Preparation method of cool-feeling anti-mosquito water-based superfine fiber synthetic leather

By adopting water-based microfiber base fabric and multi-layer structure design in the shoe material, combined with phase-change microcapsules and anti-mosquito microcapsules, the existing shoe material has solved the problem of insufficient coolness and anti-mosquito function in summer, and achieved long-lasting The cool feeling and anti-mosquito effect are improved and anti-destructive properties are improved.

CN118958007APending Publication Date: 2024-11-15ANAN CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411029935.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing shoe materials lack effective cooling and anti-mosquito functions in summer, and these functions are prone to failure after multiple washes, and cannot meet the needs of cooling and anti-mosquito needs at the same time.

Method used

The water-based microfiber base cloth is used for preparation, and the triple cooling technology is designed through impregnation, post-treatment and surface-making processes to form a multi-layer structure of phase-change microcapsules and anti-mosquito microcapsules. The intelligent constant temperature regulation of phase-change microcapsules and The sustained release effect of anti-mosquito microcapsules, combined with silicon-based feel agent and thickener, creates a lasting cool feeling and anti-mosquito effect.

Benefits of technology

It realizes the long-lasting cool feeling and anti-mosquito effect of the shoe material, is resistant to washing and damage, can be continuously effective after multiple uses, and meets the requirements of high-standard contact cool feeling detection.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of cool-feeling anti-mosquito water-based superfine fiber synthetic leather. The preparation method comprises the following steps: (1) preparing water-based superfine fiber base cloth; (2) carrying out water-based wet-process impregnation treatment on the base cloth, and then carrying out splitting treatment to obtain split base cloth; (3) carrying out post-treatment on the split base cloth to obtain a superfine fiber synthetic leather base; (4) a dry-method surface making process: sequentially coating a surface material layer and a bottom material layer on release paper to prepare a dry-method layer of the water-based cool microfiber synthetic leather; and (5) laminating and drying the water-based cool microfiber synthetic leather dry-method layer and a superfine fiber synthetic leather base, cooling, and stripping from the release paper to obtain a cool anti-mosquito water-based superfine fiber synthetic leather finished product. The synthetic leather is mainly applied to shoe materials, and has excellent, lasting and effective cool feeling and anti-mosquito effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of synthetic leather, in particular to a method for preparing cool and mosquito-proof water-based ultrafine fiber synthetic leather. Background Art

[0002] As the temperature rises in the hot summer, mosquitoes also breed in large numbers. The feeling of heat and mosquito bites are the main reasons that affect human comfort in summer. In order to improve comfort, cool clothing for dealing with the heat and mosquito repellent patches for preventing mosquito bites are available on the market. Summer clothing is mainly short skirts, and cool clothing has limited cooling performance on the lower limbs of the human body, especially the feet. Mosquito repellent patches are inconvenient to carry and also have limited mosquito repellent effect on the lower limbs of the human body. The necessary clothing for the lower limbs of the human body is footwear. At present, there are few cool or mosquito repellent functions for footwear, and the functions are relatively single, either single mosquito repellent or single cool function. In addition, the corresponding cool or mosquito repellent effect of the footwear is easily lost after the footwear is washed several times (such as five or six times).

[0003] Based on the above problems, this case conducted an in-depth study on the above problems and proposed a preparation method of cool and mosquito-proof water-based microfiber synthetic leather, which resulted in this case. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a cool and mosquito-proof water-based ultrafine fiber synthetic leather, which has excellent, lasting and effective cool feeling and mosquito-proof effects.

[0005] In order to achieve the above object, the solution of the present invention is:

[0006] A method for preparing a cool and anti-mosquito water-based microfiber synthetic leather comprises the following steps:

[0007] (1) preparing a water-based ultrafine fiber base fabric;

[0008] (2) performing an aqueous wet impregnation treatment on a water-based microfiber base fabric, and then performing a fiber opening treatment to obtain a fiber opening base fabric; the impregnation slurry for the impregnation treatment comprises the following components in parts by weight: 100 parts by weight of water-based polyurethane, 15-30 parts by weight of phase change microcapsules, 3-5 parts by weight of a water-based thickener, 3-5 parts by weight of a water-based enhancer, and 1-2 parts by weight of a water-based color paste;

[0009] (3) post-processing the open fiber base fabric, wherein the open fiber base fabric is dried in an oven, then three-immersed and three-rolled in an oil tank containing 12-20% by weight of a cool feeling treatment agent and 8-12% by weight of a silicone-based hand feeling agent, and then subjected to high temperature baking treatment to obtain an ultrafine fiber synthetic leather bass;

[0010] (4) Dry surface making process, coating the surface layer mixture on the release paper, heating and drying to obtain the surface layer; then coating the base material layer mixture on the surface layer, heating and drying to obtain the water-based cool microfiber synthetic leather dry layer; the surface layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 10-20 parts of water, 0.2-0.6 parts of water-based thickener, 1-2 parts of water-based bridging agent, 10-18 parts of phase change microcapsules, 8-12 parts of mosquito repellent microcapsules, and 5-10 parts of water-based color paste; the base material layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 2-8 parts of water, 0.4-0.8 parts of water-based thickener, 2-3 parts of water-based bridging agent, 0-2 parts of phase change microcapsules, 2-4 parts of mosquito repellent microcapsules, and 1-2 parts of water-based color paste;

[0011] (5) laminating the water-based cool feeling microfiber synthetic leather dry layer and the microfiber synthetic leather base and drying them, and peeling them off from the release paper after cooling to obtain a cool feeling anti-mosquito water-based microfiber synthetic leather finished product.

[0012] Furthermore, in the step (4), a middle material layer mixture is coated on the surface layer, and the middle material layer is obtained after heating and drying; then, the base material layer mixture is coated on the middle material layer, and the water-based cool microfiber synthetic leather dry layer is obtained after heating and drying; the middle material layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 5-15 parts of water, 0.4-0.8 parts of water-based thickener, 2-3 parts of water-based bridging agent, 2-6 parts of phase change microcapsules, 4-8 parts of mosquito repellent microcapsules, and 6-8 parts of water-based color paste.

[0013] Furthermore, the coating stripes of the surface layer mixed liquid are 0.10-0.18mm, and the drying temperature is 80-100°C; the coating stripes of the middle material layer mixed liquid are 0.15-0.20mm, and the drying temperature is 100-120°C; the coating stripes of the base material layer mixed liquid are 0.20-0.25mm, and the drying temperature is 130-140°C.

[0014] Furthermore, in the step (1), the microfibers of the water-based microfiber base cloth are sea island microfibers, which are formulated according to the following weight parts and made through a spinning production process: 45-55 weight parts of sea component slices, 42-50 weight parts of island component slices, 3-5 weight parts of nano-shaped mineral powder, and 0-1.5 weight parts of masterbatch.

[0015] Furthermore, the nano-sized mineral powder is nano-sized jade powder and / or nano-sized mica powder.

[0016] Furthermore, the sea component is LDPE, and the island component is nylon PA.

[0017] Furthermore, in the step (3), the liquid rate of the three-dipping and three-rolling process is 100-120%, and the high-temperature baking process is 150-170° C. for 3-7 minutes.

[0018] After adopting the above scheme, the beneficial effects of the present invention compared with the prior art are:

[0019] 1. Synthetic leather uses water-based microfiber base fabric, and on this basis, three processes are designed for the cool feeling function in the impregnation, post-treatment and surface making steps. The base fabric first forms a film containing phase change microcapsules through an impregnation process. The phase change microcapsules play an intelligent constant temperature regulation role, and the base fabric forms the first cool feeling base film; then in the post-finishing process, a second cool feeling reinforcement film is formed through a cool feeling treatment agent, which plays a protective and reinforcing auxiliary role for the first cool feeling base film; finally, in the surface making lamination process, at least two structural layers (face material layer and base material layer) containing phase change microcapsules are formed by lamination to form the third cool feeling main body layer. The first and third cool feeling functions echo each other, and the final synthetic leather has excellent and lasting cool feeling physical effects.

[0020] 2. In the process of laminating the surface of synthetic leather, the laminating forms at least two structural layers, which contain phase change microcapsules and anti-mosquito microcapsules in a certain ratio. The phase change microcapsules create a constant temperature environment for the anti-mosquito microcapsules, which is beneficial to the quantitative and long-lasting release of the anti-mosquito microcapsules, so that the prepared synthetic leather can achieve a long-lasting and slow-release mosquito repellent effect. Moreover, the two-layer and microcapsule-form structural design makes the prepared synthetic leather shoe material have high resistance to washing and damage.

[0021] 3. Furthermore, the synthetic leather surface is bonded to form three structural layers of outer layer, middle layer and bottom layer. The contents of phase change microcapsules and anti-mosquito microcapsules in the three layers decrease layer by layer. The outer layer has a high content and a good diffusion effect, while the contents of the middle layer and the bottom layer decrease layer by layer. This ensures that the cool feeling and anti-mosquito function remain stable for a long time, and plays a certain degree of replenishing effect after the shoe material is washed and worn many times, ensuring the continued effectiveness of the cool feeling and anti-mosquito function. DETAILED DESCRIPTION

[0022] The case is further described in detail below in conjunction with specific implementation methods.

[0023] This case involves a method for preparing a cool, mosquito-proof water-based microfiber synthetic leather, comprising the following steps:

[0024] (1) preparing a water-based ultrafine fiber base fabric;

[0025] (2) performing an aqueous wet impregnation treatment on a water-based microfiber base fabric, and then performing a fiber opening treatment to obtain a fiber opening base fabric; the impregnation slurry for the impregnation treatment comprises the following components in parts by weight: 100 parts by weight of water-based polyurethane, 15-30 parts by weight of phase change microcapsules, 3-5 parts by weight of a water-based thickener, 3-5 parts by weight of a water-based enhancer, and 1-2 parts by weight of a water-based color paste; and the phase change microcapsule film is infiltrated on the base fabric through the impregnation process;

[0026] (3) The open fiber base fabric is post-treated, and after being dried in an oven, the open fiber base fabric is subjected to three immersions and three rollings in an oil tank containing 12-20% by weight of a cool feeling treatment agent and 8-12% by weight of a silicone-based hand feeling agent, and finally subjected to a high-temperature baking treatment to obtain an ultrafine fiber synthetic leather base; preferably, the three-immersion and three-rolling liquid rate is 100-120%, and the high-temperature baking treatment is a high-temperature baking at 150-170°C for 3-7 minutes.

[0027] The open-fiber base fabric forms a continuous adsorption layer of the hand-feeling agent on the fiber surface through the combination of a silicon-based hand-feeling agent and three dips and three rolls to ensure the softness brought by the post-finishing. Through the three dips and three rolls process, a proper amount of cooling agent is added to form a continuous multi-effect (cooling and soft) adsorption layer on the fiber surface; the multi-effect adsorption layer is attached to the phase change microcapsule membrane, which protects and assists the function of the phase change microcapsule membrane;

[0028] (4) Dry surface making process, coating the surface layer and the base material layer on the release paper in sequence to obtain a water-based cool microfiber synthetic leather dry layer; specifically, coating the surface layer mixture on the release paper, heating and drying to obtain the surface layer; then coating the base material layer mixture on the surface layer, heating and drying to obtain the water-based cool microfiber synthetic leather dry layer;

[0029] The surface material layer mixed liquid comprises the following components in parts by weight: 100 parts of aqueous polyurethane resin, 10-20 parts of water, 0.2-0.6 parts of aqueous thickener, 1-2 parts of aqueous bridging agent, 10-18 parts of phase change microcapsules, 8-12 parts of mosquito repellent microcapsules, and 5-10 parts of aqueous color paste; the base material layer mixed liquid comprises the following components in parts by weight: 100 parts of aqueous polyurethane resin, 2-8 parts of water, 0.4-0.8 parts of aqueous thickener, 2-3 parts of aqueous bridging agent, 0-2 parts of phase change microcapsules, 2-4 parts of mosquito repellent microcapsules, and 1-2 parts of aqueous color paste.

[0030] (5) laminating the water-based cool feeling microfiber synthetic leather dry layer and the microfiber synthetic leather base and drying them, and peeling them off from the release paper after cooling to obtain a cool feeling anti-mosquito water-based microfiber synthetic leather finished product.

[0031] The phase change microcapsule is an existing well-known technology, in which the phase change microcapsule is a specific phase change material coated into a microcapsule through a special process. Through the phase change process of the material, the heat is temporarily stored in the microcapsule. When the external temperature changes, the state of the core material in the microcapsule changes, and the phase change material absorbs or releases a large amount of latent heat. Taking the human body's comfortable temperature of 28°C as an example, when the external ambient temperature is higher than 28°C, the phase change material will change from solid to liquid, absorb and store excess heat, and reduce the temperature; when the external ambient temperature is lower than 28°C, the phase change material will return from liquid to solid, release the stored heat, and keep the temperature constant. That is, when the external temperature rises, the core material will actively absorb heat; when the external temperature is lower than the phase change temperature point, the microcapsule will release heat and keep itself at a constant temperature, thereby achieving the effect of intelligent temperature regulation. In this way, under solar radiation, the cooling effect of the leather surface can reach up to 28°C. The phase change microcapsules of the present invention select the relevant phase change microcapsule products of Wuhan Advanced Institute.

[0032] The anti-mosquito microcapsule is an existing well-known technology. The application characteristics of the anti-mosquito microcapsule are that the anti-mosquito essence on the outer layer of the microcapsule emits fragrance at the beginning. During the wearing process, due to external forces such as friction and heat, the anti-mosquito essence inside the microcapsule is slowly released, which plays a role of long-lasting sustained release.

[0033] The synthetic leather of the present invention adopts a water-based ultrafine fiber base cloth to design a triple cooling process. First, a phase change microcapsule skin film is formed through an impregnation process, and the base cloth forms a first cooling base film, and the phase change microcapsules play an intelligent constant temperature regulation of the bottom layer; then, a second cooling reinforcement film (multi-effect adsorption layer) is formed through a cooling treatment agent in a post-finishing process, which protects and assists the first cooling base film and also plays an intermediate transition role, and accelerates the diffusion of body heat and the dissipation of sweat during use; finally, in a surface making and laminating process, at least two structural layers (a surface material layer and a base material layer) containing phase change microcapsules are laminated to form a third cooling main body layer, and the first and third cooling functions brought by the phase change microcapsules echo each other. The synthetic leather finally manufactured can reduce body temperature, give the skin a unique and lasting cool and comfortable feeling, is non-irritating to the skin, does not contain harmful substances to the human body, and the synthetic leather has excellent and lasting cooling physical effects and good washability.

[0034] The phase-change microcapsules and mosquito-proof microcapsules in a certain ratio in at least two structural layers formed by the synthetic leather surface laminating process of the present invention form a multi-effect adsorption layer, wherein the thermostatic regulating effect of the phase-change microcapsules creates a relatively constant temperature working environment for the mosquito-proof microcapsules, which is beneficial to the quantitative and lasting sustained release of the mosquito-proof microcapsules, thereby enabling the prepared synthetic leather to achieve a lasting and sustained release mosquito-repellent effect, and the two-layer and microcapsule-form structural design enables the prepared synthetic leather shoe material to have high washing resistance and anti-destruction effects.

[0035] Furthermore, in the step (4), a middle material layer is coated between the surface layer and the base material layer; the coating process of the middle material layer is to coat the surface layer with a mixed liquid of the middle material layer, and obtain the middle material layer after heating and drying; the mixed liquid of the middle material layer comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 5-15 parts of water, 0.4-0.8 parts of water-based thickener, 2-3 parts of water-based bridging agent, 2-6 parts of phase change microcapsules, 4-8 parts of mosquito repellent microcapsules, and 6-8 parts of water-based color paste. The base material layer mixed liquid is coated on the middle material layer, and heated and dried to obtain a water-based cool microfiber synthetic leather dry method layer.

[0036] By adopting the above scheme, the synthetic leather surface is bonded to form three structural layers of the outer material layer, the middle material layer and the bottom material layer. The content of phase change microcapsules and anti-mosquito microcapsules in the three layers decreases layer by layer. The outer material layer has a high content and a good diffusion effect, while the content of the middle material layer and the bottom material layer decreases layer by layer. This ensures that the cool feeling and anti-mosquito function remain stable for a long time, and plays a certain degree of effect supplement after the shoe material is washed and worn many times, ensuring the continued effectiveness of the cool feeling and anti-mosquito function.

[0037] Furthermore, in the step (4), the surface layer mixture is coated on the release paper, the number of coating strips is 0.10-0.18mm, and it is transferred to a hot air oven for heating and drying at a temperature of 80-100°C to obtain the surface layer. The middle material layer mixture is coated on the surface layer, the number of coating strips is 0.15-0.20mm, and it is transferred to a hot air oven for heating and drying at a temperature of 100-120°C to obtain the middle material layer. The base material layer compounding liquid is coated on the middle material layer, the number of coating strips is 0.20-0.25mm, and it is transferred to a hot air oven for heating and drying at a temperature of 130-140°C to obtain the water-based cool microfiber synthetic leather dry layer.

[0038] Furthermore, in the step (5), the obtained water-based cool microfiber synthetic leather dry layer is transferred to a hot air oven for semi-drying, and then laminated with the microfiber synthetic leather base for drying at a temperature of 130-145°C. After natural cooling, it is peeled off from the release paper to obtain a cool and anti-mosquito water-based microfiber synthetic leather finished product.

[0039] Furthermore, in the step (1), the water-based ultrafine fiber is a sea island ultrafine fiber, which is prepared according to the following weight parts and is made through a spinning production process: 45-55 weight parts of sea component slices, 42-50 weight parts of island component slices, 3-5 weight parts of nano-shaped mineral powder, and 0-1.5 weight parts of masterbatch. Preferably, the sea component is LDPE, and the island component is nylon PA. In addition, preferably, the nano-shaped mineral powder is nano-shaped jade powder and / or nano-shaped mica powder.

[0040] By adopting the above scheme, the water-based microfiber base cloth adopts sea island microfiber, and a certain proportion of nano-minerals are added to the sea island microfiber. The good thermal conductivity and slow heat absorption characteristics of these nano-minerals are utilized to make the fiber itself have a certain cooling function, thereby optimizing the overall cooling effect of the synthetic leather.

[0041] Embodiment 1

[0042] A method for preparing a cool and anti-mosquito water-based microfiber synthetic leather comprises the following steps:

[0043] (1) preparing a water-based microfiber base fabric; the water-based microfiber is a sea island microfiber, which is prepared according to the following weight parts and is made through a spinning production process: 50 weight parts of sea component slices, 45 weight parts of island component slices, 4 weight parts of nano-shaped jade powder, and 1 weight part of masterbatch; the sea component is LDPE, and the island component is nylon PA;

[0044] (2) performing an aqueous wet impregnation treatment on a water-based microfiber base fabric, and then performing a fiber opening treatment to obtain a fiber opening base fabric; the impregnation slurry for the impregnation treatment comprises the following components in parts by weight: 100 parts by weight of water-based polyurethane, 20 parts by weight of phase change microcapsules, 4 parts by weight of a water-based thickener, 4 parts by weight of a water-based enhancer, and 1.5 parts by weight of a water-based color paste;

[0045] (3) The open fiber base fabric is post-treated. After being dried in an oven, the open fiber base fabric is subjected to three immersions and three rollings in an oil tank containing 15% by weight of a cool feeling treatment agent and 10% by weight of a silicone-based feel agent, with a liquid carrying rate of 100-120%, and is baked at 160° C. for 5 minutes; finally, the open fiber base fabric is subjected to high temperature baking treatment to obtain an ultrafine fiber synthetic leather bass;

[0046] (4) Dry surface making process, coating the surface layer mixture on the release paper, the coating strip number is 0.10-0.18mm, and conveying it to a hot air oven for heating and drying at a drying temperature of 90°C to obtain the surface layer; then coating the base material layer mixture on the surface layer, the coating strip number is 0.20-0.25mm, and conveying it to a hot air oven for heating and drying at a drying temperature of 135°C to obtain a water-based cool microfiber synthetic leather dry layer;

[0047] The mixed liquid of the surface layer comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 15 parts of water, 0.4 parts of water-based thickener, 1.5 parts of water-based bridging agent, 15 parts of phase change microcapsules, 10 parts of mosquito repellent microcapsules, and 7 parts of water-based color paste; the mixed liquid of the base material layer comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 5 parts of water, 0.6 parts of water-based thickener, 2.5 parts of water-based bridging agent, 1 part of phase change microcapsules, 3 parts of mosquito repellent microcapsules, and 1.5 parts of water-based color paste;

[0048] (5) The water-based cool microfiber synthetic leather dry layer is transferred to a hot air oven for semi-drying, and then laminated with the microfiber synthetic leather base and dried at a temperature of 140° C. After natural cooling, the layer is peeled off from the release paper to obtain a cool anti-mosquito water-based microfiber synthetic leather finished product.

[0049] Embodiment 2

[0050] A method for preparing a cool and anti-mosquito water-based microfiber synthetic leather comprises the following steps:

[0051] (1) preparing a water-based microfiber base fabric; the water-based microfiber is a sea-island microfiber, which is prepared according to the following weight parts and is made through a spinning production process: 45 weight parts of sea component slices, 42 weight parts of island component slices, 3 weight parts of nano-mica powder, and 0.3 weight parts of masterbatch; the sea component is LDPE, and the island component is nylon PA;

[0052] (2) performing an aqueous wet impregnation treatment on a water-based microfiber base fabric, and then performing a fiber opening treatment to obtain a fiber opening base fabric; the impregnation slurry for the impregnation treatment comprises the following components in parts by weight: 100 parts by weight of water-based polyurethane, 15 parts by weight of phase change microcapsules, 3 parts by weight of a water-based thickener, 3 parts by weight of a water-based enhancer, and 1 part by weight of a water-based color paste;

[0053] (3) The open fiber base fabric is post-treated. After being dried in an oven, the open fiber base fabric is subjected to three immersions and three rollings in an oil tank containing 13% by weight of a cool feeling treatment agent and 8% by weight of a silicone-based feel agent, with a liquid carrying rate of 100-120%, and high-temperature baking at 150° C. for 4 minutes; finally, after high-temperature baking treatment, an ultrafine fiber synthetic leather base is obtained;

[0054] (4) Dry surface making process, coating the surface layer mixture on the release paper, the number of coating strips is 0.10-0.18mm, and conveying it to a hot air oven for heating and drying at a drying temperature of 95°C, thereby obtaining the surface layer; coating the middle material layer mixture on the surface layer, the number of coating strips is 0.15-0.20mm, and conveying it to a hot air oven for heating and drying at a drying temperature of 110°C, thereby obtaining the middle material layer; then coating the base material layer mixture on the surface layer, the number of coating strips is 0.20-0.25mm, and conveying it to a hot air oven for heating and drying at a drying temperature of 135°C, thereby obtaining the water-based cool microfiber synthetic leather dry layer;

[0055] The fabric layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 10 parts of water, 0.2 parts of water-based thickener, 1 part of water-based bridging agent, 10 parts of phase change microcapsules, 8 parts of mosquito repellent microcapsules, and 5 parts of water-based color paste;

[0056] The middle material layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 5 parts of water, 0.4 parts of water-based thickener, 2 parts of water-based bridging agent, 2 parts of phase change microcapsules, 4 parts of mosquito repellent microcapsules, and 6 parts of water-based color paste;

[0057] The base material layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 2 parts of water, 0.4 parts of water-based thickener, 2 parts of water-based bridging agent, 0.5 parts of phase change microcapsules, 2 parts of mosquito repellent microcapsules, and 1 part of water-based color paste;

[0058] (5) The water-based cool microfiber synthetic leather dry layer is transferred to a hot air oven for semi-drying, and then laminated with the microfiber synthetic leather base and dried at a drying temperature of 135° C. After natural cooling, the layer is peeled off from the release paper to obtain a cool anti-mosquito water-based microfiber synthetic leather finished product.

[0059] Embodiment 3

[0060] A method for preparing a cool and anti-mosquito water-based microfiber synthetic leather comprises the following steps:

[0061] (1) preparing a water-based microfiber base fabric; the water-based microfiber is a sea island microfiber, which is prepared according to the following weight parts and is made through a spinning production process: 55 weight parts of sea component slices, 50 weight parts of island component slices, 2 weight parts of nano-mica powder, 2 weight parts of nano-jade powder, and 1.5 weight parts of masterbatch; the sea component is LDPE, and the island component is nylon PA;

[0062] (2) subjecting the water-based microfiber base fabric to a water-based wet impregnation treatment, and then subjecting the water-based microfiber base fabric to a fiber-opening treatment to obtain a fiber-opening base fabric; the impregnation slurry for the impregnation treatment comprises the following components in parts by weight: 100 parts by weight of water-based polyurethane, 30 parts by weight of phase change microcapsules, 5 parts by weight of a water-based thickener, 5 parts by weight of a water-based enhancer, and 2 parts by weight of a water-based color paste;

[0063] (3) The open fiber base fabric is post-treated. After being dried in an oven, the open fiber base fabric is subjected to three immersions and three rollings in an oil tank containing 20% ​​by weight of a cool feeling treatment agent and 12% by weight of a silicone-based feel agent, with a liquid carrying rate of 100-120%, and is baked at 170° C. for 7 minutes; finally, the open fiber base fabric is subjected to high temperature baking treatment to obtain an ultrafine fiber synthetic leather base;

[0064] (4) Dry surface making process, coating the surface layer mixture on the release paper, the number of coating strips is 0.10-0.18mm, and conveying it to a hot air oven for heating and drying at a drying temperature of 100°C to obtain the surface layer; coating the middle material layer mixture on the surface layer, the number of coating strips is 0.15-0.20mm, and conveying it to a hot air oven for heating and drying at a drying temperature of 120°C to obtain the middle material layer; then coating the base material layer mixture on the surface layer, the number of coating strips is 0.20-0.25mm, and conveying it to a hot air oven for heating and drying at a drying temperature of 140°C to obtain the water-based cool microfiber synthetic leather dry layer;

[0065] The fabric layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 20 parts of water, 0.6 parts of water-based thickener, 2 parts of water-based bridging agent, 18 parts of phase change microcapsules, 12 parts of mosquito repellent microcapsules, and 10 parts of water-based color paste;

[0066] The middle material layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 15 parts of water, 0.8 parts of water-based thickener, 3 parts of water-based bridging agent, 6 parts of phase change microcapsules, 8 parts of mosquito repellent microcapsules, and 8 parts of water-based color paste;

[0067] The base material layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 8 parts of water, 0.8 parts of water-based thickener, 3 parts of water-based bridging agent, 2 parts of phase change microcapsules, 4 parts of mosquito repellent microcapsules, and 2 parts of water-based color paste;

[0068] (5) The water-based cool microfiber synthetic leather dry layer is transferred to a hot air oven for semi-drying, and then laminated with the microfiber synthetic leather base and dried at a temperature of 145° C. After natural cooling, the layer is peeled off from the release paper to obtain a cool anti-mosquito water-based microfiber synthetic leather finished product.

[0069] The present invention provides a method for preparing a water-based microfiber synthetic leather with a cool feeling and anti-mosquito effect. The processing method is simple, convenient and easy to operate. The prepared shoe material has high washing resistance and anti-damage performance, can be recycled, and has a long-lasting cool physical effect. At the same time, the anti-mosquito effect still has the anti-mosquito effect after washing for fifty or sixty times. At the same time, it can meet the detection and evaluation standard of the contact cool coefficient Qmax≥0.25 of superior clothing in the FZ / T 73067-2020 "Contact Cool Knitted Clothing" standard.

[0070] The above descriptions are only preferred embodiments of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should fall within the scope of the claims of the present invention.

Claims

1. A method for preparing a cool and anti-mosquito water-based microfiber synthetic leather, characterized in that: The following steps are involved: (1) preparing a water-based ultrafine fiber base fabric; (2) performing an aqueous wet impregnation treatment on a water-based microfiber base fabric, and then performing a fiber opening treatment to obtain a fiber opening base fabric; the impregnation slurry for the impregnation treatment comprises the following components in parts by weight: 100 parts by weight of water-based polyurethane, 15-30 parts by weight of phase change microcapsules, 3-5 parts by weight of a water-based thickener, 3-5 parts by weight of a water-based enhancer, and 1-2 parts by weight of a water-based color paste; (3) post-processing the open fiber base fabric, wherein the open fiber base fabric is dried in an oven, then three-immersed and three-rolled in an oil tank containing 12-20% by weight of a cool feeling treatment agent and 8-12% by weight of a silicone-based hand feeling agent, and then subjected to high temperature baking treatment to obtain an ultrafine fiber synthetic leather bass; (4) Dry surface making process, coating the surface layer mixture on the release paper, heating and drying to obtain the surface layer; Then, a base material layer mixture is coated on the fabric layer, and the water-based cool microfiber synthetic leather dry layer is obtained after heating and drying; the fabric layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 10-20 parts of water, 0.2-0.6 parts of water-based thickener, 1-2 parts of water-based bridging agent, 10-18 parts of phase change microcapsules, 8-12 parts of mosquito repellent microcapsules, and 5-10 parts of water-based color paste; the base material layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 2-8 parts of water, 0.4-0.8 parts of water-based thickener, 2-3 parts of water-based bridging agent, 0-2 parts of phase change microcapsules, 2-4 parts of mosquito repellent microcapsules, and 1-2 parts of water-based color paste; (5) laminating the water-based cool feeling microfiber synthetic leather dry layer and the microfiber synthetic leather base and drying them, and peeling them off from the release paper after cooling to obtain a cool feeling anti-mosquito water-based microfiber synthetic leather finished product.

2. The method for preparing a cool feeling anti-mosquito water-based microfiber synthetic leather according to claim 1, characterized in that: In the step (4), a middle material layer mixture is coated on the surface layer, and the middle material layer is obtained after heating and drying; then, the base material layer mixture is coated on the middle material layer, and the water-based cool microfiber synthetic leather dry layer is obtained after heating and drying; the middle material layer mixture comprises the following components in parts by weight: 100 parts of water-based polyurethane resin, 5-15 parts of water, 0.4-0.8 parts of water-based thickener, 2-3 parts of water-based bridging agent, 2-6 parts of phase change microcapsules, 4-8 parts of mosquito repellent microcapsules, and 6-8 parts of water-based color paste.

3. The method for preparing a cool feeling anti-mosquito water-based microfiber synthetic leather according to claim 2, characterized in that: The coating stripes of the mixed liquid of the surface layer are 0.10-0.18mm, and the drying temperature is 80-100°C; the coating stripes of the mixed liquid of the middle material layer are 0.15-0.20mm, and the drying temperature is 100-120°C; the coating stripes of the mixed liquid of the bottom material layer are 0.20-0.25mm, and the drying temperature is 130-140°C.

4. The method for preparing a cool feeling anti-mosquito water-based microfiber synthetic leather according to claim 1, characterized in that: In the step (1), the microfibers of the water-based microfiber base cloth are sea island microfibers, which are prepared according to the following weight parts and made through a spinning production process: 45-55 weight parts of sea component slices, 42-50 weight parts of island component slices, 3-5 weight parts of nano-shaped mineral powder, and 0-1.5 weight parts of masterbatch.

5. The method for preparing a cool feeling anti-mosquito water-based microfiber synthetic leather according to claim 4, characterized in that: The nano-sized mineral powder is nano-sized jade powder and / or nano-sized mica powder.

6. The method for preparing a cool feeling anti-mosquito water-based microfiber synthetic leather according to claim 4, characterized in that: The sea component is LDPE, and the island component is nylon PA.

7. The method for preparing a cool feeling anti-mosquito water-based microfiber synthetic leather according to claim 1, characterized in that: In the step (3), the liquid rate of the three-dipping and three-rolling process is 100-120%, and the high-temperature baking process is performed at 150-170° C. for 3-7 minutes.