Iron-based alloy friction material and preparation method and application thereof
By rationally formulating FeCrAlY alloy and TiC particles in ferro-based alloys, the problems of mechanical and tribological properties compatibility of ferro-based alloy friction materials are solved, and stable performance is achieved at high temperatures and is suitable for mechanical moving parts.
Patent Information
- Application Number
- CN202411041908.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
Ferro-based alloy friction materials have challenges in mechanical properties and tribological properties compatibility, especially in the high temperatures, which show lower toughness and poor wear resistance, resulting in unsatisfactory reinforcement effects.
Using a specific ratio of FeCrAlY alloy and TiC particles, they are mixed evenly through ball milling and sintering processes, adjusting the Y content and TiC particle size to improve the mechanical and tribological properties of the material and maintaining stability from room temperature to 300°C. coefficient of friction.
It realizes compatibility between mechanical properties and tribological properties of iron-based alloy friction materials, has good self-lubricating properties and wear resistance, and has high compressive strength. It is suitable for high load, low speed, high impact stress and high and low temperature alternation. Working conditions.
Smart Images

Figure CN118957439A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of alloy materials, and in particular to an iron-based alloy friction material and a preparation method and application thereof. Background Art
[0002] The main reason for the failure of the moving parts of mechanical equipment is friction and wear. Iron-based alloy friction materials have good self-lubrication and are particularly suitable for mechanical moving parts working under wear conditions such as bearings, bushings, cylinder liners, valve seats, piston rings, floating bearings, guide sleeves, crankshafts, and chain rods. Among many iron-based alloys, FeCrAl alloy is a new type of material developed on the basis of Fe-Cr and Fe-Cr-Ni alloys. This alloy system has lower density, excellent oxidation resistance and long service life. At the same time, FeCrAl alloy also has good corrosion resistance and radiation resistance, so it is also considered to be a very potential candidate structural material for reactors.
[0003] With the development of modern industry, higher requirements are put forward for the comprehensive performance of materials for mechanical moving parts. The compatibility of mechanical properties and tribological properties of iron-based alloy friction materials has always been a scientific problem that restricts its application as a structural material for mechanical moving parts. In order to improve the mechanical properties of FeCrAl alloys and make them more competitive, the prior art generally introduces reinforcing phases into FeCrAl alloys, such as adding reinforcing materials. Commonly used materials mainly include oxides, carbides, fibers, graphene, etc. Different reinforcing materials show different reinforcing mechanisms. Among them, particle reinforcing materials such as oxides and carbides have the characteristics of high melting point, high hardness, high elastic modulus, small linear thermal expansion coefficient, good stability of organization and performance at high temperature, good wear resistance and corrosion resistance, etc. Compared with fiber and whisker reinforcing materials, the preparation process and equipment of particle reinforcing materials are simpler and the cost is lower, which is conducive to industrial production and promotion and application. Introducing particle reinforcing materials with good thermal stability into FeCrAl alloys is an effective way to improve the mechanical properties of FeCrAl alloys. However, particle reinforcement materials often have problems such as accumulation and uneven distribution, and the reinforcement effect is not ideal or even has negative effects, such as reduced toughness or poor wear resistance, poor high temperature resistance, etc. Therefore, selecting appropriate reinforcement materials and optimizing the preparation process are the key to obtaining iron-based alloy friction materials with compatible mechanical and tribological properties. Summary of the invention
[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the purpose of the present invention is to provide an iron-based alloy friction material, which is a self-lubricating friction material, including a specific proportion of FeCrAlY alloy and TiC, has excellent mechanical properties, good self-lubricating properties and wear resistance, and achieves compatibility between mechanical properties and tribological properties.
[0005] A second aspect of the present invention is to provide a method for preparing an iron-based alloy friction material.
[0006] A third aspect of the present invention is to provide a structural material.
[0007] A fourth aspect of the present invention is to provide an application of an iron-based alloy friction material or structural material.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is:
[0009] A first aspect of the present invention is to provide an iron-based alloy friction material, comprising 65-85% by mass of FeCrAlY alloy and 15-35% by mass of TiC.
[0010] The wetting angle θ between TiC particles and molten Fe is 28°, and there is no interface reaction between the two, which is an ideal iron-based alloy reinforcement phase. The iron-based alloy friction material of the present invention has a specific ratio of FeCrAlY alloy and TiC, and the tribological properties and mechanical properties are improved by adjusting the content of FeCrAlY alloy and TiC, and can have a stable friction coefficient under dynamic temperature rise from room temperature to 300°C.
[0011] In some embodiments of the present invention, the mass content of Y in the FeCrAlY alloy is 0.1-1%.
[0012] In some embodiments of the present invention, the mass content of Y in the FeCrAlY alloy is 0.15-0.5%.
[0013] In some specific embodiments of the present invention, the mass content of Y in the FeCrAlY alloy is 0.2-0.25%.
[0014] For example, the mass content of Y in the FeCrAlY alloy may be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.5%, 0.8%, or 1%.
[0015] In some embodiments of the present invention, the mass ratio of Fe, Cr, Al and Y elements in the FeCrAlY alloy is (75-85):(10-20):(5-10):(0.1-1).
[0016] In some embodiments of the present invention, the mass ratio of Fe, Cr, Al and Y elements in the FeCrAlY alloy is (79-80):(14-15):(5-6):(0.2-0.25).
[0017] The content of each component in the FeCrAlY alloy will affect the performance of the final iron-based alloy friction material. For example, the mass content of Y is related to the mechanical properties of the iron-based alloy friction material. Controlling the content of Y is conducive to further improving the mechanical properties.
[0018] In some embodiments of the present invention, the TiC is nano-TiC.
[0019] In some embodiments of the present invention, the average particle size of the TiC is 35 to 55 nm.
[0020] In some embodiments of the present invention, the average particle size of the TiC is 40-50 nm.
[0021] In some specific embodiments of the present invention, the average particle size of the TiC is 45-50 nm.
[0022] For example, the average particle size of TiC may be 35 nm, 40 nm, 45 nm, 50 nm, or 55 nm.
[0023] In some embodiments of the present invention, the average particle size of the FeCrAlY alloy is 200-300 meshes.
[0024] For example, the average particle size of the FeCrAlY alloy of the present invention may be 200 mesh, 250 mesh, or 300 mesh.
[0025] The second aspect of the present invention provides a method for preparing the iron-based alloy friction material according to the first aspect of the present invention, comprising the following steps:
[0026] The FeCrAlY alloy and TiC are mixed, ball-milled, and then sintered to obtain an iron-based alloy friction material.
[0027] The present invention firstly ball-mills the FeCrAlY alloy and TiC and then sinters them. Ball milling can make the FeCrAlY alloy and TiC mix evenly, avoid local agglomeration of TiC, ensure the uniformity of phase distribution after sintering, and simultaneously select appropriate sintering process parameters to obtain a dense block material, which can ensure the mechanical properties of the material to a certain extent, such as improvement of compressive strength.
[0028] In some embodiments of the present invention, the diameter of the grinding balls of the ball mill is 3 to 10 mm.
[0029] In some embodiments of the present invention, the grinding balls of the ball mill include grinding balls with diameters of 2.5-3.5 mm, 4-5 mm, and 9-10 mm.
[0030] In some specific embodiments of the present invention, the mass ratio of the grinding balls of 2.5-3.5 mm, 4-5 mm, and 9-10 mm is 1:(0.9-1.1):(0.9-1.1).
[0031] In some embodiments of the present invention, the ball-to-material ratio of the ball mill is 1:(1-2).
[0032] In some embodiments of the present invention, the rotation speed of the ball mill is 200-400 r / min.
[0033] In some embodiments of the present invention, the rotation speed of the ball mill is 250-350 r / min.
[0034] In some specific implementations of the present invention, the rotation speed of the ball mill is 290-310 r / min.
[0035] For example, the ball mill rotation speed of the present invention can be 200r / min, 250r / min, 290r / min, 300r / min, 350r / min, 390r / min, 400r / min.
[0036] In some embodiments of the present invention, the ball milling time is 8 to 10 hours.
[0037] In some embodiments of the present invention, the ball milling time is 8 to 9 hours.
[0038] In some specific embodiments of the present invention, the ball milling time is 8 to 8.5 hours.
[0039] For example, the ball milling time in the preparation method of the present invention can be 8h, 9h, or 10h.
[0040] By adjusting the parameters of the ball milling process, such as the ball milling speed, ball milling time, grinding ball diameter, etc., the uniformity of powder mixing and the density of the sintered block can be further ensured, thereby improving the comprehensive properties of the material, such as tribological properties and mechanical properties.
[0041] In some embodiments of the present invention, the ball milling adopts a planetary low-energy ball mill; and the grinding balls are stainless steel balls.
[0042] In some embodiments of the present invention, the ball-milled FeCrAlY alloy and TiC mixture is placed in a mold with a diameter of 30 to 80 mm for sintering.
[0043] In some embodiments of the present invention, the mold with a diameter of 30 to 80 mm is a graphite cylinder mold.
[0044] In some embodiments of the present invention, the sintering temperature is 1300-1400°C.
[0045] In some embodiments of the present invention, the sintering temperature is 1300-1350°C.
[0046] For example, the sintering temperature of the present invention may be 1300°C, 1350°C, or 1400°C.
[0047] In some embodiments of the present invention, the heating rate of the sintering is 10-15° C. / min.
[0048] For example, the heating rate of the present invention may be 10°C, 12°C, or 15°C.
[0049] In some embodiments of the present invention, the sintering pressure is 25-35 MPa.
[0050] In some embodiments of the present invention, the sintering is performed under vacuum.
[0051] In some embodiments of the present invention, the vacuum degree of sintering is 10 -2 ~10 -1 Pa.
[0052] In some embodiments of the present invention, the temperature and pressure are maintained during the sintering process for 5 to 30 minutes.
[0053] For example, the time for heat preservation and pressure preservation during the sintering process can be 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, or 30 minutes.
[0054] In some embodiments of the present invention, the pressure is applied when the temperature rises to 700-800° C. during the sintering process.
[0055] In some embodiments of the present invention, the pressure is applied when the temperature rises to 700-750° C. during the sintering process.
[0056] The third aspect of the present invention is a structural material, comprising the iron-based alloy friction material described in the first aspect of the present invention, or the iron-based alloy friction material obtained by the preparation method described in the second aspect of the present invention.
[0057] The fourth aspect of the present invention provides a mechanical moving part, comprising the iron-based alloy friction material described in the first aspect of the present invention or the structural material described in the third aspect of the present invention.
[0058] Compared with the prior art, the present invention has at least the following beneficial technical effects:
[0059] (1) The iron-based alloy friction material of the present invention is an iron-based alloy self-lubricating friction material, which has good isotropic characteristics in terms of mechanical properties, and has a stable friction coefficient under different temperature conditions, good self-lubricating performance and wear resistance, and has a 10 -5 mm 3 The wear rate is low at the order of magnitude of / N·m, and the change in wear rate under dynamic heating conditions from room temperature to 300℃ does not exceed 0.7×10 -5 mm 3 / N·m; at the same time, the iron-based alloy friction material has excellent mechanical strength, high compressive strength of not less than 1100MPa, axial Vickers hardness and radial Vickers hardness of not less than 3GPa, achieving the compatibility of mechanical properties and tribological properties.
[0060] (2) The preparation method of the present invention is simple in process and can further control the mechanical properties and tribological properties of the iron-based alloy friction material by adjusting the process parameters.
[0061] (3) The iron-based alloy friction material of the present invention has excellent mechanical properties, self-lubricating properties and wear resistance, high compressive strength, and a stable friction coefficient when the temperature rises from room temperature to 300°C. It can be used as a structural material for preparing mechanical moving parts, and is particularly suitable for friction materials serving under high load, low speed, high impact stress and high and low temperature alternating working conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 The X-ray diffraction spectra of the iron-based alloy friction materials of Examples 1 to 3 of the present invention are shown.
[0063] Figure 2 The Vickers microhardness diagrams of the iron-based alloy friction materials of Examples 1 to 3 of the present invention.
[0064] Figure 3 This is a diagram of the compressive strength of the iron-based alloy friction material of Examples 1 to 3 of the present invention.
[0065] Figure 4 This is a graph of average friction coefficients of the iron-based alloy friction materials of Examples 1 to 3 of the present invention. DETAILED DESCRIPTION
[0066] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0067] Example 1
[0068] The present embodiment provides an iron-based alloy friction material, comprising 85% by mass of FeCrAlY alloy and 15% by mass of TiC; the mass content of Y in the FeCrAlY alloy is 0.2%; the mass ratio of Fe, Cr, Al and Y elements in the FeCrAlY alloy is 79.8:15:5:0.2; the average particle size of TiC is 50 nm; and the average particle size of the FeCrAlY alloy is 200 mesh.
[0069] The preparation method of the iron-based alloy friction material in this embodiment comprises the following steps:
[0070] 85% of FeCrAlY alloy powder with a mass ratio of Fe, Cr, Al and Y elements of 79.8:15:5:0.2 and 15% of TiC powder with an average particle size of 50 nm were weighed and put into a ball mill. A planetary low-energy ball mill was used with stainless steel balls with a diameter of 3 to 10 mm (the mass ratio of grinding balls of 3 mm, 5 mm and 10 mm was 1:1:1) as grinding balls, a ball-to-material ratio (i.e., the ratio of grinding balls to alloy and TiC raw materials) of 1:2, a rotation speed of 300 r / min, and after ball milling for 8 hours, the uniformly mixed powder was put into a Φ52 mm graphite mold and placed in a vacuum hot pressing sintering furnace with a furnace chamber vacuum degree of 10 -2 ~10 -1 Pa, and then the temperature was raised to 700 °C at a heating rate of 10 °C / min, and the sintering pressure was applied. When the temperature was raised to the sintering temperature of 1300 °C, the pressure increased to 25 MPa. After keeping the temperature and pressure for 5 minutes, the furnace was cooled to room temperature to obtain an iron-based alloy friction material, which was recorded as FeCrAlY-15TiC.
[0071] The mechanical properties of FeCrAlY-15TiC were tested along the axial direction (parallel to the sintering pressure direction) and radial direction (perpendicular to the sintering pressure direction). The results are as follows: Figure 2 and Figure 3 As shown: the axial Vickers hardness is 3.39GPa, the radial Vickers hardness is 3.50GPa; the axial compressive strength is 1127MPa, and the radial compressive strength is 1216MPa.
[0072] Example 2
[0073] The present embodiment provides an iron-based alloy friction material, comprising 75% by mass of a FeCrAlY alloy and 25% by mass of TiC; the mass content of Y in the FeCrAlY alloy is 0.2%; the mass ratio of Fe, Cr, Al, and Y elements in the FeCrAlY alloy is 79.8:15:5:0.2; the average particle size of TiC is 50 nm; and the average particle size of the FeCrAlY alloy is 250 mesh.
[0074] The preparation method of the iron-based alloy friction material in this embodiment comprises the following steps:
[0075] 75% of FeCrAlY alloy powder with a mass ratio of Fe, Cr, Al and Y elements of 79.8:15:5:0.2 and 25% of TiC powder with an average particle size of 50 nm were weighed and put into a ball mill. A planetary low-energy ball mill was used with stainless steel balls with a diameter of 3 to 10 mm (the mass ratio of 3 mm, 5 mm and 10 mm grinding balls was 1:1:1) as grinding balls, a ball-to-material ratio of 1:1.5, a rotation speed of 300 r / min. After ball milling for 8 hours, the mixed powder was put into a Φ52 mm graphite mold and placed in a vacuum hot pressing sintering furnace with a furnace chamber vacuum degree of 10 -2 ~10 -1 Pa, and then the temperature was raised to 700 °C at a heating rate of 12 °C / min, and the sintering pressure was applied. When the temperature was raised to the sintering temperature of 1320 °C, the pressure increased to 30 MPa. After keeping the temperature and pressure for 30 minutes, the furnace was cooled to room temperature to obtain an iron-based alloy friction material, which was recorded as FeCrAlY-25TiC.
[0076] The mechanical properties of FeCrAlY-25TiC were tested along the axial direction (parallel to the sintering pressure direction) and radial direction (perpendicular to the sintering pressure direction). The results are as follows: Figure 2 and Figure 3 As shown: the axial Vickers hardness is 5.04GPa, the radial Vickers hardness is 5.58GPa; the axial compressive strength is 1221MPa, and the radial compressive strength is 1341MPa.
[0077] Example 3
[0078] The present embodiment provides an iron-based alloy friction material, comprising a FeCrAlY alloy with a mass fraction of 65% and a TiC with a mass fraction of 35%; the mass content of Y in the FeCrAlY alloy is 0.2%; the mass ratio of Fe, Cr, Al, and Y elements in the FeCrAlY alloy is 79.8:15:5:0.2; the average particle size of TiC is 50 nm; and the average particle size of the FeCrAlY alloy is 300 mesh.
[0079] The preparation method of the iron-based alloy friction material in this embodiment comprises the following steps:
[0080] 65% of FeCrAlY alloy powder with a mass ratio of Fe, Cr, Al and Y elements of 79.8:15:5:0.2 and 35% of TiC powder with an average particle size of 50 nm were weighed and put into a ball mill. A planetary low-energy ball mill was used with stainless steel balls with a diameter of 3 to 10 mm (the mass ratio of grinding balls of 3 mm, 5 mm and 10 mm was 1:1:1) as grinding balls, a ball-to-material ratio of 1:1, a rotation speed of 300 r / min. After ball milling for 8 hours, the mixed powder was put into a Φ52 mm graphite mold and placed in a vacuum hot pressing sintering furnace. The vacuum degree of the furnace chamber was 10 -2 ~10 -1 Pa, and the temperature was raised to 700 °C at a heating rate of 15 °C / min, and the sintering pressure was applied. When the temperature was raised to the sintering temperature of 1350 °C, the pressure increased to 35 MPa. After keeping the temperature and pressure for 15 minutes, the furnace was cooled to room temperature to obtain an iron-based alloy friction material, which was recorded as FeCrAlY-35TiC.
[0081] The mechanical properties of FeCrAlY-35TiC were tested along the axial direction (parallel to the sintering pressure direction) and radial direction (perpendicular to the sintering pressure direction). The results are as follows: Figure 2 and Figure 3 As shown: the axial Vickers hardness is 5.57 GPa, the radial Vickers hardness is 5.54 GPa; the axial compressive strength is 1468 MPa, and the radial compressive strength is 1308 MPa.
[0082] Example 4
[0083] The present embodiment provides an iron-based alloy friction material, comprising 75% by mass of a FeCrAlY alloy and 25% by mass of TiC; the mass content of Y in the FeCrAlY alloy is 0.2%; the mass ratio of Fe, Cr, Al, and Y elements in the FeCrAlY alloy is 79.8:15:5:0.2; the average particle size of TiC is 40 nm; and the average particle size of the FeCrAlY alloy is 250 mesh.
[0084] The preparation method of the iron-based alloy friction material in this embodiment comprises the following steps:
[0085] 75% of FeCrAlY alloy powder with a mass ratio of Fe, Cr, Al and Y of 79.8:15:5:0.2 and 25% of TiC powder with an average particle size of 40 nm were weighed and put into a ball mill. A planetary low-energy ball mill was used with stainless steel balls with a diameter of 3 to 10 mm (the mass ratio of 3 mm, 5 mm and 10 mm grinding balls was 1:1:1) as grinding balls, a ball-to-material ratio of 1:1, a rotation speed of 300 r / min. After ball milling for 8 hours, the uniformly mixed powder was put into a Φ52 mm graphite mold and placed in a vacuum hot pressing sintering furnace. The vacuum degree of the furnace chamber was 10 -2~10 -1 Pa, and then the temperature was raised to 700°C at a heating rate of 12°C / min, and the sintering pressure was applied. When the temperature was raised to the sintering temperature of 1320°C, the pressure increased to 30MPa. After keeping the temperature and pressure for 30 minutes, the furnace was cooled to room temperature to obtain the iron-based alloy friction material.
[0086] The mechanical properties of the iron-based alloy friction material were tested in the axial direction (parallel to the sintering pressurization direction) and radial direction (perpendicular to the sintering pressurization direction). The results were as follows: the axial Vickers hardness was 3.76 GPa, and the radial Vickers hardness was 4.75 GPa; the axial compressive strength was 1168 MPa, and the radial compressive strength was 1579 MPa.
[0087] In the above-mentioned embodiments 1 to 4 of the present invention, the mass fractions of FeCrAlY alloy and TiC in the iron-based alloy friction material are shown in Table 1 below:
[0088] Table 1 Proportions of FeCrAlY alloy and TiC in Examples 1 to 4
[0089] FeCrAlY alloy / wt% TiC / wt% Example 1 85 15 Example 2 75 25 Example 3 65 35 Example 4 75 25
[0090] Matrix material comparative example 1
[0091] This comparative example provides a method for preparing a FeCrAlY ferroalloy bulk material, comprising the following steps:
[0092] FeCrAlY ferroalloy powder with a mass ratio of Fe, Cr, Al and Y elements of 79.8:15:5:0.2 was placed in a Φ52mm graphite mold, and then moved to a vacuum hot pressing sintering furnace. The temperature was raised to 700°C at a heating rate of 10°C / min, and the sintering pressure was applied. When the temperature rose to the sintering temperature of 1200°C, the pressure increased to 25MPa. After keeping the temperature and pressure for 5 minutes, the powder was cooled to room temperature with the furnace to obtain a FeCrAlY ferroalloy block material.
[0093] Through X-ray diffraction analysis, the prepared FeCrAlY ferroalloy bulk material is mainly composed of Fe-Cr, FeAl and Fe2AlCr phases, with an average Vickers hardness of 2.08±0.05GPa, a flexural strength of 1004±20MPa, and a compressive strength greater than 3700MPa.
[0094] Matrix material comparative example 2
[0095] This comparative example provides a method for preparing a FeCrAlY ferroalloy bulk material, comprising the following steps:
[0096] FeCrAlY ferroalloy powder with a mass ratio of Fe, Cr, Al and Y elements of 81.8:13:5:0.2 was placed in a Φ52mm graphite mold, and then moved to a vacuum hot pressing sintering furnace. The temperature was raised to 700°C at a heating rate of 10°C / min, and the sintering pressure was applied. When the temperature rose to the sintering temperature of 1200°C, the pressure increased to 25MPa. After keeping the temperature and pressure for 5 minutes, the powder was cooled to room temperature with the furnace to obtain a FeCrAlY ferroalloy block material.
[0097] X-ray diffraction analysis showed that the prepared bulk material was mainly composed of Fe-Cr, FeAl and Fe2AlCr phases, with an average Vickers hardness of 3.18±0.14GPa, a flexural strength of 791±160MPa and a compressive strength greater than 3700MPa.
[0098] Results
[0099] Vickers hardness: The mechanical properties of the materials obtained in the examples and comparative examples were tested in different directions; the hardness of the obtained materials was tested using a Vickers hardness tester, and the test conditions were: loading load 300g, loading duration 10s; the results of Examples 1 to 4 are shown in Table 2; Among them, the hardness test results of Examples 1 to 3 are shown in Table 2. Figure 2 shown.
[0100] Compressive strength: The compressive strength of the materials obtained in the examples and comparative examples was tested using a universal material testing machine; the results of Examples 1 to 4 are shown in Table 3; wherein the test results of Examples 1 to 3 are shown in Table Figure 3 shown.
[0101] Tribological properties: The iron-based alloy friction materials obtained in Examples 1 to 3 were subjected to tribological properties tests at room temperature and 300°C and dynamic tribological properties tests from room temperature to 300°C using a GF-I reciprocating friction and wear tester; the test conditions were: load 75N, frequency 5Hz, amplitude 1mm; friction pair: SA508Gr.3Cl.2 steel, Φ2mm surface contact; in the dynamic friction performance test, the heating rate was 10°C / min; the average friction coefficient obtained by the test was as follows: Figure 4 The wear rates are shown in Table 4.
[0102] Table 2 Vickers hardness of iron-based alloy friction materials of Examples 1 to 4
[0103] Axial Vickers hardness / GPa Radial Vickers hardness / GPa Example 1 3.39 3.50 Example 2 5.04 5.58 Example 3 5.57 5.54 Example 4 3.76 4.75
[0104] It can be seen from Table 2 above that with the increase of TiC content, the Vickers hardness first increases and then tends to be stable, indicating that the present invention is beneficial to improving the mechanical properties of the material by adjusting the mass content of alloy and TiC in the iron-based alloy friction material. At the same time, it can also be seen from the comparison between Example 4 and Example 2 that the change of TiC particle size will also lead to a change in Vickers hardness, indicating that adjusting the TiC particle size is also beneficial to improving the mechanical strength.
[0105] Table 3 Compressive strength of iron-based alloy friction materials of Examples 1 to 4
[0106] Axial compressive strength / MPa Radial compressive strength / MPa Example 1 1127 1216 Example 2 1221 1341 Example 3 1468 1308 Example 4 1168 1579
[0107] The results in Table 3 show that the iron-based alloy friction material of the present invention has excellent compressive strength, but changes in the TiC content and TiC particle size will also cause changes in the compressive strength.
[0108] Table 4 Wear rate of iron-based alloy friction materials of Examples 1 to 3 (10 -5 mm 3 / N·m)
[0109] FeCrAlY-15TiC FeCrAlY-25TiC FeCrAlY-35TiC Room temperature 1.98±0.36 2.55±0.53 1.61±0.62 300℃ 1.01±0.32 1.16±0.45 1.38±0.65 Dynamic from room temperature to 300℃ 2.05±0.61 2.99±0.76 1.44±0.65
[0110] It can be seen from Table 4 that the iron-based alloy friction material obtained by the present invention has a low wear rate at both room temperature and 300°C, and the change in wear rate under the dynamic heating condition from room temperature to 300°C does not exceed 0.7×10 -5 mm 3 / N·m, good stability, able to adapt to high and low temperature alternating conditions. Figure 2 and Figure 3 It can be seen from the results that the iron-based alloy friction material of the present invention also has excellent mechanical properties, achieving compatibility between mechanical properties and tribological properties.
[0111] In addition, it can be seen from the matrix material comparative examples 1 and 2 that changes in the ratio of each element in the matrix material, ie, the alloy material, will lead to changes in the mechanical strength of the alloy itself.
[0112] Figure 1 The X-ray diffraction spectra of the iron-based alloy friction materials of Examples 1 to 3 of the present invention are obtained by performing X-ray diffraction analysis on the materials prepared in Examples 1 to 3. Figure 1 As shown, the physical phase of the iron-based alloy friction material prepared by the present invention is mainly composed of Fe-Cr, FeAl, Fe2AlCr matrix phase and TiC phase, wherein Y is a trace element added, and the added amount is small and difficult to measure.
[0113] Figure 2 The Vickers microhardness diagram of the iron-based alloy friction material of Examples 1 to 3 of the present invention. Figure 2 It can be seen that the iron-based alloy friction material obtained by the present invention has excellent hardness, and both the axial Vickers hardness and the radial Vickers hardness are not less than 3 GPa.
[0114] Figure 3 The compressive strength diagram of the iron-based alloy friction material of Examples 1 to 3 of the present invention. Figure 3 It can be seen that the iron-based alloy friction material obtained by the present invention has excellent compressive strength, and the compressive strength is not less than 1100 MPa.
[0115] Figure 4 The average friction coefficient of the iron-based alloy friction material of Examples 1 to 3 of the present invention is shown in FIG. Figure 4 It can be seen that the iron-based alloy friction material obtained by the present invention has a small friction coefficient and good stability. Under dynamic heating conditions from room temperature to 300°C, the average friction coefficient changes less than that at room temperature. Among them, when the TiC content is 15wt%, the average friction coefficient hardly changes.
[0116] Combination Figure 2 to Figure 4 From the test results, it can be seen that the iron-based alloy friction material obtained by the present invention not only has excellent mechanical properties, but also has good tribological properties, a moderate friction coefficient and a low wear rate, high wear resistance, and can maintain stable tribological properties under dynamic heating conditions from room temperature to 300°C, with high stability.
[0117] In summary, the iron-based alloy friction material of the present invention is an iron-based alloy self-lubricating friction material, which has isotropic mechanical properties, a stable friction coefficient under different temperature conditions, good self-lubricating properties and wear resistance, a low wear rate at room temperature and a high temperature of 300°C, and the wear rate variation under the dynamic temperature increase condition from room temperature to 300°C does not exceed 0.7×10 -5 mm 3 / N·m; at the same time, the iron-based alloy friction material has excellent mechanical strength. It can be seen that the iron-based alloy friction material of the present invention achieves compatibility between mechanical properties and tribological properties.
[0118] The iron-based alloy friction material of the present invention can be used as a structural material. Its excellent mechanical properties and tribological properties enable it to be used in the preparation of mechanical moving parts. The obtained mechanical moving parts include but are not limited to shafts, bearings, gears, transmission shafts, couplings, clutches, brakes, etc. These mechanical moving parts, or the iron-based alloy friction materials or structural materials used to prepare these mechanical moving parts in the present invention, are particularly suitable for serving under high load, low speed, high impact stress and high and low temperature alternating working conditions.
[0119] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. An iron-based alloy friction material, characterized in that: The invention comprises FeCrAlY alloy with a mass fraction of 65 to 85% and TiC with a mass fraction of 15 to 35%.
2. The iron-based alloy friction material according to claim 1, characterized in that: The mass ratio of Fe, Cr, Al and Y elements in the FeCrAlY alloy is (75-85):(10-20):(5-10):(0.1-1).
3. The iron-based alloy friction material according to claim 1 or 2, characterized in that: The average particle size of the TiC is 35 to 55 nm.
4. The iron-based alloy friction material according to claim 1 or 2, characterized in that: The average particle size of the FeCrAlY alloy is 200-300 meshes.
5. A method for preparing the iron-based alloy friction material according to any one of claims 1 to 4, characterized in that: The steps include: The FeCrAlY alloy and TiC are mixed, ball-milled, and then sintered to obtain an iron-based alloy friction material.
6. The preparation method according to claim 5, characterized in that: The diameter of the grinding balls of the ball mill is 3 to 10 mm; And / or, the ball-to-material ratio of the ball mill is 1:(1-2).
7. The preparation method according to claim 5 or 6, characterized in that: The rotation speed of the ball mill is 200-400 r / min; And / or, the ball milling time is 8 to 10 hours.
8. The preparation method according to claim 5, characterized in that: The sintering temperature is 1300-1400°C; And / or, the sintering pressure is 25-35 MPa; and / or, the sintering heating rate is 10-15° C. / min.
9. A structural material, characterized in that: The invention comprises the iron-based alloy friction material as described in any one of claims 1 to 4, or the iron-based alloy friction material obtained by the preparation method as described in any one of claims 5 to 8.
10. A mechanical moving part, characterized in that: It comprises the iron-based alloy friction material according to any one of claims 1 to 4 or the structural material according to claim 9.