Method for analyzing and testing electron backscatter diffraction at bent part of ultra-thin lithium battery copper foil

Through high-temperature heat treatment and argon ion polishing technology of extremely thin electrolytic copper foil, the problem of residual stress in extremely thin copper foil was solved, and a smooth test surface suitable for electron backscattering analysis was prepared, which improved the accuracy and calibration rate of the test , fills the gap in bending analysis technology in the application of lithium battery negative electrodes.

CN118961773APending Publication Date: 2024-11-15JIUJIANG TELFORD ELECTRONICS MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411280385.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove residual stress in extremely thin electrolytic copper foils, resulting in reduced conductivity and affected microstructure structure, making it difficult to meet the requirements of high-precision electron backscattering and diffraction analysis and testing, especially in the application of negative electrodes of lithium batteries. The test and analysis technology of folds is blank.

Method used

By cutting extremely thin electrolytic copper foil and performing high-temperature heat treatment in a vacuum oven, the internal residual stress is reduced, and argon ion polishing technology is combined to prepare smooth bending samples, and cross-sectional polishing is performed on copper foils of different tensile strengths to ensure that The test surface has no stress layer, suitable for electron backscattering and diffraction analysis.

Benefits of technology

Effectively remove residual stress in extremely thin copper foil, enhance conductivity, and prepare a high-precision bending test surface, which improves the calibration rate and accuracy of EBSD test, and meets the bends of extremely thin copper foils in the negative electrode of lithium battery micromorphology and structural analysis requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961773A_ABST
    Figure CN118961773A_ABST
Patent Text Reader

Abstract

The invention discloses a method for analyzing and testing electron backscatter diffraction at a bent part of an ultra-thin lithium battery copper foil. The method comprises the following steps: preparing an ultra-thin lithium battery copper foil bent sample with stress removed and enhanced conductivity through pre-linear cutting and high-temperature heat treatment; using conductive silver paste to bond the non-bending opening end of the sample, and adopting an argon ion polishing instrument to polish the cross section of the bent ultra-thin lithium battery copper foil sample; a cross-shaped conductive path is bridged between a sample and an inclined sample table, and then a bending cross section amplification factor, a scanning surface range and a scanning surface step length are set to carry out electron backscatter diffraction (EBSD) technical test and analysis. The influence of internal residual stress on the EBSD test calibration rate and accuracy after the electrolytic copper foil is bent and stressed is effectively reduced, smooth and fine test surfaces can be prepared for extremely thin electrolytic copper foil bending samples with different tensile strengths, and the microstructure and the structure at the center of a crease are accurately tested; the internal structure and performance of the ultrathin copper foil are researched when the ultrathin copper foil is applied to the negative electrode of the lithium battery and is bent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper foil, and in particular to an electron backscatter diffraction analysis and testing method for a bending portion of an ultra-thin lithium battery copper foil. Background Art

[0002] The rapid expansion of the global new energy vehicle and grid energy storage industries has led to a growing demand for high safety, high energy density and long life for the new generation of lithium-ion batteries. As a key electronic material for the negative electrode current collector of lithium-ion batteries, lithium battery copper foil is developing towards ultra-lightness, high tensile strength, and high elongation. Ultra-thin copper foil (≤6um) with high technical barriers has accelerated its penetration and become the mainstream product in the traditional copper foil market. However, as the copper foil becomes extremely thin, mechanical properties such as decreased elongation and tearing will appear. Especially in the winding process of the negative electrode of lithium-ion batteries, the copper foil needs to have excellent bending resistance, which is closely related to the grain growth in the copper foil electrodeposition process and the changes in its microstructure morphology after force winding and extrusion.

[0003] In the field of metal material testing technology, Electron Backscatter Diffraction (EBSD) is a commonly used analytical method for characterizing the microstructure of crystalline materials, and is mainly used for texture and orientation analysis, phase identification, grain boundary characterization, strain characterization, visualization of crystal form and its distribution, quantitative analysis of grain size, etc. Since EBSD is a diffraction pattern formed by collecting the electron beam of a scanning electron microscope at a depth of tens of nanometers on the surface of a sample tilted at 70°, the requirements for sample preparation are particularly high. The test surface must be free of residual stress, oxide layer, good conductivity, flat and clean, in order to obtain a better diffraction pattern and obtain the crystal structure information of copper foil.

[0004] Among the existing testing technologies, argon ion polishing (CP) is an advantageous method suitable for surface sensitive analysis technology. By sputtering the material surface with an argon ion beam, a flat surface with little deformation and damage after removing the stress layer can be prepared. However, for electrolytic copper foil, since the copper foil needs to be bent and stretched many times during the manufacturing process, residual stress will be generated inside the copper foil, which not only reduces the conductivity and increases the brittleness of the copper foil, but also affects the microstructure of the copper foil. Furthermore, with the continuous improvement of the physical properties of ultra-thin copper foil, the internal stress and conductivity of the sample itself have caused the difficulty of EBSD sample preparation and the test time cost to continue to increase. Using only argon ion polishing technology, it is difficult to meet the requirements of preparing fine test surfaces and obtaining EBSD tests with high calibration rates and accuracy.

[0005] As far as the current EBSD research on electrolytic copper foil is concerned, the analysis of its crystal morphology is mostly concentrated on the plane and cross-section of the copper foil. There is still a lack of testing and analysis technology for the bending parts of extremely thin copper foil, especially high tensile strength copper foil used in lithium battery negative electrodes. Summary of the invention

[0006] The purpose of the present invention is to provide a stress-relieved and conductivity-enhanced ultra-thin lithium battery copper foil bending specimen, and a polishing treatment for the specimen, which can fully meet the EBSD testing requirements of ultra-thin copper foil bending parts with different tensile strengths.

[0007] The present invention provides an electron backscatter diffraction analysis and testing method for a bend of an ultra-thin lithium battery copper foil. The specific steps of the electron backscatter diffraction analysis and testing method for a bend of an ultra-thin lithium battery copper foil are as follows:

[0008] S1. Obtaining the bending sample of the ultra-thin lithium battery copper foil for stress relief and enhanced conductivity: using a sampler to cut the ultra-thin electrolytic copper foil, folding and aligning the copper foil along the edge, using a deep groove ball bearing to uniformly roll out the crease at the non-aligned end of the copper foil, cutting the crease sample into strips, and subjecting it to high-temperature heat treatment in a vacuum oven to obtain the bending sample of the ultra-thin lithium battery copper foil;

[0009] S2. Preparation of smooth and fine test surface of the sample. Cut the bent sample to be polished into the size suitable for the cross-section baffle of the argon ion polisher, and paste the sample to the cross-section baffle; perform cross-section polishing on the bent copper foil sample. Put the bent copper foil sample to be polished into the argon ion polisher, set the polishing parameters, and perform rough polishing and fine finishing on the cross section of the bent sample;

[0010] S3, Electron backscatter diffraction equipment test, the polished and bent ultra-thin lithium battery copper foil sample is pasted on a 70° inclined sample stage, the conductive path between the sample and the inclined sample stage is connected, the electron backscatter diffraction analysis technology equipment is used for testing, and the test results are processed by image.

[0011] Preferably, the crease specimen strip cutting method in S1 is wire cutting.

[0012] Preferably, the high temperature heat treatment in S1 is performed at a temperature of 120-170° C. and for a time of 10-20 minutes.

[0013] Preferably, the ultra-thin lithium battery copper foil is classified according to tensile strength into ordinary tensile strength (300-400MPa), medium tensile strength (400-500MPa), high tensile strength (500-600MPa) and ultra-high tensile strength (>600MPa) ultra-thin electrolytic copper foil.

[0014] Preferably, the copper foil sample to be polished and bent cut in S2 has a length of ≤15 mm and a width of ≤6 mm.

[0015] Preferably, in S2, conductive silver paste is used to tightly bond the open ends of the sheared bent sample away from the bending line to serve as a sample to be pasted on the cross-section baffle.

[0016] Preferably, the sample is pasted to the cross-section baffle in S2 by brushing conductive silver paste, and the bending part of the cross-section of the sample to be polished is aligned and pasted to the center of the cross-section baffle. The edge of the bent copper foil sample to be polished is exposed to the cross-section baffle of the argon ion polisher by 40-80 μm.

[0017] Preferably, when an argon ion polisher is used for polishing in S2, the ion source deflection angle is 0°, the sample stage rotation angle is -40° to +40°, and the rough polishing is performed at a voltage of 6-8KV for 20-40 minutes, followed by switching to fine polishing at a voltage of 3-5KV for 5-30 minutes.

[0018] Preferably, the conductive path in S3 is made of conductive silver paste and aluminum-based double-sided carbon conductive adhesive for cross-type connection, and the electron backscatter diffraction analysis technology test includes setting the bending section magnification, setting the scanning surface range and scanning step length, and performing noise reduction processing on the test image.

[0019] Preferably, in S3, the scanning surface range is set to a closed area along the edge of the bent cross-sectional shape, the magnification is set to ≥3Kx, and the scanning step length is set to ≤0.075 μm.

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: according to the provided ultra-thin lithium battery copper foil bending sample, the sample section is pre-wired and then subjected to high-temperature heat treatment, which can not only restore and eliminate the internal grain boundaries and defects in the test area of ​​the sample section, but also effectively reduce the influence of the internal residual stress of the electrolytic copper foil after bending and stress on the EBSD test calibration rate and accuracy. By performing cross-sectional argon ion polishing on the bending part of the ultra-thin lithium battery copper foil, a smooth and flat test section without stress layer can be prepared for the bending surface of the ultra-thin electrolytic copper foil with different tensile strengths, and the microscopic morphology and structure at the center of the crease can be accurately tested to carry out research on the internal organization and performance of the ultra-thin copper foil when it is bent in the negative electrode application of lithium batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a SEM image of the bending part of the 6-micron ultra-thin medium-resistance electrolytic copper foil prepared in Example 1;

[0022] Figure 2 This is the reverse pole figure orientation diagram at the bending point of the 6-micron ultra-thin medium-resistant electrolytic copper foil prepared in Example 1;

[0023] Figure 3 This is the reverse pole figure orientation diagram at the bending point of the 6-micron ultra-thin medium-resistant electrolytic copper foil prepared in Example 2. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0025] As analyzed in the background technology, in the existing testing technology, the difficulty of the micro-area morphology analysis test of the electrolytic copper foil continues to increase as the thickness of the copper foil becomes extremely thin and the physical property requirements become extremely high. This is because the electrolytic copper foil is a polycrystalline material randomly stacked by a large number of tiny single crystals. As the tensile strength is significantly improved, the crystal defect density increases accordingly. When the electrolytic copper foil is subjected to external force and plastic deformation, residual stress and defects such as dislocations are generated, which will cause resistance at the grain boundary, electron scattering, and affect the clarity of the Kikuchi line in the backscattered electron diffraction pattern. In particular, after the extremely thin electrolytic copper foil is bent, the crystal is deformed, and the internal grain boundaries and defects cause the EBSD test calibration rate to drop sharply. In the existing technical scheme, since the electrolytic copper foil is deposited along the light surface to the rough surface, compared with the plane, the research and analysis of the micro-area morphology of the cross-section of the electrolytic copper foil is of great significance. At present, the testing and analysis technology of extremely thin copper foil, especially high tensile strength copper foil, for such deformed samples at the bend of the negative electrode of lithium batteries is urgently needed to be popularized and developed.

[0026] Based on this, in a first typical embodiment of the present invention, the present invention provides a method for preparing an ultra-thin lithium battery copper foil bending sample:

[0027] Use a sampler to cut an extremely thin electrolytic copper foil, fold the foil along the edge and align it, use a deep groove ball bearing to roll out a crease at a uniform speed on the non-aligned end of the foil, cut the crease sample into strips, and perform high-temperature heat treatment in a vacuum oven to obtain an extremely thin lithium battery copper foil bending sample.

[0028] It should be emphasized that pre-wire cutting of the sample cross section into splines before high-temperature heat treatment can not only reduce the stress introduced in the spline by uneven deformation, but also timely restore and eliminate the internal grain boundaries and defects in the test area of ​​the spline cross section during the subsequent high-temperature heat treatment, effectively reducing the impact of the internal residual stress of the electrolytic copper foil after bending and stress on the calibration rate and accuracy of the EBSD test.

[0029] In the present application, the cutting of the splines can be performed by wire cutting, but other cutting methods such as laser cutting that cause less damage to the cross section of the copper foil are not excluded.

[0030] The thickness of the cut strip is preferably controlled within a range of ≤6 μm, for example, 6 μm, 5 μm, 4.5 μm, 4 μm, etc.

[0031] In certain specific embodiments, the high temperature heat treatment temperature is illustratively but not limited to 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, and may also be any other value within the range of 120-170°C.

[0032] In some specific embodiments, the high temperature heat treatment time is illustratively but not limited to 10 minutes, 15 minutes, 20 minutes, and can also be any other value within the range of 10-20 minutes.

[0033] In an optional embodiment, the tensile strength of the ultra-thin lithium battery copper foil used can be any one of ordinary tensile strength (300-400MPa), medium tensile strength (400-500MPa), high tensile strength (500-600MPa) and ultra-high tensile strength (>600MPa).

[0034] In a second typical embodiment of the present invention, the present invention provides a method for preparing an EBSD test sample at a bend of an ultra-thin lithium battery copper foil based on the above preparation method, comprising the following steps:

[0035] S1 Preparation of bent copper foil samples to be polished: Cut the bent copper foil strips to be polished into a size suitable for the cross-section baffle of the argon ion polisher, and paste the samples on the cross-section baffle.

[0036] S2 performs cross-sectional polishing on the bent copper foil sample: Place the bent copper foil sample to be polished into an argon ion polisher, set polishing parameters, and perform rough polishing and fine finishing on the cross-sectional surface of the bent sample.

[0037] In some specific embodiments, the length of the sheared copper foil sample to be polished and bent is preferably controlled in the range of ≤15 mm, for example, it can be 4 mm, 5 mm, 6 mm, etc., or it can be any other value in the range of >0 and ≤15 mm; the width is preferably controlled in the range of ≤6 mm, for example, it can be 3 mm, 4 mm, 5 mm, etc., or it can be any other value in the range of >0 and ≤6 mm.

[0038] Before pasting the sample to the cross-section baffle, it is worth mentioning that the present application uses conductive silver paste to tightly bond the open ends of the bent copper foil sample away from the bending line, rather than unfolding the bending part according to the traditional method of preparing cross-section samples to be polished by lithium battery copper foil. This not only effectively enhances the conductivity of the sample, but also avoids the formation of a gap between the central protrusion of the crease and the plane of the cross-section baffle when unfolding the crease to prepare the sample to be polished, thereby affecting the argon ion beam cutting effect.

[0039] Furthermore, the bending part of the sample cross section is aligned and pasted to the center of the cross section baffle, and the bonding method is to brush on the conductive silver paste.

[0040] In some specific embodiments, a micrometer is used to fix the cross-section baffle so that the edge of the bent copper foil sample to be polished is exposed to the cross-section baffle of the argon ion polisher at a distance of 40-80 μm, such as 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, etc., or any other value within the range of 40-80 μm. By setting the distance in the above range, a better range of polishing depth can be obtained. If the distance is too short, the argon ion polisher may not be able to accurately identify the position; if the distance is too long, the polishing depth may be too deep, exacerbating the unevenness of the polished cross section.

[0041] In the present application, the cross-section of the bent copper foil sample is polished, and the ion polisher used is an argon ion polisher, which has two ion guns.

[0042] In an optional embodiment, the left ion gun or the right ion gun is used alone for cross-section polishing, and the corresponding ion source gun is rotated to make the deflection angle 0°. Since the bent copper foil sample is fitted to one side starting from the center line of the cross-section baffle, in order to obtain a better polishing effect, the rotation angle of the sample stage can be continuously swung back and forth within the range of -40° to +40°.

[0043] In this application, the cross-sectional polishing of the bent copper foil sample includes rough polishing and fine polishing. Rough polishing can obtain a large polishing area at a higher voltage, and fine polishing can finely repair the polished surface at a lower voltage. The two work together to obtain the best quality polished section.

[0044] The rough polishing is carried out at a voltage of 6-8KV for 20-40 minutes, and then switched to fine polishing at a voltage of 3-5KV for 5-30 minutes.

[0045] For reference, the polishing voltage of the rough polishing process can be 6kV, 6.5kV, 7kV, 7.5kV, 8kV, etc., or any other value within the range of 6-8kV.

[0046] The time for the rough polishing treatment can be 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, etc., or any other value within the range of 20-40 minutes.

[0047] The polishing voltage of the fine polishing process can be 3kV, 3.5kV, 4kV, 4.5kV, 5kV, etc., or any other value within the range of 3-5KV.

[0048] The time for fine polishing can be 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, etc., or any other value within the range of 5-30 minutes.

[0049] It is worth noting that when performing cross-sectional polishing on the bends of extremely thin lithium battery copper foil, a high EBSD calibration rate cannot be obtained by simply using a combination of rough polishing and fine polishing. Instead, specific rough polishing process conditions and specific fine polishing process conditions need to be set for samples with different tensile strengths to obtain excellent polishing results.

[0050] In a third typical embodiment of the present invention, the present invention further provides a testing method for an EBSD test sample at a bend of an ultra-thin lithium battery copper foil obtained based on the above preparation method, the steps are as follows:

[0051] The ultra-thin lithium battery copper foil sample that was polished and bent was pasted on a 70° inclined sample stage, and the conductive path between the sample and the inclined sample stage was connected. The electron backscatter diffraction analysis technology (EBSD) equipment was used for testing, and the test results were image processed.

[0052] The EBSD image quality (calibration rate) is restricted by multiple factors, such as the sample's own state, such as electrical conductivity, residual stress, etc., the sample preparation quality, such as stress relief, no oxide layer, flatness and cleanliness of the test surface, the instrument state, such as the electron microscope performance (voltage, beam current, aperture, etc.), the sensitivity of EBSD detection, software parameters, exposure parameters, and calibration method settings.

[0053] In the actual test process, for ultra-thin lithium battery copper foil, which inevitably produces residual stress due to the manufacturing process, the frequent charging phenomenon can easily cause the electron beam to deflect, resulting in a large-scale offset of the EBSD image, making the EBSD acquisition data mismatched with the initial electron image, affecting the EBSD test results. In order to reduce the impact of the charging phenomenon when testing the EBSD sample of bent ultra-thin lithium battery copper foil, under economic conditions, this application uses conductive silver paste and aluminum-based double-sided carbon conductive glue to jointly perform a cross-type bridge between the test sample and the 70° sample stage, and the conductive path covers the surface of the bent copper foil and the non-bent end of the test section.

[0054] In some specific embodiments, the scanning surface range is set to a closed area along the edge of the bent cross-sectional shape, the magnification is set to ≥3Kx, and the scanning step length is ≤0.075μm. Limiting the scanning surface to the range of the bent cross-sectional shape can reduce the scanning time. At the same time, performing EBSD testing at a higher magnification and an appropriate step length can not only ensure that the calibration speed is not too slow while ensuring the resolution, thereby increasing the probability of image drift, but also enable the EBSD acquisition system to make a more precise step length correction for the SEM electron beam scanning, thereby improving the overall calibration rate of the image.

[0055] Furthermore, noise reduction is performed on the test image.

[0056] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0057] Example 1

[0058] This embodiment provides a method for preparing an ultra-thin lithium battery copper foil bending EBSD test sample, comprising the following steps:

[0059] (1) A sampler is used to cut an ultra-thin common resistive electrolytic copper foil with a thickness of 6 μm, and the copper foil is folded and aligned along the edge. A deep groove ball bearing is used to roll out a crease at a uniform speed at the non-aligned end of the copper foil. The crease sample is cut into strips by wire cutting, and then subjected to high-temperature heat treatment in a vacuum oven to obtain an ultra-thin lithium battery copper foil bending sample.

[0060] (2) Preparation of bent copper foil samples to be polished: Cut the bent copper foil strips to be polished into samples with a length of 5 mm and a width of 4 mm. Use conductive silver paste to bond the open ends of the samples and then stick them on the plane of the cross-section baffle so that the edge of the bent copper foil sample to be polished is exposed to a distance of 70 μm from the cross-section baffle of the argon ion polisher.

[0061] (3) Polishing the cross section of the bent copper foil sample: Place the bent copper foil sample to be polished in an argon ion polisher, set to left-gun polishing, ion source deflection angle 0°, sample stage rotation angle -40° to +40°. The rough polishing voltage is 6KV, and the polishing time is 30 minutes. The fine polishing voltage is 3.5KV, and the polishing time is 5 minutes.

[0062] (4) Preparation of EBSD test samples: The ultra-thin lithium battery copper foil sample that was bent after polishing was pasted on a 70° inclined sample stage, and the conductive path between the sample and the inclined sample stage was connected in a cross shape.

[0063] Next, the bending part of the 6μm ultra-thin electrolytic copper foil was characterized in the ZEISS FE-SEM Sigma 300 field emission scanning electron microscope EBSD system, such as Figure 1 As shown, a SEM image of the bending part of a 6-micron ultra-thin electrolytic copper foil was obtained, and the polished surface was perfectly smooth.

[0064] Then set the bending section magnification to 3Kx, set the scanning range and scanning step size. Use AztecCrystal software to perform noise reduction on the test image, such as Figure 2 As shown, the reverse pole figure orientation diagram at the bending point of the 6-micron ultra-thin electrolytic copper foil was obtained.

[0065] Example 2

[0066] This embodiment provides a method for preparing an ultra-thin lithium battery copper foil bending EBSD test sample, comprising the following steps:

[0067] (1) Using a sampler, cut an ultra-thin medium-resistance electrolytic copper foil with a thickness of 6 μm, fold the copper foil along the edge and align it, use a deep groove ball bearing to roll out a crease at a uniform speed on the non-aligned end of the copper foil, use wire cutting to cut the crease sample into strips, and heat treat it at high temperature in a vacuum oven to obtain an ultra-thin lithium battery copper foil bending sample.

[0068] (2) Preparation of bent copper foil samples to be polished: Cut the bent copper foil strips to be polished into samples with a length of 4 mm and a width of 4 mm. Use conductive silver paste to bond the open ends of the samples and then stick them on the plane of the cross-section baffle so that the edge of the bent copper foil sample to be polished is exposed to a distance of 65 μm from the cross-section baffle of the argon ion polisher.

[0069] (3) Polishing the cross section of the bent copper foil sample: Place the bent copper foil sample to be polished in an argon ion polisher, set to left-gun polishing, ion source deflection angle 0°, sample stage rotation angle -40° to +40°. Rough polishing voltage is 6KV, polishing time is 30 minutes. Fine polishing voltage is 3KV, polishing time is 10 minutes.

[0070] (4) Preparation of EBSD test samples: The ultra-thin lithium battery copper foil sample that was bent after polishing was pasted on a 70° inclined sample stage, and the conductive path between the sample and the inclined sample stage was connected in a cross shape.

[0071] The same EBSD test method as in Example 1 was used to observe whether the polished surface was flat and smooth. Figure 3 As shown, the reverse pole figure orientation diagram at the bending point of the 6-micron ultra-thin medium-resistant electrolytic copper foil was obtained.

[0072] Example 3

[0073] This embodiment provides a method for preparing an ultra-thin lithium battery copper foil bending EBSD test sample, comprising the following steps:

[0074] (1) A sampler is used to cut an ultra-thin high-resistance electrolytic copper foil with a thickness of 6 μm, and the copper foil is folded and aligned along the edge. A deep groove ball bearing is used to roll out a crease at a uniform speed at the non-aligned end of the copper foil. The crease sample is cut into strips by wire cutting, and then subjected to high-temperature heat treatment in a vacuum oven to obtain an ultra-thin lithium battery copper foil bending sample.

[0075] (2) Preparation of bent copper foil samples to be polished: Cut the bent copper foil strips to be polished into samples with a length of 4 mm and a width of 3 mm. Use conductive silver paste to bond the open ends of the samples and then stick them on the plane of the cross-section baffle so that the edge of the bent copper foil sample to be polished is exposed to a distance of 60 μm from the cross-section baffle of the argon ion polisher.

[0076] (3) Polishing the bent copper foil sample: Place the bent copper foil sample to be polished in an argon ion polisher, set it to left-gun polishing, ion source deflection angle 0°, sample stage rotation angle -40° to +40°. The rough polishing voltage is 8KV, and the polishing time is 20 minutes. The fine polishing voltage is 3KV, and the polishing time is 20 minutes.

[0077] (4) Preparation of EBSD test samples: The ultra-thin lithium battery copper foil sample that was bent after polishing was pasted on a 70° inclined sample stage, and the conductive path between the sample and the inclined sample stage was connected in a cross shape.

[0078] The same EBSD test method as in Example 1 was used to observe whether the polished surface was flat and smooth.

[0079] Example 4

[0080] This embodiment provides a method for preparing an ultra-thin lithium battery copper foil bending EBSD test sample, comprising the following steps:

[0081] (1) A sampler is used to cut an ultra-thin ultra-high electrolytic copper foil with a thickness of 6 μm, and the copper foil is folded and aligned along the edge. A deep groove ball bearing is used to roll out a crease at a uniform speed at the non-aligned end of the copper foil. The crease sample is cut into strips by wire cutting, and then subjected to high-temperature heat treatment in a vacuum oven to obtain an ultra-thin lithium battery copper foil bending sample.

[0082] (2) Preparation of bent copper foil samples to be polished: Cut the bent copper foil strips to be polished into samples with a length of 5 mm and a width of 5 mm. Use conductive silver paste to bond the open ends of the samples and then stick them on the plane of the cross-section baffle so that the edge of the bent copper foil sample to be polished is exposed to a distance of 60 μm from the cross-section baffle of the argon ion polisher.

[0083] (3) Polishing the cross section of the bent copper foil sample: Place the bent copper foil sample to be polished in an argon ion polisher, set to left-gun polishing, ion source deflection angle 0°, sample stage rotation angle -40° to +40°. The rough polishing voltage is 8KV, and the polishing time is 20 minutes. The fine polishing voltage is 4.5KV, and the polishing time is 15 minutes.

[0084] (4) Preparation of EBSD test samples: The ultra-thin lithium battery copper foil sample that was bent after polishing was pasted on a 70° inclined sample stage, and the conductive path between the sample and the inclined sample stage was connected in a cross shape.

[0085] The same EBSD test method as in Example 1 was used to observe whether the polished surface was flat and smooth.

[0086] Comparative Example

[0087] Taking Example 1 as an example, comparative examples 1-8 are set.

[0088] The difference between Comparative Example 1 and Example 1 is that no high-temperature heat treatment step is performed.

[0089] The difference between Comparative Example 2 and Example 1 is that: according to the traditional method of preparing cross-section samples to be polished of lithium battery copper foil, the bent part is unfolded to prepare the samples to be polished.

[0090] The difference between Comparative Example 3 and Example 1 is that the cross-section polishing is only performed in a rough polishing process, and no fine polishing process is performed.

[0091] The difference between Comparative Example 4 and Example 1 is that the rough polishing is carried out at 4KV for 30 minutes.

[0092] The difference between Comparative Example 5 and Example 1 is that the rough polishing is carried out at 10 KV for 30 minutes.

[0093] The difference between Comparative Example 6 and Example 1 is that the fine polishing is carried out at 7 KV for 5 minutes.

[0094] The difference between Comparative Example 7 and Example 1 is that the fine polishing is carried out at 1 KV for 5 minutes.

[0095] The difference between Comparative Example 8 and Example 1 is that the bending section magnification is set to 1Kx.

[0096] Table 1 below lists the EBSD test results of the bends obtained according to various embodiments of the present invention and comparative examples, including image calibration rate and polished surface smoothness.

[0097]

[0098]

[0099] It can be seen from Table 1 that the extremely thin electrolytic copper foil bent samples prepared by the method of the present application can prepare perfectly smooth test surfaces for different tensile strengths, and have better image quality in the EBSD test.

[0100] Comparative Example 1 does not perform the high-temperature heat treatment step and has a significantly lower EBSD calibration rate than the cross-section polishing used in Example 1; Comparative Example 2 unfolds the bend for sample preparation and cannot obtain a flat and smooth stress-relieved test surface compared with Example 1; Comparative Example 3 does not undergo fine polishing, and the obtained test surface is not flat and smooth enough; Comparative Examples 4-7 use different rough polishing and fine polishing process conditions than the rough polishing and fine polishing process conditions provided in Example 1 and have lower EBSD calibration rates; In Comparative Example 8, EBSD testing is performed at a low magnification, which also leads to a significant decrease in the calibration rate.

[0101] In summary, the present application not only effectively reduces the influence of the internal residual stress of the electrolytic copper foil after bending and stress on the calibration rate and accuracy of the EBSD test, but also can prepare smooth and fine test surfaces for ultra-thin electrolytic copper foil bent samples with different tensile strengths, and accurately test the micromorphology and structure at the center of the crease, so as to facilitate the study of the internal organization and performance of the ultra-thin copper foil when it is bent for lithium battery negative electrode application.

[0102] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An electron backscatter diffraction analysis and testing method for the bending part of an ultra-thin lithium battery copper foil, characterized in that: The specific steps of the electron backscatter diffraction analysis test method for the bending part of the ultra-thin lithium battery copper foil are as follows: S1. Obtaining the bending sample of the ultra-thin lithium battery copper foil for stress relief and enhanced conductivity: using a sampler to cut the ultra-thin electrolytic copper foil, folding and aligning the copper foil along the edge, using a deep groove ball bearing to uniformly roll out the crease at the non-aligned end of the copper foil, cutting the crease sample into strips, and subjecting it to high-temperature heat treatment in a vacuum oven to obtain the bending sample of the ultra-thin lithium battery copper foil; S2. Preparation of smooth and fine test surface of the sample. Cut the bent sample to be polished into the size suitable for the cross-section baffle of the argon ion polisher, and paste the sample to the cross-section baffle; perform cross-section polishing on the bent copper foil sample. Put the bent copper foil sample to be polished into the argon ion polisher, set the polishing parameters, and perform rough polishing and fine finishing on the cross section of the bent sample; S3, Electron backscatter diffraction equipment test, the polished and bent ultra-thin lithium battery copper foil sample is pasted on a 70° inclined sample stage, the conductive path between the sample and the inclined sample stage is connected, the electron backscatter diffraction analysis technology equipment is used for testing, and the test results are processed by image.

2. The electron backscatter diffraction analysis and testing method for the bending part of the ultra-thin lithium battery copper foil according to claim 1 is characterized in that: The crease specimen strip cutting method in S1 is wire cutting.

3. The electron backscatter diffraction analysis and testing method for the bending part of the ultra-thin lithium battery copper foil according to claim 1 is characterized in that: The high temperature heat treatment in S1 is performed at a temperature of 120-170° C. for 10-20 minutes.

4. The electron backscatter diffraction analysis and testing method for the bending part of the ultra-thin lithium battery copper foil according to claim 1 is characterized in that: The ultra-thin lithium battery copper foil is classified into ordinary tensile strength (300-400MPa), medium tensile strength (400-500MPa), high tensile strength (500-600MPa) and ultra-high tensile strength (>600MPa) ultra-thin electrolytic copper foil according to the tensile strength.

5. The electron backscatter diffraction analysis and testing method for the bending part of the ultra-thin lithium battery copper foil according to claim 1 is characterized in that: The copper foil sample to be polished and bent cut in S2 preferably has a length of ≤15 mm and a width of ≤6 mm.

6. The electron backscatter diffraction analysis and testing method for the bending part of the ultra-thin lithium battery copper foil according to claim 1 is characterized in that: In the S2, conductive silver paste is used to tightly bond the open ends of the two sides of the cut bending sample away from the bending line to serve as the sample to be pasted on the cross-section baffle.

7. The electron backscatter diffraction analysis and testing method for the bending part of ultra-thin lithium battery copper foil according to claim 1, characterized in that: In S2, the sample is pasted to the cross-section baffle by brushing conductive silver paste, and the bending part of the cross-section of the sample to be polished is aligned and pasted to the center of the cross-section baffle. The edge of the bent copper foil sample to be polished is exposed to the cross-section baffle of the argon ion polisher by 40-80 μm.

8. The electron backscatter diffraction analysis and testing method for the bending part of ultra-thin lithium battery copper foil according to claim 1, characterized in that: When S2 is polished with an argon ion polisher, the ion source deflection angle is 0°, and the sample stage rotation angle is -40° to +40°. The rough polishing is performed at a voltage of 6-8KV for 20-40 minutes, and then switched to fine polishing at a voltage of 3-5KV for 5-30 minutes.

9. The electron backscatter diffraction analysis and testing method for the bending part of the ultra-thin lithium battery copper foil according to claim 1, characterized in that: The conductive path in S3 is cross-connected using conductive silver paste and aluminum-based double-sided carbon conductive adhesive. The electron backscatter diffraction analysis technology test includes setting the bending section magnification, setting the scanning surface range and scanning step length, and performing noise reduction on the test image.

10. The electron backscatter diffraction analysis and testing method for the bending part of ultra-thin lithium battery copper foil according to claim 1, characterized in that: In S3, the scanning surface range is set to a closed area along the edge of the bent cross-sectional shape, the magnification is set to ≥3Kx, and the scanning step is set to ≤0.075 μm.