Short-process recycling method for waste lithium ion batteries

By combining high-temperature matte smelting with water immersion, the problems of long recycling processes and poor selective lithium recovery of waste lithium-ion batteries have been solved, achieving efficient separation and low-cost recycling of lithium from cobalt, nickel, and copper.

CN118957267APending Publication Date: 2024-11-15ANHUI UNIVERSITY OF TECHNOLOGY

Patent Information

Application Number
CN202411030834.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing recycling process for waste lithium-ion batteries is lengthy, and traditional pyrometallurgical processes have failed to achieve efficient recycling of valuable metal elements in a short process, especially with poor selective recycling of lithium.

Method used

Undisassembled waste lithium-ion batteries are used. After simple discharge treatment, they are smelted at high temperature with sulfur-containing compounds and slagging agents. By taking advantage of the difference in sulfur affinity between lithium and cobalt, nickel and copper, one-step separation is achieved, forming the separation of sulfide phase and oxide phase. Lithium is then extracted by water leaching.

Benefits of technology

It achieves efficient pre-separation of lithium from cobalt, nickel, and copper, shortens the recycling process, reduces energy consumption, and the resulting sulfide products can be used as high-quality intermediate materials. The lithium leaching rate exceeds 95%, with low impurity content and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957267A_ABST
    Figure CN118957267A_ABST
Patent Text Reader

Abstract

The invention discloses a short-process recycling method for waste lithium ion batteries, and belongs to the technical field of resource recycling. The method comprises the following steps: mixing the lithium-containing waste battery with a sulfur-containing compound and a slag former, carrying out high-temperature matte smelting at 1100-1400 DEG C to obtain an upper-layer lithium-rich slag phase and a lower-layer sulfurized product, carrying out sedimentation, cooling and stripping on the smelted product to obtain the upper-layer lithium-rich slag phase and the lower-layer sulfurized product, and controlling the matte smelting temperature to be 1100-1400 DEG C and the sulfur-containing compound to be sulfate or sulfide. The slag former is a silicon-containing slag former, fluoride or chloride. According to the method disclosed by the invention, the waste lithium ion battery, the sulfur-containing compound and the slag former are subjected to high-temperature matte smelting by utilizing the sulfur affinity difference between lithium and cobalt, nickel and copper, so that efficient pre-separation of lithium from cobalt, nickel and copper in the waste lithium ion battery can be realized through one-step smelting, and the recovery process of the waste lithium battery is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of resource recycling, and more specifically, relates to a short-process recycling method for waste lithium-ion batteries. Background Art

[0002] Lithium-ion batteries are widely used in electric vehicles, communications, electronic equipment and other fields because of their long cycle life, large capacity and light weight. With the sharp increase in the use of lithium-ion batteries, it is expected that waste lithium-ion batteries will reach a peak of scrapping by 2025. Waste lithium-ion batteries contain toxic electrolytes and organic diaphragms, which will cause irreversible damage to soil and water quality. In addition, they contain a large amount of strategic key metals Li (2%-3%), Co (5%-30%), Ni (0.02%-10%), and Cu (7%-17%). If they are not recycled, it will cause a huge waste of resources. Therefore, the development of a green short-process recycling process for valuable elements in waste lithium-ion batteries will not only help solve environmental pollution problems, but also alleviate the shortage of key metal resources such as cobalt, nickel, copper, and lithium.

[0003] The main recycling methods for waste lithium-ion batteries include pyrometallurgy and hydrometallurgy. The general process of the hydrometallurgical process is "discharge → disassembly → sorting → leaching → element separation → material regeneration". This method has a long process, poor adaptability, large consumption of chemical raw materials, large output of waste (waste acid, waste residue), high processing cost, and limited processing capacity. These shortcomings limit the scale of application. The pyrometallurgical recycling process has strong raw material adaptability and large processing scale, and is the most promising short-process processing method.

[0004] The core of pyrometallurgical recycling is to select the appropriate smelting slag system to maximize the alloy recovery rate and reduce the amount of slag. For example, Umicore's patent (US7169206A1), Sumitomo Metal Mining Co., Ltd.'s patent (CN112424383A, CN103370427A, CN103380218A, CN103459624A), China Changsha Research Institute of Mining and Metallurgy Co., Ltd.'s patent (CN103526035A, CN103924088A, CN104611566 A) and the patent of Anhui University of Technology (CN114891996A) both use pyrometallurgical process to recover valuable metals in waste lithium-ion batteries, and both use ternary or quaternary slag system composed of CaO-Al2O3-SiO2, FeO-Al2O3-CaO-SiO2, MnO-Al2O3-SiO2-CaO, Li2O-Al2O3-SiO2 to smelt alloys containing Co, Ni, Cu, Mn and smelting slag containing Li.

[0005] Among them, patent CN114891996A discloses a method for preparing high-grade lithium concentrate using lithium-containing waste batteries or materials, which belongs to the field of resource recycling technology. The method includes the steps of: mixing the pretreated material obtained by immersion and discharge in a salt solution with a Si-containing slag-forming agent and then smelting at high temperature, adjusting the smelting temperature to obtain an alloy and lithium-rich slag, wherein the Si content in the Si-containing slag-forming agent is ≥25%; the mass fraction ratio of Al2O3 to SiO2 in the lithium-rich slag is 0.25-3.0, the Li2O content is 5.5%-15%, and the Mn content is ≤10%.

[0006] Although the pyrometallurgical process achieves a high alloying recovery rate of cobalt, nickel, and copper, the resulting alloy still requires a relatively long subsequent process of wet separation and purification, and the resulting lithium-containing slag has a low lithium grade and is difficult to achieve selective and efficient recovery of lithium. It can be seen that the traditional pyrometallurgical recovery process has not fundamentally achieved the goal of short-process comprehensive valuable metal elements. Therefore, it is urgent to develop a process that is different from the high-temperature reduction smelting alloying recovery of cobalt, nickel, and copper and the priority and efficient extraction of lithium based on source design. Summary of the invention

[0007] 1. Problem to be solved

[0008] In view of the problem that the existing recycling process of waste lithium-ion batteries is long, the present invention provides a short-process recycling method for waste lithium-ion batteries. The method can be used to selectively extract lithium and cobalt, nickel and copper, with a short process flow and a high recovery rate.

[0009] 2. Technical solution

[0010] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0011] The object of the present invention is to provide a short-process recycling method for waste lithium-ion batteries, comprising the following steps:

[0012] S1: Raw material pretreatment:

[0013] The lithium-containing waste batteries are placed in a salt solution for immersion and discharge, and then solid-liquid separation and drying are performed to obtain pre-treated materials and discharged waste salt solution;

[0014] S2: High temperature matte smelting:

[0015] The pretreated material is subjected to high-temperature matte smelting to obtain a sulfide product phase and lithium-rich slag. The pretreated material obtained in step S1 is mixed with a sulfur-containing compound and a slag-forming agent in a certain proportion and then subjected to high-temperature matte smelting. The smelting process is conducted under an inert atmosphere, and the amount of sulfur-containing compound added, the smelting temperature and the smelting time are adjusted. The smelting product is subjected to sedimentation, cooling and stripping to obtain an upper layer of lithium-rich slag and a lower layer of sulfide product.

[0016] Wherein, the sulfur-containing compound is sulfate or sulfide, and the slag-forming agent is silicon-containing slag-forming agent, fluoride or chloride.

[0017] S3: Lithium extraction from lithium-rich slag:

[0018] The lithium-rich slag obtained in step S2 is soaked in water and filtered to obtain a lithium-containing solution with low impurity content and aluminum-silicon-containing leached slag.

[0019] Furthermore, the salt solution used in step S1 can be a mixed solution of one or more of Na2SO4, K2SO4, NaCl, and KCl, and the concentration of the salt solution is 0.2 to 1.0 mol / L.

[0020] Furthermore, the sulfur-containing compound in step S2 is sulfate or sulfide, and the mass ratio of the added amount of the sulfur-containing compound to the pretreated material obtained in S1 is 0.2-2.5.

[0021] When sulfate is selected, the sulfate used is at least one of Na2SO4, K2SO4, CaSO4, and MgSO4, and the mass ratio of the added amount of sulfate to the pretreated material obtained from S1 is 0.5-2.5, preferably 1.0-2.0.

[0022] When sulfide is selected, the sulfide is at least one of S, Na2S, K2S, Cu2S, FeS, Fe2S, ZnS, PbS, chalcopyrite, pyrite, sphalerite, and galena, and the mass ratio of the added amount of sulfide to the pretreated material obtained by S1 is 0.2-2.0, preferably 0.3-1.5.

[0023] Furthermore, the slag-forming agent in step S2 can be a silicon-containing slag-forming agent, a fluoride or a chloride, wherein when a silicon-containing slag-forming agent is selected, the silicon-containing slag-forming agent is one or more of crystalline silicon, quartz sand, amorphous silicon, silica, and silicate minerals, and they contain at least one of Si and SiO2. It forms oxide slag with oxides of oxygen-philic elements such as aluminum, lithium, and sodium. The amount of the silicon-containing slag-forming agent used is added according to the amount of Al2O3 in the pretreated material obtained in S1, satisfying the mass fraction ratio of Al2O3 to SiO2 of 0.5 to 3.5, preferably 1.5-2.5.

[0024] When fluoride or chloride is selected as a slag-forming agent, the fluoride is one or more of NaF, KF, and AlF3, and the chloride is one or more of NaCl, KCl, and AlCl3, and the fluoride or chloride forms a molten salt with aluminum and lithium oxides. The amount of fluoride added is added according to the amount of Al2O3 in the pretreated material obtained by S1, and the mass ratio of Al2O3 to fluoride is 0.2-1.0, preferably 0.4-0.6; the amount of chloride added is added according to the amount of Al2O3 in the pretreated material obtained by S1, and the mass ratio of Al2O3 to chloride is 0.01-0.1, preferably 0.02-0.05.

[0025] Furthermore, the matte smelting temperature in step S2 is 1100-1400°C, preferably 1200-1300°C; the roasting time is 0.5-3h, preferably 1.5-2h; the inert gas introduced is at least one of N2 and Ar. The waste lithium battery, sulfur-containing compound and slag-forming agent are completely melted at 1100-1400°C. In this state, the slag system has good fluidity, which is conducive to the complete reaction and the formation of uniform sulfide products.

[0026] The obtained sulfidation product mainly comprises 5%-30wt% Cu, 15%-55wt% Co, 10%-50wt% Ni and 20%-35wt% S. The sulfidation recovery rates of Cu, Co and Ni are all greater than 98%.

[0027] The obtained lithium-rich slag has a Li content of 1.5%-10wt%, and the contents of Co, Ni and Cu are all lower than 0.01%.

[0028] Furthermore, the immersion temperature of step S3 is 10-80°C, the leaching time is 2min-2h, the liquid-solid ratio is (3-50):1, and the stirring rate is 100r / min-600r / min. Preferably, the leaching temperature is 40-60°C, the leaching time is 10-30min, the liquid-solid ratio is (10-20):1, and the stirring rate is 400r / min-500r / min.

[0029] The concentrations of impurities Co, Ni and Cu in the obtained lithium-containing solution are all less than 0.1 mg / L, and the leaching recovery rate of lithium is >95%.

[0030] The method of the present invention is applicable to lithium-containing waste batteries including cobalt oxide lithium batteries, nickel oxide lithium batteries, manganese oxide lithium batteries, nickel manganese lithium batteries, nickel cobalt lithium batteries, nickel cobalt manganese ternary lithium batteries, and nickel cobalt aluminum ternary lithium batteries.

[0031] The main features of the present invention are:

[0032] (1) Short process and low energy consumption

[0033] The raw materials of the present invention are waste lithium-ion batteries that have not been disassembled. After a simple discharge treatment, they are directly subjected to high-temperature matte smelting with sulfur-containing compounds and slag-forming agents. Since they have not been disassembled, the reducing substances in the battery, including graphite electrodes, aluminum foil, and organic matter, are retained to the maximum extent. On the one hand, a good reducing smelting atmosphere can be created for the matte smelting process to ensure that Ni, Co, and Cu in the battery are fully converted into mutually molten sulfide phases; on the other hand, the oxidation and decomposition process of these reducing substances will release a large amount of heat, which can provide heat supply for the system and reduce external energy input. The sulfide product obtained by the present invention is a high-quality "matte" or "matte nickel", which can be used as a high-quality intermediate material for copper and nickel smelting enterprises, enter the blowing process of "matte" or "matte nickel", and minimize the cost of developing an independent recovery and separation technology route, so as to achieve the coordinated disposal of lithium-containing waste batteries and existing typical heavy metals. For lithium, lithium can be converted into soluble sulfate through a one-step matte smelting process and then extracted after water leaching, without the need for subsequent complicated separation procedures of heavy metals such as Cu, Co, Ni, Al, Si and other impurity elements.

[0034] (2) Good selective recovery of lithium

[0035] The present invention is based on the significant difference in sulfur affinity between lithium and cobalt, nickel and copper. In the matte smelting process, cobalt, nickel and copper have stronger affinity with sulfur, and the formed sulfide melt with a larger specific gravity settles to the bottom layer and is completely separated from the upper slag phase. More than 98% of cobalt, nickel and copper are recovered in the form of sulfides; while lithium is more oxygen-friendly and initially exists in the slag phase in the form of oxides. Under the action of added sulfate or sulfide, lithium reacts with cations (such as Na + , K + , Ca 2+ Mg 2+ ) undergoes a common ion exchange reaction and is eventually converted into soluble lithium sulfate or lithium sulfide, and a lithium sulfate or lithium hydroxide leachate is obtained after water leaching; further, when the slag-making agent is fluoride or chloride, lithium enters the fluoride or chloride molten salt in the form of a water-soluble oxide under the action of fluoride or chloride to obtain a lithium hydroxide leachate, thereby improving the leaching rate of lithium. After water leaching, the concentrations of impurities Co, Ni, and Cu in the leachate are all less than 0.1 mg / L, and the leaching rate of lithium exceeds 95%, which solves the problem of poor lithium terminal separation and recovery effect in the traditional pyrometallurgical process of lithium-ion battery recovery.

[0036] (3) The obtained Li-containing solution has a wide range of subsequent uses

[0037] The impurity ions in the obtained Li-containing solution after treatment by this method are low, and the concentrations of Ni, Co, Cu, Al and Si are all lower than 0.1 ppm. After simple impurity removal, concentration and crystallization, the introduction of CO2 or the addition of potassium and sodium carbonate can produce Li2CO3 with higher purity.

[0038] 3. Beneficial effects

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) A short-process recycling method for waste lithium-ion batteries of the present invention utilizes the difference in sulfur affinity between lithium and cobalt, nickel and copper to carry out high-temperature matte smelting of waste lithium-ion batteries, sulfur-containing compounds and slag-forming agents. The lithium and cobalt, nickel and copper in the waste lithium-ion batteries can be efficiently pre-separated through one-step smelting, thereby shortening the recycling process of waste lithium batteries.

[0041] (2) A short-process recycling method for waste lithium-ion batteries of the present invention uses undisassembled waste lithium-ion batteries, which are directly smelted into matte after simple discharge treatment. The reducing substances in the batteries can, on the one hand, create a good reducing smelting atmosphere for the matte smelting process, ensuring that Ni, Co, and Cu in the batteries are fully converted into mutually fusible sulfide phases; on the other hand, the oxidation and decomposition process of the reducing substances will release a large amount of heat, which provides heat supply for the system, reduces external energy input, and promotes the effective progress of the reaction;

[0042] (3) A short-process recycling method for waste lithium-ion batteries of the present invention, the obtained sulfide product is a high-quality "matte copper" or "matte nickel", which can be used as a high-quality intermediate material for copper and nickel smelting enterprises and enter the blowing process of "matte copper" or "matte nickel", thereby reducing the cost of developing independent recycling and separation technology routes and realizing the coordinated disposal of lithium-containing waste batteries and existing typical heavy metals;

[0043] (4) The present invention provides a short-process recycling method for waste lithium-ion batteries. The obtained soluble lithium sulfate has low impurities in the leaching solution after water leaching, and the lithium leaching rate exceeds 95%, thereby improving the lithium terminal separation and recovery effect in the lithium-ion battery recycling process. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but it should be understood that these drawings are designed only for explanation purposes and are not intended to limit the scope of the present invention. In addition, unless otherwise specified, these drawings are intended only to conceptually illustrate the structural configurations described herein and are not necessarily drawn to scale.

[0045] Figure 1 This is a flow chart of the short-process recycling method for waste lithium-ion batteries of the present invention;

[0046] Figure 2 This is a physical picture of the product after matte smelting in Example 1;

[0047] Figure 3 This is a SEM image of the upper slag after matte smelting in Example 1;

[0048] Figure 4 This is the SEM image of the lower layer sulfidation product after matte smelting in Example 1. DETAILED DESCRIPTION

[0049] The following detailed description of exemplary embodiments of the present invention refers to the accompanying drawings, which form a part of the description, and in which exemplary embodiments of the present invention that can be implemented are shown as examples. Although these exemplary embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention, it should be understood that other embodiments can be implemented and various changes can be made to the present invention without departing from the spirit and scope of the present invention. The following more detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but is only for the purpose of illustrating and not limiting the description of the characteristics and features of the present invention, so as to propose the best mode for performing the present invention and to enable those skilled in the art to implement the present invention. Therefore, the scope of the present invention is limited only by the appended claims.

[0050] It should be understood that the following text is only used to describe one or several specific embodiments of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention. As used herein, the terms "parallel" and "perpendicular" are not limited to their strict geometric definitions, but include tolerances for reasonable and inconsistent machining or human errors.

[0051] The present invention directly uses undisassembled waste lithium batteries as raw materials, and after discharge pretreatment, mixes with sulfate and silicon-containing slag-forming agent, performs matte smelting and high-temperature sedimentation separation, and obtains a sulfide melt phase (i.e., matte phase) containing cobalt, nickel and copper and a slag containing lithium sulfate salt in one step. The matte phase can be directly supplied to existing copper and nickel smelters in the form of high-grade "matte copper" or "matte nickel" for separation and recovery, while the slag containing soluble lithium manganese salt is crushed and finely ground for water leaching to obtain a lithium solution with extremely low impurity content, thereby realizing efficient separation and recovery of lithium from cobalt, nickel and copper in one step.

[0052] A short-process recycling method for waste lithium-ion batteries comprises the following steps:

[0053] S1: Raw material pretreatment: Place the lithium-containing waste batteries in a salt solution for immersion and discharge, and then obtain pretreated materials and discharged waste salt solution after solid-liquid separation and drying;

[0054] S2: high-temperature matte smelting: the pretreated material is subjected to high-temperature matte smelting to obtain a sulfide product phase and lithium-rich slag. The pretreated material obtained in step S1 is mixed with a sulfur-containing compound and a slag-forming agent in a certain proportion and then subjected to high-temperature matte smelting. The smelting process is conducted under an inert atmosphere, and the amount of sulfur-containing compound added, the smelting temperature and the smelting time are adjusted. The matte smelting temperature is 1100-1400°C. The smelting product is subjected to sedimentation, cooling and stripping to obtain an upper lithium-rich slag phase and a lower sulfide product.

[0055] S3: Lithium extraction from lithium-rich slag by water leaching: The lithium-rich slag obtained in step S2 is leached in water and filtered to obtain a lithium-containing solution with low impurity content and aluminum-silicon-containing leached slag.

[0056] Sulfur-containing compounds: The present invention is based on the significant difference in sulfur affinity between lithium and cobalt, nickel and copper. Cobalt, nickel and copper have stronger affinity for sulfur. By adding sulfur-containing compounds, cobalt, nickel, copper and sulfur form a sulfide melt with a larger specific gravity and settle to the bottom layer during the matte smelting process, and are completely separated from the upper slag.

[0057] Slag-forming agent: In the present invention, a slag-forming agent is added to form a slag system with sulfide. At a matte smelting temperature of 1100-1400°C, the slag system melts to form a molten phase with good fluidity, so that the metal cobalt, nickel, and copper in the waste lithium battery fully contact and react with the sulfur-containing compound to form a precipitate. The slag-forming agent can be a silicon-containing slag-forming agent, a fluoride, or a chloride. When a silicon-containing slag-forming agent is selected, the silicon-containing slag-forming agent forms an oxide slag with aluminum, lithium, and manganese; when a fluoride or chloride is selected as a slag-forming agent, it forms a molten salt with the oxides of aluminum and lithium.

[0058] Unless otherwise specified, the materials in the present invention are all commercially available.

[0059] Calculation method of metal recovery rate: by testing the components of waste lithium-ion batteries and sulfide products, determine the mass fractions of Cu, Co, and Ni in the two, and multiply the values ​​by the mass of waste batteries added and the mass of sulfide products respectively to obtain the mass of Cu, Co, and Ni elements added and the mass of Cu, Co, and Ni elements in the obtained sulfide products, and then divide the latter by the former and multiply by 100% to obtain the recovery rate. The lithium content in undisassembled lithium batteries is between 2wt% and 3.5wt%. The embodiment of the present invention takes waste lithium batteries with a lithium content of 2.5wt% as the research object.

[0060] Example 1

[0061] A short-process recycling method for waste lithium-ion batteries in Example 1 comprises the following steps, wherein the waste lithium-ion batteries are waste nickel-cobalt-manganese ternary lithium batteries:

[0062] S1: Raw material pretreatment:

[0063] The lithium-containing waste batteries are placed in a salt solution for immersion and discharge, and then solid-liquid separation and drying are performed to obtain pretreated materials and discharged waste salt solution; the salt solution used is NaCl, and the concentration of the salt solution is 0.8 mol / L.

[0064] S2: High temperature matte smelting:

[0065] The pretreated material is subjected to high-temperature matte smelting to obtain a sulfide product phase and lithium-rich slag. The pretreated material obtained in step S1 is mixed with a sulfur-containing compound and a slag-forming agent in a certain proportion and then subjected to high-temperature matte smelting. The smelting process is conducted under an inert atmosphere, and the amount of sulfur-containing compound added, the smelting temperature and the smelting time are adjusted. The smelting product is subjected to sedimentation, cooling and stripping to obtain an upper lithium-rich slag phase and a lower sulfide product phase.

[0066] Among them, the sulfur-containing compound is Na2SO4, and the added amount is 1.5 in the mass ratio with the pretreated material obtained from S1; the slag-forming agent is quartz sand, which is added according to the Al2O3 in the pretreated material obtained from S1 to meet the mass fraction ratio of Al2O3 to SiO2 of 2.0.

[0067] The matte smelting temperature is 1500℃, the roasting time is 1.5h, and the inert gas introduced is N2.

[0068] S3: Lithium-rich slag water leaching:

[0069] The lithium-rich slag obtained in step S2 is soaked in water and filtered to obtain a lithium-containing solution with low impurity content and aluminum-silicon-containing leached slag.

[0070] Among them, the water immersion temperature is 60°C, the leaching time is 90min, the liquid-solid ratio is 10:1, and the stirring rate is 450r / min.

[0071] The composition of the obtained sulfidation product is Cu content 28.3wt%, Co content 10.6wt%, Ni content 28.4wt%, S content 32.7wt%, and the obtained Cu, Co, Ni sulfidation recovery rate is 98.5%.

[0072] The Li content in the obtained lithium-rich slag is 3.4wt% in terms of Li2O, and the contents of Co, Ni and Cu are all lower than 0.001wt%.

[0073] The concentrations of impurities Co, Ni and Cu in the obtained lithium-containing solution were 0.012 mg / L, 0.015 mg / L and 0.013 mg / L respectively, and the leaching recovery rate of lithium was 96.5%.

[0074] Example 2

[0075] A short-process recycling method for waste lithium-ion batteries in Example 2 comprises the following steps, wherein the waste lithium-ion batteries are waste nickel-cobalt-manganese ternary lithium batteries:

[0076] S1: Raw material pretreatment:

[0077] The lithium-containing waste batteries are placed in a salt solution for immersion and discharge, and then solid-liquid separation and drying are performed to obtain pretreated materials and discharged waste salt solution; the salt solution used is KCl, and the concentration of the salt solution is 0.8 mol / L.

[0078] S2: High temperature matte smelting:

[0079] The pretreated material is subjected to high-temperature matte smelting to obtain a sulfide product phase and lithium-rich slag. The pretreated material obtained in step S1 is mixed with a sulfur-containing compound and a slag-forming agent in a certain proportion and then subjected to high-temperature matte smelting. The smelting process is conducted under an inert atmosphere, and the amount of sulfur-containing compound added, the smelting temperature and the smelting time are adjusted. The smelting product is subjected to sedimentation, cooling and stripping to obtain an upper lithium-rich slag phase and a lower sulfide product phase.

[0080] Among them, the sulfur-containing compound is Na2S, and the added amount is 1.0 in the mass ratio with the pretreated material obtained from S1; the slag-forming agent is quartz sand, which is added according to the Al2O3 in the pretreated material obtained from S1 to meet the mass fraction ratio of Al2O3 to SiO2 of 2.2.

[0081] The matte smelting temperature is 1550℃, the roasting time is 1.0h, and the inert gas introduced is N2.

[0082] S3: Lithium extraction from lithium-rich slag:

[0083] The lithium-rich slag obtained in step S2 is soaked in water and filtered to obtain a lithium-containing solution with low impurity content and aluminum-silicon-containing leached slag.

[0084] Among them, the water immersion temperature is 45°C, the leaching time is 60min, the liquid-solid ratio is 10:1, and the stirring rate is 450r / min.

[0085] The composition of the obtained sulfidation product is Cu content 27.8wt%, Co content 11.3wt%, Ni content 27.4wt%, S content 33.5wt%, and the obtained Cu, Co, Ni sulfidation recovery rate is 98.7%.

[0086] The Li content in the obtained lithium-rich slag is 5.3wt% in terms of Li2O, and the contents of Co, Ni and Cu are all lower than 0.001wt%.

[0087] The concentrations of impurities Co, Ni and Cu in the obtained lithium-containing solution were 0.014 mg / L, 0.012 mg / L and 0.013 mg / L respectively, and the leaching recovery rate of lithium was 96.5%.

[0088] Example 3

[0089] A short-process recycling method for waste lithium-ion batteries according to Example 3 comprises the following steps, wherein the waste lithium-ion batteries are waste lithium cobalt oxide batteries:

[0090] S1: Raw material pretreatment:

[0091] The lithium-containing waste batteries are placed in a salt solution for immersion and discharge, and then solid-liquid separation and drying are performed to obtain pretreated materials and discharged waste salt solution; the salt solution used is NaCl, and the concentration of the salt solution is 0.8 mol / L.

[0092] S2: High temperature matte smelting:

[0093] The pretreated material is subjected to high-temperature matte smelting to obtain a sulfide product phase and lithium-rich slag. The pretreated material obtained in step S1 is mixed with a sulfur-containing compound and a slag-forming agent in a certain proportion and then subjected to high-temperature matte smelting. The smelting process is conducted under an inert atmosphere, and the amount of sulfur-containing compound added, the smelting temperature and the smelting time are adjusted. The smelting product is subjected to sedimentation, cooling and stripping to obtain an upper lithium-rich slag phase and a lower sulfide product phase.

[0094] Among them, the sulfur-containing compound is Na2SO4, and the added amount is 1.5 in the mass ratio with the pretreated material obtained from S1; the slag-forming agent is quartz sand, which is added according to the Al2O3 in the pretreated material obtained from S1 to meet the mass fraction ratio of Al2O3 to SiO2 of 2.0.

[0095] The matte smelting temperature is 1500℃, the roasting time is 1.5h, and the inert gas introduced is N2.

[0096] S3: Lithium-rich slag water leaching:

[0097] The lithium-rich slag obtained in step S2 is soaked in water and filtered to obtain a lithium-containing solution with low impurity content and aluminum-silicon-containing leached slag.

[0098] Among them, the water immersion temperature is 60°C, the leaching time is 90min, the liquid-solid ratio is 10:1, and the stirring rate is 450r / min.

[0099] The composition of the obtained sulfidation product is Cu content 25.6wt%, Co content 44.1wt%, S content 30.3wt%, and the obtained Cu and Co sulfidation recovery rate is 99.2%.

[0100] The Li content in the obtained lithium-rich slag is 3.2wt% in terms of Li2O, and the contents of Co, Ni and Cu are all lower than 0.001%.

[0101] The concentrations of impurities Co and Cu in the obtained lithium-containing solution were 0.011 mg / L and 0.012 mg / L, respectively, and the leaching recovery rate of lithium was 97.1%.

[0102] Example 4

[0103] A short-process recycling method for waste lithium-ion batteries in Example 4 comprises the following steps, wherein the waste lithium-ion batteries are waste nickel-cobalt-manganese ternary lithium batteries:

[0104] S1: Raw material pretreatment:

[0105] The lithium-containing waste batteries are placed in a salt solution for immersion and discharge, and then solid-liquid separation and drying are performed to obtain pretreated materials and discharged waste salt solution; the salt solution used is NaCl, and the concentration of the salt solution is 0.8 mol / L.

[0106] S2: High temperature matte smelting:

[0107] The pretreated material is subjected to high-temperature matte smelting to obtain a sulfide product phase and lithium-rich slag. The pretreated material obtained in step S1 is mixed with a sulfur-containing compound and a slag-forming agent in a certain proportion and then subjected to high-temperature matte smelting. The smelting process is conducted under an inert atmosphere, and the amount of sulfur-containing compound added, the smelting temperature and the smelting time are adjusted. The smelting product is subjected to sedimentation, cooling and stripping to obtain an upper lithium-rich slag phase and a lower sulfide product phase.

[0108] Among them, the sulfur-containing compound is Na2SO4, and the added amount is 1.5 in mass ratio with the pretreated material obtained from S1; the slag-forming agent is NaF; the added amount is added according to the amount of Al2O3 in the pretreated material obtained from S1, satisfying the mass ratio of Al2O3 to fluoride of 0.5.

[0109] The matte smelting temperature is 1500℃, the roasting time is 1.5h, and the inert gas introduced is N2.

[0110] S3: Lithium-rich slag water leaching:

[0111] The lithium-rich slag obtained in step S2 is soaked in water and filtered to obtain a lithium-containing solution with low impurity content and aluminum-silicon-containing leached slag.

[0112] Among them, the water immersion temperature is 60°C, the leaching time is 90min, the liquid-solid ratio is 10:1, and the stirring rate is 450r / min.

[0113] The composition of the obtained sulfidation product is Cu content 26.5wt%, Co content 10.4wt%, Ni content 29.6wt%, S content 33.5wt%, and the obtained Cu, Co, Ni sulfidation recovery rate is 98.7%.

[0114] The Li content in the obtained lithium-rich slag is 8.2wt% in terms of Li2O, and the contents of Co, Ni and Cu are all lower than 0.001wt%.

[0115] The concentrations of impurities Co, Cu and Ni in the obtained lithium-containing solution were 0.015 mg / L, 0.015 mg / L and 0.018 mg / L respectively, and the leaching recovery rate of lithium was 96.8%.

[0116] Example 5

[0117] A short-process recycling method for waste lithium-ion batteries in Example 5 comprises the following steps, wherein the waste lithium-ion batteries are waste nickel-cobalt-manganese ternary lithium batteries:

[0118] S1: Raw material pretreatment:

[0119] The lithium-containing waste batteries are placed in a salt solution for immersion and discharge, and then solid-liquid separation and drying are performed to obtain pretreated materials and discharged waste salt solution; the salt solution used is NaCl, and the concentration of the salt solution is 0.8 mol / L.

[0120] S2: High temperature matte smelting:

[0121] The pretreated material is subjected to high-temperature matte smelting to obtain a sulfide product phase and lithium-rich slag. The pretreated material obtained in step S1 is mixed with a sulfur-containing compound and a slag-forming agent in a certain proportion and then subjected to high-temperature matte smelting. The smelting process is conducted under an inert atmosphere, and the amount of sulfur-containing compound added, the smelting temperature and the smelting time are adjusted. The smelting product is subjected to sedimentation, cooling and stripping to obtain an upper lithium-rich slag phase and a lower sulfide product phase.

[0122] Among them, the sulfur-containing compound is K2SO4, and the added amount is 1.5 in mass ratio with the pretreated material obtained from S1; the slag-forming agent is NaCl; the added amount is added according to the amount of Al2O3 in the pretreated material obtained from S1, satisfying the mass ratio of Al2O3 to fluoride of 0.5.

[0123] The matte smelting temperature is 1500℃, the roasting time is 1.5h, and the inert gas introduced is N2.

[0124] S3: Lithium-rich slag water leaching:

[0125] The lithium-rich slag obtained in step S2 is soaked in water and filtered to obtain a lithium-containing solution with low impurity content and aluminum-silicon-containing leached slag.

[0126] Among them, the water immersion temperature is 60°C, the leaching time is 90min, the liquid-solid ratio is 10:1, and the stirring rate is 450r / min.

[0127] The composition of the obtained sulfidation product is Cu content 27.1wt%, Co content 11.7wt%, Ni content 29.6wt%, S content 31.6wt%, and the obtained Cu, Co, Ni sulfidation recovery rate is 98.5%.

[0128] The obtained lithium-rich slag has a Li content of 7.8 wt% in terms of Li2O, and the contents of Co, Ni and Cu are all lower than 0.001 wt%.

[0129] The concentrations of impurities Co, Cu and Ni in the obtained lithium-containing solution were 0.011 mg / L, 0.012 mg / L and 0.017 mg / L respectively, and the leaching recovery rate of lithium was 96.3%.

[0130] Comparative Example 1

[0131] A short-process recycling method for waste lithium-ion batteries in Comparative Example 1 comprises the following steps, wherein the waste lithium-ion batteries are waste nickel-cobalt-manganese ternary lithium batteries:

[0132] S1: Raw material pretreatment:

[0133] The lithium-containing waste batteries are placed in a salt solution for immersion and discharge, and then solid-liquid separation and drying are performed to obtain pretreated materials and discharged waste salt solution; the salt solution used is NaCl, and the concentration of the salt solution is 0.8 mol / L.

[0134] S2: High temperature matte smelting:

[0135] The pretreated material is subjected to high-temperature matte smelting to obtain a sulfide product phase and lithium-rich slag. The pretreated material obtained in step S1 is mixed with a sulfur-containing compound in a certain proportion and then subjected to high-temperature matte smelting. The smelting process is conducted under an inert atmosphere, and the amount of sulfur-containing compound added, the smelting temperature and the smelting time are adjusted. Since no slag-forming agent is added, the smelting product is not stratified, and the product in this embodiment is referred to as a smelting mixture.

[0136] Wherein, the sulfur-containing compound is K2SO4, and the added amount is 1.5 in mass ratio to the pretreated material obtained from S1;

[0137] The matte smelting temperature is 1500℃, the roasting time is 1.5h, and the inert gas introduced is N2.

[0138] S3: Smelting the mixture to extract lithium by water leaching:

[0139] The smelting mixture obtained in step S2 is immersed in water and filtered to obtain a lithium-containing solution and leached slag with low impurity content.

[0140] Among them, the water immersion temperature is 60°C, the leaching time is 90min, the liquid-solid ratio is 10:1, and the stirring rate is 450r / min.

[0141] The composition of the obtained leaching residue is Cu content 7.1wt%, Co content 3.5wt%, Ni content 10.2wt%, S content 21.6wt%, Li content 0.8wt%, Al content 13%, O content 43.8%. Since the leaching residue is not a sulfide, Cu, Co, Ni cannot be completely separated from other impurity elements such as Al, Li, O, etc., and recycling is essentially not achieved.

[0142] The concentrations of impurities Co, Cu and Ni in the obtained lithium-containing solution were 8.1 mg / L, 7.2 mg / L and 9.3 mg / L respectively, and the leaching recovery rate of lithium was 16.3%.

[0143] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.

[0144] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.

Claims

1. A short-process recycling method for waste lithium-ion batteries, characterized in that: The method comprises the following steps: mixing lithium-containing waste batteries with sulfur-containing compounds and a slag-forming agent and then performing high-temperature matte smelting; and obtaining an upper layer of lithium-rich slag and a lower layer of sulfide products after sedimentation, cooling and peeling of the smelting products; the matte smelting temperature is 1100-1400°C.

2. The recycling method according to claim 1, characterized in that: The sulfur-containing compound is sulfate or sulfide, and the mass ratio of the added amount of the sulfur-containing compound to the lithium-containing waste battery is 0.2-2.

5.

3. The recycling method according to claim 3, characterized in that: The slag-forming agent is selected from one of a silicon-containing slag-forming agent, a fluoride and a chloride. The lithium-containing waste battery contains Al2O3. The amount of silicon-containing slag-forming agent added satisfies that the mass fraction ratio of Al2O3 to SiO2 is 0.5-3.5; the amount of fluoride added satisfies that the mass ratio of Al2O3 to fluoride is 0.2-1.0; and the amount of chloride added satisfies that the mass ratio of Al2O3 to chloride is 0.01-0.

1.

4. The recycling method according to claim 3, characterized in that: The silicon-containing slag-forming agent includes one or more of crystalline silicon, quartz sand, amorphous silicon, silica, and silicate minerals; the fluoride includes one or more of NaF, KF, and AlF3; and the chloride includes one or more of NaCl, KCl, and AlCl3.

5. The recycling method according to claim 1, characterized in that: An inert atmosphere is introduced during the high-temperature matte smelting process.

6. The recycling method according to claim 1, characterized in that: The time for high-temperature matte smelting is 0.5-3h.

7. The recycling method according to claim 1, characterized in that: The method also includes the step of pre-treating the lithium-containing waste batteries. The pre-treatment process includes: placing the lithium-containing waste batteries in a salt solution for immersion and discharge, and then performing solid-liquid separation and drying to obtain pre-treated materials and discharged waste salt solution.

8. The recycling method according to claim 7, characterized in that: The salt solution used in step S1 is a solution of one or more of Na2SO4, K2SO4, NaCl, and KCl, and the concentration of the salt solution is 0.2 to 1.0 mol / L.

9. The recycling method according to claim 1, characterized in that: The invention also comprises the step of leaching lithium from lithium-rich slag: leaching the obtained lithium-rich slag in water, filtering and obtaining a lithium-containing solution and aluminum-silicon-containing leached slag.

10. The recycling method according to claim 9, characterized in that: In the lithium-rich slag water leaching lithium step, the water leaching temperature is 10-80°C, the leaching time is 2min-2h, the liquid-solid ratio is (3-50):1, and the stirring rate is 100r / min-600r / min.

Citation Information

Patent Citations

  • Method for extracting valuable metal from waste lithium ion battery material

    CN114480854A

  • Synergistic resource recycling method for industrial sulfate solid waste and waste nickel-cobalt-manganese-lithium series batteries

    CN115367732A

  • Valuable metal recovery method

    CN116804243A

  • Valuable metal recovery method

    CN116926331A

  • Remote control transmitter building microphone therein

    KR1020240070335A

Cited By

  • Method for treating waste lithium battery discharge wastewater and recycling valuable metal and application

    CN120555763A

  • Method for treating waste lithium battery discharge wastewater and recovering valuable metals and application

    CN120555763B