All-vanadium titano-magnetite intensified roasting pellet and preparation method thereof

By adding blast furnace gravity dust concentrate and binder to vanadium-titanium magnetite pellets, and using a disc pelletizer for pelletizing and roasting, the problem of insufficient oxidation preheating time was solved, achieving high-efficiency production and reduced energy consumption, and improving the compressive strength and production efficiency of the pellets.

CN118957257APending Publication Date: 2024-11-15PANGANG GRP XICHANG STEEL & VANADIUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411041641.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In existing technologies, when the oxidation preheating time of vanadium-titanium magnetite pellets is less than 20 minutes, the ferrous oxide content increases, the compressive strength decreases, and a "sugar core sandwich" phenomenon occurs, making it difficult to achieve enhanced roasting, resulting in low production efficiency, high energy consumption, and increased costs.

Method used

The process involves mixing blast furnace gravity dust powder with vanadium-titanium magnetite, adding appropriate amounts of binder and pelletizing zone dust, forming pellets using a disc pelletizer, and roasting them in a belt roaster while controlling the roasting temperature and time to form fully vanadium-titanium magnetite enhanced roasted pellets.

Benefits of technology

It increases the oxidation rate of vanadium-titanium magnetite pellets, enhances compressive strength, reduces production energy consumption and costs, and improves the production efficiency of the pellet production line while reducing the amount of recycled materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957257A_ABST
    Figure CN118957257A_ABST
Patent Text Reader

Abstract

The invention discloses an all-vanadium titano-magnetite intensified roasting pellet and a preparation method thereof, and belongs to the technical field of iron ore pellet preparation. The method comprises the following steps: processing blast furnace gravitational fly ash into blast furnace gravitational fly ash fine powder, proportioning the blast furnace gravitational fly ash fine powder with vanadium titano-magnetite in proportion to obtain mixed iron powder, drying, rolling, proportioning 95-99% of the mixed iron ore powder, 1-3% of a binder and 0-2% of fly ash in a pelletizing area, uniformly mixing, pelletizing by a disc pelletizer, and sintering to obtain the vanadium titano-magnetite pellet. And the green pellets are distributed into a belt type roasting machine, and the all-vanadium titano-magnetite strengthened roasting pellets are obtained after roasting. According to the method, the oxidation speed of the vanadium-titanium magnetite pellets can be greatly increased, the oxidation preheating time can be greatly shortened, on the premise that it is guaranteed that the strength of the vanadium-titanium pellets is larger than or equal to 2000 N, vanadium-titanium magnetite intensified roasting of the pellets can be achieved, the production efficiency of a pellet production line is remarkably improved, energy consumption and the processing cost of the vanadium-titanium pellet production procedure are reduced, and meanwhile the method is suitable for industrial production. And the circulating material amount in the sintering production process can be reduced, and the sintering process processing cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron ore pellet preparation, and in particular relates to an all-vanadium titanium magnetite enhanced roasting pellet and a preparation method thereof. Background Art

[0002] The main iron-containing minerals of vanadium-titanium magnetite in Panxi area are titanomagnetite, followed by granular ilmenite. Titanomagnetite is a complex composed of magnetite, ilmenite spar and magnesia-aluminum spinel. The ilmenite content in titanium concentrate is 92.12%, of which 99% of titanium exists in the form of ilmenite, and 96.01% of ilmenite exists as a monomer. At 400-500℃, the mineral components of vanadium-titanium magnetite begin to produce a series of solid-phase reactions: ilmenite and magnesia-aluminum spinel disappear, and the magnetite-ilmenite spar-magnesia-aluminum spinel solid solution separation structure gradually disappears, forming uniform titanium hematite and titanomagnetite, and the higher the temperature, the faster the formation speed.

[0003] Vanadium-titanium magnetite concentrate usually adopts two agglomeration processes: sintering and pelletizing. By comparing the six core technical parameters of the two agglomeration processes: finished ore strength, finished product rate, process energy consumption, processing fee, pollutant generation per ton of ore and metallurgical properties of finished ore, the pelletizing process is significantly better than the sintering process. Therefore, the use of pelletizing technology for magnetite has become the development direction of agglomeration technology. Pelletized ore has the characteristics of high grade, low slag ratio and uniform particle size. Therefore, blast furnace smelting with a large proportion of pellets can play a role in energy saving and consumption reduction, and is the blast furnace smelting energy-saving and emission reduction charge structure advocated by the country.

[0004] In the production practice of all-vanadium-titanium pellets produced with the "single vanadium-titanium magnetite + bentonite + pellet area dust removal ash" structure, when the oxidation preheating + roasting time of the production line is ≤20min, the ferrous oxide content of the finished pellets will increase by about 1.0%-2.0%, and the compressive strength index will drop significantly (the compressive strength of the finished pellets is only 1500-1700N). There is a shiny "sugar core interlayer" phenomenon in the middle of the finished pellets, which makes it difficult to achieve vanadium-titanium magnetite enhanced roasting pellets, restricts the performance of the pellet production line, and leads to high processing energy consumption and processing costs of all-vanadium-titanium pellets. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a vanadium-titanium magnetite enhanced roasting pellet and a preparation method thereof. The present invention can greatly improve the oxidation rate of the vanadium-titanium magnetite pellet, shorten the oxidation preheating time, and realize the enhanced roasting of the vanadium-titanium magnetite pellet while ensuring that the strength of the vanadium-titanium pellet is ≥2000N, significantly improve the production efficiency of the pellet production line, reduce the energy consumption and processing cost of the vanadium-titanium pellet production process, and at the same time, reduce the amount of circulating materials in the sintering production process and reduce the processing cost of the sintering process.

[0006] The object of the present invention is to achieve the following:

[0007] The present invention provides a method for preparing all-vanadium titanium magnetite enhanced roasted pellets, comprising the following steps:

[0008] (1) processing blast furnace gravity dust removal ash into blast furnace gravity dust removal ash fine powder through a dry grinding process;

[0009] (2) mixing the blast furnace gravity dust removal ash powder obtained in step (1) with vanadium-titanium magnetite to form a mixed iron powder, wherein the mixed iron powder comprises: 95-99% vanadium-titanium magnetite + 5-1% blast furnace gravity dust removal ash powder;

[0010] (3) The mixed iron ore powder is dried and roller-pressed to control the moisture content of the mixed iron ore powder after drying to ≤8.5%;

[0011] (4) Mix the ingredients according to 95-99% iron ore powder + 1-3% binder + 0-2% dust removal ash from the pelletizing area and mix them evenly;

[0012] (5) The disc ball making machine makes balls, the number of raw balls falling is 5-7 times, and the raw balls with a particle size of 9-14 mm account for ≥80%;

[0013] (6) The raw balls are fed into a belt roasting machine, and after roasting, all-vanadium titanium magnetite enhanced roasted pellets are obtained.

[0014] Based on the above technical solution, further, the blast furnace gravity dust removal ash fine powder described in step (1) has a particle size of less than 200 mesh and a moisture content of ≤2%.

[0015] Based on the above technical scheme, further, the composition of the blast furnace gravity dust removal ash in step (1) is: P: 0.3-0.4%, S: 0.01-0.04%, CaO: 8-10%, MgO: 1.5-2%, TFe: 30-40%, SiO2: 6-8%, TiO2: 3-5%, Al2O3: 2-4%, C: 20-25%, and the remainder is unavoidable impurities.

[0016] Based on the above technical scheme, further, the composition of the vanadium-titanium magnetite described in step (2) is: TFe: 53-58%, CaO: 0.4-1.3%, SiO2: 2-5%, MgO: 2-4%, Al2O3: 3-4%, K: 0.01-0.3%, Na: 0.01-0.2%, Ni: 0-0.05%, S: 0.20-0.90%, P: 0-0.1%, V2O5: 0.4-0.8%, TiO2: 9-13%, and the remainder is unavoidable impurities.

[0017] Based on the above technical solution, further, the particle size of the vanadium-titanium magnetite described in step (2) is <200 mesh, and the proportion of the particle size is ≥85%.

[0018] Based on the above technical solution, further, the binder described in step (4) is bentonite.

[0019] Based on the above technical solution, further, the dust ash in the pelletizing area described in step (4) has a particle size of less than 200 mesh, accounting for more than 65%, and the composition of the dust ash in the pelletizing area is: TFe: 54-56%, CaO: 0.5-0.7%, SiO2: 3-4%, MgO: 2.5-3.5%, Al2O3: 3-4%, K: 0.01-0.1%, Na: 0.01-0.1%, S: 0-0.1%, P: 0-0.1%, V2O5: 0.5-0.7%, TiO2: 9-10%, and the remainder is unavoidable impurities.

[0020] Based on the above technical solution, further, the mixing described in step (4) is carried out in a strong mixer for 30 to 300 seconds.

[0021] Based on the above technical solution, further, in step (5) The feeding capacity of a single pelletizing plate is ≥60t / h. The feeding capacity of a single pelletizing disc is ≥90t / h.

[0022] Based on the above technical solution, further, the roasting described in step (5) mainly includes an oxidation preheating section and a roasting section, the oxidation preheating section temperature is 500-1100°C, the time is 8-10min, and the roasting section temperature is 1100-1300°C, the time is 8-10min.

[0023] The invention also provides all-vanadium titanium magnetite enhanced roasted pellets prepared by the preparation method.

[0024] The beneficial effects of the present invention compared with the prior art are as follows:

[0025] 1. The present invention can greatly improve the oxidation rate of vanadium-titanium magnetite pellets, shorten the oxidation preheating time, and realize the intensive roasting of vanadium-titanium magnetite pellets under the premise of ensuring that the strength of vanadium-titanium pellets is ≥2000N, significantly improve the production efficiency of the pellet production line, reduce the energy consumption and processing cost of the vanadium-titanium pellet production process, and at the same time, reduce the amount of circulating materials in the sintering production process and reduce the processing cost of the sintering process. This patented technology can be promoted and used in all pellet processing production lines that use vanadium-titanium magnetite as raw material and use disc pelletizing machines to make pellets.

[0026] 2. The present invention can be promoted and used in all pelletizing production lines that use vanadium-titanium magnetite as raw material and adopt a disc pelletizing machine to make pellets. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.

[0028] Figure 1 This is a schematic diagram of the preparation of the enhanced roasting pellets of all-vanadium titanium magnetite in Example 1-2.

[0029] Figure 2 It is a normality test result diagram of the experimental data of Examples 1-2 and Comparative Example 1.

[0030] Figure 3 Graph showing the variance analysis results of the test data of Examples 1-2 and Comparative Example 1. DETAILED DESCRIPTION

[0031] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.

[0032] Example 1

[0033] This embodiment provides a method for preparing all-vanadium titanium magnetite enhanced roasted pellets, comprising the following steps:

[0034] (1) The blast furnace gravity dust removal ash is finely ground into fine powder with a particle size of <200 mesh accounting for about 80% by dry grinding process; the composition of the blast furnace gravity dust removal ash is shown in Table 1;

[0035] (2) The finely ground blast furnace gravity dust ash concentrate is mixed with vanadium-titanium magnetite in a pre-mixing process to form a mixed iron powder, wherein the mixed iron powder comprises: vanadium-titanium magnetite 99% + finely ground blast furnace gravity dust 1%; the composition of the vanadium-titanium magnetite is: TFe: 53-58%, CaO: 0.4-1.3%, SiO2: 2-5%, MgO: 2-4%, Al2O3: 3-4%, K: 0.01-0.3%, Na: 0.01-0.2%, Ni: 0-0.05%, S: 0.20-0.90%, P: 0-0.1%, V2O5: 0.4-0.8%, TiO2: 9-13%, and the remainder is unavoidable impurities; the particle size of the vanadium-titanium magnetite is <200 mesh, accounting for ≥85% of the particle size;

[0036] (3) The mixed iron ore powder is dried and roller-pressed to control the moisture content of the mixed iron ore powder after drying to ≤8.5%;

[0037] (4) The ingredients are prepared according to the formula of "mixed iron ore powder 97% + binder 2% + pelletizing area dust 1%", and mixed in a powerful mixer for about 60 seconds; the binder is bentonite; the pelletizing area dust <200 mesh size accounts for 72%, and the composition of the pelletizing area dust is shown in Table 2;

[0038] (5) Disc pelletizing machine for pelletizing, The feeding capacity of a single pelletizing plate is ≥60t / h, the number of raw balls falling is 5-7 times, and the proportion of raw balls with a particle size of 9-14mm is ≥80%;

[0039] (6) Place the raw balls into a belt roasting machine and roast them according to the process in Table 3.

[0040] Table 1 Main components of blast furnace gravity dust removal ash (unit: %)

[0041]

[0042] Table 2 Main components of dust removal ash in pelletizing area (unit: %)

[0043] TFe CaO <![CDATA[SiO2]]> MgO <![CDATA[Al2O3]]> K Na Ni S P <![CDATA[V2O5]]> <![CDATA[TiO2]]> Pellet dust removal 55.01 0.64 3.52 2.91 3.36 0.03 0.06 0.00 0.00 0.01 0.61 9.62

[0044] Table 3 Calcination process parameters

[0045]

[0046] Example 2

[0047] This embodiment provides a method for preparing all-vanadium titanium magnetite enhanced roasted pellets, comprising the following steps:

[0048] (1) The blast furnace gravity dust removal ash is finely ground into fine powder with a particle size of <200 mesh accounting for about 80% by dry grinding process; the composition of the blast furnace gravity dust removal ash is shown in Table 1;

[0049] (2) the finely ground blast furnace gravity dust ash concentrate is mixed with vanadium-titanium magnetite in the pre-mixing process to form a mixed iron powder, the mixed iron powder composition is: vanadium-titanium magnetite 95% + finely ground blast furnace gravity dust 5%; the composition of the vanadium-titanium magnetite is: TFe: 53-58%, CaO: 0.4-1.3%, SiO2: 2-5%, MgO: 2-4%, Al2O3: 3-4%, K: 0.01-0.3%, Na: 0.01-0.2%, Ni: 0-0.05%, S: 0.20-0.90%, P: 0-0.1%, V2O5: 0.4-0.8%, TiO2: 9-13%, the remainder is inevitable impurities, the particle size of the vanadium-titanium magnetite is <200 mesh, accounting for ≥85%;

[0050] (3) The mixed iron ore powder is dried and roller-pressed to control the moisture content of the mixed iron ore powder after drying to ≤8.5%;

[0051] (4) The ingredients were prepared according to the formula of "97% mixed iron ore powder + 1% binder + 2% dust removal ash from the pelletizing area", and mixed in a powerful mixer for about 60 seconds; the binder was bentonite; the dust removal ash from the pelletizing area with a particle size of <200 mesh accounted for 72%, and the composition of the dust removal ash from the pelletizing area is shown in Table 2;

[0052] (5) Disc pelletizing machine for pelletizing, The feeding capacity of a single pelletizing plate is ≥90t / h, the number of raw balls falling is 5-7 times, and the proportion of raw balls with a particle size of 9-14mm is ≥80%;

[0053] (6) Place the raw balls into a belt roasting machine and roast them according to the process in Table 3.

[0054] Comparative Example 1

[0055] This comparative example provides a method for preparing all-vanadium titanium magnetite pellets, comprising the following steps:

[0056] (1) The composition of vanadium-titanium magnetite is: TFe: 53-58%, CaO: 0.4-1.3%, SiO2: 2-5%, MgO: 2-4%, Al2O3: 3-4%, K: 0.01-0.3%, Na: 0.01-0.2%, Ni: 0-0.05%, S: 0.20-0.90%, P: 0-0.1%, V2O5: 0.4-0.8%, TiO2: 9-13%, and the balance is inevitable impurities. The particle size of vanadium-titanium magnetite is <200 mesh, and the proportion of the particle size is ≥85%. The vanadium-titanium magnetite powder is dried and roller-pressed, and the moisture content of the powder after drying is controlled to be ≤8.5%;

[0057] (2) The ingredients are prepared according to the formula of "97% mineral powder + 1% binder + 2% dust removal ash from the pelletizing area", and mixed in a powerful mixer for about 60 seconds; the binder is bentonite; the dust removal ash from the pelletizing area with a particle size of less than 200 mesh accounts for 72%, and the composition of the dust removal ash from the pelletizing area is shown in Table 2;

[0058] (3) Disc pelletizing machine for pelletizing, The feeding capacity of a single pelletizing plate is ≥90t / h, the number of raw balls falling is 5-7 times, and the proportion of raw balls with a particle size of 9-14mm is ≥80%;

[0059] (4) Place the raw balls into a belt roasting machine and roast them according to the process in Table 3.

[0060] The compressive strength of the finished pellets prepared in Examples 1-2 and Comparative Example 1 is shown in Table 4.

[0061] Table 4 Compressive strength of finished pellets prepared in Examples 1-2 and Comparative Example 1 (unit: N)

[0062]

[0063] The test data of Examples 1-2 and Comparative Example 1 were subjected to data normality test and variance analysis:

[0064] The normality test results are shown in Figure 2 , it can be seen that the above test data satisfy the normal distribution, and the variance analysis results are shown in Figure 3 The data show that adding 3% and 5% blast furnace gravity dust removal ash has a significant effect on improving the compressive strength of pellets.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing vanadium-titanium magnetite intensive roasted pellets, It is characterized in that The steps include: (1) processing blast furnace gravity dust removal ash into blast furnace gravity dust removal ash fine powder through a dry grinding process; (2) mixing the blast furnace gravity dust removal ash powder obtained in step (1) with vanadium-titanium magnetite to form a mixed iron powder, wherein the mixed iron powder comprises: 95-99% vanadium-titanium magnetite + 5-1% blast furnace gravity dust removal ash powder; (3) The mixed iron ore powder is dried and roller-pressed to control the moisture content of the mixed iron ore powder after drying to ≤8.5%; (4) Mix the ingredients according to 95-99% iron ore powder + 1-3% binder + 0-2% dust removal ash from the pelletizing area and mix them evenly; (5) The disc ball making machine makes balls, the number of raw balls falling is 5-7 times, and the raw balls with a particle size of 9-14 mm account for ≥80%; (6) The raw balls are fed into a belt roasting machine, and after roasting, all-vanadium titanium magnetite enhanced roasted pellets are obtained.

2. The preparation method according to claim 1, It is characterized in that The blast furnace gravity dust removal ash powder in step (1) has a particle size of less than 200 mesh and a moisture content of ≤2%. The composition of the blast furnace gravity dust removal ash is: P: 0.3-0.4%, S: 0.01-0.04%, CaO: 8-10%, MgO: 1.5-2%, TFe: 30-40%, SiO 2 :6~8%、TiO 2 :3~5%、Al 2 O 3 : 2-4%, C: 20-25%, and the remainder are inevitable impurities.

3. The preparation method according to claim 1, It is characterized in that The composition of the vanadium-titanium magnetite in step (2) is: TFe: 53-58%, CaO: 0.4-1.3%, SiO 2 : 2~5%, MgO: 2~4%, Al 2 O 3 : 3~4%, K: 0.01~0.3%, Na: 0.01~0.2%, Ni: 0~0.05%, S: 0.20~0.90%, P: 0~0.1%, V 2 O 5 :0.4~0.8%,TiO 2 : 9-13%, the remainder is inevitable impurities.

4. The preparation method according to claim 3, It is characterized in that The particle size of the vanadium-titanium magnetite described in step (2) is <200 mesh, and the proportion of the particle size is ≥85%.

5. The preparation method according to claim 1, It is characterized in that The binder described in step (4) is bentonite.

6. The preparation method according to claim 1, It is characterized in that The pelletizing area dust ash described in step (4) has a particle size of less than 200 meshes accounting for more than 65%, and the composition of the pelletizing area dust ash is: TFe: 54-56%, CaO: 0.5-0.7%, SiO 2 : 3~4%, MgO: 2.5~3.5%, Al 2 O 3 : 3~4%, K: 0.01~0.1%, Na: 0.01~0.1%, S: 0~0.1%, P: 0~0.1%, V 2 O 5 :0.5~0.7%,TiO 2 : 9-10%, the remainder is inevitable impurities.

7. The preparation method according to claim 1, It is characterized in that The mixing in step (4) is carried out in a powerful mixer for 30 to 300 seconds.

8. The preparation method according to claim 1, It is characterized in that In step (5), the feeding capacity of a φ6m pelletizing disk is ≥60t / h, and the feeding capacity of a φ7.5m pelletizing disk is ≥90t / h.

9. The preparation method according to claim 1, It is characterized in that The roasting described in step (5) mainly includes an oxidation preheating section and a roasting section. The oxidation preheating section has a temperature of 500-1100° C. and a time of 8-10 min. The roasting section has a temperature of 1100-1300° C. and a time of 8-10 min.

10. All-vanadium titanium magnetite enhanced roasted pellets prepared by the preparation method according to any one of claims 1 to 9.