Carbon fiber fabric-based flexible electrode and preparation method thereof
By growing ZIF-L and PANI in situ on carbon fiber fabrics, the modified electrodes are formed, and the conductivity and stability problems of flexible electrodes are solved, and the preparation of high-performance flexible electrodes is realized, with good electrochemical and mechanical properties.
Patent Information
- Application Number
- CN202411034046.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing flexible electrodes have low conductivity, stability and specific capacity, making it difficult to meet the needs of high-performance flexible supercapacitors.
Carbon fiber fabric is used as the supporting structure, and the metal organic frame ZIF-L and conductive polymer PANI are grown in situ on its surface after oxidation treatment to form PANI@ZIF-L modified carbon fiber fabric to improve conductivity and electrochemical properties.
A high-performance flexible electrode with a conductivity of 500-2400S/cm, an area specific capacitance of 800-2000mF/cm-2, and a 10,000-capacitance retention rate of 60-90% in charge and discharge cycles, with good mechanical properties and electrical performance. Chemical properties.
Smart Images

Figure CN118957994A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flexible electrode materials, and in particular relates to a carbon fiber fabric-based flexible electrode and a preparation method thereof. Background Art
[0002] In order to meet the needs of wearable portable devices, energy storage devices have been developed in the direction of safety, lightweight and flexibility, further stimulating the growing demand for flexible energy storage devices; flexible supercapacitors stand out among many energy storage devices because they have comparable power density and longer cycle life as traditional capacitors, and are safe, fast charging and discharging, excellent flexibility and low environmental pollution, and perfectly meet the development needs of wearable smart devices.
[0003] In the field of high-performance flexible supercapacitors, textile materials are ideal flexible substrates and promising functional components. Compared with other flexible substrates, the most obvious feature of textile materials is the hierarchical structure fibers containing multi-scale geometric structures. Moreover, textile materials are ideal flexible substrates for carrying active materials due to their high conductivity, good flexibility and mechanical properties.
[0004] At present, flexible electrodes are constructed by growing pseudocapacitive materials on the surface of fabrics. However, their low conductivity greatly hinders their capacitive performance. Although conductive polymer electrode materials have the advantages of large theoretical specific capacitance, good conductivity, low cost, and easy preparation, they have been widely used in supercapacitors. However, conductive polymer materials themselves are too rigid and difficult to load on the surface of carbon fiber fabrics. After severe mechanical deformation, they are easily detached from the support in large quantities, resulting in low cycle stability and specific capacity of the electrode materials. Summary of the invention
[0005] In view of the technical problems existing in the prior art, the present invention provides a carbon fiber fabric-based flexible electrode and a preparation method thereof to solve the technical problems of low conductivity, stability and specific capacity of the existing flexible electrodes.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The present invention provides a method for preparing a carbon fiber fabric-based flexible electrode, comprising:
[0008] performing oxidation treatment on the carbon fiber fabric to obtain pre-oxidized carbon fiber fabric;
[0009] The pre-oxidized carbon fiber fabric is placed in a Co(NO3)2·6H2O solution for vacuum impregnation to obtain a vacuum impregnated fabric; the vacuum impregnated fabric is added to a 2-methylimidazole solution for in-situ growth of AIF-L reaction, and after washing and drying, a ZIF-L modified carbon fiber fabric is obtained;
[0010] The ZIF-L modified carbon fiber fabric is placed in an APS solution for impregnation to obtain an impregnated fabric; the impregnated fabric is added to an aniline acid solution for in-situ redox reaction to obtain a PANI@ZIF-L modified carbon fiber fabric;
[0011] The PANI@ZIF-L modified carbon fiber fabric is subjected to vacuum drying treatment to obtain the carbon fiber fabric-based flexible electrode.
[0012] Further, the carbon fiber fabric is subjected to oxidation treatment to obtain a pre-oxidized carbon fiber fabric, which is specifically as follows:
[0013] The carbon fiber fabric is immersed in a mixed acid solution, stirred in a water bath and then washed to obtain a pre-oxidized carbon fiber fabric; wherein the mixed acid solution is a mixed solution of concentrated nitric acid and concentrated sulfuric acid.
[0014] Furthermore, the carbon fiber fabric is immersed in the mixed acid solution, stirred in a water bath and then washed to obtain the pre-oxidized carbon fiber fabric. The water bath stirring temperature is 35-50° C. and the time is 1-4 hours.
[0015] Furthermore, the pre-oxidized carbon fiber fabric is placed in a Co(NO3)2·6H2O solution for vacuum impregnation. In the process of obtaining the vacuum-impregnated fabric, the vacuum degree of the vacuum impregnation is 0.01-0.1MPa and the temperature is 60-100°C; wherein the concentration of the Co(NO3)2·6H2O solution is 0.1-0.5mmol / mL.
[0016] Furthermore, the vacuum impregnated fabric is added to a 2-methylimidazole solution to perform an in-situ growth AIF-L reaction. After washing and drying, the ZIF-L modified carbon fiber fabric is obtained. The time for the in-situ growth AIF-L reaction is 2-4 hours, and the drying temperature is 60-80°C; wherein the concentration of the 2-methylimidazole solution is 8-10 mmol / mL.
[0017] Furthermore, the ZIF-L modified carbon fiber fabric is placed in an APS solution for impregnation. In the process of obtaining the impregnated fabric, the impregnation time is 1-3 hours and the temperature is 4-10°C.
[0018] Furthermore, the impregnated fabric is added to an aniline acid solution to perform an in-situ redox reaction to obtain a PANI@ZIF-L modified carbon fiber fabric. The time of the in-situ redox reaction is 2-4 hours and the temperature is 4-10°C.
[0019] Furthermore, during the vacuum drying process of the PANI@ZIF-L modified carbon fiber fabric, the drying temperature is 60-100° C., the drying time is 1-10 h, and the vacuum degree is 0.01-0.09 MPa.
[0020] The present invention also provides a carbon fiber fabric-based flexible electrode, which is prepared using the method for preparing a carbon fiber fabric-based flexible electrode.
[0021] Furthermore, the conductivity of the carbon fiber fabric-based flexible electrode is 500-2400S / cm; at a current density of 1 mA / cm 2 When the area specific capacitance is 800-2000mF / cm -2 ; at 20mA / cm 2 At a current density of , the charge and discharge cycles are 10,000 times, and the capacitance retention rate is 60-90%.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention provides a carbon fiber fabric-based flexible electrode and a preparation method thereof, wherein ZIF-L is grown in situ on pre-oxidized carbon fiber fabric to obtain ZIF-L modified carbon fiber fabric, and PANI@ZIF-L modified carbon fiber fabric is obtained by in situ redox reaction with aniline solution, and then the carbon fiber fabric-based flexible electrode is obtained by drying; wherein the carbon fiber fabric is selected as the supporting structure of the flexible electrode to improve the flexibility of the electrode; the metal organic framework ZIF-L is used as the active material to provide capacity, and a load platform with high specific surface area and porosity is provided to ensure that ions are charged and discharged. The invention relates to a method for preparing a flexible electrode for supercapacitors by using carbon fiber fabric, ZIF-L and PANI to improve the conductivity and electrochemical performance of the electrode by using PANI as a conductive layer and an active layer. ... 2 When the area specific capacitance is 800-2000mF / cm -2 ; at 20mA / cm 2 At a current density of , the charge and discharge cycles are 10,000 times, and the capacitance retention rate is 60-90%. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 is a SEM image of the carbon fiber fabric in Example 4;
[0026] Figure 2 This is the SEM image of the ZIF-L modified carbon fiber fabric in Example 4. DETAILED DESCRIPTION
[0027] In order to make the technical problems, technical solutions and beneficial effects solved by this application clearer, the technical solutions in the embodiments of this application will be described clearly and completely in combination with the drawings in the embodiments of this application; obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0028] The present invention provides a method for preparing a carbon fiber fabric-based flexible electrode, comprising the following steps:
[0029] Step 1, impregnating the carbon fiber fabric with a mixed acid solution, stirring in a water bath at 35-50° C. for 1-4 hours, and after stirring, washing with a large amount of deionized water for multiple times to obtain a pre-oxidized carbon fiber fabric; wherein the mixed acid solution is obtained by mixing concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:1-4, the mass fraction of the concentrated nitric acid is 65.0%-68.0%, and the mass fraction of the concentrated sulfuric acid is 95.0%-98.0%.
[0030] Step 2: Add 2-10 mmol of Co(NO3)2·6H2O to deionized water, and disperse it ultrasonically for 5-15 min to obtain a Co(NO3)2·6H2O solution with a concentration of 0.1-0.5 mmol / mL; add 16-20 mmol of 2-methylimidazole to deionized water, and disperse it ultrasonically for 5-15 min to obtain a 2-methylimidazole solution with a concentration of 8-10 mmol / mL.
[0031] Step 3, placing 7.5-10 mmol of ammonium persulfate (APS) in an ice water bath at 0-5°C and mechanically stirring for 0.5-2 h to obtain an APS solution; placing 3-8 mmol of aniline monomer in an ice water bath at 0-5°C and mechanically stirring for 0.5-1.5 h, and then dispersing in a hydrochloric acid solution with a concentration of 1-5 mol / L to obtain an aniline acid solution with a concentration of 0.15-0.4 mmol / mL.
[0032] Step 4, placing the pre-oxidized carbon fiber fabric in the Co(NO3)2·6H2O solution prepared in step 2, and performing vacuum impregnation for 1-4 hours at a vacuum degree of 0.01-0.1 MPa and a temperature of 60-100°C to obtain a vacuum-impregnated fabric; transferring the vacuum-impregnated fabric to the 2-methylimidazole solution prepared in step 2, and performing an in-situ growth ZIF-L reaction for 2-4 hours. After the reaction is completed, washing it with deionized water and anhydrous ethanol for multiple times, and drying it in a blast drying oven at 60-80°C to obtain a ZIF-L modified carbon fiber fabric.
[0033] Step 5, placing the ZIF-L modified carbon fiber fabric in step 4 in the APS solution prepared in step 3, and immersing it at a temperature of 4-10°C for 1-3 hours to obtain an impregnated fabric; transferring the impregnated fabric to the aniline acid solution prepared in step 3, and performing an in-situ redox reaction at 4-10°C for 2-4 hours to grow a conductive polymer polyaniline (PANI) on the surface of the ZIF-L modified carbon fiber fabric to obtain PANI@ZIF-L modified carbon fiber fabric.
[0034] Step 6: Place the PANI@ZIF-L modified carbon fiber fabric in step 5 in a vacuum drying oven, and perform vacuum drying treatment at a vacuum degree of 0.01-0.09 MPa and a drying temperature of 60-100° C. to obtain the carbon fiber fabric-based flexible electrode.
[0035] In the present invention, the carbon fiber fabric-based flexible electrode prepared by using carbon fiber fabric, ZIF-L and PANI has high conductivity and good electrochemical performance; specifically, the conductivity of the carbon fiber fabric-based flexible electrode is 500-2400S / cm; at a current density of 1mA / cm 2 When the area specific capacitance is 800-2000mF / cm -2 ; at 20mA / cm 2 At a current density of , the charge and discharge cycles are 10,000 times, and the capacitance retention rate is 60-90%.
[0036] Preparation principle:
[0037] The preparation method of the carbon fiber fabric-based flexible electrode of the present invention adopts the carbon fiber fabric as the supporting structure of the flexible electrode and uses the carbon fiber fabric as the substrate, thereby effectively improving the flexibility of the electrode; the carbon fiber fabric is pre-oxidized by using a mixed acid solution of concentrated nitric acid and concentrated sulfuric acid, and the surface of the oxidized carbon fiber fabric becomes rough, thereby improving the surface activity of the carbon fiber fabric, so that some functional groups are oxidized and can react with external compounds; the pre-oxidized carbon fiber fabric is placed in a Co(NO3)2·6H2O solution for vacuum impregnation, and then transferred to a 2-methylimidazole solution for in-situ growth of ZIF-L reaction, using the metal organic framework ZIF-L as the active The ZIF-L modified carbon fiber fabric is immersed in an APS solution and then transferred to an aniline acid solution for an in-situ redox reaction to grow a conductive polymer polyaniline on the surface of the ZIF-L modified carbon fiber fabric, thereby realizing PANI as a conductive layer and an active layer, thereby improving the conductivity and electrochemical properties of the electrode. It should be noted that by regulating the content of ZIF-L and PANI in the carbon fiber fabric, an electrode for a supercapacitor with good mechanical properties, high electrochemical properties and high cycle stability is prepared.
[0038] Example 1
[0039] This embodiment 1 provides a method for preparing a carbon fiber fabric-based flexible electrode, comprising the following steps:
[0040] Step 1, impregnating the carbon fiber fabric with a mixed acid solution, stirring it in a water bath at 35°C for 1h, and after stirring, washing it multiple times with a large amount of deionized water to obtain a pre-oxidized carbon fiber fabric; wherein the mixed acid solution is obtained by mixing concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:1, the mass fraction of the concentrated nitric acid is 65%, and the mass fraction of the concentrated sulfuric acid is 95%.
[0041] Step 2: Add 2 mmol of Co(NO3)2·6H2O to deionized water and disperse it ultrasonically for 5 minutes to obtain a Co(NO3)2·6H2O solution with a concentration of 0.1 mmol / mL; add 16 mmol of 2-methylimidazole to deionized water and disperse it ultrasonically for 5 minutes to obtain a 2-methylimidazole solution with a concentration of 8 mmol / mL.
[0042] Step 3, placing 7.5 mmol of ammonium persulfate (APS) in an ice-water bath at 0°C and mechanically stirring for 0.5 h to obtain an APS solution; placing 3 mmol of aniline monomer in an ice-water bath at 0°C and mechanically stirring for 0.5 h, and then dispersing it in a hydrochloric acid solution with a concentration of 1 mol / L to obtain an aniline acid solution with a concentration of 0.15 mmol / mL.
[0043] Step 4, placing the pre-oxidized carbon fiber fabric in the Co(NO3)2·6H2O solution prepared in step 2, and performing vacuum impregnation for 1 hour at a vacuum degree of 0.01 MPa and a temperature of 60°C to obtain a vacuum-impregnated fabric; transferring the vacuum-impregnated fabric to the 2-methylimidazole solution prepared in step 2, and performing an in-situ growth ZIF-L reaction for 2 hours. After the reaction is completed, washing it with deionized water and anhydrous ethanol for multiple times, and drying it in a blast drying oven at 60°C to obtain a ZIF-L modified carbon fiber fabric.
[0044] Step 5, placing the ZIF-L modified carbon fiber fabric in step 4 in the APS solution prepared in step 3, and immersing it at a temperature of 4°C for 1 hour to obtain an impregnated fabric; transferring the impregnated fabric to the aniline acid solution prepared in step 3, and performing an in-situ redox reaction at 4°C for 2 hours to grow a conductive polymer polyaniline (PANI) on the surface of the ZIF-L modified carbon fiber fabric to obtain PANI@ZIF-L modified carbon fiber fabric.
[0045] Step 6: Place the PANI@ZIF-L modified carbon fiber fabric in step 5 in a vacuum drying oven, and perform vacuum drying treatment at a vacuum degree of 0.01 MPa and a drying temperature of 60° C. for 1 h to obtain the carbon fiber fabric-based flexible electrode.
[0046] Performance testing:
[0047] The performance of the carbon fiber fabric-based flexible electrode prepared in Example 1 was tested, and the test results were as follows: the conductivity of the carbon fiber fabric-based flexible electrode was 500 S / m; at a current density of 1 mA / cm 2 When the area specific capacitance is 800mF / cm -2 , at 20mA / cm 2 At a current density of , the charge and discharge cycles were 10,000 times and the capacitance retention rate was 65%.
[0048] Example 2
[0049] This embodiment 2 provides a method for preparing a carbon fiber fabric-based flexible electrode, comprising the following steps:
[0050] Step 1, impregnating the carbon fiber fabric with a mixed acid solution, stirring it in a water bath at 50°C for 4 hours, and after stirring, washing it multiple times with a large amount of deionized water to obtain a pre-oxidized carbon fiber fabric; wherein the mixed acid solution is obtained by mixing concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:4, the mass fraction of the concentrated nitric acid is 68%, and the mass fraction of the concentrated sulfuric acid is 98%.
[0051] Step 2: Add 10 mmol of Co(NO3)2·6H2O to deionized water, and disperse it ultrasonically for 15 minutes to obtain a Co(NO3)2·6H2O solution with a concentration of 0.5 mmol / mL; add 20 mmol of 2-methylimidazole to deionized water, and disperse it ultrasonically for 15 minutes to obtain a 2-methylimidazole solution with a concentration of 10 mmol / mL.
[0052] Step 3, place 10 mmol of ammonium persulfate (APS) in an ice-water bath at 5°C and mechanically stir for 2 hours to obtain an APS solution; place 8 mmol of aniline monomer in an ice-water bath at 5°C and mechanically stir for 1.5 hours, then disperse it in a hydrochloric acid solution with a concentration of 5 mol / L to obtain an aniline acid solution with a concentration of 0.4 mmol / mL.
[0053] Step 4, placing the pre-oxidized carbon fiber fabric in the Co(NO3)2·6H2O solution prepared in step 2, and performing vacuum impregnation for 4 hours at a vacuum degree of 0.1 MPa and a temperature of 100°C to obtain a vacuum-impregnated fabric; transferring the vacuum-impregnated fabric to the 2-methylimidazole solution prepared in step 2, and performing an in-situ growth ZIF-L reaction for 4 hours. After the reaction, the fabric is washed with deionized water and anhydrous ethanol for multiple times, and dried in a blast drying oven at 80°C to obtain a ZIF-L modified carbon fiber fabric.
[0054] Step 5, placing the ZIF-L modified carbon fiber fabric in step 4 in the APS solution prepared in step 3, and immersing it at a temperature of 10°C for 3 hours to obtain an impregnated fabric; transferring the impregnated fabric to the aniline acid solution prepared in step 3, and performing an in-situ redox reaction at 10°C for 4 hours to grow a conductive polymer polyaniline (PANI) on the surface of the ZIF-L modified carbon fiber fabric to obtain PANI@ZIF-L modified carbon fiber fabric.
[0055] Step 6: Place the PANI@ZIF-L modified carbon fiber fabric in step 5 in a vacuum drying oven, and perform vacuum drying treatment for 10 hours at a vacuum degree of 0.09 MPa and a drying temperature of 100° C. to obtain the carbon fiber fabric-based flexible electrode.
[0056] Performance testing:
[0057] The performance of the carbon fiber fabric-based flexible electrode prepared in Example 2 was tested, and the test results were as follows: the conductivity of the carbon fiber fabric-based flexible electrode was 2200 S / m; at a current density of 1 mA / cm 2 When the area specific capacitance is 1800mF / cm -2 , at 20mA / cm 2 At a current density of , the charge and discharge cycles were 10,000 times and the capacitance retention rate was 85%.
[0058] Example 3
[0059] This embodiment 3 provides a method for preparing a carbon fiber fabric-based flexible electrode, comprising the following steps:
[0060] Step 1, impregnating the carbon fiber fabric with a mixed acid solution, stirring it in a water bath at 40°C for 2.5 hours, and after stirring, washing it multiple times with a large amount of deionized water to obtain a pre-oxidized carbon fiber fabric; wherein the mixed acid solution is obtained by mixing concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:2, the mass fraction of the concentrated nitric acid is 65%, and the mass fraction of the concentrated sulfuric acid is 98%.
[0061] Step 2: Add 6 mmol of Co(NO3)2·6H2O to deionized water, and disperse it ultrasonically for 10 min to obtain a Co(NO3)2·6H2O solution with a concentration of 0.3 mmol / mL; add 18 mmol of 2-methylimidazole to deionized water, and disperse it ultrasonically for 10 min to obtain a 2-methylimidazole solution with a concentration of 9 mmol / mL.
[0062] Step 3: Place 9 mmol of ammonium persulfate (APS) in an ice-water bath at 3°C and mechanically stir for 1.5 h to obtain an APS solution; place 6 mmol of aniline monomer in an ice-water bath at 3°C and mechanically stir for 1 h, then disperse it in a 3 mol / L hydrochloric acid solution to obtain a 0.2 mmol / mL aniline acid solution.
[0063] Step 4, placing the pre-oxidized carbon fiber fabric in the Co(NO3)2·6H2O solution prepared in step 2, and performing vacuum impregnation for 2.5 hours at a vacuum degree of 0.05 MPa and a temperature of 80°C to obtain a vacuum-impregnated fabric; transferring the vacuum-impregnated fabric to the 2-methylimidazole solution prepared in step 2, and performing an in-situ growth ZIF-L reaction for 3 hours. After the reaction is completed, washing it with deionized water and anhydrous ethanol for multiple times, and drying it in a blast drying oven at 70°C to obtain a ZIF-L modified carbon fiber fabric.
[0064] Step 5, placing the ZIF-L modified carbon fiber fabric in step 4 in the APS solution prepared in step 3, and immersing it at a temperature of 7°C for 2 hours to obtain an impregnated fabric; transferring the impregnated fabric to the aniline acid solution prepared in step 3, and performing an in-situ redox reaction at 10°C for 4 hours to grow a conductive polymer polyaniline (PANI) on the surface of the ZIF-L modified carbon fiber fabric to obtain PANI@ZIF-L modified carbon fiber fabric.
[0065] Step 6: Place the PANI@ZIF-L modified carbon fiber fabric in step 5 in a vacuum drying oven, and perform vacuum drying treatment for 5 hours at a vacuum degree of 0.05 MPa and a drying temperature of 60° C. to obtain the carbon fiber fabric-based flexible electrode.
[0066] Performance testing:
[0067] The performance of the carbon fiber fabric-based flexible electrode prepared in Example 3 was tested, and the test results were as follows: the conductivity of the carbon fiber fabric-based flexible electrode was 1700 S / m; at a current density of 1 mA / cm 2 When the area specific capacitance is 1500mF / cm -2 , at 20mA / cm 2 At a current density of , the charge and discharge cycles were 10,000 times and the capacitance retention rate was 70%.
[0068] Example 4
[0069] This embodiment 4 provides a method for preparing a carbon fiber fabric-based flexible electrode, comprising the following steps:
[0070] Step 1, impregnating the carbon fiber fabric with a mixed acid solution, stirring it in a water bath at 35°C for 4 hours, and after stirring, washing it multiple times with a large amount of deionized water to obtain a pre-oxidized carbon fiber fabric; wherein the mixed acid solution is obtained by mixing concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:2, the mass fraction of the concentrated nitric acid is 68%, and the mass fraction of the concentrated sulfuric acid is 98%.
[0071] Step 2: Add 2 mmol of Co(NO3)2·6H2O to deionized water, and disperse it ultrasonically for 15 minutes to obtain a Co(NO3)2·6H2O solution with a concentration of 0.1 mmol / mL; add 16 mmol of 2-methylimidazole to deionized water, and disperse it ultrasonically for 15 minutes to obtain a 2-methylimidazole solution with a concentration of 8 mmol / mL.
[0072] Step 3, placing 7.5 mmol of ammonium persulfate (APS) in an ice-water bath at 0°C and mechanically stirring for 2 hours to obtain an APS solution; placing 3 mmol of aniline monomer in an ice-water bath at 0°C and mechanically stirring for 1.5 hours, and then dispersing it in a hydrochloric acid solution with a concentration of 1 mol / L to obtain an aniline acid solution with a concentration of 0.15 mmol / mL.
[0073] Step 4, placing the pre-oxidized carbon fiber fabric in the Co(NO3)2·6H2O solution prepared in step 2, and performing vacuum impregnation for 4 hours at a vacuum degree of 0.1 MPa and a temperature of 60°C to obtain a vacuum-impregnated fabric; transferring the vacuum-impregnated fabric to the 2-methylimidazole solution prepared in step 2, and performing an in-situ growth ZIF-L reaction for 4 hours. After the reaction, the fabric is washed with deionized water and anhydrous ethanol for multiple times, and dried in a blast drying oven at 60°C to obtain a ZIF-L modified carbon fiber fabric.
[0074] Step 5, placing the ZIF-L modified carbon fiber fabric in step 4 in the APS solution prepared in step 3, and immersing it at a temperature of 4°C for 3 hours to obtain an impregnated fabric; transferring the impregnated fabric to the aniline acid solution prepared in step 3, and performing an in-situ redox reaction at 4°C for 3 hours to grow a conductive polymer polyaniline (PANI) on the surface of the ZIF-L modified carbon fiber fabric to obtain PANI@ZIF-L modified carbon fiber fabric.
[0075] Step 6: Place the PANI@ZIF-L modified carbon fiber fabric in step 5 in a vacuum drying oven, and perform vacuum drying treatment for 5 hours at a vacuum degree of 0.01 MPa and a drying temperature of 60° C. to obtain the carbon fiber fabric-based flexible electrode.
[0076] Performance testing:
[0077] The performance of the carbon fiber fabric-based flexible electrode prepared in Example 4 was tested, and the test results were as follows: the conductivity of the carbon fiber fabric-based flexible electrode was 2400 S / m; at a current density of 1 mA / cm 2 When the area specific capacitance is 2000mF / cm -2 , at 20mA / cm 2 At a current density of , the charge and discharge cycles are 10,000 times and the capacitance retention rate is 90%.
[0078] Example 5
[0079] This embodiment 5 provides a method for preparing a carbon fiber fabric-based flexible electrode, comprising the following steps:
[0080] Step 1, impregnating the carbon fiber fabric with a mixed acid solution, stirring it in a water bath at 50°C for 4 hours, and after stirring, washing it multiple times with a large amount of deionized water to obtain a pre-oxidized carbon fiber fabric; wherein the mixed acid solution is obtained by mixing concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:2, the mass fraction of the concentrated nitric acid is 67%, and the mass fraction of the concentrated sulfuric acid is 97%.
[0081] Step 2: Add 2 mmol of Co(NO3)2·6H2O to deionized water and disperse it ultrasonically for 5 minutes to obtain a Co(NO3)2·6H2O solution with a concentration of 0.1 mmol / mL; add 16 mmol of 2-methylimidazole to deionized water and disperse it ultrasonically for 5 minutes to obtain a 2-methylimidazole solution with a concentration of 8 mmol / mL.
[0082] Step 3, placing 7.5 mmol of ammonium persulfate (APS) in an ice-water bath at 0°C and mechanically stirring for 0.5 h to obtain an APS solution; placing 3 mmol of aniline monomer in an ice-water bath at 0°C and mechanically stirring for 0.5 h, and then dispersing it in a hydrochloric acid solution with a concentration of 5 mol / L to obtain an aniline acid solution with a concentration of 0.15 mmol / mL.
[0083] Step 4, placing the pre-oxidized carbon fiber fabric in the Co(NO3)2·6H2O solution prepared in step 2, and performing vacuum impregnation for 4 hours at a vacuum degree of 0.01 MPa and a temperature of 60°C to obtain a vacuum-impregnated fabric; transferring the vacuum-impregnated fabric to the 2-methylimidazole solution prepared in step 2, and performing an in-situ growth ZIF-L reaction for 4 hours. After the reaction, the fabric is washed with deionized water and anhydrous ethanol for multiple times, and dried in a blast drying oven at 60°C to obtain a ZIF-L modified carbon fiber fabric.
[0084] Step 5, placing the ZIF-L modified carbon fiber fabric in step 4 in the APS solution prepared in step 3, and immersing it at a temperature of 4°C for 1 hour to obtain an impregnated fabric; transferring the impregnated fabric to the aniline acid solution prepared in step 3, and performing an in-situ redox reaction at 4°C for 2 hours to grow a conductive polymer polyaniline (PANI) on the surface of the ZIF-L modified carbon fiber fabric to obtain PANI@ZIF-L modified carbon fiber fabric.
[0085] Step 6: Place the PANI@ZIF-L modified carbon fiber fabric in step 5 in a vacuum drying oven, and perform vacuum drying treatment at a vacuum degree of 0.01 MPa and a drying temperature of 60° C. for 1 h to obtain the carbon fiber fabric-based flexible electrode.
[0086] Performance testing:
[0087] The performance of the carbon fiber fabric-based flexible electrode prepared in Example 5 was tested, and the test results were as follows: the conductivity of the carbon fiber fabric-based flexible electrode was 1600 S / m; at a current density of 1 mA / cm 2 When the area specific capacitance is 1400mF / cm -2 , at 20mA / cm 2 At a current density of , the charge and discharge cycles were repeated 10,000 times, and the capacitance retention rate was 75%.
[0088] Example 6
[0089] This embodiment 6 provides a method for preparing a carbon fiber fabric-based flexible electrode, comprising the following steps:
[0090] Step 1, impregnating the carbon fiber fabric with a mixed acid solution, stirring it in a water bath at 35°C for 4 hours, and after stirring, washing it multiple times with a large amount of deionized water to obtain a pre-oxidized carbon fiber fabric; wherein the mixed acid solution is obtained by mixing concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:2, the mass fraction of the concentrated nitric acid is 67%, and the mass fraction of the concentrated sulfuric acid is 98%.
[0091] Step 2: Add 2 mmol of Co(NO3)2·6H2O to deionized water and disperse it ultrasonically for 5 minutes to obtain a Co(NO3)2·6H2O solution with a concentration of 0.1 mmol / mL; add 16 mmol of 2-methylimidazole to deionized water and disperse it ultrasonically for 5 minutes to obtain a 2-methylimidazole solution with a concentration of 8 mmol / mL.
[0092] Step 3, placing 7.5 mmol of ammonium persulfate (APS) in an ice-water bath at 0°C and mechanically stirring for 2 hours to obtain an APS solution; placing 3 mmol of aniline monomer in an ice-water bath at 0°C and mechanically stirring for 1.5 hours, and then dispersing it in a hydrochloric acid solution with a concentration of 1 mol / L to obtain an aniline acid solution with a concentration of 0.15 mmol / mL.
[0093] Step 4, placing the pre-oxidized carbon fiber fabric in the Co(NO3)2·6H2O solution prepared in step 2, and performing vacuum impregnation for 4 hours at a vacuum degree of 0.1 MPa and a temperature of 60°C to obtain a vacuum-impregnated fabric; transferring the vacuum-impregnated fabric to the 2-methylimidazole solution prepared in step 2, and performing an in-situ growth ZIF-L reaction for 4 hours. After the reaction, the fabric is washed with deionized water and anhydrous ethanol for multiple times, and dried in a blast drying oven at 60°C to obtain a ZIF-L modified carbon fiber fabric.
[0094] Step 5, placing the ZIF-L modified carbon fiber fabric in step 4 in the APS solution prepared in step 3, and immersing it at a temperature of 10°C for 1 hour to obtain an impregnated fabric; transferring the impregnated fabric to the aniline acid solution prepared in step 3, and performing an in-situ redox reaction at 10°C for 2 hours to grow a conductive polymer polyaniline (PANI) on the surface of the ZIF-L modified carbon fiber fabric to obtain PANI@ZIF-L modified carbon fiber fabric.
[0095] Step 6: Place the PANI@ZIF-L modified carbon fiber fabric in step 5 in a vacuum drying oven, and perform vacuum drying treatment at a vacuum degree of 0.01 MPa and a drying temperature of 60° C. for 1 h to obtain the carbon fiber fabric-based flexible electrode.
[0096] Performance testing:
[0097] The performance of the carbon fiber fabric-based flexible electrode prepared in Example 6 was tested, and the test results were as follows: the conductivity of the carbon fiber fabric-based flexible electrode was 1650 S / m; at a current density of 1 mA / cm 2 When the area specific capacitance is 1500mF / cm -2 , at 20mA / cm 2 At a current density of , the charge and discharge cycles were 10,000 times and the capacitance retention rate was 82%.
[0098] As attached Figure 1-2 As shown, attached Figure 1 The SEM image of the carbon fiber fabric in Example 4 is given in Figure 2 The SEM image of the ZIF-L modified carbon fiber fabric in Example 4 is given in FIG. Figure 1 It can be seen from the figure that carbon fiber fabric is a three-dimensional mesh structure formed by interweaving carbon fibers. The surface of the carbon fiber is smooth when it is not treated, and the surface of the carbon fiber is inert. Figure 2 It can be seen that the surface of the carbon fiber becomes rough, which reflects that the surface activity of the carbon fiber fabric is improved, some functional groups are oxidized, and can react with external compounds. At the same time, the fiber surface is covered with a two-dimensional blade-like structure material in an array, which shows that ZIF-L is successfully loaded on the surface of the carbon fiber. Among them, the metal organic framework ZIF-L, as an active material, provides capacity and a loading platform with high specific surface area and porosity, which ensures the rapid transfer and diffusion of ions during the charge and discharge process, laying the foundation for the preparation of flexible electrodes with good mechanical properties, high electrochemical properties, and high cycle stability.
[0099] The carbon fiber fabric-based flexible electrode and preparation method thereof described in the present invention, taking into account the requirements that energy storage materials should meet, namely, high specific capacity and low cost, selects polyaniline with high specific capacitance, adjustable conductivity and low price and a metal organic framework ZIF-L that is simple to prepare for compounding, so as to improve the disadvantages of low capacitance and low rate characteristics caused by low conductivity of the metal organic framework. The organic combination of the two makes it difficult for the conductive polymer to expand and collapse in the process of long-term charging and discharging, thereby increasing the stability of the flexible energy storage material.
[0100] The above embodiment is only one of the implementation methods that can realize the technical solution of the present invention. The scope of protection claimed by the present invention is not limited only to this embodiment, but also includes changes, replacements and other implementation methods that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed by the present invention.
Claims
1. A method for preparing a carbon fiber fabric-based flexible electrode, characterized in that: include: performing oxidation treatment on the carbon fiber fabric to obtain pre-oxidized carbon fiber fabric; The pre-oxidized carbon fiber fabric is placed in a Co(NO3)2·6H2O solution for vacuum impregnation to obtain a vacuum impregnated fabric; the vacuum impregnated fabric is added to a 2-methylimidazole solution for in-situ growth of AIF-L reaction, and after washing and drying, a ZIF-L modified carbon fiber fabric is obtained; The ZIF-L modified carbon fiber fabric is placed in an APS solution for impregnation to obtain an impregnated fabric; the impregnated fabric is added to an aniline acid solution for in-situ redox reaction to obtain a PANI@ZIF-L modified carbon fiber fabric; The PANI@ZIF-L modified carbon fiber fabric is subjected to vacuum drying treatment to obtain the carbon fiber fabric-based flexible electrode.
2. The method for preparing a carbon fiber fabric-based flexible electrode according to claim 1, characterized in that: The process of oxidizing the carbon fiber fabric to obtain the pre-oxidized carbon fiber fabric is as follows: The carbon fiber fabric is immersed in a mixed acid solution, stirred in a water bath and then washed to obtain a pre-oxidized carbon fiber fabric; wherein the mixed acid solution is a mixed solution of concentrated nitric acid and concentrated sulfuric acid.
3. The method for preparing a carbon fiber fabric-based flexible electrode according to claim 2, characterized in that: The carbon fiber fabric is immersed in the mixed acid solution, stirred in a water bath and then washed to obtain the pre-oxidized carbon fiber fabric. The water bath stirring temperature is 35-50° C. and the time is 1-4 hours.
4. The method for preparing a carbon fiber fabric-based flexible electrode according to claim 1, characterized in that: The pre-oxidized carbon fiber fabric is placed in a Co(NO3)2·6H2O solution for vacuum impregnation. In the process of obtaining the vacuum-impregnated fabric, the vacuum degree of the vacuum impregnation is 0.01-0.1MPa and the temperature is 60-100°C; wherein the concentration of the Co(NO3)2·6H2O solution is 0.1-0.5mmol / mL.
5. The method for preparing a carbon fiber fabric-based flexible electrode according to claim 1, characterized in that: The vacuum impregnated fabric is added to a 2-methylimidazole solution to perform an in-situ growth AIF-L reaction. After washing and drying, the ZIF-L modified carbon fiber fabric is obtained. The time for the in-situ growth AIF-L reaction is 2-4 hours, and the drying temperature is 60-80°C; wherein the concentration of the 2-methylimidazole solution is 8-10 mmol / mL.
6. The method for preparing a carbon fiber fabric-based flexible electrode according to claim 1, characterized in that: The ZIF-L modified carbon fiber fabric is placed in an APS solution for impregnation. In the process of obtaining the impregnated fabric, the impregnation time is 1-3 hours and the temperature is 4-10°C.
7. The method for preparing a carbon fiber fabric-based flexible electrode according to claim 1, characterized in that: The impregnated fabric is added to a aniline acid solution to perform an in-situ redox reaction to obtain a PANI@ZIF-L modified carbon fiber fabric. The time of the in-situ redox reaction is 2-4 hours and the temperature is 4-10°C.
8. The method for preparing a carbon fiber fabric-based flexible electrode according to claim 1, characterized in that: During the vacuum drying process of the PANI@ZIF-L modified carbon fiber fabric, the drying temperature is 60-100° C., the drying time is 1-10 h, and the vacuum degree is 0.01-0.09 MPa.
9. A carbon fiber fabric-based flexible electrode, characterized in that: The electrode is prepared by the method for preparing a carbon fiber fabric-based flexible electrode as described in any one of claims 1 to 8.
10. The carbon fiber fabric-based flexible electrode according to claim 9, characterized in that: The conductivity of the carbon fiber fabric-based flexible electrode is 500-2400S / cm; at a current density of 1mA / cm 2 When the area specific capacitance is 800-2000mF / cm -2 ; at 20mA / cm 2 At a current density of , the charge and discharge cycles are 10,000 times, and the capacitance retention rate is 60-90%.
Citation Information
Patent Citations
Novel method for preparing polyaniline composite conductive fabric
CN102337679A
Production method of metal-based carbon fiber composite electrode, and product and application thereof
CN112992558A
CoSx / PANI / MF composite flexible electrode and preparation method and application thereof
CN117936286A
Flexible conductive fiber membrane material and preparation method therefor
WO2021114321A1
Cited By
Flexible electric heating material and preparation method and application thereof
CN119824682A
Medical-grade PEEK composite material with developing property and preparation method of medical-grade PEEK composite material
CN120754329A