Flexible ion tactile sensor and preparation method thereof

By using flexible composite electrodes and multi-stage microstructured ion dielectric layer in ion tactile sensors, combined with magnetic field induction technology, the problem of sensor sensitivity reduction in high-voltage environments is solved, achieving high sensitivity and rapid response effects.

CN118963595APending Publication Date: 2024-11-15WUYI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410983256.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In high-voltage environments, existing ion tactile sensors are difficult to maintain high sensitivity, and there are performance bottlenecks.

Method used

Designed with flexible ion tactile sensors, including flexible encapsulation layer from top to bottom, composite electrode, multi-stage microstructured ion dielectric layer and carbon cloth electrode, needle formation is induced by ionic liquid inverted and magnetic field doped with nano iron powder. The microstructure is enhanced to enhance the electrochemical activity of the electrode and the dielectric layer, and improve the sensitivity and response speed of the sensor.

Benefits of technology

In high-voltage environments, the sensitivity and response speed of the sensor are significantly improved, the response ability to magnetic field changes is enhanced, and the linearity and detection range of the sensor are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118963595A_ABST
    Figure CN118963595A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses a flexible ion tactile sensor and a preparation method thereof, and the flexible ion tactile sensor comprises an upper flexible packaging layer, a first flexible electrode, a frame layer, an ion dielectric layer of a multi-stage microstructure, a second flexible electrode and a lower flexible packaging layer which are sequentially arranged from top to bottom. Wherein the ionic dielectric layer of the multi-stage microstructure comprises a first-stage microstructure formed by reverse molding of an ionic liquid doped with nano iron powder, and a second-stage needle-shaped microstructure formed by magnetic field induction of the first-stage microstructure, so that high sensitivity of the sensor can still be ensured in a high-pressure environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the technical field of tactile sensors, and in particular to a flexible ionic tactile sensor and a method for preparing the same. Background Art

[0002] In the field of intelligent sensing, interfacial capacitive sensing technology has rapidly emerged due to its unique advantages in achieving precise tactile perception. This technology uses the strong electrostatic interaction between electrons and ions at the interface between electrodes and dielectric layers to form a double-layer region with supercapacitive characteristics. This capacitive sensing mechanism provides a solid theoretical basis for the development of a new generation of high-sensitivity, high-resolution tactile sensors.

[0003] As a typical representative of interfacial capacitive sensing technology, ionic tactile sensors (ITSs) have attracted extensive attention from the scientific research and industrial communities for their rapid response capabilities to static and dynamic stimuli, as well as their broad application prospects in the fields of human-computer interaction, health monitoring, and motion tracking. These sensors achieve significant changes in capacitance through the double electric layer formed at the electrode-dielectric layer interface, and can achieve higher sensitivity and a wider measurement range than traditional capacitive sensors.

[0004] However, despite the significant advantages of ITSs in terms of sensitivity and response speed, they still face challenges in practical applications. Especially in high-voltage environments, how to ensure the high sensitivity of sensors is a key bottleneck in the current technological development. Summary of the invention

[0005] The main purpose of the embodiments of the present application is to propose a flexible ionic tactile sensor and a preparation method thereof, aiming to ensure the sensitivity of the sensor under high pressure environment.

[0006] In a first aspect, a flexible ionic tactile sensor is provided, comprising an upper flexible packaging layer, a first flexible electrode, a frame layer, a multi-level microstructured ionic dielectric layer, a second flexible electrode and a lower flexible packaging layer, which are arranged in sequence from top to bottom; wherein the multi-level microstructured ionic dielectric layer comprises a primary microstructure formed by molding an ionic liquid doped with nano-iron powder, and a secondary needle-shaped microstructure formed by inducing the nano-iron powder by a magnetic field.

[0007] In a possible implementation, the first flexible electrode is a flexible composite electrode, and the second flexible electrode is a flexible carbon cloth electrode.

[0008] In a possible implementation, the flexible composite electrode is nickel manganese oxide (NiMnO x ) and multi-walled carbon nanotube (CNT) composite electrode, wherein NiMnO xThe specific capacitance of the electrode was significantly increased, while the doping of CNTs significantly improved the pseudocapacitance of the electrode and enhanced the overall performance of the sensor.

[0009] In a possible implementation, the framework layer is a polydimethylsiloxane hollow framework layer.

[0010] In a second aspect, a method for preparing a flexible ionic tactile sensor is provided, comprising the following steps:

[0011] Prepare an upper flexible packaging layer, a first flexible electrode, a frame layer, a multi-level microstructured ionic dielectric layer, a second flexible electrode and a lower flexible packaging layer;

[0012] The first flexible electrode, the frame layer, the multi-level microstructured ionic dielectric layer and the second flexible electrode are bonded into an integrated structure;

[0013] Leading wires from the first flexible electrode and the second flexible electrode;

[0014] Sealing and packaging the integrated structure by the upper flexible packaging layer and the lower flexible packaging layer;

[0015] The multi-level microstructured ionic dielectric layer is prepared by the following steps:

[0016] The ionic liquid doped with nano-iron powder is poured into the mold to form an initial model with a primary microstructure;

[0017] Inducing the nano-iron powder in the initial model through a magnetic field to form a target model with a secondary needle-shaped microstructure;

[0018] The target model is heated and cured, and then demolded to obtain the ionic dielectric layer of the multi-level microstructure;

[0019] The nano iron powder doped with the ionic liquid gives the sensor magnetic sensitivity. Under the action of the magnetic field, the dielectric layer undergoes displacement changes, increasing the effective contact area and improving the linearity, sensitivity and response speed of the sensor.

[0020] The primary microstructure and the secondary needle-shaped microstructure can generate a uF-level high capacitance signal output when subjected to a large pressure. This high output is achieved by enhancing the electrochemically active area between the electrode and the dielectric layer and utilizing the microstructure induced by the magnetic field, thereby significantly improving the sensitivity of the sensor.

[0021] In a possible implementation, the second flexible electrode is prepared by the following steps:

[0022] Immersing the carbon cloth cut to a specific size in a first mixed solution for chemical modification, wherein the first mixed solution is a mixed solution of hydrochloric acid and nitric acid;

[0023] The modified carbon cloth is ultrasonically cleaned with deionized water at room temperature to obtain a carbon cloth electrode substrate;

[0024] The second flexible electrode is prepared by using the carbon cloth electrode substrate.

[0025] In a possible implementation, the first flexible electrode is prepared by the following steps:

[0026] Nickel nitrate hexahydrate (Ni(NO3)2·6H2O), ammonium fluoride (NH4F), manganese sulfate (MnSO4·H2O), urea and carbon nanotubes (CNTs) are mixed in deionized water to form a precursor solution;

[0027] Immersing the pretreated carbon cloth in the precursor solution and performing a hydrothermal reaction in a hydrothermal reactor, wherein the pretreated carbon cloth is prepared using the carbon cloth electrode substrate;

[0028] The carbon cloth is taken out from the precursor solution, rinsed with deionized water, and dried with a heating plate to obtain the first flexible electrode.

[0029] In a possible implementation, the ionic liquid doped with nano iron powder is prepared by the following steps:

[0030] Mixing polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and dimethylacetamide (DMF) and heating them in an oil bath to obtain a second mixed solution;

[0031] After the second mixed solution is cooled to room temperature, 1-ethyl-3-methylimidazole bisimide salt is added to the second mixed solution and stirred evenly to obtain a third mixed solution;

[0032] The nano iron powder is uniformly dispersed in the third mixed liquid by using heating and ultrasonic treatment to obtain an ionic liquid doped with the nano iron powder.

[0033] In a possible implementation, the step of pouring the ionic liquid doped with nano iron powder into a mold to form an initial model having a primary microstructure includes:

[0034] The ionic liquid doped with nano-iron powder is poured into the 3D printed model to form an initial model with a primary microstructure;

[0035] The method of inducing the nano-iron powder in the initial model by means of a magnetic field to form a target model having a secondary needle-shaped microstructure comprises:

[0036] In a heating environment, a magnet is used to induce the nano-iron powder in the initial model to form a target model with a secondary needle-shaped microstructure.

[0037] In a possible implementation, the framework layer is prepared by the following steps:

[0038] uniformly mixing the polydimethylsiloxane and the curing agent to obtain a fourth mixed liquid;

[0039] The fourth mixed liquid is spread flat in a mold, heated using a heating plate, demoulded after solidification, and cut into a desired shape to obtain the frame layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 is a structural schematic diagram of a flexible ionic tactile sensor provided in an embodiment of the present application;

[0041] Figure numerals: flexible packaging layer 1, flexible composite electrode 2, polydimethylsiloxane hollow framework layer 3, multi-level microstructured ionic dielectric layer 4, flexible carbon cloth electrode 5.

[0042] Figure 2 Schematic diagrams of ionic dielectric layers of embodiments of the present application, wherein (a) is a schematic diagram of an ionic dielectric layer having a multi-level microstructure, and (b) is a schematic diagram of an ionic dielectric layer having a primary microstructure;

[0043] Figure 3 is a schematic diagram comparing the sensitivity of the sensors in the embodiments of the present application;

[0044] Figure 4 Schematic diagram of the principle of the flexible ionic tactile sensor of the embodiment of the present application; wherein (a) is a schematic diagram of the original state, and (b) is a schematic diagram of the loaded state;

[0045] Figure 5 is a schematic diagram comparing the sensitivity of sensors of two embodiments of the present application;

[0046] Figure 6 It is a performance diagram of the response and recovery capability of the sensor of the embodiment of the present application;

[0047] Figure 7 It is a schematic diagram of the response of the sensor of the embodiment of the present application to the magnetic field. DETAILED DESCRIPTION

[0048] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0049] It should be noted that, although the functional modules are divided in the device schematic diagram and the logical order is shown in the flowchart, in some cases, the steps shown or described may be performed in a different order than the module division in the device or the order in the flowchart. The terms "first", "second", etc. in the specification, claims and the above drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence.

[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.

[0051] The present application provides a flexible ionic tactile sensor, such as Figure 1 As shown, it includes a flexible packaging layer 1, a flexible composite electrode 2, a polydimethylsiloxane hollow framework layer 3, a multi-level microstructured ion dielectric layer 4, and a flexible carbon cloth electrode 5. The flexible packaging layer 1 includes an upper flexible packaging layer and a lower flexible packaging layer.

[0052] In this embodiment, Figure 1 , Figure 2 , Figure 4 , Figure 6 and Figure 7 As shown, a flexible ionic tactile sensor comprises an upper flexible packaging layer, a first flexible electrode, a frame layer, a multi-level microstructured ionic dielectric layer 4, a second flexible electrode and a lower flexible packaging layer arranged in sequence from top to bottom; wherein the multi-level microstructured ionic dielectric layer 4 comprises a primary microstructure formed by molding an ionic liquid doped with nano-iron powder, and a secondary needle-shaped microstructure formed by inducing the nano-iron powder with a magnetic field.

[0053] Among them, the first flexible electrode is a flexible composite electrode 2, the second flexible electrode is a flexible carbon cloth electrode 5, and the flexible composite electrode 2 and the flexible carbon cloth electrode 5 are two upper and lower asymmetric flexible electrodes, and the upper flexible packaging layer and the lower flexible packaging layer use PI tape to seal and package the upper and lower asymmetric flexible electrodes to ensure the overall airtightness and long-term stability of the flexible ion tactile sensor, and the asymmetric electrode packaging structure further expands the detection range of the flexible ion tactile sensor.

[0054] In addition, the flexible composite electrode 2 is nickel manganese oxide (NiMnO x ) and multi-walled carbon nanotube (CNT) composite electrode, wherein NiMnO x The specific capacitance of the electrode was significantly increased, while the doping of CNTs significantly improved the pseudocapacitance of the electrode, enhancing the overall performance of the flexible ionic tactile sensor.

[0055] The frame layer is a polydimethylsiloxane hollow frame layer 3.

[0056] In addition, if Figure 3 As shown, the ionic dielectric layer 4 of the multi-level microstructure is precisely molded by 3D printing technology to form the primary microstructure, and the nano-iron powder doped inside the film forms the secondary needle-shaped microstructure under the action of the magnetic field. These structures can generate high capacitance signal output when subjected to high pressure, thereby improving the linearity, sensitivity and response speed of the sensor. The nano-iron powder doped in the ionic dielectric layer 4 of the multi-level microstructure gives the flexible ionic tactile sensor magnetic sensitivity. Under the action of the magnetic field, the dielectric layer undergoes displacement changes, increasing the effective contact area, resulting in a significant change in the capacitance signal, thereby improving the responsiveness of the flexible ionic tactile sensor to changes in the magnetic field.

[0057] The present application provides a method for preparing a flexible ionic tactile sensor, such as Figure 2 and Figure 4 As shown, the method comprises the following steps:

[0058] Step S1, preparing an upper flexible packaging layer, a first flexible electrode, a frame layer, a multi-level microstructured ionic dielectric layer, a second flexible electrode and a lower flexible packaging layer;

[0059] Specifically, the multi-level microstructured ionic dielectric layer is prepared by the following steps:

[0060] Step S11, pouring the ionic liquid doped with nano iron powder into a mold to form an initial model with a primary microstructure;

[0061] Step S12, inducing the nano-iron powder in the initial model through a magnetic field to form a target model with a secondary needle-shaped microstructure;

[0062] Step S13, heating and curing the target model and then demolding the model to obtain the ionic dielectric layer of the multi-level microstructure;

[0063] The nano iron powder doped with the ionic liquid gives the sensor magnetic sensitivity. Under the action of the magnetic field, the dielectric layer undergoes displacement changes, increasing the effective contact area and improving the linearity, sensitivity and response speed of the sensor.

[0064] like Figure 3 As shown, the primary microstructure and the secondary needle-shaped microstructure can generate a high capacitance signal output of uF level when subjected to a large pressure. This high output is achieved by enhancing the electrochemical active area between the electrode and the dielectric layer and utilizing the microstructure induced by the magnetic field, thereby significantly improving the sensitivity of the sensor;

[0065] Step S2, pasting the first flexible electrode, the frame layer, the multi-level microstructured ionic dielectric layer and the second flexible electrode into an integrated structure, completing the combination of the key layers of the flexible ionic tactile sensor, and enhancing the stability and consistency of the overall structure;

[0066] Step S3, leading out wires from the first flexible electrode and the second flexible electrode;

[0067] Step S4, sealing and packaging the integrated structure by the upper flexible packaging layer and the lower flexible packaging layer to ensure the overall air tightness and long-term stability of the flexible ionic tactile sensor.

[0068] The present application also provides a method for preparing a second flexible electrode, such as Figure 1 As shown, the method for preparing the second flexible electrode of each of the above embodiments includes the following steps:

[0069] Step S1: immersing the carbon cloth cut to a specific size in a first mixed solution for 30 minutes to perform chemical modification, wherein the first mixed solution is a mixed solution of hydrochloric acid and nitric acid, and the volume ratio of the hydrochloric acid to the nitric acid is 3:1;

[0070] Step S2: ultrasonically cleaning the modified carbon cloth with deionized water at room temperature for 10 minutes to remove surface residues and form a hydrophilic surface, thereby obtaining a carbon cloth electrode substrate;

[0071] Step S3: preparing the second flexible electrode using the carbon cloth electrode substrate.

[0072] The present application also provides a method for preparing a first flexible electrode, such as Figure 1 As shown, the method for preparing the first flexible electrode of each of the above embodiments includes the following steps:

[0073] Step S1: accurately weigh 0.8724 g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 0.0741 g of ammonium fluoride (NH4F), 0.254 g of manganese sulfate (MnSO4·H2O), 0.36 g of urea and 0.088 g of carbon nanotubes (CNT), add them to 45 ml of deionized water, and stir magnetically at room temperature for 2 hours to form a precursor solution, wherein the mass ratio of the mixed solution of Ni(NO3)2·6H2O, NH4F, MnSO4·H2O, urea and CNT is precisely 8.7:0.7:2.5:3.6:0.9, and the precise ratio of each component in the solution is crucial to the electrochemical activity and structural stability of the electrode material;

[0074] Step S2: immersing the pretreated carbon cloth in the precursor solution and performing a hydrothermal reaction at 200 degrees Celsius in a hydrothermal reactor for 24 hours, wherein the pretreated carbon cloth is prepared using the carbon cloth electrode substrate. This step ensures that each component is uniformly deposited on the carbon cloth substrate and forms a preliminary structure of the composite electrode;

[0075] Step S3: taking out the carbon cloth from the precursor solution, rinsing the carbon cloth with deionized water to remove residues, then placing it in a culture dish, and using a heating plate to dry the carbon cloth at 70 degrees Celsius for 4 hours to obtain the first flexible electrode. This step ensures thorough drying of the flexible electrode and uniform distribution of the composite material.

[0076] The present application also provides a method for preparing an ionic liquid doped with nano iron powder, such as Figure 1 As shown, the method for preparing the ionic liquid doped with nano iron powder in the above embodiments comprises the following steps:

[0077] Step S1: polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and dimethylacetamide (DMF) are mixed in a weight ratio of 1:7.2, 1 g of PVDF-HFP and 7.2 g of DMF are accurately weighed, and after mixing, they are heated in an oil bath to 70 degrees Celsius and stirred for 2 hours to ensure that the materials are fully dissolved to form a uniform solution, thereby obtaining a second mixed solution;

[0078] Step S2: After the second mixed solution is cooled to room temperature, 4 g of 1-ethyl-3-methylimidazolium bisimide salt is added to the second mixed solution, and magnetic stirring is performed at room temperature for 30 minutes to ensure that the ionic liquid is evenly dispersed in the solution, thereby obtaining a third mixed solution;

[0079] Step S3: Using heating ultrasonic treatment at 50 degrees Celsius for 1 hour, 0.25 grams of nano iron powder with a particle size of 50 nanometers is evenly dispersed in the third mixed liquid, so as to achieve uniform dispersion of the nano iron powder in the solution, lay the foundation for forming a multi-level microstructure, and obtain an ionic liquid doped with nano iron powder.

[0080] The present application also provides a method of pouring an ionic liquid doped with nano iron powder into a mold to form an initial model with a primary microstructure, comprising:

[0081] The ionic liquid doped with nano-iron powder is poured into a 3D printed model with a size of 6 cm × 6 cm to form an initial model with a primary microstructure;

[0082] The present application also provides a method for inducing the nano-iron powder in the initial model by a magnetic field to form a target model with a secondary needle-like microstructure, comprising:

[0083] In a heating environment, a magnet is used to induce the nano-iron powder in the initial model at 50 degrees Celsius to form a target model with a secondary needle-like microstructure.

[0084] The present application also provides a method for preparing a frame layer, such as Figure 1 As shown, the method for preparing the frame layer of the above embodiments includes the following steps:

[0085] Step S1: uniformly mixing polydimethylsiloxane and a curing agent at a weight ratio of 10:1 to obtain a fourth mixed solution;

[0086] Step S2: Spread the fourth mixed liquid in a mold formed by a 1 mm thick 3M tape attached to the surface of an aluminum plate, heat it at 150 degrees Celsius for 2 hours using a heating plate, demold it after curing and cut it into a desired shape to obtain the frame layer.

[0087] In a specific embodiment, Figure 1 , Figure 2 , Figure 3 and Figure 4 As shown, the flexible composite electrode 2 and the flexible carbon cloth electrode 5 are two upper and lower asymmetric flexible electrodes.

[0088] In this embodiment, the flexible composite electrode 2 and the flexible carbon cloth electrode 5 are two upper and lower asymmetric flexible electrodes. If the flexible composite electrode 2 and the flexible carbon cloth electrode 5 do not introduce the design of two upper and lower asymmetric flexible electrodes, no large energy difference is formed inside the device, so the sensitivity is reduced.

[0089] In a specific embodiment, Figure 1 , Figure 2 , Figure 3 and Figure 4 As shown, the flexible composite electrode 2 is NiMnO deposited on the surface of the carbon cloth. x The flexible composite electrode 2 and the flexible carbon cloth electrode 5 are two upper and lower asymmetric flexible electrodes.

[0090] In this embodiment, the flexible composite electrode 2 is NiMnO deposited on the surface of the carbon cloth. x The flexible composite electrode 2 and the flexible carbon cloth electrode 5 are two upper and lower asymmetric flexible electrodes. If the flexible composite electrode 2 is not doped, and the flexible composite electrode 2 and the flexible carbon cloth electrode 5 do not introduce the design of two upper and lower asymmetric flexible electrodes, the composite electrode specific capacitance is relatively reduced, so the device performance is relatively worse.

[0091] In a specific embodiment, Figure 1 , Figure 2 , Figure 3 and Figure 4As shown, the flexible ionic tactile sensor uses a flexible composite electrode 2 and a flexible carbon cloth electrode 5 as electrodes, and the flexible composite electrode 2 and the flexible carbon cloth electrode 5 are two upper and lower asymmetric flexible electrodes.

[0092] In this embodiment, the flexible ion tactile sensor uses a flexible composite electrode 2 and a flexible carbon cloth electrode 5 as electrodes, and the flexible composite electrode 2 and the flexible carbon cloth electrode 5 are two upper and lower asymmetric flexible electrodes. If the flexible ion tactile sensor only uses the flexible carbon cloth electrode 5 as an electrode and does not use the design of the upper and lower two asymmetric flexible electrodes, the sensitivity of the flexible tactile sensor is greatly reduced.

[0093] In a specific embodiment, Figure 1 , Figure 2 and Figure 5 As shown, the multi-level microstructured ionic dielectric layer 4 includes a primary microstructure formed by molding an ionic liquid doped with nano-iron powder, and a secondary needle-shaped microstructure formed by inducing the nano-iron powder with a magnetic field.

[0094] In this embodiment, the multi-level microstructured ionic dielectric layer 4 includes a primary microstructure formed by molding an ionic liquid doped with nano-iron powder, and a secondary needle-shaped microstructure formed by inducing the nano-iron powder with a magnetic field. If the multi-level microstructured ionic dielectric layer 4 is not doped with nano-iron powder and the secondary needle-shaped microstructure is not formed, the sensitivity of the flexible tactile sensor is relatively reduced, and the flexible tactile sensor does not have magnetic sensitivity.

[0095] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0096] It is further understood that, although the operations are described in a specific order in the drawings in the embodiments of the present disclosure, it should not be understood as requiring the operations to be performed in the specific order shown or in a serial order, or requiring the execution of all the operations shown to obtain the desired results. In certain environments, parallel processing may be advantageous.

[0097] The preferred embodiments of the present application are described above with reference to the accompanying drawings, but the scope of the present application is not limited thereby. Any modification, equivalent substitution and improvement made by a person skilled in the art without departing from the scope and essence of the present application shall be within the scope of the present application.

Claims

1. A flexible ionic tactile sensor, characterized in that: It includes an upper flexible packaging layer, a first flexible electrode, a frame layer, an ionic dielectric layer with a multi-level microstructure, a second flexible electrode and a lower flexible packaging layer, which are arranged in sequence from top to bottom; The multi-level microstructured ionic dielectric layer includes a primary microstructure formed by molding an ionic liquid doped with nano-iron powder, and a secondary needle-shaped microstructure formed by inducing the nano-iron powder with a magnetic field.

2. The flexible ionic tactile sensor according to claim 1, characterized in that: The first flexible electrode is a flexible composite electrode, and the second flexible electrode is a flexible carbon cloth electrode.

3. The flexible ionic tactile sensor according to claim 2, characterized in that: The flexible composite electrode is a composite electrode of nickel manganese oxide and multi-walled carbon nanotubes deposited on the surface of carbon cloth.

4. The flexible ionic tactile sensor according to claim 1, characterized in that: The frame layer is a polydimethylsiloxane hollow frame layer.

5. A method for preparing a flexible ionic tactile sensor, characterized in that: The following steps are involved: Prepare an upper flexible packaging layer, a first flexible electrode, a frame layer, a multi-level microstructured ionic dielectric layer, a second flexible electrode and a lower flexible packaging layer; The first flexible electrode, the frame layer, the multi-level microstructured ionic dielectric layer and the second flexible electrode are bonded into an integrated structure; Leading wires from the first flexible electrode and the second flexible electrode; sealing and packaging the integrated structure by the upper flexible packaging layer and the lower flexible packaging layer; The multi-level microstructured ionic dielectric layer is prepared by the following steps: The ionic liquid doped with nano-iron powder is poured into the mold to form an initial model with a primary microstructure; Inducing the nano-iron powder in the initial model through a magnetic field to form a target model having a secondary needle-shaped microstructure; The target model is heated and solidified, and then demolded to obtain the ionic dielectric layer of the multi-level microstructure.

6. The method for preparing the flexible ionic tactile sensor according to claim 5, characterized in that: The second flexible electrode is prepared by the following steps: Immersing the carbon cloth cut to a specific size in a first mixed solution for chemical modification, wherein the first mixed solution is a mixture of hydrochloric acid and nitric acid; The modified carbon cloth is ultrasonically cleaned using deionized water at room temperature to obtain a carbon cloth electrode substrate; The second flexible electrode is prepared by using the carbon cloth electrode substrate.

7. The method for preparing the flexible ionic tactile sensor according to claim 6, characterized in that: The first flexible electrode is prepared by the following steps: Nickel nitrate hexahydrate (Ni(NO3)2·6H2O), ammonium fluoride (NH4F), manganese sulfate (MnSO4·H2O), urea, and carbon nanotubes (CNTs) were mixed in deionized water to form a uniform precursor solution; Immersing the pretreated carbon cloth in the precursor solution and performing a hydrothermal reaction in a hydrothermal reactor, wherein the pretreated carbon cloth is prepared using the carbon cloth electrode substrate; The carbon cloth is taken out from the precursor solution, rinsed with deionized water, and dried with a heating plate to obtain the first flexible electrode.

8. The method for preparing the flexible ionic tactile sensor according to claim 5, characterized in that: The ionic solution doped with nano-iron powder is prepared by the following steps: Mixing polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and dimethylacetamide (DMF) and heating them in an oil bath to obtain a second mixed solution; After the second mixed solution is cooled to room temperature, 1-ethyl-3-methylimidazolium bisimide salt is added to the second mixed solution and stirred uniformly to obtain a third mixed solution; The nano iron powder is uniformly dispersed in the third mixed liquid by using heating and ultrasonic treatment to obtain an ionic liquid doped with the nano iron powder.

9. The method for preparing the flexible ionic tactile sensor according to claim 8, wherein: The step of pouring the ionic liquid doped with nano-iron powder into a mold to form an initial model having a primary microstructure comprises: The ionic liquid doped with nano-iron powder is poured into the 3D printed model to form an initial model with a primary microstructure; The method of inducing the nano-iron powder in the initial model by a magnetic field to form a target model having a secondary needle-shaped microstructure includes: Under a heating environment, a magnet is used to induce the nano-iron powder in the initial model to form a target model with a secondary needle-shaped microstructure.

10. The method for preparing the flexible ionic tactile sensor according to claim 5, characterized in that: The frame layer is prepared by the following steps: uniformly mixing polydimethylsiloxane and a curing agent to obtain a fourth mixed liquid; The fourth mixed liquid is spread flatly in a mold, heated using a heating plate, demoulded after solidification, and cut into a desired shape to obtain the frame layer.