Hydrophobic slow-release type self-snow-melting and ice-inhibiting material and preparation method thereof
By combining modified diatomaceous earth with surface-modified materials, a hydrophobic slow-release self-melting snow and ice suppressing material was prepared, solving the problems of large material consumption and component loss in existing technologies, and achieving efficient snow melting and ice suppression as well as environmentally friendly effects.
Patent Information
- Application Number
- CN202411012162.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
Existing technologies for preparing snow-melting and ice-suppressing materials for asphalt mixtures suffer from problems such as large material consumption, low utilization rate, and rapid loss of effective components during hot and humid seasons, resulting in environmental pollution and poor snow-melting effect.
The material employs a hydrophobic, slow-release, self-melting snow and ice suppressing agent. By combining modified diatomaceous earth with surface-modified materials, a stable coating structure is formed, controlling the release of chlorides and ensuring effective snow melting in low-temperature winter environments, while reducing component loss during hot and rainy summer seasons.
It achieves rapid snow melting and ice suppression in low-temperature winter environments, while reducing material loss during hot and rainy summer seasons, thus reducing the amount of traditional snow melting agents used and minimizing environmental pollution.
Smart Images

Figure CN118956346A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road pavement antifreezing and deicing, and specifically relates to a hydrophobic slow-release self-snow-melting and ice-inhibiting material and a preparation method thereof. Background Art
[0003] Traditional methods of clearing ice and snow from roads are mainly mechanical snow removal and spreading snow-melting agents. However, mechanical snow removal requires a large amount of machinery and manual labor, which is time-consuming and inefficient. Although spreading snow-melting agents can improve the efficiency of snow removal to a certain extent, a large amount of snow-melting agents is required for roads with thicker ice and snow, which may cause corrosion damage to roads and ancillary facilities, and may also damage and pollute the ecological environment of farmland crops and green vegetation on both sides of the road.
[0004] Patent CN109135674A discloses a hydrophobic multifunctional snow-melting agent, including the following components: a hydrophobic salt composite snow-melting agent, a hydrophobic composite slow-freezing agent, and a hydrophobic composite ice layer softener; the ice-suppressing coating formed by brushing on the road surface can significantly reduce the freezing point, slow freezing, and soften the ice layer. Patent CN109233600B discloses a long-lasting hydrophobic ice-suppressing coating, including paraffin powder, polyurethane, a long-lasting hydrophobic ice-suppressing agent and a polyurethane curing agent, a water-based epoxy resin, and a water-based epoxy resin curing agent; the long-lasting hydrophobic ice-suppressing coating is obtained, which can effectively inhibit the formation of ice layers on the road surface even in extremely bad weather. The coating can be directly adhered to the asphalt pavement and rolled on the asphalt pavement to effectively reduce the freezing disaster of the road surface. The above snow-melting and ice-suppressing materials are all used as coatings, and there are relatively few products that are directly added to asphalt mixtures.
[0005] Therefore, there is an urgent need to prepare a self-melting snow and ice-suppressing material that can be directly added to asphalt mixtures, has excellent moisture and heat resistance, and can reduce the amount of traditional snow-melting agents used. Summary of the invention
[0006] In order to overcome the deficiencies of the above-mentioned prior art, the present invention provides a hydrophobic slow-release self-snow-melting and ice-inhibiting material, which has a slow-release function and excellent moisture and heat resistance, avoids the rapid loss of effective salt in the hot and rainy summer season, can reduce the amount of traditional snow-melting agents used, and reduce environmental pollution.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] The first aspect of the present invention provides a hydrophobic slow-release self-snow-melting and ice-inhibiting material, which comprises the following raw materials in parts by weight: 50-80 parts of chloride, 95-105 parts of water, 18-22 parts of ethanol, 25-35 parts of modified diatomaceous earth, 10-15 parts of surface modification material, and 2-4 parts of coupling agent.
[0009] In some embodiments, the method for preparing the modified diatomaceous earth comprises the following steps:
[0010] (1) adding tetrapropylammonium hydroxide into water to dissolve it, then adding ethyl orthosilicate under stirring at 300-400 r / min, and continuing stirring for 23-25 hours to obtain a precursor solution;
[0011] (2) adding diatomaceous earth to a tetrapropylammonium hydroxide aqueous solution and stirring for 2-3 hours, then filtering and drying to obtain a solid, adding the precursor solution obtained in step (1) to the dried solid, reacting at 110-120° C. for 47-49 hours, filtering, washing, and drying to obtain a crude product;
[0012] (3) calcining the crude product obtained in step (2) at 380-420° C. for 3-5 h, then adding sulfuric acid solution for immersion treatment at 75-85° C. for 1.5-2.5 h, filtering with suction, and then continuing to immerse with sodium hydroxide solution at 65-75° C. for 5-9 min, then filtering with suction, washing and drying to obtain zeolite-modified diatomaceous earth;
[0013] (4) Add the zeolite-modified diatomaceous earth and sodium methyl silicate obtained in step (3) into a reaction vessel and stir at 50-60° C. for 1-2 h to obtain modified diatomaceous earth.
[0014] Preferably, the concentration of the tetrapropylammonium hydroxide aqueous solution in step (2) is 0.1-0.3 wt %, the concentration of the sulfuric acid solution in step (3) is 13-17 wt %, and the concentration of the 5 wt % sodium hydroxide solution is 4-6 wt %.
[0015] The present invention does not impose any special restrictions on the source of the diatomaceous earth, which can be purchased commercially.
[0016] Preferably, the particle size of the diatomaceous earth is 300-350 mesh.
[0017] Diatomaceous earth can be used as a carrier for adsorbing chloride due to its rich pore structure and large specific surface area. However, in fact, many pore structures of diatomaceous earth are filled with impurities, resulting in its weak ability to adsorb effective components of chloride, which further limits its long-term use in snow melting and deicing in winter. The present invention modifies diatomaceous earth by zeolite to increase the adsorption amount of chloride, which can be released for a long time in winter. On the one hand, the possible reason is that after the diatomaceous earth is modified by zeolite, it is subjected to high-temperature calcination, acid washing and alkali washing under specific conditions, which can reduce the pores of zeolite entering the diatomaceous earth during the loading process and reduce the accommodation volume, thereby ensuring that the zeolite-modified diatomaceous earth still has a large specific surface area and adsorption capacity. On the other hand, it may be due to the modification The modified diatomaceous earth forms a multi-level pore structure and increases the capillary action. In snowy weather, water penetrates into the coating structure through capillary action and is absorbed by the adsorbed sodium chloride, which can be quickly transferred from the inside of the structure to the road surface, which is conducive to the timely release of snow-melting components. In addition, the addition of sodium methyl silicate not only makes the modified diatomaceous earth more compatible with the surface modification material and easier to coat, but also the modified diatomaceous earth acts as a filler of the surface modification material, increases the crystallinity of the surface modification material, increases the low-temperature brittleness, and is more prone to rupture in winter. In the hot and rainy weather in summer, due to the micro-expansion of sodium methyl silicate, the density of the material is increased, the release of chloride is reduced, and the sustained-release effect is further improved.
[0018] In some embodiments, the mass ratio of tetrapropylammonium hydroxide, tetraethyl orthosilicate and water in step (1) is 1:(2.8-3):(4.5-5).
[0019] In some embodiments, the mass ratio of diatomaceous earth to precursor solution in step (2) is 1:(180-190).
[0020] The present invention controls the concentration of the precursor solution by limiting the mass ratio of tetrapropylammonium hydroxide, ethyl orthosilicate and water, and simultaneously controls the mass ratio of diatomaceous earth and the precursor solution, so that the zeolite-modified diatomaceous earth has a larger specific surface area and pore volume. The possible reason is that under a specific mass ratio, the zeolite can be uniformly attached to the surface of the diatomaceous earth and will not block the pores of the diatomaceous earth.
[0021] In some embodiments, the mass ratio of zeolite-modified diatomaceous earth to sodium methyl silicate in step (4) is (43-46):1.
[0022] The present invention controls the mass ratio of zeolite-modified diatomaceous earth and sodium methyl silicate, and can form a certain hydrophobic layer on the surface of the zeolite-modified diatomaceous earth in rainy summer to prevent the loss of effective components, and will not affect the precipitation of salt water in winter.
[0023] In some embodiments, the preparation method of the surface modified material comprises the following steps: adding 4-fluorostyrene, 2,4-hexadien-1-ol, allyl acetate and an initiator into ethanol, stirring and reacting at 60-70° C., controlling the number average molecular weight to 2600-2800, and obtaining a surface modified material.
[0024] In some embodiments, the mass ratio of 4-fluorostyrene, 2,4-hexadien-1-ol, and allyl acetate is 1:(2.7-3.2):(3-3.5).
[0025] The traditional way to remove snow and ice from roads is generally to spread snow-melting agents on the road surface or to roll an ice-suppressing coating on the road surface. This method requires a large amount of materials and has a low utilization rate. People in this field add certain deicing materials to the road surface materials, and through vehicle load and capillary action, the effective ingredients are gradually precipitated from the inside of the road surface to achieve the purpose of removing ice and snow. However, in hot and humid seasons, the effective ingredients added to the road surface are prone to rapid loss, affecting the winter snow-melting and ice-suppressing effect. The applicant forms a special water-resistant structure on the surface of the snow-melting and ice-suppressing material to reduce the release of chloride effective ingredients under rainy conditions in summer. The present invention prepares a surface modified material by making 4-fluorostyrene, 2,4-hexadiene-1-ol, and allyl acetate The ester is polymerized to form a polymer of limited molecular weight, and then a stable coating structure is formed on the surface of the modified diatomite that adsorbs chloride, which can effectively reduce the loss of the effective ingredient of chloride in hot and rainy summer. It may be due to the hydrogen bonding between the fluoride ion and the ester group and the modified diatomite that the polymer is evenly attached to the surface of the modified diatomite that adsorbs chloride to form a uniform coating layer. At the same time, the mass ratio of 4-fluorostyrene, 2,4-hexadiene-1-ol, and allyl acetate is controlled so that the coating layer is not only resistant to moisture and heat, but also can maintain a certain low-temperature brittleness. In the low-temperature environment of winter, the rolling of the moving vehicles causes the coating layer to partially rupture and produce cracks, which promotes the rapid release of the effective ingredient chloride, and achieves the effect of melting snow and inhibiting ice in winter.
[0026] In some embodiments, the coupling agent is γ-methacryloxypropyltrimethoxysilane.
[0027] The present application can improve the compatibility between the surface modified material and the modified diatomite by adding a specific coupling agent, and can react with the surface modified material and the modified diatomite to form a uniform water-resistant structural layer on the surface of the modified diatomite that adsorbs chloride.
[0028] The second aspect of the present invention provides a method for preparing a hydrophobic slow-release self-melting snow and ice-inhibiting material, comprising the following steps:
[0029] S1, dissolving chloride in water to obtain a chloride solution, adding the chloride solution dropwise to the modified diatomaceous earth while grinding, the addition is completed over 20-30 minutes, and then continuing to grind for 4-6 minutes, and drying to obtain a mixture;
[0030] S2. Mix the solvent, coupling agent and surface modification material and heat to 50-60° C., cool to room temperature, add the mixture obtained in step S1, stir at 190-210 r / min for 40-50 min, and then dry to obtain a hydrophobic slow-release self-snow-melting and ice-inhibiting material.
[0031] In some embodiments, the particle size distribution of the hydrophobic slow-release self-snow-melting and ice-suppressing material is as follows: in terms of weight percentage, particles with a size less than 0.6 mm account for 100%, particles with a size less than 0.15 mm account for 95%-98%, and particles with a size less than 0.075 mm account for 80%-98%.
[0032] The third aspect of the present invention provides an application of a hydrophobic slow-release self-melting snow and ice-inhibiting material, wherein the hydrophobic slow-release self-melting snow and ice-inhibiting material accounts for 5-7wt% in the asphalt mixture.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1. The present invention prepares a hydrophobic slow-release self-snow-melting and ice-inhibiting material by using surface modification materials and modified diatomaceous earth. The material has a slow-release function and excellent resistance to moisture and heat, which avoids the rapid loss of effective salt in the hot and rainy summer season, can reduce the amount of traditional snow-melting agents used, and reduce environmental pollution.
[0035] 2. The present invention enhances the specific surface area and adsorption capacity of the modified diatomaceous earth by modifying the diatomaceous earth, thereby increasing the adsorption amount of chloride. In snowy weather, water penetrates into the coating structure through capillary action and is absorbed by the adsorbed sodium chloride, and can be quickly transferred from the inside of the structure to the road surface, which is conducive to the timely release of snow-melting components.
[0036] 3. The present invention prepares a surface modified material by using 4-fluorostyrene, 2,4-hexadiene-1-ol and allyl acetate, which can form a stable coating structure on the surface of modified diatomaceous earth, effectively reduce the loss of effective components of chloride in hot and rainy summer, and can also maintain a certain low-temperature brittleness. In the low-temperature environment of winter, the rolling of moving vehicles causes local rupture and cracks in the coating layer, which promotes the rapid release of the effective component chloride, and achieves the effect of melting snow and suppressing ice in winter. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is the result of spraying water on the surface of specimen 5 and freezing it in a -5℃ low-temperature constant temperature box for 8 hours;
[0038] Figure 2 This is the result of spraying water on the surface of specimen 6 and freezing it in a -5℃ low-temperature incubator for 8 hours. DETAILED DESCRIPTION
[0039] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following examples and comparative examples are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0040] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments and comparative examples are described as follows: the compounds and related reagents used in the present invention can be purchased from the market, among which diatomaceous earth was purchased from Xuyi Taihe High-tech Technology Co., Ltd. with a particle size of 325 mesh.
[0041] Preparation Example 1
[0042] The preparation method of modified diatomite-1 comprises the following steps:
[0043] (1) 50 g of tetrapropylammonium hydroxide was added to 240 g of water to dissolve, and then 145 g of ethyl orthosilicate was added under stirring at 350 r / min, and stirring was continued for 24 h to obtain a precursor solution;
[0044] (2) Add 1 g of diatomaceous earth to 50 ml of 0.2 wt% tetrapropylammonium hydroxide aqueous solution and stir for 3 h, then filter and dry to obtain a solid, add 185 g of the precursor solution obtained in step (1) to the dried solid, react at 115° C. for 48 h, filter, wash and dry to obtain a crude product;
[0045] (3) 5 g of the crude product was calcined at 400° C. for 4 h, then 50 g of a 15 wt % sulfuric acid solution was added at 80° C. for immersion treatment for 2 h, and then 50 g of a 5 wt % sodium hydroxide solution was added at 70° C. for 8 min after suction filtration, and then zeolite-modified diatomite was obtained after suction filtration, washing and drying;
[0046] (4) 4.5 g of zeolite-modified diatomaceous earth obtained in step (3) and 0.1 g of sodium methyl silicate were added to a reaction vessel and stirred at 55° C. for 1.5 h to obtain modified diatomaceous earth-1.
[0047] Preparation Example 2
[0048] The preparation method of modified diatomite-2 comprises the following steps:
[0049] (1) 50 g of tetrapropylammonium hydroxide was added to 240 g of water to dissolve, and then 180 g of tetraethyl orthosilicate was added under stirring at 350 r / min, and stirring was continued for 24 h to obtain a precursor solution;
[0050] (2) Add 1 g of diatomaceous earth to 50 ml of 0.2 wt% tetrapropylammonium hydroxide aqueous solution and stir for 3 h, then filter and dry to obtain a solid, add 185 g of the precursor solution obtained in step (1) to the dried solid, react at 115° C. for 48 h, filter, wash and dry to obtain a crude product;
[0051] (3) 5 g of the crude product was calcined at 400° C. for 4 h, then 50 g of a 15 wt % sulfuric acid solution was added at 80° C. for immersion treatment for 2 h, and then 50 g of a 5 wt % sodium hydroxide solution was added at 70° C. for 8 min after suction filtration, and then zeolite-modified diatomite was obtained after suction filtration, washing and drying;
[0052] (4) 4.5 g of zeolite-modified diatomaceous earth obtained in step (3) and 0.1 g of sodium methyl silicate were added to a reaction vessel and stirred at 55° C. for 1.5 h to obtain modified diatomaceous earth-2.
[0053] Preparation Example 3
[0054] The preparation method of modified diatomite-3 comprises the following steps:
[0055] (1) 50 g of tetrapropylammonium hydroxide was added to 240 g of water to dissolve, and then 180 g of tetraethyl orthosilicate was added under stirring at 350 r / min, and stirring was continued for 24 h to obtain a precursor solution;
[0056] (2) Add 1 g of diatomaceous earth to 50 ml of 0.2 wt% tetrapropylammonium hydroxide aqueous solution and stir for 3 h, then filter and dry to obtain a solid, add 200 g of the precursor solution obtained in step (1) to the dried solid, react at 115° C. for 48 h, filter, wash and dry to obtain a crude product;
[0057] (3) 5 g of the crude product was calcined at 400° C. for 4 h, then 50 g of a 15 wt % sulfuric acid solution was added at 80° C. for immersion treatment for 2 h, and then 50 g of a 5 wt % sodium hydroxide solution was added at 70° C. for 8 min after suction filtration, and then zeolite-modified diatomite was obtained after suction filtration, washing and drying;
[0058] (4) 4.5 g of zeolite-modified diatomaceous earth obtained in step (3) and 0.1 g of sodium methyl silicate were added to a reaction vessel and stirred at 55° C. for 1.5 h to obtain modified diatomaceous earth-3.
[0059] Preparation Example 4
[0060] The preparation method of modified diatomite-4 comprises the following steps:
[0061] (1) 50 g of tetrapropylammonium hydroxide was added to 240 g of water to dissolve, and then 145 g of ethyl orthosilicate was added under stirring at 350 r / min, and stirring was continued for 24 h to obtain a precursor solution;
[0062] (2) Add 1 g of diatomaceous earth to 50 ml of 0.2 wt% tetrapropylammonium hydroxide aqueous solution and stir for 3 h, then filter and dry to obtain a solid, add 185 g of the precursor solution obtained in step (1) to the dried solid, react at 115° C. for 48 h, filter, wash and dry to obtain a crude product;
[0063] (3) 5 g of the crude product was calcined at 400° C. for 4 h, then 50 g of a 15 wt % sulfuric acid solution was added at 80° C. for immersion treatment for 2 h, and then 50 g of a 5 wt % sodium hydroxide solution was added at 70° C. for 8 min after suction filtration, and then zeolite-modified diatomite was obtained after suction filtration, washing and drying;
[0064] (4) 4 g of zeolite-modified diatomaceous earth obtained in step (3) and 0.1 g of sodium methyl silicate were added to a reaction vessel and stirred at 55° C. for 1.5 h to obtain modified diatomaceous earth-4.
[0065] Preparation Example 5
[0066] The preparation method of surface modified material-1 comprises the following steps: adding 1 g of 4-fluorostyrene, 3 g of 2,4-hexadiene-1-ol, 3.3 g of allyl acetate and 0.35 g of azobisisobutyronitrile to 30 g of anhydrous ethanol, stirring and reacting at 65° C. to obtain surface modified material-1 with a number average molecular weight of 2768.
[0067] Preparation Example 6
[0068] The preparation method of surface modified material-2 comprises the following steps: adding 1 g of 4-fluorostyrene, 6 g of 2,4-hexadiene-1-ol, 3.3 g of allyl acetate and 0.35 g of azobisisobutyronitrile to 30 g of anhydrous ethanol, stirring and reacting at 65° C. to obtain surface modified material-2 with a number average molecular weight of 2749.
[0069] Preparation Example 7
[0070] The preparation method of surface modified material-3 comprises the following steps: adding 1 g of 4-fluorostyrene, 3 g of 2,4-hexadiene-1-ol, 3.3 g of allyl acetate and 0.35 g of azobisisobutyronitrile to 30 g of anhydrous ethanol, stirring and reacting at 65° C. to obtain surface modified material-3 with a number average molecular weight of 3084.
[0071] Example 1
[0072] A hydrophobic slow-release self-snow-melting and ice-inhibiting material comprises the following raw materials, measured by weight: 65 parts of sodium chloride, 100 parts of water, 20 parts of anhydrous ethanol, 130 parts of modified diatomaceous earth, 113 parts of surface modification materials, and 3 parts of gamma-methacryloxypropyltrimethoxysilane.
[0073] The method for preparing the hydrophobic slow-release self-melting snow and ice-inhibiting material of this embodiment comprises the following steps:
[0074] S1, dissolving sodium chloride in water to obtain a sodium chloride solution, grinding the modified diatomite-1 while dropping the sodium chloride solution, the dropping is completed within 25 minutes, and then continuing to grind for 5 minutes, and drying to obtain a mixture;
[0075] S2. Mix anhydrous ethanol, γ-methacryloxypropyltrimethoxysilane and surface modification material-1 and heat to 55° C., then add the mixture obtained in step S1 and stir at 200 r / min for 45 min, and dry to obtain a hydrophobic slow-release self-snow-melting and ice-inhibiting material.
[0076] Example 2
[0077] A hydrophobic slow-release self-snow-melting and ice-inhibiting material comprises the following raw materials, measured by weight: 50 parts of sodium chloride, 95 parts of water, 18 parts of anhydrous ethanol, 125 parts of modified diatomaceous earth, 110 parts of surface modification materials, and 2 parts of gamma-methacryloxypropyltrimethoxysilane.
[0078] The method for preparing the hydrophobic slow-release self-melting snow and ice-inhibiting material of this embodiment comprises the following steps:
[0079] S1, dissolving sodium chloride in water to obtain a sodium chloride solution, grinding the modified diatomite-1 while dropping the sodium chloride solution, the dropping is completed within 20 minutes, and then continuing to grind for 4 minutes, and drying to obtain a mixture;
[0080] S2. Mix anhydrous ethanol, γ-methacryloxypropyltrimethoxysilane and surface modification material-1 and heat to 50° C., then add the mixture obtained in step S1 and stir at 190 r / min for 50 min, dry and grind to obtain a hydrophobic slow-release self-snow-melting and ice-inhibiting material.
[0081] Example 3
[0082] A hydrophobic slow-release self-snow-melting and ice-inhibiting material comprises the following raw materials, measured by weight: 80 parts of sodium chloride, 105 parts of water, 22 parts of anhydrous ethanol, 135 parts of modified diatomaceous earth, 115 parts of surface modification materials, and 4 parts of gamma-methacryloxypropyltrimethoxysilane.
[0083] The method for preparing the hydrophobic slow-release self-melting snow and ice-inhibiting material of this embodiment comprises the following steps:
[0084] S1, dissolving sodium chloride in water to obtain a sodium chloride solution, grinding the modified diatomite-1 while adding the sodium chloride solution dropwise, the addition is completed within 30 minutes, and then continuing to grind for 6 minutes, and drying to obtain a mixture;
[0085] S2. Mix anhydrous ethanol, γ-methacryloxypropyltrimethoxysilane and surface modification material-1 and heat to 60°C, then add the mixture obtained in step S1 and stir at 210 r / min for 40 min, and dry to obtain a hydrophobic slow-release self-snow-melting and ice-inhibiting material.
[0086] Example 4
[0087] A hydrophobic slow-release self-snow-melting and ice-inhibiting material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified diatomaceous earth-1 is replaced by modified diatomaceous earth-2.
[0088] Example 5
[0089] A hydrophobic slow-release self-snow-melting and ice-inhibiting material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified diatomaceous earth-1 is replaced by modified diatomaceous earth-3 in equal amounts.
[0090] Example 6
[0091] A hydrophobic slow-release self-snow-melting and ice-inhibiting material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified diatomaceous earth-1 is replaced by modified diatomaceous earth-4 in equal amounts.
[0092] Example 7
[0093] A hydrophobic slow-release self-snow-melting and ice-inhibiting material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the surface modified material-1 is replaced by the surface modified material-2 in equal amounts.
[0094] Example 8
[0095] A hydrophobic slow-release self-snow-melting and ice-inhibiting material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the surface modified material-1 is replaced by the surface modified material-3 in equal amounts.
[0096] Comparative Example 1
[0097] A hydrophobic slow-release self-snow-melting and ice-inhibiting material and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 1, except that an equal amount of modified diatomaceous earth-1 is replaced by diatomaceous earth.
[0098] Performance Testing
[0099] 1. Sustained release time
[0100] The time for the conductivity to reach equilibrium is taken as the sustained release time of the material. 1 g of the self-melting snow and ice suppression material prepared in each embodiment and comparative example is added to 150 ml of distilled water and stirred to form a solution. The conductive electrode and temperature electrode of the conductivity meter are inserted into the solution to test the conductivity and sustained release time. The test results are shown in Table 1.
[0101] Table 1
[0102]
[0103]
[0104] From the data comparison of Examples 1-3 in Table 1, it can be seen that the proportion of each material changes, and the material still has a good sustained release effect. The use of modified diatomite-2 in Example 4 may cause the zeolite to be not evenly distributed on the surface of the diatomite, and the accumulation and blocking of the pores, resulting in a decrease in the amount of chloride adsorption and a shortened sustained release time; the use of modified diatomite-3 in Example 5 may cause the zeolite to have an excessive load, a reduced pore size, a reduced amount of chloride adsorption, and an increased sustained release time; the use of modified diatomite-4 in Example 6, the change in the ratio of zeolite-modified diatomite to sodium methyl silicate, resulting in a slower release of chloride and a slower rate of snow melting and de-icing; the use of surface modified material-2 in Example 7, the moisture resistance decreases, the chloride is released faster, and the sustained release time is shortened; the use of surface modified material-3 in Example 8, the increase in the number average molecular weight, may result in a denser coating and a slower sustained release; in Comparative Example 1, the modified diatomite-1 is replaced by diatomite in equal amounts, the amount of chloride adsorption is reduced, and the sustained release time is increased.
[0105] 2. Ice melting rate
[0106] (1) Ice melting rate at -5℃
[0107] The self-melting snow and ice suppression material prepared in Example 1 was added to the asphalt mixture in an amount of 6 wt %, and stirred evenly to prepare a Marshall specimen, which was recorded as specimen 1;
[0108] The asphalt mixture without the addition of self-melting snow and ice suppression material was made into a Marshall specimen, which was recorded as specimen 2;
[0109] Place 40g of water at -18℃ and freeze it into ice cubes for later use. Place Marshall specimens 1 and 2 at -5℃ and keep them at a constant temperature for 4 hours. Take out the ice cubes and weigh them quickly. Place them at -5℃ and keep them at a constant temperature for 2h, 24h, 48h and 72h. Take out the ice cubes and weigh them immediately. Calculate the ice melting rate of the material at -5℃. Ice melting rate = weight difference before and after ice cubes / initial weight of ice cubes. The test results are shown in Table 2.
[0110] Table 2
[0111]
[0112] (2) Ice melting rate at -10℃
[0113] The self-melting snow and ice suppression material prepared in Example 1 was added to the asphalt mixture in an amount of 6 wt %, and stirred evenly to prepare a Marshall specimen, which was recorded as specimen 3;
[0114] The asphalt mixture without the addition of self-melting snow and ice suppression material was made into a Marshall specimen, which was recorded as specimen 4;
[0115] 40g of water was placed at -18℃ and frozen into ice cubes for later use. Marshall specimens 3 and 4 were placed at -10℃ and kept at a constant temperature for 4 hours. The ice cubes were taken out and weighed quickly. They were also placed at -10℃ and kept at a constant temperature for 2h, 24h, 48h and 72h. The ice cubes were taken out and weighed immediately. The melting rate of the material at -10℃ was calculated. The melting rate = the difference in weight before and after the ice cube / the initial weight of the ice cube. The test results are shown in Table 3.
[0116] Table 3
[0117]
[0118] It can be seen from Tables 2 and 3 that the ice melting rate of the Marshall specimens with the material added is greater than that of the Marshall specimens without the material added, indicating that the material has a good ice and snow melting effect.
[0119] 3. Road deicing effect
[0120] The self-melting snow and ice suppression material prepared in Example 1 of the present invention was added to the asphalt mixture in an amount of 6 wt %, and stirred evenly to prepare a rutting specimen, which was recorded as specimen 5;
[0121] The asphalt mixture without the addition of self-melting snow and ice suppression material was made into a rutting specimen, which was recorded as specimen 6;
[0122] Sprinkle an equal amount of water on the surface of rutting specimens 5 and 6, and then freeze the specimens in a -5℃ low temperature constant temperature box for 8 hours. The results are as follows: Figure 1 , Figure 2 As shown, it is shown that there is no ice on the surface of the rutting specimen with the material added, while there is an obvious ice layer on the surface of the rutting specimen without the material added.
[0123] The temperature of the low-temperature constant temperature box was adjusted to -10℃, -8℃, -2℃, and 0℃ in sequence to test whether the rutting specimens 5 and 6 with water sprinkled on the surface would freeze under the corresponding temperature environment. The test steps were the same as above. The test results showed that the surfaces of the rutting specimens with the material added were not frozen, while the surfaces of the rutting specimens without the material added had obvious ice layers.
[0124] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A hydrophobic slow-release self-melting snow and ice-inhibiting material, characterized in that: The invention comprises the following raw materials by weight: 50-80 parts of chloride, 95-105 parts of water, 18-22 parts of ethanol, 25-35 parts of modified diatomaceous earth, 10-15 parts of surface modification material and 2-4 parts of coupling agent.
2. The hydrophobic slow-release self-melting ice-inhibiting material according to claim 1, characterized in that: The preparation method of the modified diatomite comprises the following steps: (1) adding tetrapropylammonium hydroxide into water to dissolve it, then adding ethyl orthosilicate under stirring at 300-400 r / min, and continuing stirring for 23-25 hours to obtain a precursor solution; (2) adding diatomaceous earth to a tetrapropylammonium hydroxide aqueous solution and stirring for 2-3 hours, then filtering and drying to obtain a solid, adding the precursor solution obtained in step (1) to the dried solid, reacting at 110-120° C. for 47-49 hours, filtering, washing, and drying to obtain a crude product; (3) calcining the crude product obtained in step (2) at 380-420° C. for 3-5 h, then adding sulfuric acid solution for immersion treatment at 75-85° C. for 1.5-2.5 h, filtering with suction, and then continuing to immerse with sodium hydroxide solution at 65-75° C. for 5-9 min, then filtering with suction, washing and drying to obtain zeolite-modified diatomaceous earth; (4) Add the zeolite-modified diatomaceous earth and sodium methyl silicate obtained in step (3) into a reaction vessel and stir at 50-60° C. for 1-2 h to obtain modified diatomaceous earth.
3. The hydrophobic slow-release self-melting snow and ice-inhibiting material according to claim 2, characterized in that: In the step (1), the mass ratio of tetrapropylammonium hydroxide, ethyl orthosilicate and water is 1:(2.8-3):(4.5-5).
4. The hydrophobic slow-release self-melting snow and ice-inhibiting material according to claim 3, characterized in that: In the step (2), the mass ratio of diatomaceous earth to precursor solution is 1:(180-190).
5. The hydrophobic slow-release self-melting ice-inhibiting material according to claim 2, characterized in that: In the step (4), the mass ratio of zeolite-modified diatomaceous earth to sodium methyl silicate is (43-46):
1.
6. The hydrophobic slow-release self-melting snow and ice-inhibiting material according to claim 1, characterized in that: The preparation method of the surface modified material comprises the following steps: adding 4-fluorostyrene, 2,4-hexadiene-1-ol, allyl acetate and an initiator into ethanol, stirring and reacting at 60-70° C., and controlling the number average molecular weight to be 2600-2800 to obtain the surface modified material.
7. The hydrophobic slow-release self-melting snow and ice-inhibiting material according to claim 6, characterized in that: The mass ratio of 4-fluorostyrene, 2,4-hexadiene-1-ol and allyl acetate is 1:(2.7-3.2):(3-3.5).
8. The hydrophobic slow-release self-melting snow and ice-inhibiting material according to claim 1, characterized in that: The coupling agent is γ-methacryloxypropyltrimethoxysilane.
9. A method for preparing the hydrophobic slow-release self-melting snow and ice-inhibiting material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, dissolving chloride in water to obtain a chloride solution, adding the chloride solution dropwise to the modified diatomaceous earth while grinding, the addition is completed over 20-30 minutes, and then continuing to grind for 4-6 minutes, and drying to obtain a mixture; S2. Mix ethanol, coupling agent and surface modification material and heat to 50-60° C., cool to room temperature, add the mixture obtained in step S1, stir at 190-210 r / min for 40-50 min, dry and grind to obtain a hydrophobic slow-release self-snow-melting and ice-inhibiting material.
10. An application of the hydrophobic slow-release self-melting snow and ice-inhibiting material according to any one of claims 1 to 8 or the hydrophobic slow-release self-melting snow and ice-inhibiting material prepared by the preparation method according to claim 9, characterized in that: The hydrophobic slow-release self-melting snow and ice-inhibiting material accounts for 5-7wt% in the asphalt mixture.
Citation Information
Cited By
Slow-release snow-melting ice-melting coffee residue porous carbon material as well as preparation method and application thereof