Preparation method of (ZrTi) C reinforced titanium alloy compound gear

By preparing (ZrTi)C enhanced composite layer on the surface of titanium alloy gear, the problems of high friction coefficient and poor interface bonding of titanium alloy gear are solved, the friction coefficient and wear resistance are reduced, and the composite layer and substrate are ensured. Stable combination.

CN118957577AActive Publication Date: 2024-11-15XIAN UNIV OF TECH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411021674.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The friction coefficient of existing titanium alloy gears is large, resulting in low transmission efficiency and insufficient wear resistance, and poor bonding between the composite layer and the substrate interface, making it easy to crack or detach.

Method used

Using the preparation method of (ZrTi)C enhanced titanium alloy composite gear, carbonization is formed by sandpaper removal of oxide layer, ultrasonic cleaning, automatic wire feeding arc clad zirconium titanium alloy coating, hot forging, fine forging, solid solution treatment and gas carburizing. The layer is formed to form a composite carbide layer and a zirconium titanium cladding layer to improve the interface bonding strength.

Benefits of technology

The friction coefficient of titanium alloy gear is significantly reduced to 0.08~0.1, the wear resistance and stability of the gear are improved, the good combination of the composite layer and the substrate are ensured, and the service life of the gear is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957577A_ABST
    Figure CN118957577A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a (ZrTi) C reinforced titanium alloy compound gear, which comprises the following steps: cladding a zirconium-titanium alloy coating on the cylindrical side surface of a titanium alloy, then carrying out hot forging processing to form a gear blank with a required shape, then carrying out precision forging and solid solution treatment on the gear blank, placing the forged gear in a gas carburizing furnace, carburizing by taking acetylene gas as a carbon source, and carrying out high-temperature sintering to obtain the (ZrTi) C reinforced titanium alloy compound gear. The preparation method comprises the following steps: preparing a zirconium-titanium alloy cladding layer, forming a carbonized layer on the surface of the zirconium-titanium alloy cladding layer to obtain a carbide-titanium alloy gear taking the (ZrTi) C carburized layer and the zirconium-titanium alloy cladding layer as tooth surfaces, cleaning, finishing and polishing the tooth surfaces to obtain the (ZrTi) C reinforced titanium alloy compound gear, and forming a layered gradient structure of a complex-phase carbide layer, the zirconium-titanium cladding layer and a matrix from outside to inside of the gear. The complex-phase carbide (ZrTi) C and the zirconium-titanium alloy cladding layer as well as the cladding layer and the matrix have good bonding interfaces, so that the use stability of the titanium alloy gear under different working conditions is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of gear materials and relates to a method for preparing a (ZrTi)C reinforced titanium alloy composite gear. Background Art

[0002] With the development of lightweight military electronic equipment, the weight reduction requirements of servo transmission mechanisms are getting higher and higher. Using titanium alloy gears to replace steel alloy gears can achieve a weight reduction of about 60%, effectively reducing the quality of the mechanical system and improving the performance and efficiency of the system. In terms of performance, titanium alloy gears can meet the product index requirements, but the friction coefficient of titanium alloy is relatively large (0.6-0.8), and the gear transmission efficiency is low, resulting in large friction losses and even functional failure. Therefore, reducing the surface friction coefficient of titanium alloy gears is an urgent problem to be solved in the application engineering of titanium alloy gears.

[0003] The main strategy to reduce the friction coefficient of the titanium alloy gear surface is to prepare a composite material, that is, to add a layer of low friction coefficient material to the surface of the titanium alloy gear. For example, the Chinese patent with publication number CN113981441B discloses a method for preparing a gear surface coating, which uses an ultra-high-speed laser cladding method to form a surface iron-based coating on the surface of a nickel-based gear, greatly improving the wear resistance of the gear surface. The Chinese patent with publication number CN116100267A discloses a method for preparing a lightweight and wear-resistant titanium alloy gear, which improves the wear resistance of the titanium alloy gear by cladding a layer of alloy steel coating on the titanium alloy gear blank and directly processing the cladding layer into the tooth surface. The Chinese patent with publication number CN114231898A discloses a method for depositing a carbon-based film on the tooth surface by magnetron sputtering to form a low-friction-coefficient, wear-resistant carbon-based film modified layer on the surface of the titanium alloy gear. The Chinese patent with publication number CN109295343A discloses that a mixed powder (titanium powder, nickel powder, titanium carbide powder) is clad on the surface of a titanium alloy gear to prepare a hardened layer with good wear resistance and low friction coefficient on the gear surface.

[0004] As can be seen from the above, the preparation of composite gears is a feasible method to reduce the friction coefficient, but for titanium alloy gears, the bonding force between the composite layer and the tooth surface (blank) must be considered, otherwise the composite layer will experience interface cracking, peeling and other phenomena during service. For example, during the steel / iron-titanium composite process, due to the large difference in the thermal physical properties of the interface and the metallurgical reaction that easily forms hard and brittle intermetallic compounds, the composite layer is very easy to crack and fail; although the sputtering method can avoid the generation of brittle phases on the tooth surface, the film and the substrate are mechanically bonded and easily separated, and the coating thickness is too thin to serve for a long time; cladding the titanium alloy gear tooth surface with a mixed powder of an appropriate system can improve the wear resistance of the tooth surface, but powder cladding is prone to produce defects such as pore inclusions, resulting in poor density of the composite layer, which will greatly reduce the wear resistance of the tooth surface. How to reduce the friction coefficient of the titanium alloy gear tooth surface and ensure sufficient thickness and excellent interface bonding is a technical problem that urgently needs to be solved. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a (ZrTi)C reinforced titanium alloy composite gear, which solves the problems of high friction coefficient and poor interface bonding between the matrix and the composite layer of the titanium alloy composite gear prepared by the existing method.

[0006] The technical solution adopted by the present invention is a method for preparing a (ZrTi)C reinforced titanium alloy composite gear, comprising the following steps:

[0007] Step 1, using sandpaper to remove the oxide layer on the surface of the titanium alloy cylinder, and then ultrasonically cleaning it in an ethanol solution and drying it;

[0008] Step 2, using automatic wire feeding arc cladding equipment to clad a zirconium-titanium alloy coating on the side of the titanium alloy cylinder to obtain a titanium alloy prefabricated gear blank, and the thickness of the cladding layer exceeds the full tooth height of the titanium alloy gear blank by 3 mm to 5 mm;

[0009] Step 3, hot forging the titanium alloy prefabricated gear blank at 800-880° C. to form a gear blank of a desired shape;

[0010] Step 4, performing precision forging at 900-980° C. on the gear blank, and then performing solid solution treatment to obtain a forged gear;

[0011] Step 5, placing the forged gear in a gas carburizing furnace, using acetylene gas as a carbon source for carburizing, and forming a carbide layer with a thickness of 100 μm to 200 μm on the surface of the zirconium-titanium alloy cladding layer, that is, obtaining a carbide-titanium alloy gear with a (ZrTi)C carburized layer and a zirconium-titanium alloy cladding layer as the tooth surface;

[0012] Step 6, cleaning and finishing the carbide-titanium alloy gear, and polishing the tooth surface to obtain a (ZrTi)C reinforced titanium alloy composite gear.

[0013] In step 2, the power of arc cladding is 10-18 kW, the arc column diameter is 3-7 mm, the wire feeding method is side wire feeding, the wire material is pure zirconium wire or zirconium-titanium alloy wire, the wire diameter is 0.8 mm-4 mm, the wire feeding speed is 50-80 mm / s, the scanning speed is 20-50 mm / s, argon is used as the shielding gas, and the shielding gas flow rate is 25-35 SCFH.

[0014] The zirconium content in the zirconium-titanium alloy wire is ≥40wt.%.

[0015] In step 4, solution treatment is performed, including placing the finely forged gear blank into an atmosphere heating furnace, raising the furnace temperature to 680-880°C, keeping the temperature for 2 hours, and then cooling to room temperature at a cooling rate of 80-120°C / min.

[0016] In step 5, before placing the forged gear in the gas carburizing furnace, the non-tooth part is first coated with an anti-seepage coating, and after the coating material is dried in the shade for 20h-24h, the forged gear is placed in the gas carburizing furnace.

[0017] In step 5, carburizing is performed using acetylene gas as a carbon source, the carburizing temperature is 850-1050°C, the holding time is 1h-6h, the carbon potential is controlled at 0.4-0.6 during the holding stage, and the heating rate is 5-10°C / min.

[0018] In step 6, the tooth surface is polished to a surface roughness of Ra=0.020.

[0019] The material of the titanium alloy cylinder is Ti6Al4V.

[0020] The titanium alloy prefabricated gear blank is hot forged at 800-880°C, and the forging ratio is 1.2-1.3.

[0021] The gear blank is finely forged at 900-980°C, with a forging ratio of 1.1-1.2.

[0022] The beneficial effects of the present invention are as follows:

[0023] (1) A composite wear-resistant layer was prepared on the surface of titanium alloy gears by arc cladding and gas carburizing methods, forming a layered gradient structure of complex phase carbide layer → zirconium-titanium cladding layer → substrate from the outside to the inside. The complex phase carbide (ZrTi)C and the zirconium-titanium alloy cladding layer and the cladding layer and the substrate had a good bonding interface, which improved the stability of titanium alloy gears under different working conditions.

[0024] (2) Hot forging is used to form the gears. Compared with machined gears, the streamline characteristics of the material are greatly retained. The existence of streamlines makes the grain arrangement inside the gears more uniform, and the crystal direction is consistent with the stress direction, which improves the toughness of the gears. In the temperature range of the solution treatment, the cladding layer undergoes a β phase transformation, and combined with rapid cooling treatment, the solid solution ratio of zirconium and titanium elements is increased, which improves the preparation efficiency of the subsequent (ZrTi)C carburized layer.

[0025] (3) The friction coefficient of the (ZrTi)C reinforced titanium alloy composite gear prepared by the present invention can be reduced to 0.08-0.1, which significantly improves the wear resistance of the titanium alloy gear. The thickness of the carbide layer is 100-200 μm, which meets the use requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the internal structure of the (ZrTi)C reinforced titanium alloy composite gear in the present invention;

[0027] Figure 2 is a SEM image of the transition zone between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer in Example 2 of the present invention;

[0028] Figure 3 This is a SEM image of the transition zone between the zirconium-titanium alloy cladding layer and the titanium alloy substrate in Example 2 of the present invention.

[0029] In the figure, 1. titanium alloy substrate, 2. zirconium-titanium alloy cladding layer, 3. (ZrTi)C carburized layer. DETAILED DESCRIPTION

[0030] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0031] The method for preparing the (ZrTi)C reinforced titanium alloy composite gear of the present invention comprises the following steps:

[0032] Step 1, using sandpaper to remove the oxide layer on the surface of the Ti6Al4V titanium alloy cylinder, and then ultrasonically cleaning it in an ethanol solution and drying it;

[0033] Step 2, using automatic wire feeding arc cladding equipment to clad the zirconium-titanium alloy coating on the side of the titanium alloy cylinder, the arc cladding power is 10-18kW, the arc column diameter is 3-7mm, and the side wire feeding method is adopted. The wire material is pure zirconium wire or zirconium-titanium alloy wire, the zirconium content in the zirconium-titanium alloy wire is ≥40wt.%, the wire diameter is 0.8mm-4mm, the wire feeding speed is 50-80mm / s, the scanning speed is 20-50mm / s, argon is used as the protective gas, and the protective gas flow rate is 25-35SCFH, and finally a titanium alloy prefabricated gear blank is obtained, and the thickness of the cladding layer exceeds the full tooth height of the titanium alloy gear blank by 3mm-5mm;

[0034] Step 3, placing the titanium alloy prefabricated gear blank in a heating furnace, heating it to 800-880° C. and keeping it warm for 1-2 hours, taking it out after the end of the heat preservation, placing it in the initial forging die, and using a hydraulic press for hot forging, with the forging ratio controlled between 1.2 and 1.3, and air cooling after forging to obtain the gear blank of the desired shape;

[0035] Step 4, heating the gear blank to 900-980°C and keeping it warm for 1h-2h, taking it out after the heat preservation, putting it into the precision forging die, and using a hydraulic press for hot forging, controlling the forging ratio between 1.1 and 1.2, air cooling after forging to obtain a precision forged gear, and then performing a solid solution treatment, including placing the precision forged gear blank into an atmosphere heating furnace, raising the furnace temperature to 680-880°C, keeping it warm for 2h, and then cooling it to room temperature at a cooling rate of 80-120°C / min to obtain a forged gear;

[0036] Step 5, first use an anti-seepage coating to coat the non-tooth part for anti-seepage treatment, the anti-seepage coating is AC100 water-soluble anti-seepage coating, after the coating material is dried in the shade for 20h-24h, the forged gear is placed in a gas carburizing furnace, and acetylene gas is used as a carbon source for carburizing, the carburizing temperature is 850-1050°C, the holding time is 1h-6h, the carbon potential is controlled at 0.4-0.6 during the holding stage, the heating rate is 5-10°C / min, and a carbide layer with a thickness of 100μm-200μm is formed on the surface of the zirconium-titanium alloy cladding layer, that is, a carbide-titanium alloy gear with a (ZrTi)C carburized layer and a zirconium-titanium alloy cladding layer as the tooth surface is obtained;

[0037] Step 6: Clean and finish the carbide-titanium alloy gear, and polish the tooth surface to a surface roughness of Ra=0.020, thereby obtaining a (ZrTi)C reinforced titanium alloy composite gear.

[0038] See also Figure 1 The (ZrTi)C reinforced titanium alloy composite gear consists of a titanium alloy substrate 1, a zirconium-titanium alloy cladding layer 2 and a (ZrTi)C carburized layer 3.

[0039] Example 1

[0040] A method for preparing a (ZrTi)C reinforced titanium alloy composite gear comprises the following steps:

[0041] Step 1, select a Ti6Al4V titanium alloy cylinder with a cross-sectional diameter of 20 mm and a height of 10 mm as a substrate, polish it step by step with sandpaper to 1000 mesh to remove the oxide layer on the surface of the Ti6Al4V titanium alloy cylinder, then put it into an ethanol solution for ultrasonic cleaning for 30 minutes and then dry it;

[0042] Step 2, use automatic wire feeding arc cladding equipment to uniformly clad the zirconium-titanium alloy coating on the side of the titanium alloy cylinder, the arc cladding power is 10kW, the arc column diameter is 3mm, the wire feeding method is side wire feeding, the wire material is pure zirconium wire, the wire diameter is 0.8mm, the wire feeding speed is 50mm / s, the scanning speed is 20mm / s, argon is used as the shielding gas, and the shielding gas flow rate is 25SCFH. Finally, a titanium alloy prefabricated gear blank is obtained, and the thickness of the cladding layer on the surface of the titanium alloy prefabricated gear blank exceeds the full tooth height of the titanium alloy gear blank by 3mm.

[0043] Step 3, placing the titanium alloy prefabricated gear blank in a heating furnace and heating it to 800° C. for 1 hour, taking it out after the end of the heat preservation, placing it in the initial forging die, and using a hydraulic press for hot forging, with the forging ratio controlled between 1.2 and 1.3, and air cooling after forging to obtain the gear blank of the desired shape;

[0044] Step 4, heating the gear blank to 900°C and keeping it for 1 hour, taking it out after the heat preservation, putting it into the precision forging die and using a hydraulic press for hot forging, controlling the forging ratio between 1.1 and 1.2, air cooling after forging to obtain a precision forged gear, and then performing a solid solution treatment, including placing the precision forged gear blank into an atmosphere heating furnace, raising the furnace temperature to 880°C, keeping it for 2 hours, and then cooling it to room temperature at a cooling rate of 80°C / min, to obtain a forged gear;

[0045] Step 5, first use an anti-seepage coating to coat the non-tooth part for anti-seepage treatment, after the coating material is dried in the shade for 20 hours, the forged gear is placed in a gas carburizing furnace, carburized with acetylene gas as the carbon source, and the furnace temperature is raised to 850°C at 8°C / min, and kept warm for 1 hour. The carbon potential is controlled at 0.4 during the insulation stage, and a carbide-titanium alloy gear with a (ZrTi)C carburized layer and a zirconium-titanium alloy cladding layer as the tooth surface is obtained;

[0046] Step 6: Clean and finish the carbide-titanium alloy gear, and polish the tooth surface to a surface roughness of Ra=0.020, thereby obtaining a (ZrTi)C reinforced titanium alloy composite gear.

[0047] The microstructure of the (ZrTi)C reinforced titanium alloy composite gear prepared in Example 1 was observed. The thickness of the zirconium-titanium alloy cladding layer on the surface of the titanium alloy substrate was about 8 mm, and the thickness of the (ZrTi)C carburized layer on the surface of the cladding layer was about 100 μm. The mechanical properties of the (ZrTi)C reinforced titanium alloy composite gear were tested, and the tooth surface friction coefficient was 0.1.

[0048] Example 2

[0049] A method for preparing a (ZrTi)C reinforced titanium alloy composite gear comprises the following steps:

[0050] Step 1, select a Ti6Al4V titanium alloy cylinder with a cross-sectional diameter of 40 mm and a height of 20 mm as a substrate, polish it step by step with sandpaper to 1000 mesh to remove the oxide layer on the surface of the Ti6Al4V titanium alloy cylinder, then put it into an ethanol solution for ultrasonic cleaning for 30 minutes and then dry it;

[0051] Step 2, use automatic wire feeding arc cladding equipment to uniformly clad the zirconium-titanium alloy coating on the side of the titanium alloy cylinder, the arc cladding power is 12kW, the arc column diameter is 4mm, the wire feeding method is side wire feeding, the wire material is Zr50Ti50 wire, the wire diameter is 1mm, the wire feeding speed is 55mm / s, the scanning speed is 25mm / s, argon is used as the shielding gas, and the shielding gas flow rate is 27SCFH. Finally, a titanium alloy prefabricated gear blank is obtained, and the thickness of the cladding layer on the surface of the titanium alloy prefabricated gear blank exceeds the full tooth height of the titanium alloy gear blank by 4mm.

[0052] Step 3, placing the titanium alloy prefabricated gear blank in a heating furnace, heating it to 820° C. and keeping it warm for 1.5 hours, taking it out after the end of the heat preservation, placing it in the initial forging die, and using a hydraulic press for hot forging, with the forging ratio controlled between 1.2 and 1.3, and air cooling after forging to obtain the gear blank of the desired shape;

[0053] Step 4, heating the gear blank to 920°C and keeping it warm for 1.5 hours, taking it out after the heat preservation, putting it into the precision forging die, and using a hydraulic press for hot forging, controlling the forging ratio between 1.1 and 1.2, air cooling after forging to obtain a precision forged gear, and then performing a solid solution treatment, including placing the precision forged gear blank into an atmosphere heating furnace, raising the furnace temperature to 850°C, keeping it warm for 2 hours, and then cooling it to room temperature at a cooling rate of 90°C / min, to obtain a forged gear;

[0054] Step 5, first use an anti-seepage coating to coat the non-tooth part for anti-seepage treatment, after the coating material is dried in the shade for 24 hours, the forged gear is placed in a gas carburizing furnace, carburized with acetylene gas as the carbon source, and the furnace temperature is raised to 900°C at 8°C / min, and kept warm for 2 hours. The carbon potential is controlled at 0.4 during the insulation stage, and a carbide-titanium alloy gear with a (ZrTi)C carburized layer and a zirconium-titanium alloy cladding layer as the tooth surface is obtained;

[0055] Step 6: Clean and finish the carbide-titanium alloy gear, and polish the tooth surface to a surface roughness of Ra=0.020, thereby obtaining a (ZrTi)C reinforced titanium alloy composite gear.

[0056] The microstructure of the (ZrTi)C reinforced titanium alloy composite gear prepared in Example 2 was observed. Figure 2 This is the SEM image of the transition zone between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer. Figure 3 This is the SEM image of the transition zone between the zirconium-titanium alloy cladding layer and the titanium alloy substrate. Figure 2 and Figure 3 It can be seen that the (ZrTi)C reinforced titanium alloy composite gear prepared by the method of the present invention has a dense structure, the zirconium-titanium alloy cladding layer and the titanium alloy substrate have a good interface bond, and a dense transition zone is formed between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer, which greatly improves the interface bonding strength between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer. The thickness of the zirconium-titanium alloy cladding layer in the (ZrTi)C reinforced titanium alloy composite gear is about 12mm, and the thickness of the (ZrTi)C carburized layer is about 135μm. The mechanical properties of the (ZrTi)C reinforced titanium alloy composite gear are tested, and the tooth surface friction coefficient is 0.092.

[0057] Example 3

[0058] A method for preparing a (ZrTi)C reinforced titanium alloy composite gear comprises the following steps:

[0059] Step 1, select a Ti6Al4V titanium alloy cylinder with a cross-sectional diameter of 60 mm and a height of 30 mm as a substrate, polish it step by step with sandpaper to 1000 mesh to remove the oxide layer on the surface of the Ti6Al4V titanium alloy cylinder, then put it into an ethanol solution for ultrasonic cleaning for 30 minutes and then dry it;

[0060] Step 2, use automatic wire feeding arc cladding equipment to uniformly clad the zirconium-titanium alloy coating on the side of the titanium alloy cylinder, the arc cladding power is 14kW, the arc column diameter is 5mm, the wire feeding method is side wire feeding, the wire material is Zr60Ti40 wire, the wire diameter is 2mm, the wire feeding speed is 60mm / s, the scanning speed is 30mm / s, argon is used as the shielding gas, the shielding gas flow rate is 29SCFH, and finally a titanium alloy prefabricated gear blank is obtained. The thickness of the cladding layer on the surface of the titanium alloy prefabricated gear blank exceeds the full tooth height of the titanium alloy gear blank by 4mm.

[0061] Step 3, placing the titanium alloy prefabricated gear blank in a heating furnace, heating it to 840° C. and keeping it warm for 1.2 hours, taking it out after the end of the heat preservation, placing it in the initial forging die, and using a hydraulic press for hot forging, with the forging ratio controlled between 1.2 and 1.3, and air cooling after forging to obtain the gear blank of the desired shape;

[0062] Step 4, heating the gear blank to 940°C and keeping it warm for 1.6 hours, taking it out after the end of the heat preservation, putting it into the precision forging die, using a hydraulic press for hot forging, controlling the forging ratio between 1.1 and 1.2, air cooling after forging to obtain a precision forged gear, and then performing a solid solution treatment, including placing the precision forged gear blank into an atmosphere heating furnace, raising the furnace temperature to 800°C, keeping it warm for 2 hours, and then cooling it to room temperature at a cooling rate of 100°C / min, to obtain a forged gear;

[0063] Step 5, first use an anti-seepage coating to coat the non-tooth part for anti-seepage treatment, after the coating material is dried in the shade for 22 hours, the forged gear is placed in a gas carburizing furnace, carburized with acetylene gas as the carbon source, and the furnace temperature is raised to 950°C at 5°C / min, and kept warm for 4 hours. The carbon potential is controlled at 0.5 during the insulation stage, and a carbide-titanium alloy gear with a (ZrTi)C carburized layer and a zirconium-titanium alloy cladding layer as the tooth surface is obtained;

[0064] Step 6: Clean and finish the carbide-titanium alloy gear, and polish the tooth surface to a surface roughness of Ra=0.020, thereby obtaining a (ZrTi)C reinforced titanium alloy composite gear.

[0065] The microstructure of the (ZrTi)C reinforced titanium alloy composite gear prepared in Example 3 was observed, and it was found that the interface between the zirconium-titanium alloy cladding layer and the titanium alloy substrate was well bonded, and a dense transition zone was formed between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer, which improved the interface bonding strength between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer. The thickness of the zirconium-titanium alloy cladding layer in the (ZrTi)C reinforced titanium alloy composite gear was about 14 mm, and the thickness of the (ZrTi)C carburized layer was about 165 μm. The mechanical properties of the (ZrTi)C reinforced titanium alloy composite gear were tested, and the tooth surface friction coefficient was 0.09.

[0066] Example 4

[0067] A method for preparing a (ZrTi)C reinforced titanium alloy composite gear comprises the following steps:

[0068] Step 1, select a Ti6Al4V titanium alloy cylinder with a cross-sectional diameter of 80 mm and a height of 40 mm as a substrate, polish it step by step with sandpaper to 1000 mesh to remove the oxide layer on the surface of the Ti6Al4V titanium alloy cylinder, then put it into an ethanol solution for ultrasonic cleaning for 30 minutes and then dry it;

[0069] Step 2, use automatic wire feeding arc cladding equipment to uniformly clad the zirconium-titanium alloy coating on the side of the titanium alloy cylinder, the arc cladding power is 16kW, the arc column diameter is 6mm, the wire feeding method is side wire feeding, the wire material is Zr70Ti30 wire, the wire diameter is 3mm, the wire feeding speed is 65mm / s, the scanning speed is 35mm / s, argon is used as the shielding gas, the shielding gas flow rate is 28SCFH, and finally a titanium alloy prefabricated gear blank is obtained. The thickness of the cladding layer on the surface of the titanium alloy prefabricated gear blank exceeds the full tooth height of the titanium alloy gear blank by 4mm.

[0070] Step 3, placing the titanium alloy prefabricated gear blank in a heating furnace, heating it to 860° C. and keeping it warm for 1.8 hours, taking it out after the end of the heat preservation, placing it in the initial forging die, and using a hydraulic press for hot forging, with the forging ratio controlled between 1.2 and 1.3, and air cooling after forging to obtain the gear blank of the desired shape;

[0071] Step 4, heating the gear blank to 960°C and keeping it warm for 1.8 hours, taking it out after the end of the heat preservation, putting it into the precision forging die, and using a hydraulic press for hot forging, the forging ratio is controlled between 1.1 and 1.2, and air cooling after forging to obtain a precision forged gear, and then performing a solid solution treatment, including placing the precision forged gear blank into an atmosphere heating furnace, raising the furnace temperature to 750°C, keeping it warm for 2 hours, and then cooling it to room temperature at a cooling rate of 110°C / min, so as to obtain a forged gear;

[0072] Step 5, first use an anti-seepage coating to coat the non-tooth part for anti-seepage treatment, after the coating material is dried in the shade for 23 hours, the forged gear is placed in a gas carburizing furnace, carburized with acetylene gas as the carbon source, and the furnace temperature is raised to 1000°C at 9°C / min, and kept warm for 5 hours. The carbon potential is controlled at 0.6 during the insulation stage, and a carbide-titanium alloy gear with a (ZrTi)C carburized layer and a zirconium-titanium alloy cladding layer as the tooth surface is obtained;

[0073] Step 6: Clean and finish the carbide-titanium alloy gear, and polish the tooth surface to a surface roughness of Ra=0.020, thereby obtaining a (ZrTi)C reinforced titanium alloy composite gear.

[0074] The microstructure of the (ZrTi)C reinforced titanium alloy composite gear prepared in Example 4 was observed, and it was found that the interface between the zirconium-titanium alloy cladding layer and the titanium alloy substrate was well bonded, and a dense transition zone was formed between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer, which improved the interface bonding strength between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer. The thickness of the zirconium-titanium alloy cladding layer in the (ZrTi)C reinforced titanium alloy composite gear was about 16 mm, and the thickness of the (ZrTi)C carburized layer was about 180 μm. The mechanical properties of the (ZrTi)C reinforced titanium alloy composite gear were tested, and the tooth surface friction coefficient was 0.085.

[0075] Example 5

[0076] A method for preparing a (ZrTi)C reinforced titanium alloy composite gear comprises the following steps:

[0077] Step 1, select a Ti6Al4V titanium alloy cylinder with a cross-sectional diameter of 100 mm and a height of 50 mm as a substrate, polish it step by step with sandpaper to 1000 mesh to remove the oxide layer on the surface of the Ti6Al4V titanium alloy cylinder, then put it into an ethanol solution for ultrasonic cleaning for 30 minutes and then dry it;

[0078] Step 2, use automatic wire feeding arc cladding equipment to uniformly clad the zirconium-titanium alloy coating on the side of the titanium alloy cylinder, the arc cladding power is 18kW, the arc column diameter is 7mm, the wire feeding method is side wire feeding, the wire material is Zr80Ti20 wire, the wire diameter is 4mm, the wire feeding speed is 70mm / s, the scanning speed is 40mm / s, and argon is used as the shielding gas and plasma gas. The shielding gas flow rate is 30SCFH, and the plasma gas flow rate is 2.0SCFH. Finally, a titanium alloy prefabricated gear blank is obtained, and the thickness of the cladding layer on the surface of the titanium alloy prefabricated gear blank exceeds the full tooth height of the titanium alloy gear blank by 5mm.

[0079] Step 3, placing the titanium alloy prefabricated gear blank in a heating furnace and heating it to 880° C. for 2 hours, taking it out after the end of the heat preservation, placing it in the initial forging die, and using a hydraulic press for hot forging, with the forging ratio controlled between 1.2 and 1.3, and air cooling after forging to obtain the gear blank of the desired shape;

[0080] Step 4, heating the gear blank to 980°C and keeping it for 2 hours, taking it out after the heat preservation, putting it into the precision forging die, and using a hydraulic press for hot forging, controlling the forging ratio between 1.1 and 1.2, air cooling after forging to obtain a precision forged gear, and then performing a solid solution treatment, including placing the precision forged gear blank into an atmosphere heating furnace, raising the furnace temperature to 680°C, keeping it for 2 hours, and then cooling it to room temperature at a cooling rate of 120°C / min, to obtain a forged gear;

[0081] Step 5, first use an anti-seepage coating to coat the non-tooth part for anti-seepage treatment, after the coating material is dried in the shade for 24 hours, the forged gear is placed in a gas carburizing furnace, carburized with acetylene gas as the carbon source, and the furnace temperature is raised to 1050°C at 10°C / min, and kept warm for 6 hours. The carbon potential is controlled at 0.6 during the insulation stage, and a carbide-titanium alloy gear with a (ZrTi)C carburized layer and a zirconium-titanium alloy cladding layer as the tooth surface is obtained;

[0082] Step 6: Clean and finish the carbide-titanium alloy gear, and polish the tooth surface to a surface roughness of Ra=0.020, thereby obtaining a (ZrTi)C reinforced titanium alloy composite gear.

[0083] The microstructure of the (ZrTi)C reinforced titanium alloy composite gear prepared in Example 5 was observed, and it was found that the interface between the zirconium-titanium alloy cladding layer and the titanium alloy substrate was well bonded, and a dense transition zone was formed between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer, which improved the interface bonding strength between the (ZrTi)C carburized layer and the zirconium-titanium alloy cladding layer. The thickness of the zirconium-titanium alloy cladding layer in the (ZrTi)C reinforced titanium alloy composite gear was about 20 mm, and the thickness of the (ZrTi)C carburized layer was about 200 μm. The mechanical properties of the (ZrTi)C reinforced titanium alloy composite gear were tested, and the tooth surface friction coefficient was 0.08.

Claims

1. A method for preparing a (ZrTi)C reinforced titanium alloy composite gear, characterized in that: The following steps are involved: Step 1, using sandpaper to remove the oxide layer on the surface of the titanium alloy cylinder, and then ultrasonically cleaning it in an ethanol solution and drying it; Step 2, using automatic wire feeding arc cladding equipment to clad a zirconium-titanium alloy layer on the side of the titanium alloy cylinder to obtain a titanium alloy prefabricated gear blank, and the thickness of the cladding layer exceeds the full tooth height of the titanium alloy gear blank by 3 mm to 5 mm; Step 3, hot forging the titanium alloy prefabricated gear blank at 800-880° C. to form a gear blank of a desired shape; Step 4, performing precision forging at 900-980° C. on the gear blank, and then performing solid solution treatment to obtain a forged gear; Step 5, placing the forged gear in a gas carburizing furnace, using acetylene gas as a carbon source for carburizing, and forming a carbide layer with a thickness of 100 μm to 200 μm on the surface of the zirconium-titanium alloy cladding layer, that is, obtaining a carbide-titanium alloy gear with a (ZrTi)C carburized layer and a zirconium-titanium alloy cladding layer as the tooth surface; Step 6, cleaning and finishing the carbide-titanium alloy gear, and polishing the tooth surface to obtain a (ZrTi)C reinforced titanium alloy composite gear.

2. The method for preparing a (ZrTi)C reinforced titanium alloy composite gear according to claim 1, characterized in that: In the step 2, the power of the arc cladding is 10-18 kW, the arc column diameter is 3-7 mm, the wire feeding method is side wire feeding, the wire material is pure zirconium wire or zirconium-titanium alloy wire, the wire diameter is 0.8 mm-4 mm, the wire feeding speed is 50-80 mm / s, the scanning speed is 20-50 mm / s, argon is used as the shielding gas, and the shielding gas flow rate is 25-35 SCFH.

3. The method for preparing a (ZrTi)C reinforced titanium alloy composite gear according to claim 2, characterized in that: The zirconium content in the zirconium-titanium alloy wire is ≥40wt.%.

4. The method for preparing a (ZrTi)C reinforced titanium alloy composite gear according to claim 3, characterized in that: In step 4, the solution treatment includes placing the finely forged gear blank into an atmosphere heating furnace, raising the furnace temperature to 680-880° C., keeping the temperature for 2 hours, and then cooling to room temperature at a cooling rate of 80-120° C. / min.

5. The method for preparing a (ZrTi)C reinforced titanium alloy composite gear according to claim 4, characterized in that: In step 5, before placing the forged gear in the gas carburizing furnace, the non-tooth part is first coated with an anti-seepage coating, and after the coating material is dried in the shade for 20h-24h, the forged gear is placed in the gas carburizing furnace.

6. The method for preparing a (ZrTi)C reinforced titanium alloy composite gear according to claim 5, characterized in that: In step 5, carburizing is performed using acetylene gas as a carbon source, the carburizing temperature is 850-1050° C., the holding time is 1 h-6 h, the carbon potential is controlled at 0.4-0.6 during the holding stage, and the heating rate is 5-10° C. / min.

7. The method for preparing a (ZrTi)C reinforced titanium alloy composite gear according to claim 1, characterized in that: In step 6, the tooth surface is polished to a surface roughness of Ra=0.

020.

8. The method for preparing a (ZrTi)C reinforced titanium alloy composite gear according to claim 1, characterized in that: The titanium alloy cylinder is made of Ti6Al4V.

9. The method for preparing a (ZrTi)C reinforced titanium alloy composite gear according to claim 1, characterized in that: The titanium alloy prefabricated gear blank is hot forged at 800-880° C., and the forging ratio is 1.2-1.

3.

10. The method for preparing a (ZrTi)C reinforced titanium alloy composite gear according to claim 9, characterized in that: The gear blank is finely forged at 900-980° C., with a forging ratio of 1.1-1.2.

Citation Information

Patent Citations

  • Titanium alloy gear and preparation method thereof

    CN109295343A

  • Preparation method of gear surface strengthening coating and gear

    CN113981441B

  • High-precision high-wear-resistance titanium alloy gear forming method

    CN114231898A

  • Preparation method of light wear-resistant titanium alloy gear

    CN116100267A

  • Gear machining process

    CN108607997A