Cadmium-containing iron oxide-based composite magnetic material as well as preparation method and application thereof
The preparation of cadmium-containing iron oxide-based composite magnetic materials was solved by one-step method, and the problems of complex preparation and uneven dispersion in the prior art were solved, and the stability and magnetization were improved, which was suitable for photocatalytic degradation of organic matter.
Patent Information
- Application Number
- CN202411256334.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-15
AI Technical Summary
The existing preparation method for ferromagnetic materials containing cadmium-containing surface layer is complex and has the problem of uneven dispersion of precipitates, making it difficult to effectively adjust the coercive force and stability of the magnetic materials.
A one-step method is used to prepare iron oxide-based composite magnetic materials containing cadmium. By preparing a specific ratio of FeCl3, Mg(NO3)2, NaOH, FeCl2 and Cd(NO3)2 aqueous solutions, the reaction conditions such as temperature and pH value are controlled, and precipitation is carried out. Clean and dry to form nanoparticles with stable magnetic properties and adjustable magnetization.
Simple and controllable process conditions are achieved, and iron oxide-based composite magnetic material with stable magnetic properties and adjustable magnetization is prepared. It is suitable for catalysis of degradation of organic matter and significantly improves the coercive force and photocatalytic properties of the material.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of nanomaterials and specifically relates to a cadmium-containing iron oxide-based composite magnetic material and a preparation method and application thereof. Background Art
[0002] Iron oxide-based composite magnetic material is a magnetic nanomaterial with a particle size of less than 100 nanometers. Due to its excellent thermally stable magnetic properties, it has been used in the fields of cell separation, magnetic colloid synthesis, information recording, etc. In addition to maintaining excellent thermally stable magnetic properties, the iron oxide-based composite magnetic material containing a cadmium surface layer can also increase its coercivity. This kind of particle whose properties are modulated by cadmium in the surface layer has more stable magnetic properties than the particles doped with cadmium inside the iron oxide particles, including temperature characteristics, magnetostriction and aging characteristics. This is because the cadmium-containing modulation of the surface layer belongs to the epitaxial growth of a layer of cadmium-based iron oxide on the surface of the iron oxide, while the addition of cadmium inside the iron oxide particles will change the internal structure of the iron oxide and make the iron oxide metastable.
[0003] The usual method for preparing cadmium-containing surface iron oxide magnetic materials is to perform secondary treatment on the prepared iron oxide magnetic powder to form a cadmium-coated iron oxide material. This method has a relatively complicated preparation process and has the problem that the iron oxide magnetic material precursor is difficult to disperse evenly during the secondary treatment. Summary of the invention
[0004] The invention provides a cadmium-containing iron oxide-based composite magnetic material and a preparation method and application thereof.
[0005] Based on the above purpose, the present invention adopts the following technical solutions: A method for preparing a cadmium-containing iron oxide-based composite magnetic material comprises the following steps: (1) Prepare FeCl3 aqueous solution, Mg(NO3)2 aqueous solution, NaOH aqueous solution, FeCl2 aqueous solution, Cd(NO3)2 aqueous solution and dilute nitric acid; (2) Pour the Mg(NO3)2 aqueous solution into the FeCl3 aqueous solution at a molar ratio of Fe to Mg of (1-3):1, and stir thoroughly to obtain solution A; (3) Pour the NaOH aqueous solution into solution A at a volume ratio of (8-12):1, and stir thoroughly to obtain solution B; heat solution B to boiling while stirring; keep boiling for 5-10 minutes, then stop heating and cool naturally to room temperature. The molar ratio of NaOH to FeCl3 is 8-10:1; (4) Filter and wash the precipitate with dilute nitric acid; (5) heating the FeCl2 aqueous solution to boiling, and then adding the precipitate obtained in step (4), wherein the volume ratio of the FeCl2 aqueous solution to the precipitate is (20-10):1, and the molar ratio of FeCl2 to FeCl3 is (2-3):1; (6) Keep boiling for 15-25 minutes and then add Cd(NO3)2 aqueous solution; the molar ratio of Cd(NO3)2 to FeCl2 is 1:(2-3); (7) Continue boiling for 5-10 minutes and then add NaOH aqueous solution, with the molar ratio of NaOH to FeCl2 being (0.5-1.5):5; (8) After boiling for 5 to 10 minutes, stop heating, cool naturally to room temperature, filter, wash and dry the precipitate to obtain a cadmium-containing iron oxide-based composite magnetic material.
[0006] Preferably, in step (1), the concentration of the FeCl3 aqueous solution is 0.4~2 mol / L, the concentration of the Mg(NO3)2 aqueous solution is 1~3 mol / L, and hydrochloric acid is added to the Mg(NO3)2 solution at a ratio of 0.05~2 mol HCl per liter of Mg(NO3)2 aqueous solution, and the concentration of the hydrochloric acid is 10~12 mol / L; the concentration of the NaOH aqueous solution is 0.1~2 mol / L, the concentration of the FeCl2 aqueous solution is 0.1~2 mol / L, the concentration of the Cd(NO3)2 aqueous solution is 0.05~2 mol / L, and the concentration of nitric acid is 0.01~0.05 mol / L.
[0007] Furthermore, in step (4), the specific process of cleaning is: adding dilute nitric acid to the precipitate, stirring evenly, then centrifuging, and adding dilute nitric acid again until the pH value of the solution after centrifugation is 7-8.
[0008] Furthermore, in step (8), the cleaning and drying are specifically performed as follows: S1. Use 0.01~0.05 mol / L nitric acid as a cleaning solution for the precipitate, stir evenly, then centrifuge, and add 0.01~0.05 mol / L nitric acid again until the pH value of the solution after centrifugation is 7~8; S2, dehydration with acetone; S3, transferring the dehydrated product into a silica gel dryer for natural drying; S4, drying for at least 24 hours, grinding, and obtaining an anhydrous cadmium-containing iron oxide composite magnetic material.
[0009] The cadmium-containing iron oxide composite magnetic material is prepared by the above preparation method.
[0010] The application of the above cadmium-containing iron oxide composite magnetic material in the degradation of organic matter.
[0011] The organic substance is rhodamine B.
[0012] Furthermore, under light, a cadmium-containing iron oxide composite magnetic material is added to the waste liquid containing rhodamine B, and under light and stirring, an adsorption-desorption equilibrium is reached, wherein the amount of the cadmium-containing iron oxide composite magnetic material added is 1 mg to 2 mg per 10 mL of waste liquid, and the concentration of rhodamine B in the waste liquid is 1 to 20 mg / L. -1 .
[0013] Preferably, a 300 W xenon lamp equipped with a 1.5G filter is used as the light source.
[0014] The cadmium content in the final product can be changed by adding different amounts of cadmium nitrate or sodium hydroxide in the above synthesis steps. The magnetic properties of the prepared composite magnetic material, namely the magnetization intensity, change with the cadmium content.
[0015] The method uses common raw materials, adopts a one-step preparation method, has a simple process, and the process conditions are easy to control. No toxic gas is formed, and the generated wastewater is easy to collect. The magnetic properties of the prepared composite magnetic material are stable, and the magnetization intensity σ can be changed with the preparation conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 3 is a curve showing the relationship between the specific magnetization intensity σ and the magnetic field H of the composite magnetic material synthesized in Example 1.
[0017] Figure 2 is a transmission electron microscope image of the composite magnetic material synthesized in Example 1; Figure 3 is an X-ray energy dispersive spectrum (EDX) image of the composite magnetic material synthesized in Example 1; Figure 4 is a degradation curve diagram of Rhodamine B degraded by the composite magnetic material synthesized in Example 1; Figure 5 is a curve showing the relationship between the specific magnetization intensity σ and the magnetic field H of the composite magnetic material synthesized in Example 2; Figure 6 is a transmission electron microscope image of the composite magnetic material synthesized in Example 2; Figure 7 is an X-ray energy dispersive spectrum (EDX) image of the composite magnetic material synthesized in Example 2; Figure 8 is a degradation curve diagram of Rhodamine B degraded by the composite magnetic material synthesized in Example 2; Fig. 9 is a curve showing the relationship between the specific magnetization intensity σ and the magnetic field H of the composite magnetic material synthesized in Example 3; Fig.10This is a degradation curve of Rhodamine B by the composite magnetic material synthesized in Example 3. DETAILED DESCRIPTION
[0018] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. It should be understood that these preferred embodiments are only intended to illustrate the present invention rather than to limit the protection scope of the present invention.
[0019] Example 1 A method for preparing a cadmium-containing iron oxide-based composite magnetic material comprises the following steps: 1. Solution preparation Solution ①: 40 mL of 1 mol / L FeCl3 aqueous solution.
[0020] Solution ②: 10 mL of 2 mol / L Mg(NO3)2 aqueous solution, add 4.2 mL (0.05 mol) of 12 mol / L HCl aqueous solution; Solution ③: 520 mL of 0.7 mol / L NaOH aqueous solution.
[0021] Solution ④: 400 mL of 0.25 mol / L FeCl2 aqueous solution.
[0022] Solution ⑤: 50 mL of 1 mol / L Cd(NO3)2 aqueous solution.
[0023] Solution ⑥: 1000 mL of 0.01 mol / L HNO3 cleaning solution.
[0024] 2. Synthesis (1) Pour solution ② into solution ① and stir thoroughly to obtain solution A.
[0025] (2) Pour 500 mL of solution ③ into solution A quickly (within 10 seconds) while stirring, and obtain solution B after thorough stirring.
[0026] (3) Heat solution B to boiling while stirring.
[0027] (4) Keep boiling for 5 minutes, then stop heating and let it cool naturally to room temperature. During the cooling process, a precipitate will gradually precipitate. After 2 hours, the precipitation is complete.
[0028] (5) Mix the precipitate and the cleaning solution (solution ⑥) in a volume ratio of 1:5, stir thoroughly, and then separate in a centrifuge. Wash several times until the pH value of the solution after centrifugation is about 7.5.
[0029] (6) Heat solution ④ to boiling and add the precipitate obtained in step (5).
[0030] (7) Keep boiling for 20 minutes and then add solution ⑤.
[0031] (8) Continue boiling for 10 minutes and then add 20 mL of solution ③.
[0032] (9) After boiling for 10 minutes, stop heating and cool naturally to room temperature. The composite material gradually precipitates. The precipitation is complete after 2 hours.
[0033] 3. Cleaning and drying (1) Mix the precipitate and the cleaning solution (0.01 mol / L HNO3 aqueous solution) in a volume ratio of 1:5, stir thoroughly and centrifuge. Repeat this step three times until the pH value reaches about 7.5.
[0034] (2) Mix the precipitate and acetone in a volume ratio of 1:5. Stir thoroughly and separate using a centrifuge. Repeat this step twice.
[0035] (3) The dehydrated product is transferred to a silica gel dryer for drying.
[0036] (4) After 24 hours, the mixture is completely dried and ground to obtain a dry and anhydrous cadmium-modulated iron oxide-based composite magnetic material.
[0037] The magnetization curve of the composite magnetic material synthesized in Example 1 is as follows: Figure 1 As shown, the specific saturation magnetization σ s 35.2 emu / g, coercivity H c The transmission electron microscope image is as follows Figure 2 As shown in Figure 2, nanoparticles tend to aggregate and have poor dispersion. The X-ray energy dispersion spectrum is shown in Figure 2. Figure 3 As shown in Figure 2, the molar content of Cd is 8.08%. The performance of photocatalytic degradation of organic matter (Rhodamine B) is shown in Figure 2. Figure 4 As shown in the figure, 84.8% of the degradation was observed within 50 min. The concentration of rhodamine B was 10 mg L -1 , the volume was 200 mL, 30 mg of the prepared magnetic catalyst was added into a double-layer quartz catalytic vessel. Under light, the sample and rhodamine B were fully stirred to reach adsorption-desorption equilibrium. A 300 W xenon lamp equipped with a 1.5G filter was used as the light source.
[0038] Example 2 A method for preparing a cadmium-containing iron oxide-based composite magnetic material comprises the following steps: 1. Solution preparation Solution ①: 20 mL of 2 mol / L FeCl3 aqueous solution; Solution ②: 20 mL of 1 mol / L Mg(NO3)2 aqueous solution, add 5 mL (0.06 mol) of 12 mol / L HCl aqueous solution; Solution ③: 540 mL of 0.7 mol / L NaOH aqueous solution; Solution ④: 400 mL of 0.25 mol / L FeCl2 aqueous solution; Solution ⑤: 25 mL of 2 mol / L Cd(NO3)2 aqueous solution; Solution ⑥: 1000 mL of 0.01 mol / L HNO3 cleaning solution.
[0039] 2. Synthesis (1) Pour solution ② into solution ① and stir thoroughly to obtain solution A; (2) Pour 500 mL of solution ③ into solution A quickly (within 10 seconds) while stirring, and obtain solution B after sufficient stirring; (3) Heat solution B to boiling while stirring.
[0040] (4) Keep boiling for 5 minutes, then stop heating and let it cool naturally to room temperature. During the cooling process, a precipitate will gradually precipitate. After 2 hours, the precipitation is complete.
[0041] (5) Mix the precipitate and the cleaning solution in a volume ratio of 1:5, stir thoroughly, and then separate on a centrifuge. Wash several times until the pH value is about 7.5.
[0042] (6) Heat solution ④ to boiling and add the precipitate obtained in step (5).
[0043] (7) Keep boiling for 20 minutes and then add solution ⑤.
[0044] (8) Continue boiling for 20 minutes and then add 40 mL of solution ③.
[0045] (9) After boiling for 10 minutes, stop heating and cool naturally to room temperature. The composite magnetic material will gradually precipitate. The precipitation is complete after 2 hours.
[0046] 3. Cleaning and drying Same as Example 1.
[0047] The magnetization curve of the composite magnetic material synthesized in Example 2 is as follows: Figure 5 As shown, its saturation magnetization is larger than σ s 58.2 emu / g, coercivity H c The magnetic field of the sample in Example 2 is 48.6 Oe, indicating that the sample in Example 2 has strong magnetic properties. Figure 6 As shown in Figure 2, the nanoparticles have good dispersion. The X-ray energy dispersion spectrum is shown in Figure 2 Figure 7 As shown in Figure 2, the molar content of Cd is 12.34%. The performance of photocatalytic degradation of organic matter (Rhodamine B) is shown in Figure 2. Figure 8 As shown in the figure, 91.7% of the degradation was achieved within 50 min, which is better than the catalytic performance of the sample in Example 1, indicating that the modulation of Cd is beneficial to the photocatalytic degradation of organic matter. -1 30 mg of the prepared magnetic catalyst was added to a double-layer quartz catalytic vessel with a volume of 200 mL. The sample and rhodamine B were fully stirred to reach adsorption-desorption equilibrium. A 300 W xenon lamp equipped with a 1.5G filter was used as the light source.
[0048] In order to prove that the prepared composite material has iron oxide as the core and its surface layer is a cadmium-containing layer, the present application performs XPS characterization on Example 1 and Example 2. The atomic percentages of each element are shown in the table below. As the NaOH content in Example 2 increases, the content of cadmium oxide generated on the surface also increases. Since the detection depth of XPS is about 3nm, it can only detect the surface / interface area, so the increased cadmium oxide exists on the surface. In addition, the sample contains Cl elements, which is because the Cl ions in the solution are partially attached to the sample surface, and the Cd / Cl in Example 2 is greater than that in Example 1, which further illustrates that the surface of the prepared sample is a cadmium layer. Therefore, the composite magnetic material prepared by this method has iron oxide as the core and its surface layer is a cadmium-containing layer.
[0049] Example 3 A method for preparing a pure iron oxide magnetic material (as a comparative study) comprises the following steps: 1. Solution preparation Solution ①: 100 mL of 0.4 mol / L FeCl3 aqueous solution.
[0050] Solution ②: 10 mL of 2 mol / L Mg(NO3)2 aqueous solution, add 4.2 mL of 12 mol / L HCl aqueous solution; Solution ③: 500 mL of 0.7 mol / L NaOH aqueous solution.
[0051] Solution ④: 400 mL of 0.25 mol / L FeCl2 aqueous solution; Solution ⑤: 1000mL of 0.01mol / L HNO3 cleaning solution.
[0052] 2. Synthesis (1) Pour solution ② into solution ① and stir thoroughly to obtain solution A.
[0053] (2) Pour 500 mL of solution ③ into solution A quickly (within 10 seconds) while stirring, and obtain solution B after thorough stirring.
[0054] (3) Heat solution B to boiling while stirring.
[0055] (4) Keep boiling for 5 minutes, then stop heating and let it cool naturally to room temperature. During the cooling process, a precipitate will gradually precipitate. After 2 hours, the precipitation is complete.
[0056] (5) Mix the precipitate and the cleaning solution (solution ⑤) in a volume ratio of 1:5, stir thoroughly, and then separate in a centrifuge. Wash several times until the pH value of the solution after centrifugation is about 7.5.
[0057] (6) Heat solution ④ to boiling and add the precipitate obtained in step (5).
[0058] (7) Continue boiling for 10 minutes and then add 20 mL of solution ③.
[0059] (8) After boiling for 10 minutes, stop heating and cool naturally to room temperature. The composite material gradually precipitates. The precipitation is complete after 2 hours.
[0060] 3. Cleaning and drying Same as Example 1.
[0061] The magnetization curve of the magnetic material synthesized in Example 3 is as follows Fig. 9 As shown, the specific saturation magnetization σ s 42.6emu / g, coercivity H c As a comparative study, the photocatalytic degradation performance of organic matter (rhodamine B) by cadmium-free iron oxide magnetic materials is as follows Fig.10 As shown in the figure, the degradation rate was 59.3% within 50 min, which was much lower than that of cadmium-containing materials and met the catalytic performance of magnetic materials. -1 , the volume was 200 mL, 30 mg of the prepared magnetic catalyst was added into a double-layer quartz catalytic vessel. Under light, the sample and rhodamine B were fully stirred to reach adsorption-desorption equilibrium. A 300 W xenon lamp equipped with a 1.5G filter was used as the light source.
[0062] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a cadmium-containing iron oxide-based composite magnetic material, characterized in that: The steps include: (1) Prepare FeCl3 aqueous solution, Mg(NO3)2 aqueous solution, NaOH aqueous solution, FeCl2 aqueous solution, Cd(NO3)2 aqueous solution and dilute nitric acid; (2) Pour the Mg(NO3)2 aqueous solution into the FeCl3 aqueous solution at a molar ratio of Fe to Mg of (1-3):1, and stir thoroughly to obtain solution A; (3) Pour the NaOH aqueous solution into solution A at a volume ratio of (8-12):1, and stir thoroughly to obtain solution B; heat solution B to boiling while stirring; keep boiling for 5-10 minutes, then stop heating and cool naturally to room temperature. The molar ratio of NaOH to FeCl3 is 8-10:1; (4) Filter and wash the precipitate with dilute nitric acid; (5) heating the FeCl2 aqueous solution to boiling, and then adding the precipitate obtained in step (4), wherein the volume ratio of the FeCl2 aqueous solution to the precipitate is (20-10):1, and the molar ratio of FeCl2 to FeCl3 is (2-3):1; (6) Keep boiling for 15-25 minutes and then add Cd(NO3)2 aqueous solution; the molar ratio of Cd(NO3)2 to FeCl2 is 1:(2-3); (7) Continue boiling for 5-10 minutes and then add NaOH aqueous solution, with the molar ratio of NaOH to FeCl2 being (0.5-1.5):5; (8) After boiling for 5 to 10 minutes, stop heating, cool naturally to room temperature, filter, wash and dry the precipitate to obtain a cadmium-containing iron oxide-based composite magnetic material.
2. The method for preparing the cadmium-containing iron oxide composite magnetic material according to claim 1, characterized in that: In step (1), the concentration of the FeCl3 aqueous solution is 0.4~2 mol / L, the concentration of the Mg(NO3)2 aqueous solution is 1~3 mol / L, and hydrochloric acid is added to the Mg(NO3)2 solution at a ratio of 0.05~2 mol HCl per liter of Mg(NO3)2 aqueous solution, and the concentration of the hydrochloric acid is 10~12 mol / L; the concentration of the NaOH aqueous solution is 0.1~2 mol / L, the concentration of the FeCl2 aqueous solution is 0.1~2 mol / L, the concentration of the Cd(NO3)2 aqueous solution is 0.05~2 mol / L, and the concentration of nitric acid is 0.01~0.05 mol / L.
3. The method for preparing the cadmium-containing iron oxide composite magnetic material according to claim 1, characterized in that: In step (4), the specific process of cleaning is: adding dilute nitric acid to the precipitate, stirring evenly, then centrifuging, and adding dilute nitric acid again until the pH value of the solution after centrifugation is 7-8.
4. The method for preparing the cadmium-containing iron oxide composite magnetic material according to claim 1, characterized in that: In step (8), cleaning and drying, the specific process is as follows: S1. Use 0.01~0.05 mol / L nitric acid as a cleaning solution for the precipitate, stir evenly, then centrifuge, and add 0.01~0.05 mol / L nitric acid again until the pH value of the solution after centrifugation is 7~8; S2, dehydration with acetone; S3, transferring the dehydrated product into a silica gel dryer for natural drying; S4, drying for at least 24 hours, grinding, and obtaining an anhydrous cadmium-containing iron oxide composite magnetic material.
5. The cadmium-containing iron oxide composite magnetic material obtained by the preparation method according to any one of claims 1 to 4.
6. Use of the cadmium-containing iron oxide composite magnetic material according to claim 5 in degrading organic matter.