Method for accurately observing carbon-coated lithium iron phosphate material by using transmission electron microscope

Through resin embedding method and microscope parameter optimization, the problem of difficult to measure the thickness and uniformity of the carbon-coated lithium iron phosphate material in transmission electron microscope is solved, and the clear observation and accurate evaluation of lithium iron phosphate material is achieved, which improves the The authenticity and reliability of the experiment.

CN118961768APending Publication Date: 2024-11-15BEIJING MINING & METALLURGICAL TECH GRP CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411011243.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to clearly observe and accurately measure the thickness and uniformity of the coating layer of carbon-coated lithium iron phosphate material through transmission electron microscopy, resulting in the inability to effectively evaluate its conductivity.

Method used

Transmission electron microscope samples were prepared by resin embedding method, and standard cross-sectional samples were formed by mechanical thinning and double-sided ion thinning, and the samples were continuously tilted in the transmission electron microscope, so that the electron beam was coated with lithium iron phosphate along the carbon. The exponential crystal belt is incident, and the microscope parameters are adjusted to enhance the image contrast.

Benefits of technology

Clear observation and accurate measurement of the carbon coating layer of lithium iron phosphate material is achieved, ensuring reliable evaluation of the thickness and uniformity of the coating layer, avoiding the problem of image contrast superposition, and improving the authenticity of the transmission electron microscopy experiment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961768A_ABST
    Figure CN118961768A_ABST
Patent Text Reader

Abstract

The invention provides a method for accurately observing a carbon-coated lithium iron phosphate material by using a transmission electron microscope, and relates to the field of analysis and detection. The method for accurately observing the carbon-coated lithium iron phosphate material by using the transmission electron microscope comprises the following steps: mixing G1 glue and a carbon-coated lithium iron phosphate powder material, and stirring to obtain composite glue; pressing the composite colloid into a film, and thinning to obtain an observation sample; placing an observation sample in a transmission electron microscope, and tilting the sample until an electron beam just enters along a low-index crystal zone axis of the carbon-coated lithium iron phosphate material at the tilting angle; and adjusting the shooting state and parameters of the transmission electron microscope, and then observing to obtain a corresponding result. According to the method, the interface contrast on the two sides of the carbon layer is clearly presented, so that the coating effectiveness, uniformity and thickness condition of the carbon-coated lithium iron phosphate material can be accurately evaluated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of analysis and detection, and in particular to a method for accurately observing carbon-coated lithium iron phosphate materials using a transmission electron microscope. Background Art

[0002] As a type of positive electrode material for lithium-ion batteries, lithium iron phosphate exhibits good cycle stability and long cycle life during the charge and discharge process; however, lithium iron phosphate also has the disadvantages of poor conductivity and low ion diffusion rate. In order to improve the conductivity of lithium iron phosphate materials, coating amorphous carbon on the surface of particles is the most common solution. The performance of carbon-coated lithium iron phosphate produced by different manufacturers varies greatly, mainly due to the effectiveness, uniformity and thickness of the carbon coating.

[0003] At present, the evaluation of the amorphous carbon coating (LiFePO4 / C) on the surface of lithium iron phosphate crystal materials is mainly measured by measuring the carbon content in the material. However, this method has limitations and can only determine the total amount of amorphous carbon in the material (including free carbon and carbon coating on the surface of LiFePO4), and cannot provide more valuable relevant information for evaluating the conductivity of lithium iron phosphate materials (effectiveness of carbon coating on the surface of LiFePO4, uniformity of carbon coating and thickness of carbon coating layer). In theory, the microscopic characterization of the amorphous carbon coating of nanomaterial LiFePO4 / C by transmission electron microscopy can accurately observe and measure the coating effectiveness and uniformity of amorphous carbon on the surface of lithium iron phosphate crystals and measure the thickness of the coating layer. In actual situations, the amorphous carbon coating layer usually has the following two characteristics: (1) The carbon film does not have a crystal structure and is in an amorphous state; (2) The thickness of the carbon film is very thin, generally around 5 nanometers. For amorphous ultra-thin samples composed of light element carbon atoms, the dynamic scattering effect is very weak, and the image contrast is also very weak, so that in the conventional observation experiment of transmission electron microscopy, whether it is direct naked eye observation or CCD shooting, the boundary of the carbon coating layer in LiFePO4 / C will be unclear or even invisible, which ultimately leads to the inability to carry out the observation experiment smoothly. At present, the transmission electron microscope observation of the carbon coating layer in LiFePO4 / C usually adopts the following experimental scheme: first, the ultrasonic dispersion method is used to disperse LiFePO4 / C on a carbon support film or a micro-grating film to make a sample observable by a transmission electron microscope, and then the image contrast is improved by adjusting the state of the transmission electron microscope, increasing the objective lens aperture, adjusting the focus state, and reducing the acceleration voltage. As a result, on the one hand, the true thickness of the carbon coating layer in LiFePO4 / C cannot be obtained, and on the other hand, the contrast enhancement effect of the ultra-thin amorphous carbon film is not good, and it also causes the undesirable result of reduced image resolution.

[0004] Except for LiFePO4 / C amorphous carbon-coated materials, similar problems exist in the observation of other surface-coated nanoparticle materials.

[0005] In summary, it is necessary to explore an experimental method that can clearly observe the surface coating of carbon-coated lithium iron phosphate and then accurately evaluate its coating effectiveness, uniformity, and thickness. Summary of the invention

[0006] The purpose of this application is to provide a method for accurately observing carbon-coated lithium iron phosphate materials using a transmission electron microscope to solve the above problems.

[0007] To achieve the above objectives, this application adopts the following technical solutions:

[0008] A method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope, comprising:

[0009] Resin-G1 in G1 glue is mixed with Hardener-G1 and a carbon-coated lithium iron phosphate material sample, and stirred to obtain a carbon-coated lithium iron phosphate material composite colloid;

[0010] The carbon-coated lithium iron phosphate material composite colloid is pressed and solidified to form a composite colloid film, and then mechanical thinning and double-sided ion thinning are sequentially performed until a center hole is perforated to obtain an observation sample;

[0011] The observation sample is placed in a transmission electron microscope, the observation sample is tilted continuously, and the morphology of the observation sample is observed in real time. According to the principle of the best contrast of the coating layer of the observation sample, the appropriate tilting angle is finally determined as: an angle at which the electron beam is incident along the low-index crystal zone axis of the carbon-coated lithium iron phosphate;

[0012] Adjust the shooting state, parameters and focusing state of the transmission electron microscope, and then observe and obtain the corresponding results.

[0013] Preferably, the volume ratio of the Resin-G1 to the Hardener-G1 is 1:(0.5-1.5).

[0014] Preferably, the ratio of the volume of the carbon-coated lithium iron phosphate material sample to the total volume of the Resin-G1 and the Hardener-G1 is (1-2):1.

[0015] Preferably, the pressing comprises:

[0016] The carbon-coated lithium iron phosphate material composite colloid is placed between two pieces of sulfuric acid paper to form a sandwich structure, and pressure is applied uniformly to the structure to press the carbon-coated lithium iron phosphate material composite colloid into the film with a thickness of micrometer level.

[0017] Preferably, the film has a thickness of 100-200 μm.

[0018] Preferably, the curing time is 24-48 hours.

[0019] Preferably, the mechanical thinning comprises:

[0020] The composite colloid film is polished to 30-50 μm using sandpaper.

[0021] Preferably, the continuous tilting comprises:

[0022] Converging the electron beam on the surface of the observed sample into a nanobeam, and switching the electron microscope mode to the DIFF mode to clearly observe the Kikuchi flower pattern of the observed sample;

[0023] According to the distribution and trend characteristics of the Kikuchi pattern, the observation sample is tilted, and the observed Kikuchi pattern changes in real time until the electron beam is incident along the low-index crystal zone axis of the carbon-coated lithium iron phosphate at this tilting angle (such as

[100] ,

[001] ,

[010] ,

[110] ,

[111] ).

[0024] Preferably, the adjusting the shooting state, parameters and focusing state of the transmission electron microscope comprises:

[0025] Adjust voltage center, one-five axis, focusing image astigmatism, and object image astigmatism;

[0026] Comparative analysis is performed on the morphology contrast under different objective lens aperture numbers, and a suitable objective lens aperture number is determined according to the principle that the contrast of the coating layer of the observed sample is optimal;

[0027] Observe and photograph the observation sample under different image focusing states, and determine a suitable focusing state based on the photographing results and taking the contrast of the coating layer of the observation sample as the best principle;

[0028] The magnification is determined based on the thickness and contrast characteristics of the carbon coating.

[0029] Compared with the prior art, the beneficial effects of this application include:

[0030] The present application provides a method for accurately observing carbon-coated lithium iron phosphate materials using a transmission electron microscope. The transmission electron microscope samples prepared by the resin embedding method can more effectively ensure the true thickness of the lithium iron phosphate carbon coating layer in the TEM experiment compared with the transmission electron microscope samples prepared by the conventional ultrasonic dispersion sample preparation method; the sample has been successfully cut into a standard cross-section sample with the top and bottom removed after mechanical pre-thinning and ion thinning steps. Obviously, this cross-section sample presents a structure with a clear interface of the coated lithium iron phosphate as the core and the ultra-thin coating amorphous carbon as the shell. Therefore, in the transmission electron microscope experiment, the electron beam penetrates the sample for imaging and no longer has the problem of contrast superposition. The interface between the lithium iron phosphate crystal and the amorphous carbon coating layer can be clearly and accurately observed, so that the thickness of the ultra-thin coating layer can be accurately measured; the sample is continuously tilted to observe so that the specific crystallographic orientation of the sample is parallel to the incident direction of the electron beam, which can achieve the purpose of greatly improving the image contrast of the amorphous coating layer, which is conducive to clearly and accurately observing and recording the coating effectiveness, uniformity and true thickness of the coating layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0032] Figure 1 This is a schematic diagram of the observation effect of preparing samples by ultrasonic dispersion method;

[0033] Figure 2 This is the TEM photo of the sample prepared by ultrasonic dispersion method;

[0034] Figure 3 A theoretical schematic diagram of a method for accurately observing carbon-coated lithium iron phosphate materials using a transmission electron microscope provided in this application;

[0035] Figure 4 This is a TEM photo of the sample obtained in Example 1 of the present application;

[0036] Figure 5 This is a TEM photo of the sample obtained in Comparative Example 2 of the present application;

[0037] Figure 6 This is a TEM photo of the sample obtained in Example 2 of the present application;

[0038] Figure 7 This is a TEM photo of the sample obtained in Comparative Example 3 of the present application;

[0039] Figure 8 This is the observed TEM photo of the sample obtained in Comparative Example 4 of the present application. DETAILED DESCRIPTION

[0040] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:

[0041] A method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope, comprising:

[0042] Resin-G1 in G1 glue is mixed with Hardener-G1 and a carbon-coated lithium iron phosphate material sample, and stirred to obtain a carbon-coated lithium iron phosphate material composite colloid;

[0043] The carbon-coated lithium iron phosphate material composite colloid is pressed and solidified to form a composite colloid film, and then mechanical thinning and double-sided ion thinning are sequentially performed until a center hole is perforated to obtain an observation sample;

[0044] Placing the observed sample in a transmission electron microscope, continuously tilting the observed sample, and observing the morphology of the observed sample in real time, and finally determining the appropriate tilt angle as an angle that enables the electron beam to be incident along the low-index crystal zone axis of the carbon-coated lithium iron phosphate according to the principle that the coating layer contrast of the observed sample is optimal;

[0045] At this time, the interfaces on both sides of the amorphous carbon film on the surface of the carbon-coated lithium iron phosphate (1. the interface between the carbon layer and the lithium iron phosphate, 2. the interface between the carbon layer and the amorphous coating medium) can be clearly presented, and the results are observed and recorded.

[0046] Adjust the shooting state, parameters and focusing state of the transmission electron microscope, and then observe and obtain the corresponding results.

[0047] The following uses carbon-coated LiFePO4 as an example to explain the technical solution of this application:

[0048] Ultrasonic dispersion method is used to prepare transmission electron microscope samples. In the experiment, the electron beam penetrates the carbon-coated lithium iron phosphate material and interacts with the sample layer by layer. Then the transmitted electron beam carrying the sample information is imaged on the image plane and observed by the experimenter. Obviously, the boundary between the amorphous carbon coating layer and the LiFePO4 crystal observed on the image plane is actually two layers of amorphous carbon film plus LiFePO4 crystal, which is the image contrast superposition of a total of three areas parallel to the electron beam direction (such as Figure 1 When the thickness of the ultra-thin carbon film is measured by the electron image collected on the image plane, it is found that the interface between the amorphous carbon coating layer and the LiFePO4 crystal is fuzzy, and the real and exact interface between the two cannot be determined (as shown in Figure 1). Figure 2 shown).

[0049] The transmission electron microscope sample was prepared by resin embedding method. After mechanical pre-thinning and ion thinning steps, the sample was successfully cut into a standard cross-section sample with the top and bottom removed. Obviously, this cross-section sample showed a structure with LiFePO4 crystal as the core and ultra-thin amorphous carbon film as the shell with a clear interface (such as Figure 3 Therefore, in the transmission electron microscope experiment, the electron beam penetrates the sample to avoid the problem of contrast superposition in different regions, and the interface between LiFePO4 and the ultra-thin amorphous carbon film can be clearly and accurately observed (as shown in Figure 2). Figure 4 shown).

[0050] In the method provided in the present application, the sample can be continuously tilted so that the incident electron beam is parallel to the specific crystallographic orientation of nanocrystalline LiFePO4, thereby greatly improving the image contrast of the ultra-thin carbon film coated on the surface of LiFePO4 / C, which is conducive to clearly and accurately observing and recording the coating effectiveness, uniformity and true thickness of the amorphous carbon layer in LiFePO4 / C.

[0051] The specific explanation is as follows:

[0052] 1. The conventional experimental method (Comparative Example 2) is: first adjust the appropriate electron microscope state, objective lens aperture, magnification, acceleration voltage, beam spot size, and then directly observe the carbon film of LiFePO4 / C with any crystallographic orientation. At this time, the thickness contrast is the main factor affecting the image contrast. According to the transmission intensity formula of the electron wave after penetrating the sample, I = I0exp (-μt), where t is the propagation thickness, ρ is the mass density, M is the local relative molecular weight, L is the Avogadro constant, and σ is the local elastic scattering cross section. It can be seen that when the sample thickness is extremely thin, even if a series of parameters such as the electron microscope state are adjusted, the difference in the emission intensity of the transmitted wave in the extremely thin samples on both sides is extremely small. Therefore, it is impossible to form a contrast difference that can distinguish two adjacent areas only by the mass thickness contrast. Therefore, for samples with very thin thickness of LiFePO4 crystals and amorphous carbon layers on the surface (the thickness of the amorphous carbon layer and the thickness of the carbon layer near the LiFePO4 crystal are both about 5nm), conventional experimental methods cannot clearly and accurately observe the situation where the LiFePO4 crystal is coated with an amorphous carbon layer, such as Figure 5 shown.

[0053] 2. The method provided in the present application is, first, to converge the electron beam into a nanobeam on the surface of the LiFePO4 crystal, and switch the electron microscope mode to the DIFF mode, so that the Kikuchi pattern of the LiFePO4 crystal can be clearly observed; secondly, according to the distribution trend characteristics of the Kikuchi pattern, the sample is mechanically tilted, and the observed Kikuchi pattern changes in real time, and tilted to an arbitrary low-index Kikuchi pole of the sample is parallel to the incident electron beam, that is, the low-index crystal band axis of the LiFePO4 crystal is parallel to the incident direction of the electron beam; finally, adjust the electron microscope state, select the appropriate objective lens aperture and magnification, modulate the focus state to be underfocus, and then take a transmission electron microscope image. This is because when the electron beam is incident on the crystal surface parallel to the low-index crystal zone axis of the LiFePO4 crystal, the diffraction contrast and mass thickness contrast simultaneously affect the image contrast of the LiFePO4 crystal. Further using the objective lens aperture to allow the transmitted beam and part of the diffracted electron beam to participate in the imaging can greatly reduce the grayscale value of the LiFePO4 crystal in the electron image, and increase the contrast difference at the interface between the LiFePO4 crystal and the amorphous carbon film. At the same time, the ultra-thin amorphous carbon film coated on the surface of the LiFePO4 crystal is not only irradiated by the incident electron beam, but also by part of the outgoing electron beam after diffraction from the LiFePO4 crystal. The interaction between the two electron beams with a phase relationship increases the contrast difference at the interface between the amorphous carbon film and the embedding agent. Therefore, this experimental method can clearly and accurately observe the two boundaries of the amorphous carbon film, thereby determining its coating effectiveness, uniformity and thickness, such as Figure 6 shown.

[0054] In summary, the method provided in this application can clearly and accurately observe and record the coating effectiveness, uniformity and true thickness of the amorphous carbon layer in LiFePO4 / C, and can realize the microscopic fine characterization and evaluation of materials such as LiFePO4 / C, and can ensure its authenticity and reliability.

[0055] In the embodiment of the present application, lithium iron phosphate coated amorphous carbon with nanometer thickness is taken as an example, but it is not limited to this sample and may also include other nanoparticle surface coating materials, such as boron nitride coated lithium aluminum titanium phosphate powder material, amorphous titanium dioxide coated nano silicon material, etc.

[0056] In an optional embodiment, the volume ratio of the Resin-G1 to the Hardener-G1 is 1:(0.5-1.5).

[0057] Optionally, the volume ratio of the Resin-G1 to the Hardener-G1 can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5 or any value between 1:(0.5-1.5).

[0058] In an optional embodiment, the ratio of the volume of the core-shell structure material sample to the total volume of the Resin-G1 and the Hardener-G1 is (1-2):1.

[0059] Optionally, the ratio of the volume of the carbon-coated lithium iron phosphate material sample to the total volume of the Resin-G1 and the Hardener-G1 can be any value between 1:1, 1.5:1, 2:1 or (1-2):1.

[0060] In an optional embodiment, the pressing comprises:

[0061] The carbon-coated lithium iron phosphate material composite colloid is placed between two pieces of sulfuric acid paper to form a sandwich structure, and pressure is applied uniformly to the structure to press the carbon-coated lithium iron phosphate material composite colloid into the film with a thickness of micrometer level.

[0062] In an optional embodiment, the film has a thickness of 100-200 μm.

[0063] Optionally, the thickness of the film may be 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm or any value between 100-200 μm.

[0064] In an optional embodiment, the curing time is 24-48 hours.

[0065] Optionally, the curing time can be 24 hours, 26 hours, 28 hours, 30 hours, 32 hours, 34 hours, 36 hours, 38 hours, 40 hours, 42 hours, 44 hours, 46 hours, 48 ​​hours or any value between 24 and 48 hours.

[0066] In an optional embodiment, the mechanical thinning comprises:

[0067] The composite colloid film is polished to 30-50 μm using sandpaper.

[0068] Optionally, the end point thickness of sandpaper polishing can be 30 μm, 40 μm, 50 μm or any value between 30-50 μm.

[0069] In an optional embodiment, the continuous tilting includes:

[0070] Converging the electron beam on the surface of the observed sample into a nanobeam, and switching the electron microscope mode to the DIFF mode to clearly observe the Kikuchi flower pattern of the observed sample;

[0071] According to the distribution trend characteristics of the Kikuchi pattern, the observation sample is tilted so that the Kikuchi pattern changes in real time until the electron beam is incident along any low-index crystal band axis of the carbon-coated lithium iron phosphate at the tilting angle.

[0072] In an optional embodiment, adjusting the shooting state, parameters and focusing state of the transmission electron microscope includes:

[0073] Adjust voltage center, one-five axis, focusing image astigmatism, and object image astigmatism;

[0074] Comparative analysis is performed on the morphology contrast under different objective lens aperture numbers, and a suitable objective lens aperture number is determined according to the principle that the contrast of the coating layer of the observed sample is optimal;

[0075] Observe and photograph the observation sample under different image focusing states, and determine a suitable focusing state based on the photographing results and taking the contrast of the coating layer of the observation sample as the best principle;

[0076] The magnification is determined based on the thickness and contrast characteristics of the carbon coating.

[0077] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0078] Example 1

[0079] This embodiment provides a method for accurately observing an amorphous carbon-coated lithium iron phosphate material using a transmission electron microscope, comprising the following steps:

[0080] (1) Mix Resin-G1 and Hardener-G1 in the G1 gel in a ratio of 1:1.5, and stir them thoroughly with a pin to form a light yellow colloid for later use;

[0081] (2) quickly mixing the powder sample LiFePO4 / C with the light yellow colloid obtained in step 1 in a volume ratio of 1:1, and stirring for multiple times in a clockwise, counterclockwise and up and down manner using a pin to expel the bubbles between the colloid and the powder sample LiFePO4 / C, so that the LiFePO4 / C and the colloid are fully infiltrated to form a LiFePO4 / C composite colloid;

[0082] (3) Placing the LiFePO4 / C composite colloid between two pieces of sulfuric acid paper to form a sandwich structure, applying slight pressure evenly to the above structure to press the composite colloid into a 100 μm thick film, and curing for 24 hours;

[0083] (4) The composite colloidal film cured in step (3) is polished with water sandpaper to a thickness of about 50 μm, and then placed in an ion thinning instrument to perform double-sided ion thinning on the composite film until a micropore is formed in the center;

[0084] (5) placing the sample processed in step (4) under a transmission electron microscope for observation;

[0085] (6) The sample LiFePO4 / C was continuously tilted so that the low-index crystal zone axis

[100] of the nanocrystalline LiFePO4 was parallel to the incident direction of the electron beam, and the morphology of the ultra-thin amorphous carbon layer was observed and recorded.

[0086] (7) Adjust the transmission electron microscope to a state suitable for shooting, including: voltage center, one-five axis, focusing image astigmatism, and object image astigmatism;

[0087] (8) Observe the morphology of LiFePO4 / C, compare and analyze the morphology contrast under different objective lens aperture numbers, and determine that the appropriate objective lens aperture number is a two-stage objective lens aperture according to the principle that the contrast of ultra-thin amorphous carbon layer is the best;

[0088] (9) Observe and photograph LiFePO4 / C under different image focusing states, and determine the appropriate focusing state as the underfocus state based on the shooting results and the principle of the best contrast of the ultra-thin amorphous carbon layer;

[0089] (10) Based on the thickness and uniformity of the ultra-thin carbon layer on the surface of LiFePO4 / C and the shooting requirements, the appropriate magnification is determined to be 400,000 times;

[0090] (11) Under the above-determined appropriate conditions, the experimental results of LiFePO4 / C were photographed and recorded to obtain the true and reliable coating conditions of the amorphous carbon coating layer of LiFePO4: Under the condition of a magnification of 400,000 times, it can be observed that the amorphous carbon in the LiFePO4 / C material forms a layer of uniform texture, thickness, and effective coating on the surface of LiFePO4 with a thickness of about 5 nanometers.

[0091] Observation photos such as Figure 4 shown.

[0092] Example 2

[0093] This embodiment provides a method for accurately observing a core-shell structure material using a transmission electron microscope, comprising the following steps:

[0094] (1) Mix Resin-G1 and Hardener-G1 in the G1 gel in a ratio of 1:1, and stir them thoroughly with a pin to form a light yellow colloid, which is set aside;

[0095] (2) quickly mixing the powder sample LiFePO4 / C with the light yellow colloid obtained in step 1 in a volume ratio of 2:1, and stirring for multiple times in a clockwise, counterclockwise and up and down manner using a pin to expel the bubbles between the colloid and the powder sample LiFePO4 / C, so that the LiFePO4 / C and the colloid are fully infiltrated to form a LiFePO4 / C composite colloid;

[0096] (3) The LiFePO4 / C composite colloid was placed between two pieces of sulfuric acid paper to form a sandwich structure, and a slight pressure was evenly applied to the above structure to press the composite colloid into a 150 μm thick film, and cured for 36 hours;

[0097] (4) The composite colloidal film cured in step (3) is polished with water sandpaper to a thickness of about 50 μm, and then placed in an ion thinning instrument to perform double-sided ion thinning on the composite film until a micropore is formed in the center;

[0098] (5) placing the sample processed in step (4) under a transmission electron microscope for observation;

[0099] (6) Continuously tilting the sample LiFePO4 / C so that the

[010] of the nanocrystalline LiFePO4 is parallel to the incident direction of the electron beam, and observing and recording the morphology of the ultrathin amorphous carbon layer;

[0100] (7) Adjust the transmission electron microscope to a state suitable for shooting, including: voltage center, one-five axis, focusing image astigmatism, and object image astigmatism;

[0101] (8) The morphology of LiFePO4 / C was observed, and the morphology contrast was compared and analyzed under different objective lens aperture levels. According to the principle that the contrast of ultra-thin amorphous carbon layer is the best, the objective lens aperture level is determined to be 2;

[0102] (9) Observe and photograph LiFePO4 / C under different image focusing states, and determine the appropriate focusing state as underfocus based on the shooting results with the ultra-thin amorphous carbon layer contrast as the best principle;

[0103] (10) According to the thickness and uniformity of the ultra-thin carbon layer on the surface of LiFePO4 / C and the shooting requirements, the appropriate magnification is determined to be 50,000 times;

[0104] (11) Under the above-determined appropriate conditions, the experimental results of LiFePO4 / C were photographed and recorded to obtain the true and reliable coating conditions of the LiFePO4 amorphous carbon coating layer: Under the condition of a magnification of 50,000 times, it can be observed that the amorphous carbon in the LiFePO4 / C material forms a layer of uniform texture, thickness, and effective coating on the surface of LiFePO4 with a thickness of about 5-7 nanometers.

[0105] Observation photos such as Figure 6 shown.

[0106] Comparative Example 1

[0107] Ultrasonic dispersion method was used as a control. Take an appropriate amount of powder sample LiFePO4 / C, and use anhydrous ethanol as a dispersant; use an ultrasonic cleaner to fully disperse the LiFePO4 / C powder in anhydrous ethanol to form a uniform suspension, draw the suspension and drop it on a copper grid with an ultra-thin carbon film, and bake the grid film with the suspension under an infrared lamp for about 1 hour. Subsequently, the treated sample was placed in a transmission electron microscope for observation. It can be seen that there is a large range of image contrast overlap between the amorphous carbon coating and the LiFePO4 crystals, which leads to a blurred boundary between the two. It is impossible to determine the real and exact interface between the two, so it is impossible to accurately measure the actual thickness of the coating. Figure 2 shown.

[0108] Comparative Example 2

[0109] The conventional observation method was used as a control. The prepared LiFePO4 / C transmission electron microscope sample was placed in the electron microscope for observation. First, the state of the transmission electron microscope was adjusted: the acceleration voltage was adjusted to 200 keV, a five-axis operation was performed, the focusing image astigmatism was eliminated, the objective image astigmatism was eliminated, the voltage center was adjusted to the concentric scaling of the light spot under HT wob, a two-stage objective lens aperture was inserted, and the magnification was adjusted to 50,000 times. On this basis, the carbon film of LiFePO4 / C was directly observed. It can be seen that under the condition of 50,000 times, it is impossible to effectively observe whether the carbon film of LiFePO4 / C forms an effective coating, and it is even more impossible to judge the important microstructural information such as the thickness and uniformity of the coating layer. The results are as follows Figure 5 shown.

[0110] Comparative Example 3

[0111] The improper tilting position of the sample was used as a control. The prepared LiFePO4 / C transmission electron microscope sample was placed in the electron microscope for observation. With other electron microscope and shooting conditions unchanged, the sample was tilted along ±X (the maximum tilting angle of the sample stage in the X direction of the high-resolution transmission electron microscope is ±30°). During the entire tilting process, the image contrast of the amorphous carbon film on the surface of the carbon-coated lithium iron phosphate did not show a significant improvement, such as Figure 7As shown in (a), the sample stage is tilted along ±Y (the maximum tilt angle in the Y direction is ±30°), and the image contrast of the amorphous carbon film does not show a significant improvement during the entire tilting process. Figure 7 As shown in (b); when observing and photographing the LiFePO4 / C powder under the above two conditions, it is impossible to observe the amorphous carbon film on the powder surface, let alone determine its coating condition. For comparison, we observe and photograph the same LiFePO4 / C powder by tilting it 11.2° along +X and 5.3° along +Y. At this time, the low-index crystal band axis

[110] of LiFePO4 is parallel to the incident direction of the electron beam. The coating condition of the amorphous carbon film on the surface of LiFePO4 / C can be clearly observed, as shown in Figure 1. Figure 7 As shown in (c).

[0112] Comparative Example 4

[0113] Improper focus adjustment was used as a control. The prepared LiFePO4 / C transmission electron microscope sample was placed in the electron microscope for observation. With other electron microscope and shooting conditions unchanged, the same LiFePO4 / C powder was observed and photographed under three focusing states: underfocus, right focus, and overfocus. It can be seen that the carbon film coating can be clearly observed under the right focus condition, the carbon film cannot be observed under the right focus condition, and the carbon film can be vaguely observed under the underfocus condition, but the image is distorted. Figure 8 shown.

[0114] The present application adopts a resin embedding method to prepare samples required for transmission electron microscopy. First, the powder sample and G1 glue are fully stirred and infiltrated to form a mixed colloid of G1 glue and powder sample. After the mixed colloid is completely solidified, mechanical pre-thinning and ion fine thinning are performed to finally obtain a sample observable by transmission electron microscopy. This step plays a leading role in solving the problem of superposition of image contrast in three regions along the direction of the electron beam. Secondly, the transmission electron microscopy experimental method is innovative compared with the current experimental method. In addition to the basic steps for improving contrast, it is proposed that the angle of the sample to be tested must be adjusted so that the electron beam is incident on the sample surface along a specific angle. This step has a significant leading role in improving the contrast of ultra-thin amorphous carbon film. The transmission electron microscopy experimental method needs to be implemented in the following steps in sequence: (1) Adjust the angle of the sample to be tested so that the electron beam is incident on the sample surface along a specific angle; (2) Adjust the state of the electron microscope; (3) Determine the appropriate objective lens aperture level; (4) Adjust to a suitable focusing state; (5) Adjust the appropriate magnification to observe and record the amorphous carbon layer coated on the surface of the sample to be tested. This method can significantly and effectively improve the contrast of ultra-thin amorphous carbon layers in transmission electron microscopy, making carbon layers with unclear boundaries or even invisible carbon layers stand out. This allows accurate observation of whether the lithium iron phosphate powder is coated with a carbon layer, whether the coating is uniform, and accurate measurement of the thickness of the coated carbon layer, thus ensuring the authenticity and reliability of transmission electron microscopy observation and analysis.

[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for accurately observing carbon-coated lithium iron phosphate materials using a transmission electron microscope, characterized in that: include: Resin-G1 in G1 glue is mixed with Hardener-G1 and a carbon-coated lithium iron phosphate material sample, and stirred to obtain a carbon-coated lithium iron phosphate material composite colloid; The carbon-coated lithium iron phosphate material composite colloid is pressed and solidified to form a composite colloid film, and then mechanical thinning and double-sided ion thinning are sequentially performed until a center hole is perforated to obtain an observation sample; The observation sample is placed in a transmission electron microscope, the observation sample is tilted continuously, and the morphology of the observation sample is observed in real time. According to the principle of the best contrast of the coating layer of the observation sample, the appropriate tilting angle is finally determined as: an angle at which the electron beam is incident along the low-index crystal zone axis of the carbon-coated lithium iron phosphate; Adjust the shooting state, parameters and focusing state of the transmission electron microscope, and then observe to obtain the corresponding results.

2. The method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope according to claim 1, characterized in that: The volume ratio of the Resin-G1 to the Hardener-G1 is 1:(0.5-1.5).

3. The method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope according to claim 1, characterized in that: The ratio of the volume of the carbon-coated lithium iron phosphate material sample to the total volume of the Resin-G1 and the Hardener-G1 is (1-2):

1.

4. The method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope according to claim 1, characterized in that: The pressing comprises: The carbon-coated lithium iron phosphate material composite colloid is placed between two pieces of sulfuric acid paper to form a sandwich structure, and pressure is applied uniformly to the structure to press the carbon-coated lithium iron phosphate material composite colloid into the film with a thickness of micrometer level.

5. The method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope according to claim 4, characterized in that: The thickness of the film is 100-200 μm.

6. The method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope according to claim 1, characterized in that: The curing time is 24-48 hours.

7. The method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope according to claim 1, characterized in that: The mechanical thinning comprises: The composite colloid film is polished to 30-50 μm using sandpaper.

8. The method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope according to claim 1, characterized in that: The continuous tilting comprises: Converging the electron beam on the surface of the observed sample into a nanobeam, and switching the electron microscope mode to the DIFF mode to clearly observe the Kikuchi flower pattern of the observed sample; According to the distribution and trend characteristics of the Kikuchi pattern, the observation sample is tilted, and the observed Kikuchi pattern changes in real time until the electron beam is incident along any low-index crystal band axis of the carbon-coated lithium iron phosphate at the tilting angle.

9. The method for accurately observing carbon-coated lithium iron phosphate material using a transmission electron microscope according to any one of claims 1 to 8, characterized in that: The adjusting of the shooting state, parameters and focusing state of the transmission electron microscope comprises: Adjust voltage center, one-five axis, focusing image astigmatism, and object image astigmatism; Comparative analysis is performed on the morphology contrast under different objective lens aperture numbers, and a suitable objective lens aperture number is determined according to the principle that the contrast of the coating layer of the observed sample is optimal; Observing and photographing the observation sample in a defocused image focusing state; The magnification is determined based on the thickness and contrast characteristics of the carbon coating.

Citation Information

Cited By

  • Method for measuring thickness of gate oxide layer

    CN121089636A

  • A method for measuring the thickness of a gate oxide layer

    CN121089636B

  • Method for characterizing carbon coating layer of carbon-coated positive electrode material and application thereof

    CN121114094A