Electrode assembly and device for preparing hydrogen peroxide by electrolyzing water
By modifying the hydrophobic polymer and porous metal oxide layer on the electrode assembly, optimizing the oxygen mass transfer and production efficiency, the problems of low oxygen utilization and insufficient disinfection efficiency in the prior art are solved, and the water treatment and disinfection technology are expanded Application scope.
Patent Information
- Application Number
- CN202411373342.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing electrolytic technology, the electrode materials have limited capacity to capture oxygen, resulting in low hydrogen peroxide production efficiency, which limits its application in the fields of water treatment and disinfection.
By modifying the hydrophobic polymer layer on the cathode electrode body and forming a porous metal oxide and electrocatalytic active material layer on the anode electrode body, a gas-liquid-solid three-phase interface and nanoporous structure are constructed, and the mass transfer of oxygen and Generate efficiency.
It improves the efficiency of oxygen capture and mass transfer, enhances the production rate and disinfection efficiency of hydrogen peroxide, and expands the application potential in the fields of water treatment, medical disinfection and environmental purification.
Smart Images

Figure CN118957671A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical technology, and in particular to an electrode assembly and a device for preparing hydrogen peroxide by electrolyzing water. Background Art
[0002] In the process of rapid urbanization and industrialization, water safety issues have become increasingly prominent, especially the disinfection of domestic water. Traditional disinfection methods, such as chlorination, can effectively kill pathogens, but may produce harmful disinfection byproducts. Therefore, the development of a green and efficient water treatment technology is of great practical significance.
[0003] Electrolysis of water has gradually become a hot topic of research due to its environmental friendliness and easy operation. In particular, the method of producing hydrogen peroxide by electrochemical cathode reduction of oxygen has attracted widespread attention due to its strong disinfection ability and no secondary pollution. However, the electrode materials in the prior art have limited oxygen capture capacity, resulting in low efficiency in the production of hydrogen peroxide, which limits its promotion in practical applications. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes an electrode assembly and device for preparing hydrogen peroxide by electrolyzing water. On the one hand, the cathode electrode body is modified by a hydrophobic polymer so that the electrode has excellent oxygen adsorption and mass transfer efficiency. On the other hand, the anode electrode body is modified by a porous metal oxide and an electrocatalytically active material so that a reaction interface that promotes the generation of micro-nano bubbles is formed on the electrode surface. Finally, through the two-way optimization of the cation and cathode electrodes, not only the problems of low oxygen utilization and insufficient disinfection efficiency in the prior art are solved, but also the application scope of disinfection technology under different water quality conditions is expanded. It is expected to demonstrate its excellent performance and broad market application potential in multiple fields such as water treatment, medical disinfection, and environmental purification.
[0005] The present invention provides an electrode assembly for preparing hydrogen peroxide by electrolyzing water, comprising a modified cathode and a modified anode;
[0006] The modified cathode comprises a cathode electrode body and a hydrophobic polymer layer loaded on the cathode electrode body, and the modified anode comprises an anode electrode body, a porous metal oxide layer loaded on the anode electrode body and an electrocatalytic activator layer loaded on the porous metal oxide layer.
[0007] In the present invention, the cathode electrode body is modified by using a hydrophobic polymer material, and an aerophilic layer can be formed at the cathode electrode interface to modify and construct a gas diffusion channel. The electrode interface is transformed from the traditional liquid-solid two-phase to the gas-liquid-solid three-phase, thereby promoting the mass transfer and capture of oxygen at the electrode interface, and ultimately improving the electrochemical reaction efficiency of the obtained electrode. In addition, since the restriction of gas mass transfer from the interface to the electrochemical reaction is greatly weakened, the obtained electrode overcomes the problem of low dissolved oxygen concentration, and the current density and current efficiency are also greatly improved.
[0008] At the same time, by loading a porous metal oxide layer on the anode electrode body, a nanoporous structure is constructed on the anode surface to increase the gas-liquid contact area, promote the release of oxygen and the formation of micro-nano bubbles, and further load highly catalytically active materials such as RuO2 and IrO2 on the porous metal oxide layer, the efficiency of oxygen generation can be improved.
[0009] Preferably, the modified cathode is obtained by coating the surface of the cathode electrode body with a hydrophobic polymer slurry and then sintering;
[0010] Preferably, the cathode electrode body is at least one of a titanium plate, a carbon felt, a nickel sheet or nickel foam, and the hydrophobic polymer is at least one of polytetrafluoroethylene PTFE, polyvinylidene fluoride PVDF, fluorinated ethylene propylene copolymer or polyhexafluoropropylene;
[0011] Preferably, the content of the hydrophobic polymer in the hydrophobic polymer slurry is 1-10 wt %.
[0012] Preferably, the hydrophobic polymer slurry further comprises a surfactant, and the surfactant is at least one of sucrose monolaurate, sucrose monooleate, polyethylene glycol distearate, hydroxyethyl cellulose ether, nonylphenol polyoxyethylene ether or fatty alcohol polyoxyethylene ether;
[0013] Preferably, the content of surfactant in the hydrophobic polymer slurry is 0.1-1 wt %.
[0014] Preferably, the hydrophobic polymer slurry further comprises an ionic fluorine-containing additive, wherein the ionic fluorine-containing additive is a copolymer of perfluorooctylethyl methacrylate, methacrylate and methacryloyloxyethyl trimethylammonium chloride;
[0015] Preferably, the molar ratio of perfluorooctylethyl methacrylate, methacrylate and methacryloyloxyethyltrimethylammonium chloride is 10:1-3:1-3;
[0016] Preferably, the content of the ionic fluorine-containing additive in the hydrophobic polymer slurry is 0.1-2 wt %.
[0017] In the present invention, the hydrophobic polymer slurry also includes an ionic fluorine-containing additive. On the one hand, the ionic chain ends contained in the ionic fluorine-containing additive can form effective adsorption on the polar surface of the electrode body. On the other hand, the fluoroalkyl chain ends contained in the ionic fluorine-containing additive can enhance the compatibility with the hydrophobic polymer material, which can not only improve the uniform adhesion effect of the hydrophobic polymer on the surface of the electrode body, but also improve the stability of the electrode and extend the service life of the electrode, thereby further enhancing the gas affinity of the electrode, increasing the gas-liquid-solid three-phase interface formed by it, and finally obtaining a higher reaction efficiency and hydrogen peroxide yield.
[0018] Preferably, the sintering temperature is 280-350° C., and the sintering time is 0.5-2 h.
[0019] Preferably, the modified anode is obtained by depositing a porous metal oxide on the surface of the anode electrode body, and then coating the surface with an electrocatalytic activator slurry and curing the surface;
[0020] Preferably, the anode electrode body is at least one of a titanium plate, a nickel sheet, a stainless steel mesh or a graphite plate, the porous metal oxide is at least one of TiO2, Co3O4, MnO2, SnO2, ZrO2 or SiO2, and the electrocatalyst is at least one of RuO2 or IrO2.
[0021] Preferably, the electrocatalyst activator slurry further includes polyaniline;
[0022] Preferably, the content of the electrocatalyst activator in the electrocatalyst activator slurry is 1-5 wt %, and the content of the polyaniline is 0.1-0.5 wt %.
[0023] In the present invention, the electrocatalyst activator slurry further includes a conductive polymer such as polyaniline, which can further improve the bubble generation performance.
[0024] Preferably, the porous metal oxide is deposited by physical vapor deposition, chemical vapor deposition, impregnation reduction method or impregnation sintering method;
[0025] Preferably, the curing temperature is 80-120° C. and the curing time is 6-12 hours.
[0026] The present invention also provides a device for preparing hydrogen peroxide by electrolyzing water, and the device comprises the electrode assembly.
[0027] Preferably, the device comprises a modified cathode, a modified anode, a separator and a housing;
[0028] The separator is located between the modified cathode and the modified anode and separates the modified cathode from the modified anode; the shell is a hollow shell and fixes the modified cathode, the modified anode and the separator as a whole.
[0029] Beneficial effects:
[0030] (1) In the electrode assembly described in the present invention, by forming a hydrophobic polymer material layer on the surface of the cathode electrode body, not only the gas affinity of the electrode is enhanced, but also a gas-liquid-solid three-phase interface is formed, thereby enhancing the electrode's oxygen capture and mass transfer efficiency, prolonging the residence time of oxygen on the electrode surface, overcoming the limited solubility of oxygen, and improving its electrochemical reduction reaction efficiency of oxygen, thereby increasing the generation rate of hydrogen peroxide; by forming a porous metal oxide layer on the surface of the anode electrode body, a nanoporous structure is constructed on the anode surface, thereby increasing the gas-liquid contact area, promoting the release of oxygen and the formation of micro-nano bubbles, and at the same time, a polyaniline / RuO2 or polyaniline / IrO2 layer is formed on the surface of the anode electrode body. On the one hand, polyaniline, as a conductive polymer, can improve the bubble generation performance, and on the other hand, RuO2 or IrO2, as a material with high catalytic activity, can improve the oxygen generation efficiency.
[0031] (2) The electrode assembly of the present invention can not only react the oxygen dissolved in water through bidirectional optimization of the anode and cathode, but also enhance the capture ability of gaseous micro-nano bubbles, thereby further improving the efficiency of the electrochemical reaction.
[0032] (3) The electrode assembly of the present invention solves the problems of low oxygen utilization and insufficient disinfection efficiency in traditional disinfection technology, and also expands the application scope of disinfection technology under different water quality conditions. It is expected to demonstrate its excellent performance and broad market application potential in multiple fields such as water treatment, medical disinfection, and environmental purification. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The present invention is a schematic diagram of the device for preparing hydrogen peroxide by electrolyzing water; wherein, 1 is a modified cathode, 2 is a modified anode, 3 is a separator, and 4 is a casing.
[0034] Figure 2 This is a partial enlarged view of the modified anode (a) and the anode electrode body (b) described in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.
[0036] Example 1
[0037] An electrode assembly for preparing hydrogen peroxide by electrolyzing water, comprising a modified cathode and a modified anode;
[0038] The modified cathode is prepared by the following method:
[0039] (1) A carbon felt (size: 2 cm × 2 cm × 2 mm) was used as a cathode electrode body and was immersed in deionized water for ultrasonic cleaning for 30 min to remove surface dirt, and then placed in an oven at 150° C. for drying for 3 h to obtain a pretreated carbon felt;
[0040] (2) adding polytetrafluoroethylene (PTFE) powder (average particle size of 1 μm) and nonylphenol polyoxyethylene ether in a mass ratio of 10:1 to ethanol and ultrasonically dispersing for 30 minutes to obtain a PTFE slurry with a PTFE content of 7 wt%;
[0041] (3) Spray the PTFE slurry evenly on both sides of the pretreated carbon felt so that the PTFE loading is 5 wt %. First, dry it naturally in a fume hood for 20 min, and then dry it in an oven at 180 ° C for 0.5 h to ensure that the solvent is completely volatilized;
[0042] (4) sintering the dried carbon felt at 320° C. for 1.5 h in a nitrogen atmosphere to enhance the bonding strength between the PTFE coating and the carbon felt substrate, and after naturally cooling to room temperature, rinsing the surface with deionized water to remove loose particles and residues, thereby obtaining the modified cathode;
[0043] The modified anode is prepared by the following method:
[0044] (1) A titanium plate (size of 2 cm×2 cm×2 mm) was used as the anode electrode body and polished with 500-mesh metallographic sandpaper to remove the surface oxide film, then rinsed with water, immersed in a 40 wt% NaOH solution, treated at 90° C. for 1 h, degreased, rinsed with water, and dried in an oven at 120° C. for 1 h to obtain a pretreated titanium plate;
[0045] (2) Install the pretreated titanium plate and TiO2 sputtering target on the corresponding fixtures in the magnetron sputtering chamber and evacuate to 0.5×10 -3 Pa, then nitrogen was injected to make the pressure of the sputtering chamber 1.5Pa, the sputtering system was turned on and the current was maintained at 25mA, the voltage was maintained at 25V, and after sputtering for 20min, porous TiO2 layers (thickness of 1μm) were formed on both sides of the titanium plate;
[0046] (3) adding RuO2 nanoparticles (average particle size of 20 nm) into N-methylpyrrolidone and ultrasonically dispersing for 1 h to obtain an electrocatalyst activator slurry with a RuO2 nanoparticle content of 3 wt%;
[0047] (4) The electrocatalytic activator slurry was scraped onto the surface of the porous TiO2 layer to form a wet film with a thickness of 5 μm, and the film was placed in a vacuum drying oven at 100° C. for curing for 10 h to obtain the modified anode.
[0048] Example 2
[0049] An electrode assembly for preparing hydrogen peroxide by electrolyzing water, comprising a modified cathode and a modified anode;
[0050] The modified cathode is prepared by the following method:
[0051] (1) A nickel foam (size: 2 cm×2 cm×2 mm) was used as a cathode electrode body and was respectively immersed in acetone and ethanol for ultrasonic cleaning for 15 min each to remove surface grease, and then placed in an oven at 110° C. for drying for 3 h to obtain a pretreated nickel foam;
[0052] (2) adding polytetrafluoroethylene PTFE powder (average particle size of 1 μm), polyvinylidene fluoride PVDF (average particle size of 1 μm) and nonylphenol polyoxyethylene ether to ethanol in a mass ratio of 2:8:1 and ultrasonically dispersing for 30 minutes to obtain a PTFE and PVDF slurry with a PTFE content of 1.4 wt% and a PVDF content of 5.6 wt%;
[0053] (3) spraying PTFE and PVDF slurry evenly on both sides of the pretreated nickel foam so that the loading amount of PTFE is 1wt% and the loading amount of PVDF is 4wt%, first drying it naturally in a fume hood for 20min, and then drying it in an oven at 180°C for 0.5h to ensure that the solvent is completely volatilized;
[0054] (4) sintering the dried carbon felt at 320° C. for 1.5 h in a nitrogen atmosphere to enhance the bonding strength between the PTFE and PVDF coatings and the carbon felt substrate, and after naturally cooling to room temperature, rinsing the surface with deionized water to remove loose particles and residues, thereby obtaining the modified cathode;
[0055] The modified anode is prepared by the following method:
[0056] (1) A nickel sheet (size: 2 cm×2 cm×2 mm) was used as an anode electrode body and was immersed in a 15 wt % HCl solution for ultrasonic cleaning for 20 min. After being taken out, it was rinsed with ethanol and water and dried in an oven at 60° C. for 1 h to obtain a pretreated nickel sheet;
[0057] (2) Immerse the pretreated nickel sheet in a 0.5 mol / L Co(NO3)2 solution and a 0.05 mol / L KNO3 solution, and use a three-electrode system, with the pretreated nickel sheet as the working electrode, the Pt sheet as the counter electrode, and the saturated calomel electrode as the reference electrode. At room temperature, keep the voltage at 1.5 V, and perform electrochemical deposition on the surface of the pretreated nickel sheet for 10 minutes. After completion, rinse with ethanol and water, place in an oven at 80°C to dry for 1 hour, and then place in a muffle furnace and calcine at 250°C for 5 hours to form a porous Co3O4 layer (1 μm thick) on both sides of the nickel sheet.
[0058] (3) adding IrO2 nanoparticles (average particle size of 10 nm) to ethanol in N-methylpyrrolidone and ultrasonically dispersing for 1.5 h to obtain an electrocatalyst activator slurry with an IrO2 nanoparticle content of 3 wt%;
[0059] (4) The electrocatalytic activator slurry was scraped onto the surface of the porous Co3O4 layer to form a wet film with a thickness of 5 μm, and then placed in a vacuum drying oven at 90° C. for curing for 10 h to obtain the modified anode.
[0060] Example 3
[0061] An electrode assembly for preparing hydrogen peroxide by electrolyzing water, comprising a modified cathode and a modified anode;
[0062] The modified cathode is prepared by the following method:
[0063] (1) immersing graphite felt (size: 2 cm×2 cm×2 mm) as the cathode electrode body in deionized water for ultrasonic cleaning for 30 min to remove surface dirt, and then drying it in an oven at 150° C. for 3 h to obtain pretreated graphite felt;
[0064] (2) adding polytetrafluoroethylene PTFE powder (average particle size of 1 μm) and polyethylene glycol distearate to ethanol at a mass ratio of 10:1 and ultrasonically dispersing for 30 minutes to obtain a PTFE slurry with a PTFE content of 7 wt%;
[0065] (3) Spray the PTFE slurry evenly on both sides of the pretreated graphite felt so that the PTFE loading is 5 wt %. First, dry it naturally in a fume hood for 20 min, and then dry it in an oven at 180° C. for 0.5 h to ensure that the solvent is completely evaporated;
[0066] (4) sintering the dried carbon felt at 320° C. for 1.5 h in a nitrogen atmosphere to enhance the bonding strength between the PTFE coating and the carbon felt substrate, and after naturally cooling to room temperature, rinsing the surface with deionized water to remove loose particles and residues, thereby obtaining the modified cathode;
[0067] The modified anode is prepared by the following method:
[0068] (1) A 304 stainless steel mesh (size: 2 cm×2 cm×2 mm) was used as the anode electrode body and was immersed in acetone for ultrasonic cleaning for 30 min to remove surface organic impurities, then immersed in a 3 wt % HCl solution for ultrasonic cleaning for 20 min to remove surface oxide impurities, then rinsed with ethanol, and dried in an oven at 60° C. for 2 h to obtain a pretreated stainless steel mesh;
[0069] (2) adding manganese acetate and citric acid to deionized water in a mass ratio of 1.5:1, stirring evenly, adding 25 wt% ammonia water to adjust the pH to 6.5, and then heating in a 60°C water bath until the solution is in a sol-like state; immersing the pretreated stainless steel mesh in the sol-like solution, allowing it to stand for adsorption for 0.5 h, and then drying it at room temperature for 0.5 h, and repeating the above operation until a porous MnO2 layer with a thickness of 1 μm is formed on both sides of the stainless steel mesh;
[0070] (3) adding RuO2 nanoparticles (average particle size of 20 nm) and polyaniline in a mass ratio of 10:1 to N-methylpyrrolidone in ethanol and ultrasonically dispersing for 1 h to obtain an electrocatalyst slurry with a RuO2 nanoparticle content of 3 wt%;
[0071] (4) The electrocatalytic activator slurry is scraped onto the surface of the porous MnO2 layer to form a wet film with a thickness of 5 μm, and then placed in a vacuum drying oven at 120° C. for curing for 8 hours to obtain the modified anode.
[0072] Example 4
[0073] An electrode assembly for preparing hydrogen peroxide by electrolyzing water, comprising a modified cathode and a modified anode;
[0074] The modified cathode is prepared by the following method:
[0075] (1) A carbon felt (size: 2 cm × 2 cm × 2 mm) was used as a cathode electrode body and was immersed in deionized water for ultrasonic cleaning for 30 min to remove surface dirt, and then placed in an oven at 150° C. for drying for 3 h to obtain a pretreated carbon felt;
[0076] (2) adding polytetrafluoroethylene (PTFE) powder (average particle size of 1 μm), ionic fluorine-containing additive and nonylphenol polyoxyethylene ether in a mass ratio of 10:2:1 to ethanol and ultrasonically dispersing for 30 minutes to obtain a PTFE slurry with a PTFE content of 7 wt%;
[0077] Wherein, the ionic fluorine-containing additive is a copolymer of perfluorooctylethyl methacrylate, methacrylate and methacryloyloxyethyl trimethylammonium chloride, and the molar ratio of perfluorooctylethyl methacrylate, methacrylate and methacryloyloxyethyl trimethylammonium chloride is 5:1:1;
[0078] The preparation method comprises: adding perfluorooctylethyl methacrylate, methacrylate and methacryloyloxyethyl trimethylammonium chloride into water at a molar ratio of 5:1:1, stirring and mixing evenly, adding a redox initiator (a mixture of potassium persulfate and sodium bisulfite, with a mass ratio of potassium persulfate and sodium bisulfite of 2:1) with a mass percentage of 5wt% of methyl methacrylate under a nitrogen protective atmosphere, stirring and reacting at 50°C for 4h, concentrating, and vacuum drying to obtain the ionic fluorine-containing additive;
[0079] (3) Spray the PTFE slurry evenly on both sides of the pretreated carbon felt so that the PTFE loading is 5 wt %. First, dry it naturally in a fume hood for 20 min, and then dry it in an oven at 180 ° C for 0.5 h to ensure that the solvent is completely volatilized;
[0080] (4) sintering the dried carbon felt at 320° C. for 1.5 h in a nitrogen atmosphere to enhance the bonding strength between the PTFE coating and the carbon felt substrate, and after naturally cooling to room temperature, rinsing the surface with deionized water to remove loose particles and residues, thereby obtaining the modified cathode;
[0081] The modified anode is prepared by the following method:
[0082] (1) A titanium plate (size of 2 cm×2 cm×2 mm) was used as the anode electrode body and polished with 500-mesh metallographic sandpaper to remove the surface oxide film, then rinsed with water, immersed in a 40 wt% NaOH solution, treated at 90° C. for 1 h, degreased, rinsed with water, and dried in an oven at 120° C. for 1 h to obtain a pretreated titanium plate;
[0083] (2) Install the pretreated titanium plate and TiO2 sputtering target on the corresponding fixtures in the magnetron sputtering chamber and evacuate to 0.5×10 -3 Pa, then nitrogen was injected to make the pressure of the sputtering chamber 1.5Pa, the sputtering system was turned on and the current was maintained at 25mA, the voltage was maintained at 25V, and after sputtering for 20min, porous TiO2 layers (thickness of 1μm) were formed on both sides of the titanium plate;
[0084] (3) adding RuO2 nanoparticles (average particle size of 20 nm) into N-methylpyrrolidone and ultrasonically dispersing for 1 h to obtain an electrocatalyst activator slurry with a RuO2 nanoparticle content of 3 wt%;
[0085] (4) The electrocatalytic activator slurry was scraped onto the surface of the porous TiO2 layer to form a wet film with a thickness of 5 μm, and the film was placed in a vacuum drying oven at 100° C. for curing for 10 h to obtain the modified anode.
[0086] Comparative Example 1
[0087] An electrode assembly for preparing hydrogen peroxide by electrolyzing water, comprising a cathode and an anode;
[0088] The cathode is carbon felt (size is 2cm×2cm×2mm);
[0089] The anode is a modified anode, which is prepared by the following method:
[0090] (1) A titanium plate (size of 2 cm×2 cm×2 mm) was used as the anode electrode body and polished with 500-mesh metallographic sandpaper to remove the surface oxide film, then rinsed with water, immersed in a 40 wt% NaOH solution, treated at 90° C. for 1 h, degreased, rinsed with water, and dried in an oven at 120° C. for 1 h to obtain a pretreated titanium plate;
[0091] (2) Install the pretreated titanium plate and TiO2 sputtering target on the corresponding fixtures in the magnetron sputtering chamber and evacuate to 0.5×10 -3 Pa, then nitrogen was injected to make the pressure of the sputtering chamber 1.5Pa, the sputtering system was turned on and the current was maintained at 25mA, the voltage was maintained at 25V, and after sputtering for 20min, porous TiO2 layers (thickness of 1μm) were formed on both sides of the titanium plate;
[0092] (3) adding RuO2 nanoparticles (average particle size of 20 nm) into N-methylpyrrolidone and ultrasonically dispersing for 1 h to obtain an electrocatalyst activator slurry with a RuO2 nanoparticle content of 3 wt%;
[0093] (4) The electrocatalytic activator slurry was scraped onto the surface of the porous TiO2 layer to form a wet film with a thickness of 5 μm, and the film was placed in a vacuum drying oven at 100° C. for curing for 10 h to obtain the modified anode.
[0094] Comparative Example 2
[0095] An electrode assembly for preparing hydrogen peroxide by electrolyzing water, comprising a cathode and an anode;
[0096] The cathode is a modified cathode, which is prepared by the following method:
[0097] (1) A carbon felt (size: 2 cm × 2 cm × 2 mm) was used as a cathode electrode body and was immersed in deionized water for ultrasonic cleaning for 30 min to remove surface dirt, and then placed in an oven at 150° C. for drying for 3 h to obtain a pretreated carbon felt;
[0098] (2) adding polytetrafluoroethylene (PTFE) powder (average particle size of 1 μm) and nonylphenol polyoxyethylene ether in a mass ratio of 10:1 to ethanol and ultrasonically dispersing for 30 minutes to obtain a PTFE slurry with a PTFE content of 7 wt%;
[0099] (3) Spray the PTFE slurry evenly on both sides of the pretreated carbon felt so that the PTFE loading is 5 wt %. First, dry it naturally in a fume hood for 20 min, and then dry it in an oven at 180 ° C for 0.5 h to ensure that the solvent is completely volatilized;
[0100] (4) sintering the dried carbon felt at 320° C. for 1.5 h in a nitrogen atmosphere to enhance the bonding strength between the PTFE coating and the carbon felt substrate, and after naturally cooling to room temperature, rinsing the surface with deionized water to remove loose particles and residues, thereby obtaining the modified cathode;
[0101] The anode is a modified anode, which is prepared by the following method:
[0102] (1) A titanium plate (size of 2 cm×2 cm×2 mm) was used as the anode electrode body and polished with 500-mesh metallographic sandpaper to remove the surface oxide film, then rinsed with water, immersed in a 40 wt% NaOH solution, treated at 90° C. for 1 h, degreased, rinsed with water, and dried in an oven at 120° C. for 1 h to obtain a pretreated titanium plate;
[0103] (2) adding RuO2 nanoparticles (average particle size of 20 nm) into N-methylpyrrolidone and ultrasonically dispersing for 1 h to obtain an electrocatalyst activator slurry with a RuO2 nanoparticle content of 3 wt%;
[0104] (4) The electrocatalytic activator slurry was scraped onto both sides of the pretreated titanium plate to form a wet film with a thickness of 5 μm, and the film was placed in a vacuum drying oven at 100° C. for curing for 10 h to obtain the modified anode.
[0105] Comparative Example 3
[0106] An electrode assembly for preparing hydrogen peroxide by electrolyzing water, comprising a modified cathode and a modified anode;
[0107] The modified cathode is prepared by the following method:
[0108] (1) A carbon felt (size: 2 cm × 2 cm × 2 mm) was used as a cathode electrode body and was immersed in deionized water for ultrasonic cleaning for 30 min to remove surface dirt, and then placed in an oven at 150° C. for drying for 3 h to obtain a pretreated carbon felt;
[0109] (2) adding polytetrafluoroethylene PTFE powder (average particle size of 1 μm), fluorine-containing additives and nonylphenol polyoxyethylene ether in a mass ratio of 10:2:1 to ethanol and ultrasonically dispersing for 30 minutes to obtain a PTFE slurry with a PTFE content of 7 wt%;
[0110] Wherein, the fluorine-containing additive is a copolymer of perfluorooctylethyl methacrylate and methacrylate, and the molar ratio of perfluorooctylethyl methacrylate to methacrylate is 5:1;
[0111] The preparation method comprises: adding perfluorooctylethyl methacrylate and methyl acrylate into water at a molar ratio of 5:1, stirring and mixing evenly, adding a redox initiator (a mixture of potassium persulfate and sodium bisulfite, with a mass ratio of potassium persulfate and sodium bisulfite of 2:1) with a mass percentage of 5wt% of methyl methacrylate under a nitrogen protective atmosphere, stirring and reacting at 50°C for 4h, concentrating, and vacuum drying to obtain the fluorine-containing additive;
[0112] (3) Spray the PTFE slurry evenly on both sides of the pretreated carbon felt so that the PTFE loading is 5 wt %. First, dry it naturally in a fume hood for 20 min, and then dry it in an oven at 180 ° C for 0.5 h to ensure that the solvent is completely volatilized;
[0113] (4) sintering the dried carbon felt at 320° C. for 1.5 h in a nitrogen atmosphere to enhance the bonding strength between the PTFE coating and the carbon felt substrate, and after naturally cooling to room temperature, rinsing the surface with deionized water to remove loose particles and residues, thereby obtaining the modified cathode;
[0114] The modified anode is prepared by the following method:
[0115] (1) A titanium plate (size of 2 cm×2 cm×2 mm) was used as the anode electrode body and polished with 500-mesh metallographic sandpaper to remove the surface oxide film, then rinsed with water, immersed in a 40 wt% NaOH solution, treated at 90° C. for 1 h, degreased, rinsed with water, and dried in an oven at 120° C. for 1 h to obtain a pretreated titanium plate;
[0116] (2) Install the pretreated titanium plate and TiO2 sputtering target on the corresponding fixtures in the magnetron sputtering chamber and evacuate to 0.5×10 -3 Pa, then nitrogen was injected to make the pressure of the sputtering chamber 1.5Pa, the sputtering system was turned on and the current was maintained at 25mA, the voltage was maintained at 25V, and after sputtering for 20min, porous TiO2 layers (thickness of 1μm) were formed on both sides of the titanium plate;
[0117] (3) adding RuO2 nanoparticles (average particle size of 20 nm) into N-methylpyrrolidone and ultrasonically dispersing for 1 h to obtain an electrocatalyst activator slurry with a RuO2 nanoparticle content of 3 wt%;
[0118] (4) The electrocatalytic activator slurry was scraped onto the surface of the porous TiO2 layer to form a wet film with a thickness of 5 μm, and the film was placed in a vacuum drying oven at 100° C. for curing for 10 h to obtain the modified anode.
[0119] The modified anode and the modified cathode obtained in the above examples and comparative examples were respectively prepared according to Figure 1 The schematic diagram of the device shown is assembled at intervals of 1 mm, with a polytetrafluoroethylene PTFE film mesh as a partition, the modified anode, the modified cathode and the partition are fixed as a whole inside the integrally hollowed-out shell, and then added to the electrolytic cell, the electrolyte is 300 mL of 150 TDS sodium bicarbonate solution, the stirring rate is 1500 rpm, and electrolysis is performed at a constant voltage of 12 V. The electrolyte is rapidly stirred in the electrochemical reaction tank, and the current and hydrogen peroxide yield of each embodiment and comparative example after 6 minutes of reaction are shown in Table 1 below.
[0120] Table 1 Corresponding current and hydrogen peroxide production of the electrode assembly in the embodiment and comparative example
[0121]
[0122]
[0123] From the results in Table 1 above, it can be seen that the electrode assembly of the present invention can not only react the oxygen dissolved in water through the bidirectional optimization of the cathode and anode, but also enhance the capture ability of gaseous micro-nano bubbles, further improving the efficiency of the electrochemical reaction. And compared with ionic fluorine-containing additives, the simple addition of fluorine-containing additives does not contribute to the efficiency of hydrogen peroxide production of the obtained electrode assembly.
[0124] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An electrode assembly for preparing hydrogen peroxide by electrolyzing water, It is characterized in that including a modified cathode and a modified anode; The modified cathode comprises a cathode electrode body and a hydrophobic polymer layer loaded on the cathode electrode body, and the modified anode comprises an anode electrode body, a porous metal oxide layer loaded on the anode electrode body and an electrocatalytic activator layer loaded on the porous metal oxide layer.
2. The electrode assembly for preparing hydrogen peroxide by electrolyzing water according to claim 1, It is characterized in that The modified cathode is obtained by coating the surface of the cathode electrode body with a hydrophobic polymer slurry and then sintering; Preferably, the cathode electrode body is at least one of a titanium plate, a carbon felt, a nickel sheet or nickel foam, and the hydrophobic polymer is at least one of polytetrafluoroethylene PTFE, polyvinylidene fluoride PVDF, fluorinated ethylene propylene copolymer or polyhexafluoropropylene; Preferably, the content of the hydrophobic polymer in the hydrophobic polymer slurry is 1-10 wt %.
3. The electrode assembly for preparing hydrogen peroxide by electrolyzing water according to claim 2, It is characterized in that The hydrophobic polymer slurry also includes a surfactant, and the surfactant is at least one of sucrose monolaurate, sucrose monooleate, polyethylene glycol distearate, hydroxyethyl cellulose ether, nonylphenol polyoxyethylene ether or fatty alcohol polyoxyethylene ether; Preferably, the content of surfactant in the hydrophobic polymer slurry is 0.1-1 wt %.
4. The electrode assembly for preparing hydrogen peroxide by electrolyzing water according to claim 2 or 3, It is characterized in that The hydrophobic polymer slurry also includes an ionic fluorine-containing additive, which is a copolymer of perfluorooctylethyl methacrylate, methacrylate and methacryloyloxyethyl trimethylammonium chloride; Preferably, the molar ratio of perfluorooctylethyl methacrylate, methacrylate and methacryloyloxyethyltrimethylammonium chloride is 10:1-3:1-3; Preferably, the content of the ionic fluorine-containing additive in the hydrophobic polymer slurry is 0.1-2 wt %.
5. The electrode assembly for preparing hydrogen peroxide by electrolyzing water according to any one of claims 2 to 4, It is characterized in that The sintering temperature is 280-350° C., and the sintering time is 0.5-2 h.
6. The electrode assembly for preparing hydrogen peroxide by electrolyzing water according to any one of claims 1 to 5, It is characterized in that The modified anode is obtained by depositing porous metal oxide on the surface of the anode electrode body, coating it with electrocatalytic activator slurry and then curing it; Preferably, the anode electrode body is at least one of a titanium plate, a nickel sheet, a stainless steel mesh or a graphite plate, and the porous metal oxide is TiO 2 、Co 3 O 4 、MnO 2 SnO 2 、ZrO 2 or SiO 2 At least one of the electrocatalysts, wherein the electrocatalyst is RuO 2 or IrO 2 At least one of .
7. The electrode assembly for preparing hydrogen peroxide by electrolyzing water according to claim 6, It is characterized in that The electrocatalyst activator slurry also includes polyaniline; Preferably, the content of the electrocatalyst activator in the electrocatalyst activator slurry is 1-5 wt %, and the content of the polyaniline is 0.1-0.5 wt %.
8. The electrode assembly for preparing hydrogen peroxide by electrolyzing water according to claim 6 or 7, It is characterized in that The porous metal oxide is obtained by physical vapor deposition, chemical vapor deposition, impregnation reduction or impregnation sintering; Preferably, the curing temperature is 80-120° C. and the curing time is 6-12 hours.
9. A device for preparing hydrogen peroxide by electrolyzing water, It is characterized in that The device comprises the electrode assembly according to any one of claims 1 to 8.
10. The device for preparing hydrogen peroxide by electrolyzing water according to claim 9, It is characterized in that The device comprises a modified cathode, a modified anode, a separator and a housing; The separator is located between the modified cathode and the modified anode and separates the modified cathode from the modified anode; The shell is a hollow shell and integrally fixes the modified cathode, the modified anode and the separator therein.