Groove type silicon carbide MOSFET device and preparation method thereof

By introducing inverted T-type electric field modulation region and body diode region into the trench SiC MOSFET device, the premature breakdown problem caused by the electric field aggregation effect of the trench bottom angle is solved, and the reliability and conduction performance of the device are improved , the effect of electric field modulation and the well region being distant is achieved.

CN118969847APending Publication Date: 2024-11-15NARI LIANYAN SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076000.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Trench SiC MOSFET devices are prone to premature breakdown and burning due to the electric field aggregation effect of the trench bottom angle electric field, and gate oxygen breakdown leads to device failure. How to modulate the electric field at the bottom of the trench to reduce this risk is difficult.

Method used

Adopting an inverted T-type electric field modulation zone structure, by setting an inverted T-type electric field modulation zone and body diode zone in the epitaxial layer, modulate the internal electric field of the device, reduce the electric field strength of the bottom angle of the trench, and avoid the natural electric field modulation zone and the well zone. depletion effect, thereby improving device reliability and conduction capability.

Benefits of technology

Effectively eliminate the electric field aggregation effect of the bottom angle of the trench, reduce the risk of gate oxygen breakdown, improve the reliability and conduction performance of the device, avoid premature breakdown and burning of the device, and ensure that the electric field modulation area is away from the trap area, and prevent the deterioration of the conduction performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969847A_ABST
    Figure CN118969847A_ABST
Patent Text Reader

Abstract

According to the trench type silicon carbide MOSFET device and the preparation method thereof, an inverted T-shaped electric field modulation region effectively modulates an internal electric field of the device, eliminates an electric field aggregation effect at a trench bottom corner, shields the electric field intensity in gate oxide, and avoids gate oxide breakdown, so that the device is prevented from being broken down and burnt out too early, and the reliability of the device is improved; the inverted T-shaped electric field modulation region is far away from the well region of the device while modulating the electric field, so that the natural depletion effect of the electric field modulation structure and the well region is effectively relieved, and the conduction performance of the device is prevented from being deteriorated; the body diode region serves as a body diode structure in the device and transmits reverse current when the device is in a working blocking state; the device structure and the preparation method are simple, the improvement effect is obvious, high-performance and batch preparation of the groove type SiC MOSFET device can be realized, and the device has huge market potential and wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a semiconductor device, and in particular to a trench-type silicon carbide MOSFET device and a preparation method thereof. Background Art

[0002] The development of third-generation semiconductor materials, represented by silicon carbide (SiC), has ushered in a new era for the semiconductor industry, becoming a cutting-edge and key core technology for vigorous development in the semiconductor industry and presenting new development opportunities for power electronics device technology and industry. SiC power devices simultaneously achieve excellent performance, including high breakdown voltage, low on-resistance, high switching speed, and easy heat dissipation. They are highly competitive in high-efficiency, high-power, and high-temperature power electronics, and have become a research hotspot in power semiconductor technology. Compared to planar-gate SiC MOSFETs, trench-gate SiC MOSFETs lack a parasitic junction field-effect transistor (JFET) region, significantly reducing device on-resistance. Furthermore, the further reduction in unit cell size further increases device power density and reduces system power consumption, offering significant performance advantages and promising application prospects. However, trench-gate SiC MOSFETs are susceptible to premature device breakdown and even burnout due to electric field concentration effects at the bottom corners of the trench. Furthermore, the high electric field within the gate oxide at the bottom of the trench can easily cause gate oxide breakdown, leading to device failure. Therefore, how to modulate the electric field at the bottom of the trench of the trench SiC MOSFET device and reduce the risk of gate oxide breakdown is a difficult and hot issue for trench SiC MOSFET devices. Patent application number 202110726765.3 discloses a trench SiC MOSFET device that introduces a column area electric field modulation structure, which can effectively alleviate the electric field distribution at the bottom of the trench, eliminate the electric field concentration effect, and shield the electric field strength in the gate oxide, reduce the electric field strength in the gate oxide, and avoid gate oxide breakdown, thereby preventing the device from breaking down and burning prematurely and improving device reliability. However, the introduced column area structure will naturally deplete the original well area of ​​the device, thereby deteriorating the device's conduction capability. Summary of the Invention

[0003] Purpose of the invention: The purpose of the present invention is to prevent the device from premature breakdown and burning, improve the reliability of the device, and at the same time improve the conduction capability of the device, and provide a trench silicon carbide MOSFET device; another purpose of the present invention is to provide a method for preparing the device.

[0004] Technical solution: The trench-type silicon carbide MOSFET device of the present invention comprises a drain electrode, a drain ohmic contact layer, a heavily doped substrate of the first doping type, a lightly doped epitaxial layer of the first doping type, and a passivation layer, which are arranged in sequence from bottom to top; a well region of the second doping type is arranged in the middle of the top of the epitaxial layer, a source region of the first doping type is arranged on the top of the well region, a gate trench is arranged in the middle of the top of the epitaxial layer through the well region and the source region, a gate dielectric layer is arranged in the trench, and polysilicon of the first doping type fills the gate trench; source windows are arranged at both ends of the passivation layer, a source ohmic contact layer is arranged thereon, and the source electrode is placed on the source ohmic contact layer; a gate window is arranged in the middle of the passivation layer and above the polysilicon, and the gate electrode is placed on the gate window; it is characterized in that in the epitaxial layer, an inverted T-shaped electric field modulation region of the second doping type is symmetrically arranged at both ends of the well region and the source region, and a body diode region of the second doping type is arranged at the top of the inverted T-shaped electric field modulation region.

[0005] Furthermore, a buffer layer is provided between the substrate and the epitaxial layer for transitioning doping concentration and preventing abnormal growth due to concentration gradient changes.

[0006] Furthermore, the first doping type is P-type and the second doping type is N-type, or the first doping type is N-type and the second doping type is P-type.

[0007] Furthermore, the longitudinal region of the inverted T-shaped electric field modulation region has a depth of 0.8 to 2.0 μm, a width of 0.3 to 1.0 μm, and a doping concentration of 1e17 to 1e19 cm -3 The depth of the lateral region is 0.2 to 1.0 μm, and the doping concentration is 1e17 to 1e19 cm -3 The distance between the boundary of the lateral region and the longitudinal region is 0.2 to 0.6 μm. As an electric field modulation structure, the inverted T-shaped electric field modulation region can pull the maximum electric field peak from the bottom corner of the trench to the bottom of the electric field modulation region when the device is in the blocked state, thereby reducing the electric field concentration effect at the bottom corner of the trench and modulating the internal electric field of the device. At the same time, the electric field strength at the bottom corner of the trench is reduced, further reducing the electric field strength in the gate oxide at the bottom of the trench, thereby avoiding gate oxide breakdown. In addition, due to the inverted T-shaped structure, while modulating the electric field, the longitudinal region can be made narrower, thereby ensuring that the electric field modulation region is far away from the device well region, thereby effectively alleviating the natural depletion effect between the electric field modulation region and the well region, and avoiding the deterioration of the device conduction performance.

[0008] Furthermore, the body diode region has a depth of 0.2 to 0.5 μm, a width of 0.3 to 1.0 μm, and a doping concentration of 1e18 to 1e20 cm -3The width of the body diode region is less than or equal to the longitudinal width of the inverted T-shaped electric field modulation region. The body diode region serves as the body diode structure inside the device and transmits reverse current when the device is in the blocking state.

[0009] Furthermore, the gate dielectric layer is a silicon oxide layer or an aluminum oxide layer, and has a thickness of 30 to 100 nm.

[0010] The method for preparing a trench silicon carbide MOSFET device according to the present invention comprises the following steps:

[0011] 1) preparing a heavily doped substrate of a first doping type, and growing a lightly doped epitaxial layer of the first doping type on the upper surface of the substrate;

[0012] 2) forming an inverted T-shaped electric field modulation region of a second doping type in the epitaxial layer;

[0013] 3) forming a body diode region of a second doping type in the inverted T-shaped electric field modulation region;

[0014] 4) forming a well region of the second doping type in the epitaxial layer and between the inverted T-shaped electric field modulation regions, and forming a source region of the first doping type in the well region;

[0015] 5) forming a gate trench in the epitaxial layer;

[0016] 6) forming a gate dielectric layer on the inner surface of the gate trench;

[0017] 7) Filling the gate trench with polysilicon of the first doping type;

[0018] 8) forming a passivation layer on the upper surface of the epitaxial layer;

[0019] 9) forming source windows at both ends of the passivation layer, forming a source ohmic contact layer on the upper surface thereof, and forming a source electrode on the surface of the source ohmic contact layer;

[0020] 10) forming a gate window in the middle of the passivation layer and above the polysilicon, and forming a gate electrode on its upper surface;

[0021] 11) Thinning the bottom of the substrate;

[0022] 12) A drain ohmic contact layer is formed on the bottom surface of the thinned substrate, and a drain electrode is formed on the lower surface thereof.

[0023] Furthermore, a buffer layer is provided between the substrate and the epitaxial layer for transitioning doping concentration and preventing abnormal growth due to concentration gradient changes.

[0024] Furthermore, the step 2) includes the following steps:

[0025] 2-1) forming an ion implantation mask layer on the surface of the epitaxial layer, wherein the ion implantation mask layer is composed of two dielectric film layers: a first dielectric film layer is silicon nitride or polysilicon, having a thickness of 0.5 to 1.5 μm; and a second dielectric film layer is silicon oxide, having a thickness of 3 to 5 μm;

[0026] The first dielectric film layer is used as an etch stop layer in the etching process in step 2-3). That is, after the etching process completely etches the second dielectric film layer, when the etching process reaches the first dielectric film layer, the etching process will automatically terminate because the etching process cannot etch the first dielectric film layer. At the same time, the first dielectric film layer is used as an ion implantation shielding layer during the aluminum ion implantation process in the epitaxial layer in step 2-5). The second dielectric film layer of a specific thickness is used to shield the implanted ions, thereby regulating the motion trajectory and distribution of the ions implanted into the epitaxial layer to form the desired first stepped region.

[0027] The second dielectric film layer will serve as an ion implantation barrier layer for blocking implanted ions and preventing the ions from being implanted into the epitaxial layer;

[0028] 2-2) coating a photoresist on the upper surface of the ion implantation mask layer, and patterning the photoresist using a photolithography process such as exposure, development, and hardening to form a patterned photoresist;

[0029] 2-3) etching the ion implantation mask layer using an etching process based on the patterned photoresist to form an ion implantation window: the etching process completely etches the second dielectric film layer in 2-1), and the etching process automatically stops at the surface of the first dielectric layer;

[0030] 2-4) removing the patterned photoresist and retaining the ion implantation mask layer after etching;

[0031] 2-5) performing a first aluminum ion implantation process on the epitaxial layer based on the etched ion implantation mask layer to form a vertical region of an inverted T-shaped electric field modulation region;

[0032] 2-6) depositing and growing a third dielectric film layer on the surface of the etched ion implantation mask layer: the dielectric film layer is silicon nitride, silicon oxide or polysilicon, and has a thickness of 0.2 to 1.0 μm;

[0033] 2-7) etching the third dielectric film layer formed in 2-6) using an etching process to form ion implantation windows in the lateral regions of the inverted T-shaped electric field modulation region;

[0034] 2-8) Based on the formed ion implantation window of the lateral region of the inverted T-shaped electric field modulation region, a second aluminum ion implantation process is performed on the epitaxial layer to form the lateral region of the inverted T-shaped electric field modulation region.

[0035] Furthermore, steps 2-6), 2-7, and 2-8) utilize a self-alignment process. After step 2-5), a further ion implantation mask layer is formed on the surface of the etched ion implantation mask layer to form lateral regions of the inverted-T electric field structure. The ion implantation mask layer in the lateral regions of the inverted-T electric field structure is then etched using an etching process to form ion implantation windows in the lateral regions of the inverted-T electric field structure. The self-alignment process effectively ensures symmetry in the left-right spacing of the inverted-T structure, while automatically adjusting the size of the lateral regions of the inverted-T structure by adjusting the thickness of the third dielectric film layer.

[0036] Furthermore, forming the gate dielectric layer in step 6) includes the following steps:

[0037] 6-1) Depositing a silicon oxide layer on the gate trench surface using a low-pressure chemical vapor deposition (LPCVD) process at a growth temperature of 600-800° C., a pressure of 200-500 mTorr, and tetraethoxysilane (TEOS) as a growth source;

[0038] 6-2) Annealing process of the silicon oxide layer: the annealing temperature is 1100-1300° C., the annealing time is 30-60 min, and the annealing atmosphere is a mixture of NO / Ar.

[0039] Furthermore, forming the gate dielectric layer in step 6) includes the following steps:

[0040] 6-1) Depositing an aluminum oxide layer on the gate trench surface using an atomic layer deposition (ALD) process. The growth source is trimethylaluminum (TMA). The ALD process can be a thermal process or a plasma process. The growth temperature of the thermal process is 200-400°C, and the plasma power of the plasma process is 150-300W.

[0041] 6-2) Annealing process of the aluminum oxide layer: the annealing temperature is 600-900°C, the annealing time is 10-30 minutes, and the annealing atmosphere is Ar or N2.

[0042] Furthermore, the annealing process for the silicon oxide layer or the aluminum oxide layer has two purposes: one is to improve the density of the oxide layer to improve the ability of the film layer to withstand voltage; the other is to optimize and modify the interface characteristics between the silicon oxide layer and the epitaxial layer to reduce the interface state density, interface defects, etc.

[0043] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: 1. The inverted T-shaped electric field modulation region effectively modulates the internal electric field of the device, eliminates the electric field concentration effect at the bottom corner of the trench, shields the electric field strength in the gate oxide, avoids gate oxide breakdown, thereby preventing the device from premature breakdown and burning, and improving device reliability; 2. While modulating the electric field, the inverted T-shaped electric field modulation region keeps it away from the device well region, thereby effectively alleviating the natural depletion effect between the electric field modulation structure and the well region, thereby preventing the deterioration of the device conduction performance; 3. The body diode region serves as the body diode structure inside the device, and transmits reverse current when the device is in the blocking state; 4. The device structure and preparation method are simple, and the improvement effect is significant, which can realize the high-performance, batch-scale preparation of trench SiCMOSFET devices, and has huge market potential and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a production flow chart of the present invention;

[0045] Figures 2 to 13 Schematic diagram of the device structure obtained in different steps of the manufacturing method of the present invention. DETAILED DESCRIPTION

[0046] The technical solution of the present invention will be further described below with reference to the accompanying drawings.

[0047] Example 1

[0048] like Figure 13A trench silicon carbide MOSFET device is shown, comprising a heavily doped substrate 101 of a first doping type, a buffer layer 102, a lightly doped epitaxial layer 103 of a first doping type, and a passivation layer 111 arranged sequentially from bottom to top; an inverted T-shaped electric field modulation region 104 of a second doping type is symmetrically arranged on the top of the epitaxial layer 103, a body diode region 105 of a second doping type is arranged on the top of the inverted T-shaped electric field modulation region 104, a well region 106 of a second doping type is arranged between the inverted T-shaped electric field modulation regions 104, and a source region 106 of a first doping type is arranged on the top of the well region 106. 07; A gate trench 108 is provided in the middle of the epitaxial layer 103, a gate dielectric layer 109 is provided in the trench, and polysilicon 110 of the first doping type fills the gate trench 108; source windows 112 are provided at both ends of the passivation layer 111, a source ohmic contact layer 113 is provided thereon, and a source electrode 116 is placed on the source ohmic contact layer 113; a gate window 114 is provided in the middle of the passivation layer 111 and above the polysilicon 110, and a gate electrode 115 is placed on the gate window 114; a drain ohmic contact layer 117 and a drain electrode 118 are provided in sequence from top to bottom at the bottom of the substrate 101. The first doping type is P-type, the second doping type is N-type, and the vertical region of the inverted T-shaped electric field modulation region 104 has a depth of 1um (set to 0.8-2.0um as required), a width of 0.5um (set to 0.3-1.0um as required), and a doping concentration of 1e19cm -3 (Set to 1e17~1e19cm according to requirements -3 ); the depth of the lateral region is 0.5 μm (can be set to 0.2 to 1.0 μm according to requirements), and the doping concentration is 1e18 cm -3 (Set to 1e17~1e19cm according to requirements -3 ), the distance between the boundary of the lateral region and the longitudinal region is 0.4um (set to 0.2-0.6um according to requirements). The depth of the body diode region 105 is 0.4um (set to 0.2-0.5um according to requirements), the width is 0.5um (set to 0.3-1.0um according to requirements), and the doping concentration is 1e18cm -3 (Set to 1e18~1e20cm according to requirements -3 ), the width of the body diode region 105 is smaller than the longitudinal width of the inverted T-shaped electric field modulation region 104. The gate dielectric layer 109 is a silicon oxide layer with a thickness of 30 μm.

[0049] The method for preparing the above-mentioned trench silicon carbide MOSFET device comprises the following steps:

[0050] 1) preparing a heavily doped substrate 101 of a first doping type, and growing a lightly doped epitaxial layer 103 of the first doping type on the upper surface thereof;

[0051] 2) forming an inverted T-shaped electric field modulation region 104 of a second doping type in the lightly doped epitaxial layer 103 of a first doping type, specifically comprising the following steps:

[0052] 2-1) Two ion implantation mask layers are formed on the surface of the epitaxial layer 103: the first dielectric film layer is silicon nitride or polysilicon, with a thickness of 1 μm (which can be set to 0.5-1.5 μm as required); the second dielectric film layer is silicon oxide, with a thickness of 4 μm (which can be set to 3-5 μm as required);

[0053] 2-2) coating a photoresist on the upper surface of the ion implantation mask layer, and patterning the photoresist using a photolithography process such as exposure, development, and hardening to form a patterned photoresist;

[0054] 2-3) etching the ion implantation mask layer using an etching process based on the patterned photoresist to form an ion implantation window: the etching process completely etches the second dielectric film layer in 2-1), and the etching process automatically stops at the surface of the first dielectric layer;

[0055] 2-4) removing the patterned photoresist and retaining the ion implantation mask layer after etching;

[0056] 2-5) performing a first aluminum ion implantation process on the epitaxial layer 103 based on the etched ion implantation mask layer to form a vertical region of the inverted T-shaped electric field modulation region 104;

[0057] 2-6) After completing step 2-5), a third dielectric film layer is deposited and grown on the surface of the etched ion implantation mask layer: the dielectric film layer is silicon nitride, silicon oxide, or polysilicon, and has a thickness of 0.5 μm (can be set to 0.2 to 1.0 μm according to requirements);

[0058] 2-7) etching the third dielectric film layer formed in 2-6) using an etching process to form ion implantation windows in the lateral regions of the inverted T-shaped electric field modulation region 104;

[0059] 2-8) Based on the formed ion implantation window of the lateral region of the inverted T-shaped electric field modulation region 104, a second aluminum ion implantation process is performed on the epitaxial layer 103 to form the lateral region of the inverted T-shaped electric field modulation region 104;

[0060] 3) forming a body diode region 105 of a second doping type in the inverted T-shaped electric field modulation region 104;

[0061] 4) forming a well region 106 of the second doping type in the lightly doped epitaxial layer 103 of the first doping type and between the inverted T-shaped electric field modulation regions 104 , and forming a source region 107 of the first doping type in the well region 106 of the second doping type;

[0062] 5) forming a gate trench 108 in the lightly doped epitaxial layer 103 of the first doping type;

[0063] 6) Forming a gate dielectric layer 109 on the inner surface of the gate trench 108, including the following steps:

[0064] 6-1) depositing a silicon oxide layer on the surface of the gate trench 108 using a low-pressure chemical vapor deposition process at a growth temperature of 600-800° C., a pressure of 200-500 mTorr, and tetraethoxysilane as a growth source;

[0065] 6-2) Annealing process of silicon oxide layer: annealing temperature is 1100-1300°C, annealing time is 30-60 minutes, and annealing atmosphere is a mixture of NO / Ar gas;

[0066] 7) Filling the gate trench 108 with polysilicon 110 of the first doping type;

[0067] 8) forming a passivation layer 111 on the upper surface of the lightly doped epitaxial layer 103 of the first doping type;

[0068] 9) Generating source windows 112 at both ends of the passivation layer 111 , forming a source ohmic contact layer 113 on the upper surface thereof, and forming a source electrode 116 on the surface of the source ohmic contact layer 113 ;

[0069] 10) A gate window 114 is formed in the middle of the passivation layer 111 and above the polysilicon 110 , and a gate electrode 115 is formed on the upper surface thereof;

[0070] 11) Thinning the bottom of the heavily doped substrate 101 of the first doping type;

[0071] 12) A drain ohmic contact layer 117 is formed on the bottom surface of the thinned substrate, and a drain electrode 118 is formed on the lower surface thereof.

[0072] Example 2

[0073] Different from Example 1, the first doping type of Example 2 is N-type and the second doping type is P-type; the width of the body diode region 105 is equal to the longitudinal width of the inverted T-type electric field modulation region 104, which is set to 1um; the gate dielectric layer 109 is an aluminum oxide layer with a thickness of 100nm.

[0074] In the preparation method, the gate dielectric layer 109 in step 6 includes the following steps:

[0075] 6-1) Depositing an aluminum oxide layer using a thermal atomic layer deposition process at a growth temperature of 200-400° C. using trimethylaluminum as a growth source;

[0076] 6-2) Annealing process of the aluminum oxide layer: the annealing temperature is 600-900°C, the annealing time is 10-30 minutes, and the annealing atmosphere is Ar or N2.

[0077] Example 3

[0078] The difference from Example 2 is that in the preparation method, the gate dielectric layer 109 in step 6 includes the following steps:

[0079] 6-1) Depositing an aluminum oxide layer using a plasma atomic layer deposition process, wherein the plasma power of the plasma process is 150 to 300 W and the growth source is trimethylaluminum;

[0080] 6-2) Annealing process of the aluminum oxide layer: the annealing temperature is 600-900°C, the annealing time is 10-30 minutes, and the annealing atmosphere is Ar or N2.

Claims

1. A trench silicon carbide MOSFET device, comprising a drain electrode (118), a drain ohmic contact layer (117), a heavily doped substrate (101) of a first doping type, a lightly doped epitaxial layer (103) of a first doping type, and a passivation layer (111) arranged in sequence from bottom to top; a well region (106) of a second doping type is arranged in the middle of the top of the epitaxial layer (103), a source region (107) of a first doping type is arranged on the top of the well region (106), and a well region (106) of a second doping type is arranged in the middle of the top of the epitaxial layer (103). A gate trench (108) is provided in the region (107), a gate dielectric layer (109) is provided in the trench, and polysilicon (110) of a first doping type fills the gate trench (108); source windows (112) are provided at both ends of the passivation layer (111), a source ohmic contact layer (113) is provided thereon, and a source electrode (116) is placed on the source ohmic contact layer (113); a gate window (114) is provided in the middle of the passivation layer (111) and above the polysilicon (110), and a gate electrode (115) is placed on the gate window (114); It is characterized in that An inverted T-shaped electric field modulation region (104) of a second doping type is symmetrically arranged at both ends of the well region (106) and the source region (107) in the epitaxial layer (103), and a body diode region (105) of a second doping type is arranged at the top of the inverted T-shaped electric field modulation region (104).

2. The trench silicon carbide MOSFET device according to claim 1, It is characterized in that A buffer layer (102) is provided between the substrate (101) and the epitaxial layer (103) for transition of doping concentration and preventing abnormal growth caused by concentration gradient changes.

3. The trench silicon carbide MOSFET device according to claim 1, It is characterized in that The doping type is N-type or P-type, and the first doping type and the second doping type are different doping types.

4. The trench silicon carbide MOSFET device according to claim 1, It is characterized in that The inverted T-shaped electric field modulation region (104) has a longitudinal region depth of 0.8 to 2.0 um, a width of 0.3 to 1.0 um, and a doping concentration of 1e17 to 1e19 cm -3 ; The depth of the lateral region is 0.2 to 1.0 μm, and the doping concentration is 1e17 to 1e19 cm -3 , the distance between the boundary of the transverse area and the longitudinal area is 0.2 to 0.6 um.

5. The trench silicon carbide MOSFET device according to claim 1, It is characterized in that The body diode region (105) has a depth of 0.2-0.5 um, a width of 0.3-1.0 um, and a doping concentration of 1e18-1e20 cm -3 ; The width of the body diode region (105) is less than or equal to the longitudinal width of the inverted T-type electric field modulation region (104).

6. The trench silicon carbide MOSFET device according to claim 1, It is characterized in that The gate dielectric layer (109) is a silicon oxide layer or an aluminum oxide layer, and has a thickness of 30 to 100 nm.

7. A method for preparing a trench silicon carbide MOSFET device, It is characterized in that The steps include: 1) preparing a heavily doped substrate (101) of a first doping type, and forming a lightly doped epitaxial layer (103) of the first doping type on its upper surface; 2) forming an inverted T-shaped electric field modulation region (104) of a second doping type in the epitaxial layer (103); 3) forming a body diode region (105) of a second doping type in the inverted T-shaped electric field modulation region (104); 4) forming a well region (106) of the second doping type in the epitaxial layer (103) and between the inverted T-shaped electric field modulation regions (104), and forming a source region (107) of the first doping type in the well region (106); 5) forming a gate trench (108) in the epitaxial layer (103); 6) forming a gate dielectric layer (109) on the inner surface of the gate trench (108); 7) Filling the gate trench (108) with polysilicon (110) of a first doping type; 8) forming a passivation layer (111) on the upper surface of the epitaxial layer (103); 9) generating source windows (112) at both ends of the passivation layer (111), generating a source ohmic contact layer (113) on the upper surface thereof, and forming a source electrode (116) on the surface of the source ohmic contact layer (113); 10) forming a gate window (114) in the middle of the passivation layer (111) and above the polysilicon (110), and forming a gate electrode (115) on the upper surface thereof; 11) Thinning the bottom of the substrate (101); 12) A drain ohmic contact layer (117) is formed on the bottom surface of the thinned substrate, and a drain electrode (118) is formed on the lower surface thereof.

8. The method for preparing a trench silicon carbide MOSFET device according to claim 7, It is characterized in that A buffer layer (102) is provided between the substrate (101) and the epitaxial layer (103) for transition of doping concentration and preventing abnormal growth caused by concentration gradient changes.

9. The method for preparing a trench silicon carbide MOSFET device according to claim 7, It is characterized in that The step 2) comprises the following steps: 2-1) forming an ion implantation mask layer on the surface of the epitaxial layer (103), the ion implantation mask layer being composed of two dielectric film layers: the first dielectric film layer being silicon nitride or polysilicon with a thickness of 0.5 to 1.5 um; and the second dielectric film layer being silicon oxide with a thickness of 3 to 5 um; 2-2) coating a photoresist on the upper surface of the ion implantation mask layer, and patterning the photoresist by using photolithography processes such as exposure, development and hardening to form a patterned photoresist; 2-3) etching the ion implantation mask layer using an etching process according to the patterned photoresist to form an ion implantation window: the etching process completely etches the second dielectric film layer in 2-1), and the etching process automatically stops on the surface of the first dielectric layer; 2-4) removing the patterned photoresist and retaining the ion implantation mask layer after etching; 2-5) performing a first aluminum ion implantation process on the epitaxial layer (103) based on the etched ion implantation mask layer to form a vertical region of an inverted T-shaped electric field modulation region (104); 2-6) After completing step 2-5), a third dielectric film layer is deposited and grown on the surface of the etched ion implantation mask layer: the dielectric film layer is silicon nitride, silicon oxide or polysilicon, and has a thickness of 0.2 to 1.0 um; 2-7) etching the third dielectric film layer formed in 2-6) by an etching process to form an ion implantation window in the lateral region of the inverted T-shaped electric field modulation region (104); 2-8) Based on the ion implantation window of the lateral region of the inverted T-type electric field modulation region (104) formed, a second aluminum ion implantation process is performed on the epitaxial layer (103) to form the lateral region of the inverted T-type electric field modulation region (104).

10. The method for preparing a trench silicon carbide MOSFET device according to claim 7, It is characterized in that The step 6) of forming the gate dielectric layer comprises the following steps: 6-1) depositing a silicon oxide layer on the surface of the gate trench (108) by using a low pressure chemical vapor deposition process, or depositing an aluminum oxide layer by using an atomic layer deposition process; 6-2) Annealing the silicon oxide layer or the aluminum oxide layer.