high viscosity vinyl-terminated polydimethylsiloxane with a viscosity of 500mPa·s and above, and the low volatile content of the medium and high viscosity vinyl-terminated polydimethylsiloxane is low, the vinyl retention rate is high, and the hardness reaches a normal level, because the present invention adopts low-viscosity vinyl-terminated polysiloxane as a capping agent, which greatly improves the boiling point of the capping agent, and is not easy to volatilize under vacuum and heating conditions, thereby reducing the loss of the capping agent and improving the vinyl retention rate. At the same time, the reaction mode of low-temperature vacuum makes the linear phosphazene catalyst have a good catalytic activity, and then effectively reduces the low volatile ring body generation amount, so that there is no need to carry out the operation of additional vacuum removal of the ring body after the termination reaction ends, simplifying the whole production process. In addition, the terminator shown in Formula 1 can not only neutralize the linear phosphazene catalyst and stop the reaction, but also a small amount of reaction ends can be vinyl-terminated, so that the hardness reaches a normal level.
[0105] Comparing Example 1 with Comparative Examples 1 to 2, it can be seen that the volatile matter in the vinyl-terminated polydimethylsiloxane prepared by catalyzing octamethylcyclotetrasiloxane or a linear system with an alkaline catalyst is relatively high (above 12%), so it needs to be vacuum-removed before it can be used in industry. Therefore, the present invention uses linear phosphazene as a catalyst to react the linear body and the capping agent to prepare medium- and high-viscosity vinyl-terminated polydimethylsiloxane, which can be directly used in industry after the reaction is completed without post-treatment, which effectively avoids the ring-opening-backbiting equilibrium problem existing in the alkaline method, avoids the production of the ring body, and eliminates the neutralization step and the vacuum ring-removing operation, as well as the poisoning effect of the presence of trace alkali on the linear phosphazene catalyst.
[0106] By comparing Example 1 with Comparative Example 3, it can be seen that although the viscosity, volatile matter, and vinyl retention rate of the vinyl-terminated polydimethylsiloxanes prepared in Example 1 and Comparative Example 3 are similar, the hardness of the two is quite different, which indicates that the use of conventional alkali (such as potassium hydroxide) can only neutralize the linear phosphazene to stop the reaction, but cannot vinyl-terminate a small amount of the reaction ends, which also indicates that a small amount of non-vinyl-terminated polysiloxane has a great influence on the hardness of the rubber compound.
[0107] Comparing Example 1 with Comparative Example 4, it can be seen that the vinyl retention rate of the vinyl-terminated polydimethylsiloxane prepared in Comparative Example 4 is only 69%, which indicates that conventional capping agents (such as vinyl double capping agents) are not suitable for linear condensation systems with vacuum and heating. This is because in the LPNC catalytic process, the condensation rate will be greater than the rearrangement rate, resulting in a relatively slow disconnection of the vinyl double capping agent, which will result in a large amount of loss under vacuum heating conditions. At the same time, the inventors of the present application also found that the low-viscosity capping agent prepared by the alkali method is also not suitable for this system, because the residual alkali will affect the catalytic activity of the linear phosphazene and even inactivate it.
[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane, characterized in that the steps include: (1) heating the linear body to 35-60° C. and then performing a dehydration treatment; (2) adding a capping agent, a linear phosphazene catalyst, and a vinyl-terminated side-chain vinyl polysiloxane to the linear product after step (1), and then reacting under vacuum conditions; (3) adding a terminator to the product after the reaction in step (2) to react to obtain a medium-high viscosity vinyl-terminated polydimethylsiloxane with a viscosity of 500 mPa·s or more; The linear body is a straight-chain hydroxyl-terminated polydimethylsiloxane with a viscosity of 40 to 200 mPa·s; The capping agent is a vinyl-terminated polysiloxane with a viscosity of 2 to 50 mPa·s; The structure of the terminator is shown in Formula 1: The value of n1 ranges from 30 to 150.
2. The method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane according to claim 1, characterized in that: The dehydration treatment includes: vacuum stirring and dehydrating the linear body so that the linear body loses less than 0.2% of its weight after being dried in an oven at 100° C. for 1 hour.
3. The method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane according to claim 1, characterized in that: The preparation raw materials include 100 parts by weight of the linear body, 0.1-10 parts by weight of the capping agent, 0-10 parts by weight of the vinyl-terminated side-chain vinyl polysiloxane, 0.05-2 parts by weight of the terminator, and 10-80 ppm of the linear phosphazene catalyst.
4. The method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane according to claim 1, characterized in that: The vacuum degree under the vacuum conditions in step (2) is greater than 0.08 MPa, and the reaction time is 2 to 10 hours.
5. The method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane according to claim 1, characterized in that: The preparation of the capping agent comprises: mixing vinyl double capping, vinyl terminated dimethyl silicone oil and linear phosphazene catalyst and reacting them at 50-80° C. for 2-10 hours.
6. The method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane according to claim 5, characterized in that: The raw materials for preparing the capping agent include 100 parts by mass of the vinyl double capping agent, 120 to 2000 parts by mass of the vinyl-terminated dimethyl silicone oil, and 40 to 120 ppm of the linear phosphazene catalyst.
7. The method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane according to claim 1, characterized in that: The preparation of the terminator comprises: putting cyclic siloxane and potassium hydroxide into a reactor, introducing nitrogen, evacuating, introducing nitrogen again and heating, stopping introducing nitrogen after the potassium hydroxide is completely dissolved, adding a vinyl double end cap to react, and continuing to introduce nitrogen after the reaction is completed.
8. The method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane according to claim 7, characterized in that: The raw materials for preparing the terminator include 100 parts by mass of the cyclic siloxane, 1.5 to 3.5 parts by mass of the potassium hydroxide, and 2.5 to 5.83 parts by mass of the vinyl double cap.
9. The method for preparing a medium-high viscosity vinyl-terminated polydimethylsiloxane according to claim 8, characterized in that: The molar ratio of the potassium hydroxide to the vinyl double end cap is 1.9 to 2.1:
1.
10. The method for preparing medium-high viscosity vinyl-terminated polydimethylsiloxane according to claim 1, characterized in that: The reaction time in step (3) is 2 to 5 hours.
Citation Information
Patent Citations
Polyvinylsilicone oil preparation method
CN105384936A
Preparation method of ultralow-viscosity vinyl silicone oil
CN112280039A
Preparation method of phosphonitrile chloride catalyst and application of phosphonitrile chloride catalyst in preparation of vinyl-terminated polydimethylsiloxane
CN115572390A
Method for preparing polysiloxane through composite catalysis of phosphazene salt / strong base
CN117777449A
New catalysts for polycondensation and redistribution of organosiloxane polymers
GB9623505D0
Cited By
Vinyl-terminated silicone oil with side chain containing silicon-hydrogen bond, preparation method and liquid silicone rubber of vinyl-terminated silicone oil
CN121270926A
Segmented preparation method of low-ring polysiloxane and segmented telomerization reaction kettle