Self-supporting CoP nanowire catalytic electrode, preparation method thereof and application of self-supporting CoP nanowire catalytic electrode in synthesis of 1, 2, 3, 4-tetrahydroquinoline through hydrogenation of electrocatalytic quinoline

By growing CoP nanowire catalytic electrodes on graphite felt, using electrochemical methods to achieve efficient hydrogenation conversion of quinoline under normal temperature and pressure, the problems of high temperature and high pressure and side reactions in the existing quinoline hydrogenation process were solved, and the problem of high temperature and high pressure and side reactions in the existing quinoline hydrogenation process was achieved. High selectivity and high conversion rate of quinoline electrocatalytic hydrogenation reaction.

CN118957636AActive Publication Date: 2024-11-15ZHEJIANG UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411290482.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-15
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

The existing quinoline hydrogenation process is carried out under high temperature and high pressure conditions, and there are problems such as many side reactions, poor product selectivity and low conversion rate. The electrochemical reduction hydrogenation method is harsh and complex in the reaction conditions, so additional organic matter is required.

Method used

A self-supported CoP nanowire catalytic electrode was designed, and graphite felt as a support was used to achieve efficient hydrogenation conversion of quinoline at room temperature and pressure by electrochemical methods. The H-type electrolytic cell, platinum electrode and Hg/HgO electrode were used. , the reaction is performed using constant voltage electrolysis method.

Benefits of technology

The high selectivity and high conversion rate of quinoline are achieved, the generation of by-products is avoided, the process is simple, the production cost is reduced, and good catalytic performance and industrial application prospects are shown.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005044429020000031
    Figure BDA0005044429020000031
  • Figure HDA0005044429030000011
    Figure HDA0005044429030000011
  • Figure HDA0005044429030000012
    Figure HDA0005044429030000012
Patent Text Reader

Abstract

The invention discloses a self-supporting CoP nanowire catalytic electrode, a preparation method thereof and application of electrocatalytic quinoline hydrogenation synthesis of 1, 2, 3, 4-tetrahydroquinoline, the self-supporting CoP nanowire catalytic electrode is composed of a carrier and an active component growing on the carrier, the carrier is graphite felt, and the active component is of a CoP nanowire structure; the preparation process of the electrode material is simple and convenient, the raw materials are low in price and easy to obtain, the electrode material has a very good industrial application prospect, the CoP nano material is very excellent in performance in electrolytic reaction, and the selectivity and the conversion rate of the CoP nano material are very ideal, which means that the material has a good application potential in many chemical reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic electrocatalytic synthesis, and specifically relates to a CoP nanowire catalytic electrode supported on graphite felt and a preparation method thereof, as well as application in the electrocatalytic hydrogenation of quinoline to synthesize 1,2,3,4-tetrahydroquinoline. Background Art

[0002] Nitrogen-containing heterocyclic compounds with high added value occupy an important position in the pharmaceutical and fine chemical fields. Most of these compounds are natural products with unique structures and properties, and can be synthesized artificially in a variety of ways. Quinoline and its derivatives are important components of nitrogen-containing heterocyclic compounds. One of its hydrogenation products, 1,2,3,4-tetrahydroquinoline, is an important pharmaceutical intermediate and has a wide range of applications in the synthesis of drugs with antibacterial activity, neuroprotectants and immunomodulators. And because 1,2,3,4-tetrahydroquinoline has a unique molecular structure with a chromophore with good electron-donating ability, it can be used as an important intermediate in the field of dye synthesis. In industrial production, 1,2,3,4-tetrahydroquinoline, as an important organic compound, is mainly prepared by chemical catalytic quinoline hydrogenation process. However, the reaction conditions of this process are very harsh, usually requiring an external hydrogen source, and being carried out under high temperature and high pressure conditions. In addition, the chemical catalytic quinoline hydrogenation reaction is usually not unidirectional, and there are many side reactions, poor product selectivity, and low conversion rate.

[0003] In order to solve these problems, electrochemical reduction hydrogenation has attracted people's attention in recent years as a very promising method. Compared with traditional chemical hydrogenation methods, electrochemical reduction hydrogenation is inherently more gentle and green, because it does not require the use of high-temperature and high-pressure containers, nor does it require an additional hydrogen source. Instead, it reduces the compounds through electron transfer to generate the desired products, reduces the occurrence of side reactions, improves product selectivity, and improves conversion rate and yield. Electrochemical synthesis methods also have many other advantages, such as easy separation of products, simple process flow, and easy automation. Therefore, electrochemical reduction hydrogenation is expected to become an important method for the industrial production of 1,2,3,4-tetrahydroquinoline in the future.

[0004] At present, some patent documents, such as CN117143015A, report the reaction example of thermal catalytic reduction of quinoline to generate 1,2,3,4-tetrahydroquinoline, and the product separation yield reaches 82%. However, the reaction conditions are harsh and multiple organic substances need to be added during the reaction. Considering the complexity of this process, we envision the synthesis of a new material that can effectively promote the activation of quinoline and water, and use it for electrochemical methods to achieve efficient and highly selective quinoline hydrogenation reactions.

[0005] Specifically, the structural design and preparation process of the new electrocatalytic material we envision synthesizing should ensure that it can effectively capture and transfer electrons during the electrochemical reaction, thereby promoting the hydrogenation reaction of quinoline. This new material should have high catalytic activity and be able to achieve efficient conversion of quinoline at room temperature and pressure while maintaining high selectivity. In the field of organic electrochemical synthesis, transition metals show many unique characteristics. In particular, in the electrochemical reduction process of nitrates and organic matter, Co-based catalysts have been widely studied due to their low cost and high stability. These catalysts can achieve efficient electron transfer in electrochemical reactions and promote the reaction. The application of Co-based catalysts in organic electrochemical synthesis lies not only in their catalytic performance, but also in their tunable coordination environment and reaction conditions. For example, Co-based phosphides show high conductivity and high stability, which enable them to enhance electrocatalytic performance. Flexible carbon support graphite felt (GF) has the characteristics of conductivity close to metal, high volume porosity, and excellent corrosion resistance, which make GF a very attractive catalyst support for organic electrochemical synthesis.

[0006] Based on the research of such electrocatalytic materials, the present invention designs a CoP catalytic electrode, and uses electrode materials and reaction microenvironment design to control the selectivity and conversion rate of the reaction. Currently, there is no report on the use of GF to improve the CoP electrochemical selective hydrogenation conversion system of quinoline. Summary of the invention

[0007] In view of the problems of "difficult reaction, low yield and poor selectivity" in the prior art of quinoline hydrogenation reaction, the present invention provides a self-supporting CoP nanowire catalytic electrode and a preparation method thereof, as well as the application of the self-supporting CoP nanowire catalytic electrode as a cathode electrode for electrocatalytic hydrogenation of quinoline to synthesize 1,2,3,4-tetrahydroquinoline.

[0008] The technical solution of the present invention is as follows:

[0009] A self-supporting CoP nanowire catalytic electrode consists of a carrier and an active component grown on the carrier; wherein the carrier is graphite felt (GF) and the active component is a CoP nanowire structure.

[0010] The catalytic electrode of the present invention is characterized in that the CoP nanowires are evenly distributed on the substrate, which makes the catalyst have a larger specific surface area and electrochemical active area; this nanostructure provides more active sites for the active substance, promotes the diffusion of the active substance, and also helps the transmission of protons in the electrolyte, which makes the catalyst show a higher reaction rate and lower reaction activation energy in the electrochemical reaction.

[0011] The preparation method of the self-supporting CoP nanowire catalytic electrode of the present invention is as follows:

[0012] Dissolve Co(NO3)2·6H2O, NH4F and urea in deionized water to obtain a mixed solution; add the obtained mixed solution and graphite felt into an autoclave, keep at 120°C for 6 hours, then cool to room temperature, take out the graphite felt, rinse and dry to obtain a catalytic electrode precursor; put the catalytic electrode precursor and a porcelain boat containing NaH2PO2 into a muffle furnace, calcine at 300°C for 2 hours in an Ar gas atmosphere to obtain the self-supporting CoP nanowire catalytic electrode;

[0013] The preferred mass ratio of Co(NO3)2·6H2O, NH4F, urea, and NaH2PO2 is 0.291:0.093:0.30:0.5;

[0014] The graphite felt was pretreated as follows before use: the graphite felt was immersed in HNO3 solution (40wt%), then transferred to an autoclave and kept at 120°C for 2h, followed by ultrasonication in acetone, H2O, and ethanol in sequence, and dried for use.

[0015] The self-supporting CoP nanowire catalytic electrode of the present invention can be used in the reaction of electrocatalytic quinoline hydrogenation to synthesize 1,2,3,4-tetrahydroquinoline; the specific method is as follows:

[0016] The electrocatalytic reaction device uses an H-type electrolyzer (such as Figure 2 As shown), the electrolyte is separated by a N117 cationic membrane between the cathode and anode reaction tanks, the anode is a platinum electrode, the cathode is a self-supporting CoP nanowire catalytic electrode, and the reference electrode is a Hg / HgO electrode. The electrolyte is added to the cathode and anode reaction tanks, and the electrocatalytic reaction is carried out in a constant voltage electrolysis mode at room temperature and under stirring conditions;

[0017] The reaction equation is Figure 1 As shown;

[0018] Electrolyte in the anode reaction tank: 1 mol / L KOH solution;

[0019] The electrolyte in the cathode reaction tank is a mixed solution of quinoline, 1 mol / L KOH solution and 1,4-dioxane; wherein the concentration of quinoline is 14.14 mmol / L, and the volume ratio of 1 mol / L KOH solution to 1,4-dioxane is 26:4;

[0020] The constant voltage bias of the electrocatalytic reaction was set to -1.1 to -1.3 V;

[0021] The electrolysis time is 3 to 6 hours.

[0022] The beneficial effects of the present invention are mainly reflected in:

[0023] First, compared with the thermochemical catalytic method, the electrochemical method is green, environmentally friendly, gentle and efficient. The process of the present invention is simpler and convenient, and is also conducive to reducing production costs. Secondly, in the process of realizing the electrocatalytic selective hydrogenation reduction of quinoline, satisfactory conversion rate and selectivity are obtained, which shows that the process of the present invention can effectively convert quinoline into the desired product while avoiding the generation of by-products.

[0024] Compared with other materials reported previously, the CoP nanomaterials we prepared have significant advantages. The preparation process is very simple, and metal Co is cheap and easily available in the market, which has good industrial application prospects. In addition, the performance of CoP nanomaterials in electrolysis reactions is also very good, with ideal selectivity and conversion rate, which means that this material may have good application potential in many chemical reactions. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 : The electrochemical reaction equation of quinoline of the present invention.

[0026] Figure 2 : The electrolytic cell device in the embodiment of the present invention.

[0027] Figure 3 : SEM image of CoP-GF prepared in the embodiment of the present invention. DETAILED DESCRIPTION

[0028] The present invention is further described below by means of specific embodiments, but the protection scope of the present invention is not limited thereto.

[0029] The graphite felt used in the following examples was from the Science and Materials Station (carbon felt GF 030).

[0030] Embodiment 1

[0031] 1. Preparation of CoP nanowire materials grown on GF.

[0032] GF pretreatment: GF (40 × 10 × 3 mm) was immersed in 40 mL of HNO3 solution (40%) and then transferred to a stainless steel autoclave with a polytetrafluoroethylene liner, kept at 120 °C for 2 h, and then ultrasonicated in acetone, H2O and ethanol for 30 min in sequence.

[0033] Preparation of CoP material: Co(NO3)2·6H2O (0.291 g), NH4F (0.093 g) and urea (0.30 g) were dissolved in deionized water (20 mL). After continuous stirring for ten minutes, the solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and a piece of pretreated GF, kept at 120°C for 6 hours, cooled to room temperature, and the precursor was rinsed with deionized water several times to remove free particles and residual reactants. Finally, 0.5 g NaH2PO2 was added to the porcelain boat under an Ar gas atmosphere at 300°C and the precursor was calcined for 2 hours to obtain CoP nanowire material. The morphology of the material is as shown in FIG. Figure 3 As shown, the Co content in the material prepared by this method is 44.67%, and the P content is 55.33%. CoP maintains the characteristics of the nanowire array and is well dispersed on the GF, ensuring that it has abundant active sites, which is an important reason why the material can achieve good catalytic performance.

[0034] 2. Using CoP nanowires grown on GF as cathode, quinoline was electrocatalytically hydrogenated. An H-type electrolytic reaction cell was used, and N117 cationic membrane was used to separate the cathode and anode electrolytes. The anode was a platinum electrode, and the reference electrode was Hg / HgO. The electrolyte in the anode reaction cell was a 1 mol / L potassium hydroxide solution (30 mL, the same below); the cathode electrolyte was a 14.14 mmol / L quinoline mixed solution with 26 ml of 1M KOH and 4 ml of 1,4-dioxane (30 mL, the same below). The electrolysis potential was controlled at -1.2 V, and the electrolysis was carried out at room temperature (25 ° C, the same below) at a constant speed of 500 r / min for 6 hours. High performance liquid chromatography was used for detection, and the results showed that the selectivity of 1,2,3,4-tetrahydroquinoline was 99.99%, and the yield was 86.81%.

[0035] Table 1 Effect of different thickness GF on hydrogenation reduction of quinoline

[0036]

[0037] Except for the different thickness of graphite felt, all the experiments in Table 1 were operated the same as in Example 1. The amount of catalyst grown by GFs of different thicknesses was different, resulting in different catalytic performances. However, the performance of the GF of 6.5 mm may be reduced due to its excessive thickness, which reduced the permeability of the solution and the transfer efficiency of protons.

[0038] Embodiment 2

[0039] 1. Preparation of CoP nanowire materials grown on GF.

[0040] GF pretreatment: GF (40×10×3 mm) was ultrasonicated in HNO3 solution (40%), acetone, H2O and ethanol for 30 min in sequence.

[0041] CoP material preparation: Material preparation is the same as in Example 1.

[0042] 2. Using CoP nanowires grown on GF as cathode, quinoline was electrocatalyzed for hydrogenation. An H-type electrolytic reaction cell was used, with N117 cationic membrane to separate the cathode and anode electrolytes, a platinum electrode as the anode, and Hg / HgO as the reference electrode. Figure 2 The diagram of the H-type electrolytic cell is shown in Figure 1. The electrolyte in the anode reaction tank is a potassium hydroxide solution with a concentration of 1 mol / L; the cathode electrolyte is a mixed solution of quinoline with a concentration of 14.14 mmol / L, 26 ml of 1M KOH and 4 ml of 1,4-dioxane. The electrolysis potential is controlled at -1.2 V, and the electrolysis is carried out at a constant stirring speed for 6 hours at room temperature. The results of the high performance liquid chromatography test showed that the selectivity of 1,2,3,4-tetrahydroquinoline was 99.99% and the yield was 58.41%. The hydrophobic surface properties of GF in this embodiment and the insufficient electrochemical activity in the electrolyte are the main reasons for the decline in the performance of the catalyst material.

[0043] Embodiment 3

[0044] 1. Preparation of CoP nanowire materials grown on GF.

[0045] GF pretreatment: The graphite felt (40×10×3 mm) was ultrasonically cleaned in deionized water for 10 min, dried and calcined in a tubular furnace at 400°C in an argon atmosphere for two hours, taken out and ultrasonically placed in HNO3 solution (40%) for 30 min, and then ultrasonically placed in acetone, deionized water and ethanol for 15 min in turn.

[0046] CoP material preparation: Material preparation is the same as in Example 1.

[0047] 2. Using CoP nanowires grown on GF as cathode, quinoline was electrocatalyzed for hydrogenation. An H-type electrolytic reaction cell was used, with N117 cationic membrane to separate the cathode and anode electrolytes, a platinum electrode as the anode, and Hg / HgO as the reference electrode. Figure 2 The diagram of the H-type electrolytic cell is shown in FIG. 1. The electrolyte in the anode reaction tank is a potassium hydroxide solution with a concentration of 1 mol / L; the cathode electrolyte is a mixed solution of quinoline with a concentration of 14.14 mmol / L, 26 ml of 1M KOH and 4 ml of 1,4-dioxane. The electrolysis potential is controlled at -1.2 V, and the electrolysis is carried out at a constant stirring speed for 6 hours at room temperature. The results of the high performance liquid chromatography test show that the selectivity of 1,2,3,4-tetrahydroquinoline is 99.99% and the yield is 59.61%. The reason for the reduction in yield is the same as in Example 2.

[0048] Embodiment 4

[0049] 1. Preparation of CoP nanowire materials grown on GF.

[0050] GF pretreatment: GF (40 × 10 × 3 mm) was soaked in a mixed acid solution (1:3) of HNO3 (65%) and H2SO4 (98%) for 12 h, then rinsed with deionized water and dried in vacuum.

[0051] CoP material preparation: Material preparation is the same as in Example 1.

[0052] 2. Using CoP nanowires grown on GF as cathode, quinoline was electrocatalyzed for hydrogenation. An H-type electrolytic reaction cell was used, with N117 cationic membrane to separate the cathode and anode electrolytes, a platinum electrode as the anode, and Hg / HgO as the reference electrode. Figure 2 The diagram of the H-type electrolytic cell is shown in FIG. 1. The electrolyte in the anode reaction tank is a potassium hydroxide solution with a concentration of 1 mol / L; the cathode electrolyte is a mixed solution of quinoline with a concentration of 14.14 mmol / L, 26 ml of 1M KOH and 4 ml of 1,4-dioxane. The electrolysis potential is controlled at -1.2 V, and the electrolysis is carried out at a constant stirring speed for 6 hours at room temperature. The results of the high performance liquid chromatography test show that the selectivity of 1,2,3,4-tetrahydroquinoline is 99.99% and the yield is 42.65%. The reason for the reduction in yield is the same as in Example 2.

Claims

1. A self-supporting CoP nanowire catalytic electrode, characterized in that: It consists of a carrier and an active component grown on the carrier; wherein the carrier is graphite felt and the active component is a CoP nanowire structure.

2. The method for preparing the self-supporting CoP nanowire catalytic electrode according to claim 1, characterized in that: The preparation method is as follows: Dissolve Co(NO3)2·6H2O, NH4F and urea in deionized water to obtain a mixed solution; add the obtained mixed solution and graphite felt into an autoclave, maintain at 120°C for 6 hours, then cool to room temperature, take out the graphite felt, rinse and dry to obtain a catalytic electrode precursor; put the catalytic electrode precursor and a porcelain boat containing NaH2PO2 into a muffle furnace, calcine at 300°C for 2 hours in an Ar gas atmosphere to obtain the self-supporting CoP nanowire catalytic electrode.

3. The preparation method according to claim 2, characterized in that: The mass ratio of Co(NO3)2·6H2O, NH4F, urea and NaH2PO2 is 0.291:0.093:0.30:0.

5.

4. The preparation method according to claim 2, characterized in that: The graphite felt was pretreated as follows before use: the graphite felt was immersed in HNO3 solution, then transferred to an autoclave and kept at 120°C for 2h, then ultrasonicated in acetone, H2O, and ethanol in sequence, and dried for use.

5. Use of the self-supporting CoP nanowire catalytic electrode as claimed in claim 1 in the electrocatalytic hydrogenation reaction of quinoline to synthesize 1,2,3,4-tetrahydroquinoline.

6. The use according to claim 5, characterized in that The application method is as follows: The electrocatalytic reaction device adopts an H-type electrolytic cell, and an N117 cationic membrane is used to separate the electrolyte between the cathode and anode reaction cells. The anode is a platinum electrode, the cathode is a self-supporting CoP nanowire catalytic electrode, and the reference electrode is a Hg / HgO electrode. The electrolyte is added to the cathode and anode reaction cells, and the electrocatalytic reaction is carried out in a constant voltage electrolysis mode at room temperature and under stirring conditions. Electrolyte in the anode reaction tank: 1 mol / L KOH solution; The electrolyte in the cathode reaction tank: a mixed solution of quinoline, 1 mol / L KOH solution and 1,4-dioxane.

7. The use according to claim 6, characterized in that In the cathode reaction tank electrolyte, the quinoline concentration was 14.14 mmol / L, and the volume ratio of 1 mol / L KOH solution and 1,4-dioxane was 26:

4.

8. The use according to claim 6, characterized in that The constant voltage bias of the electrocatalytic reaction was set to -1.1 to -1.3 V, and the electrolysis time was 3 to 6 h.

Citation Information

Patent Citations

  • Synthesis method of tetrahydroquinoline

    CN117143015A

  • Supported catalyst and application thereof in selective hydrogenation of quinoline compounds

    CN112742422A

  • Method for synthesizing 1, 2, 3, 4-tetrahydroquinoline through hydrogenation of quinoline under electro-catalysis of copper-based bimetallic

    CN116590723A

  • Electrode device based on phosphorus cobalt sulfide and application of electrode device in electro-catalytic dechlorination reaction system

    CN118064928A

  • tetrahydroquinolines

    DE102005027168A1