Groove type MOSFET device and preparation method thereof
By introducing L-shaped structure regions and current expansion regions into trench SiC MOSFET devices, the problem of premature breakdown and degradation of the device is solved, electric field modulation and carrier enhancement are achieved, and the reliability of the device is improved. and performance.
Patent Information
- Application Number
- CN202411076080.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-15
AI Technical Summary
The trench SiC MOSFET device is prone to premature breakdown due to the electric field aggregation effect at the bottom of the trench gate, and the structure of the electric field modulation region and the well region are naturally depleted, resulting in deterioration of conduction performance.
Using a combined design of the L-shaped structure area and the current expansion area, the internal electric field of the device is modulated through the L-shaped structure area, the electric field intensity of the gate trench bottom angle is reduced, and the carrier concentration is increased in the current expansion area to enhance the conduction performance.
It effectively avoids premature breakdown and degradation of the device's conductivity, improves the reliability and conductivity of the device, and simplifies the preparation process.
Smart Images

Figure CN118969848A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a semiconductor device, in particular to a trench MOSFET device and a preparation method thereof. Background Art
[0002] SiC MOSFET (Metal-Oxide-Semiconductor Field-Effect Transistor, MOSFET) devices have the advantages of high current density, high breakdown voltage, low loss, good high temperature characteristics and radiation resistance. Compared with traditional Si-based power MOSFET devices, they can simplify the topology of power electronic systems, reduce system volume and reduce power loss. Therefore, SiC MOSFET devices are very competitive in the fields of electric vehicles, photovoltaic inverters, rail transportation and aerospace. There are two types of SiCMOSFET device structures: flat gate type and trench type. Flat gate SiC MOSFET devices have a parasitic junction field effect transistor (Junction Field Electric Transistor, JFET) structure, which increases the device on-resistance and device power consumption. Trench SiC MOSFET uses a trench gate structure and does not have a JFET region. The device on-resistance can be significantly reduced, and the conductive channel is changed from horizontal to vertical, which effectively saves the device area and greatly improves the power density. It has obvious performance advantages and broad application prospects. However, due to the influence of the electric field concentration effect at the bottom corner of the trench gate, the trench SiC MOSFET is very likely to cause premature breakdown or even burnout of the device; in addition, the high electric field in the gate oxide at the bottom of the trench gate is very likely to cause gate oxide breakdown, which can easily lead to device failure. Therefore, how to modulate the electric field at the bottom of the trench gate of the trench SiC device and reduce the risk of gate oxide breakdown is a difficult and hot issue for trench SiC devices. Application No. ZL202110746585.1 discloses the use of a secondary epitaxial method to introduce an electric field modulation area structure into a trench SiC device to modulate the internal electric field of the device and eliminate the electric field concentration effect at the bottom of the trench. It can also reduce the electric field strength in the gate oxide at the bottom of the trench and avoid gate oxide breakdown, thereby preventing the device from breaking down and burning prematurely and improving device reliability. However, the electric field modulation area structure introduced is a columnar type, which causes the columnar structure to naturally deplete the original well area of the device, thereby deteriorating the device's conduction capability. Summary of the invention
[0003] Purpose of the invention: The purpose of the present invention is to provide a trench MOSFET device in order to avoid gate oxide breakdown of the device and improve the conduction performance at the same time; another purpose of the present invention is to provide a method for preparing the trench MOSFET device.
[0004] Technical solution: The trench MOSFET device described in the present invention comprises a drain electrode, a drain ohmic contact layer, a heavily doped substrate of a first doping type, a lightly doped first epitaxial layer of a first doping type, a lightly doped second epitaxial layer of a first doping type and a passivation layer, which are arranged in sequence from bottom to top; a well region of a second doping type is arranged in the second epitaxial layer, a group of contact regions of a second doping type are symmetrically arranged on the top of the well region of the second doping type, and a source region of a first doping type is arranged between the two groups of contact regions of the second doping type; a gate trench is arranged between the first epitaxial layer and the second epitaxial layer, penetrating the second epitaxial layer, a gate dielectric layer is arranged in the trench, and a polysilicon layer of a first doping type is filled in the gate trench; source windows are arranged at both ends of the passivation layer, a source ohmic contact layer is arranged on the surface of the source window, and a source electrode is arranged on the source ohmic contact layer; a gate window is arranged in the middle of the passivation layer and above the polysilicon layer, and the gate electrode is arranged in the gate window; a group of L-shaped structural regions of a second doping type are symmetrically arranged on the top of the first epitaxial layer, and a current extension region of a first doping type is arranged between the two L-shaped structural regions.
[0005] Furthermore, a buffer layer is provided between the substrate and the first epitaxial layer for transition of doping concentration and prevention of abnormal growth due to concentration gradient change.
[0006] Furthermore, the vertical region of the L-shaped structure region has a depth of 0.8 to 2.0 um, a width of 0.3 to 1.0 um, and a doping concentration of 1e17 to 1e19 cm -3 The spacing between the vertical region and the gate trench is 0.2 to 1.0 um; the depth of the lateral region is 0.2 to 1.0 um, and the doping concentration is 1e17 to 1e19 cm -3 , the distance between the boundary of the lateral region and the vertical region is 0.2 to 0.6um. In the L-shaped structural region, when the device is in the blocked state, the maximum electric field peak can be pulled from the bottom corner of the trench to the bottom of the L-shaped structural region, thereby reducing the electric field concentration effect at the bottom corner of the gate trench, playing a role in modulating the internal electric field of the device; in addition, the electric field strength at the bottom corner of the gate trench is reduced, which further promotes the reduction of the electric field strength in the gate oxide at the bottom of the gate trench, thereby avoiding gate oxide breakdown. More importantly, due to the use of the L-shaped structure electric field modulation region, while meeting the purpose of modulating the electric field, the vertical region can be made narrower, thereby ensuring that the electric field modulation region is far away from the device well region, so that the natural depletion effect between the electric field modulation region and the well region can be effectively alleviated, avoiding the deterioration of the device conduction performance.
[0007] Furthermore, the distance between the upper boundary of the current extension region and the lower boundary of the well region is 0-0.5 um, the depth of the current extension region is 0.2-0.6 um, and the doping concentration is 1e16-1e17 cm -3, the lower boundary of the current extension region can be deeper or shallower than the depth of the gate trench. The doping concentration of the current extension region is higher than that of the first epitaxial layer, which can provide more carriers for transmitting current when the device is turned on, thereby achieving the purpose of increasing the device current; at the same time, the current extension region is located between the well region and the L-shaped structure region, which can further weaken the natural depletion effect between the two, thereby also achieving the purpose of increasing the device current and enhancing the device conduction performance.
[0008] Furthermore, the width of the gate trench is 0.5-2.0um, and the aspect ratio of the depth to the width is 0.8-2um; the bottom corner of the gate trench is in an arc shape, and the curvature radius of the arc shape is 0.1-0.5um. The arc shape at the bottom corner of the gate trench can help alleviate the electric field concentration effect at the bottom of the trench, and can further reduce the electric field strength at the bottom of the trench.
[0009] Furthermore, the doping type is N-type or P-type, the first doping type is N-type and the second doping type is P-type, or the first doping type is P-type and the second doping type is N-type.
[0010] The method for preparing the trench MOSFET device of the present invention comprises the following steps:
[0011] 1) preparing a heavily doped substrate of a first doping type, and growing a lightly doped first epitaxial layer of the first doping type on the upper surface of the substrate;
[0012] 2) forming an L-shaped structure region of the second doping type and a current extension region of the first doping type in the first epitaxial layer;
[0013] 3) forming a lightly doped second epitaxial layer of the first doping type on the upper surface of the first epitaxial layer;
[0014] 4) forming a well region of the second doping type in the second epitaxial layer, and forming a contact region of the second doping type and a source region of the first doping type in the well region;
[0015] 5) a gate trench is formed between the first epitaxial layer and the second epitaxial layer, a gate dielectric layer is disposed in the trench, and then a polysilicon layer of a first doping type is filled in the gate trench;
[0016] 6) forming a passivation layer on the surface of the second epitaxial layer;
[0017] 7) forming source windows at both ends of the passivation layer, forming a source ohmic contact layer therein, and forming a source electrode on the surface of the source ohmic contact layer;
[0018] 8) forming a gate window in the middle of the passivation layer and above the polysilicon layer, and forming a gate electrode in the gate window;
[0019] 9) Thinning the bottom of the substrate;
[0020] 10) After thinning, a drain ohmic contact layer and a drain electrode are formed on the bottom surface of the substrate.
[0021] Furthermore, a buffer layer is provided between the substrate and the first epitaxial layer for transition of doping concentration and prevention of abnormal growth due to concentration gradient change.
[0022] Further, the step 2) comprises the following steps:
[0023] 2-1) forming three ion implantation mask layers on the surface of the first epitaxial layer, wherein the first dielectric film layer is silicon oxide or silicon nitride with a thickness of 0.2 to 1.0 um, the second dielectric film layer is polysilicon with a thickness of 1.5 to 3 um, and the third dielectric film layer is silicon oxide or silicon nitride with a thickness of 0.2 to 1.0 um;
[0024] The first dielectric film layer in step 2-1) has two functions: first, it serves as an etching stop layer for the etching process in step 2-5): that is, after the etching process etches the second dielectric film layer cleanly, when etching to the first dielectric film layer, the etching process will automatically terminate because the etching process cannot etch the first dielectric film layer; second, it serves as an ion implantation shielding layer for the aluminum ion implantation process in steps 2-8) and 2-9), that is, the first dielectric film layer of a specific thickness is used to shield the implanted ions, thereby regulating the movement trajectory and distribution of the ions implanted into the epitaxial layer to form the required L-shaped structural area; the second dielectric film layer serves as an ion implantation blocking layer for blocking the implanted ions to prevent the ions from being implanted into the epitaxial layer; the third dielectric film layer serves as an etching mask layer for the second dielectric film layer, and after etching the third dielectric film layer according to the patterned photoresist, an etching window for etching the second dielectric film layer can be formed, and the second dielectric film layer is subsequently etched according to the etching window;
[0025] 2-2) coating a photoresist on the upper surface of the mask layer, and patterning the photoresist by using photolithography processes such as exposure, development and hardening to form a patterned photoresist;
[0026] 2-3) etching the third dielectric film layer of the ion implantation mask layer using an etching process according to the patterned photoresist to form an etching window for etching the second dielectric film layer;
[0027] 2-4) removing the patterned photoresist;
[0028] 2-5) etching the second dielectric film layer using an etching process according to the etching window formed in step 2-3) to form an ion implantation window;
[0029] 2-6) According to the ion implantation window formed in step 2-5), aluminum ions are implanted into the first epitaxial layer for the first time to form a vertical region of the L-shaped structure region;
[0030] 2-7) depositing and growing a fourth dielectric film layer on the surface of the etched ion implantation mask layer, the dielectric film layer being silicon nitride, silicon oxide or polysilicon with a thickness of 0.2 to 1.0 um;
[0031] 2-8) The fourth dielectric film layer is etched by an etching process to form an ion implantation window in the lateral region of the L-shaped structure area; the fourth dielectric film layer is used to form an ion implantation mask layer for ion implantation in the lateral region of the L-shaped structure area; steps 2-7) and 2-8) use a self-alignment process, and after completing step 2-6), another ion implantation mask layer for forming the lateral region of the L-shaped structure area is formed on the surface of the etched ion implantation mask layer; the ion implantation mask layer in the lateral region of the L-shaped structure area is etched by an etching process to form an ion implantation window in the lateral region of the L-shaped structure area, and the self-alignment process can automatically ensure that the spacing between the lateral region of the L-shaped structure area and the vertical region of the L-shaped structure area is consistent, thereby avoiding the problem of dimensional overlay deviation caused by the photolithography process. In addition, the spacing between the vertical region and the lateral region of the L-shaped structure area can be automatically adjusted by adjusting the thickness of the ion implantation mask layer used to form the lateral region of the L-shaped structure area;
[0032] 2-9) According to the ion implantation window of the lateral region of the formed L-shaped structure region, the first epitaxial layer is implanted with aluminum ions for a second time to form the lateral region of the L-shaped structure region;
[0033] 2-10) forming two layers of ion implantation mask layers of the current extension region on the surface of the first epitaxial layer formed in step 2-9): the first dielectric film layer is silicon oxide with a thickness of 0.2 to 1.0 um, and the second dielectric film layer is polysilicon with a thickness of 1.0 to 2.0 um; the first dielectric film layer is used as an etching stop layer in the etching process in step 2-12), and the second dielectric film layer is used as an etching layer in the etching process in step 2-12). Because the etching process used has a higher etching selectivity ratio between the first dielectric film layer and the second dielectric film layer, the etching process can etch the first dielectric film layer, but cannot etch the second dielectric film layer, thereby achieving the purpose of automatically stopping the etching process at the second dielectric film layer;
[0034] 2-11) coating a photoresist on the upper surface of the ion implantation mask layer, and patterning the photoresist by using photolithography processes such as exposure, development and hardening to form a patterned photoresist;
[0035] 2-12) etching the ion implantation mask layer using an etching process according to the patterned photoresist to form an ion implantation window, the second dielectric film layer is completely etched, and the etching process automatically stops at the surface of the first dielectric film layer;
[0036] 2-13) removing the patterned photoresist and retaining the ion implantation mask layer after etching;
[0037] 2-14) Based on the etched ion implantation mask layer, nitrogen ions are implanted into the first doping type lightly doped first epitaxial layer to form a current extension region.
[0038] Furthermore, the forming of the gate dielectric layer in step 5) comprises the following steps:
[0039] 5-1) A silicon oxide layer with a thickness of 10 to 20 nm is grown on the surface of the gate trench by a dry or wet thermal oxidation process (TO);
[0040] 5-2) Annealing the silicon oxide layer in a gas atmosphere of NO or N 2 A mixed gas of O and Ar, the gas flow rate is 100-200 sccm, the annealing temperature is 1100-1400°C, and the annealing time is 60-120 min;
[0041] 5-3) After annealing, an atomic layer deposition (ALD) process is used to grow another silicon oxide layer, aluminum oxide layer or hafnium oxide layer on the surface of the silicon oxide layer formed by the thermal oxidation process, and the thickness of the oxide layer is 40 to 80 nm; the ALD process can be a thermal growth ALD process with a growth temperature of 300 to 500° C., or a plasma enhanced growth ALD process with a plasma driving power of 150 to 350 W; the growth source for growing the silicon oxide layer is bis(diethylamino)silane (Bis(diethylamino)silane, BDEAS), the growth source for growing aluminum oxide is trimethylaluminum (Trimethylaluminium, TMA), and the growth source for growing hafnium oxide is tetrakis(diMethylaMino)hafnium (Tetrakis(diMethylaMino)hafnium, TDMAH);
[0042] The oxide layer grown by the ALD process is a silicon oxide layer, that is, a conventional gate dielectric layer; the grown aluminum oxide layer or hafnium oxide layer is a high dielectric constant (high κ) film layer, that is, using a high κ film layer as a gate dielectric film layer can reduce the electric field strength inside the gate dielectric layer of the device in the blocking state compared to a conventional silicon oxide layer, thereby improving the breakdown strength and reliability of the gate dielectric layer;
[0043] 5-4) Annealing the oxide layer formed in step 5-3) to form a gate dielectric layer (111), wherein the gas atmosphere is an inert gas Ar or N 2 , the gas flow rate is 50-100 sccm, the annealing temperature is 600-900°C, and the annealing time is 10-30 min; on the one hand, the density of the silicon oxide layer, aluminum oxide layer, or hafnium oxide layer formed by the ALD process can be improved, and on the other hand, the stress inside the silicon oxide layer, aluminum oxide layer, or hafnium oxide layer formed by the ALD process can be eliminated, thereby improving the stability and reliability of the device.
[0044] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: 1. The L-type structure can effectively modulate the internal electric field of the device, eliminate the electric field concentration effect at the bottom corner of the groove, shield the electric field strength in the gate oxide, avoid gate oxide breakdown, thereby preventing the device from being broken down and burned prematurely and improving the reliability of the device; 2. Under the premise of playing the role of electric field modulation, the L-type structure maintains a farther distance from the device well region, thereby effectively alleviating the natural depletion effect of the columnar structure and the well region, thereby preventing the device from deteriorating in conduction performance; 3. A new current extension region is added, and its doping concentration is higher than that of the first epitaxial layer, which can provide more carriers for transmitting current when the device is turned on, thereby improving the conduction performance of the device; 4. The current extension region is located between the well region and the L-type structure region, further weakening the natural depletion effect between the two, thereby also achieving the purpose of increasing the device current and enhancing the conduction performance of the device; 5. The structure and preparation method are simple and the effect is significant, and the preparation of high-performance, batch trench SiC MOSFET devices can be realized, which has huge market potential and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is a flow chart of the preparation method of the present invention;
[0046] Figures 2 to 15 Schematic diagram of the device structure obtained in different steps of the manufacturing method of the present invention. DETAILED DESCRIPTION
[0047] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0048] Example 1
[0049] like Fig.15A trench MOSFET device is shown, comprising a substrate 101 heavily doped with a first doping type, a buffer layer 102, a first epitaxial layer 103 lightly doped with a first doping type, a second epitaxial layer 106 lightly doped with a first doping type, and a passivation layer 113 arranged from bottom to top; a group of L-shaped structural regions 104 of a second doping type are symmetrically arranged on the top of the first epitaxial layer 103, and a current extension region 105 of a first doping type is arranged between the two L-shaped structural regions 104; a well region 107 of a second doping type is arranged in the second epitaxial layer 106, a group of contact regions 108 of a second doping type are symmetrically arranged on the top of the well region 107 of the second doping type, and a current extension region 105 of a first doping type is arranged between the two groups of contact regions 108 of the second doping type. A source region 109 of a first doping type is disposed; a gate trench 110 is disposed between the first epitaxial layer 103 and the second epitaxial layer 106 and penetrates the second epitaxial layer 106, a gate dielectric layer 111 is disposed in the trench, and a polysilicon layer 112 of a first doping type is filled in the gate trench 110; source windows 114 are disposed at both ends of the passivation layer 113, a source ohmic contact layer 115 is disposed on the surface of the source window 114, and a source electrode 118 is disposed on the source ohmic contact layer 115; a gate window 116 is formed in the middle of the passivation layer 113 and above the polysilicon layer 112, and a gate electrode 117 is disposed on the gate window 116; a drain ohmic contact layer 119 and a drain electrode 120 are disposed in sequence from top to bottom at the bottom of the substrate 101. The vertical region of the L-shaped structure region 104 has a depth of 1 um (can be set to 0.8-2.0 um according to requirements), a width of 0.5 um (can be set to 0.3-1.0 um according to requirements), and a doping concentration of 1e18 cm -3 (It can be set to 1e17~1e19cm according to needs -3 ), the spacing between the vertical region and the gate trench 110 is 0.5um (can be set to 0.2-1.0um according to requirements); the depth of the lateral region is 0.5um (can be set to 0.2-1.0um according to requirements), the spacing between the boundary of the lateral region and the vertical region is 0.4um (can be set to 0.2-0.6um according to requirements), and the doping concentration is 1e18cm -3 (It can be set to 1e17~1e19cm according to needs -3 The distance between the upper boundary of the first doping type current extension region 105 and the lower boundary of the second doping type well region 107 is 0.3um (can be set to 0-0.5um according to requirements), the depth of the current extension region 105 is 0.4um (can be set to 0.2-0.6um according to requirements), and the doping concentration is 1e16cm -3 (It can be set to 1e16~1e17cm according to requirements -3). The width of the gate trench 110 is 1um (can be set to 0.5-2.0um according to requirements), and the aspect ratio of the depth to the width is 1 (can be set to 0.8-2 according to requirements); the bottom corner of the gate trench 110 is arc-shaped, and the curvature radius of the arc is 0.3um (can be set to 0.1-0.5um according to requirements). The first doping type is N-type and the second doping type is P-type.
[0050] like Figure 2-Figure 15 As shown, the method for preparing the above trench MOSFET device comprises the following steps:
[0051] 1) preparing a heavily doped substrate 101 of a first doping type, and forming a buffer layer 102 and a lightly doped first epitaxial layer 103 of the first doping type on the upper surface thereof;
[0052] 2) forming an L-shaped structure region 104 of a second doping type and a current extension region 105 of a first doping type in the first epitaxial layer 103, specifically comprising:
[0053] 2-1) forming three ion implantation mask layers on the surface of the first epitaxial layer 103, wherein the first dielectric film layer is silicon oxide or silicon nitride, and has a thickness of 0.5 um (can be set to 0.2-1.0 um as required) and serves as an etching stop layer for the etching process in step 2-5) and an ion implantation shielding layer for the aluminum ion implantation process in steps 2-8) and 2-9); the second dielectric film layer is polysilicon, and has a thickness of 2 um (can be set to 1.5-3 um as required) and serves as an ion implantation blocking layer; the third dielectric film layer is silicon oxide or silicon nitride, and has a thickness of 0.6 um (can be set to 0.2-1.0 um as required) and serves as an etching mask layer for the second dielectric film layer;
[0054] 2-2) coating a photoresist on the upper surface of the mask layer, and performing patterning by a photolithography process to form a patterned photoresist;
[0055] 2-3) etching the third dielectric film layer of the ion implantation mask layer using an etching process according to the patterned photoresist to form an etching window for etching the second dielectric film layer;
[0056] 2-4) removing the patterned photoresist;
[0057] 2-5) etching the second dielectric film layer using an etching process according to the etching window formed in step 2-3) to form an ion implantation window;
[0058] 2-6) According to the ion implantation window formed in step 2-5), aluminum ions are implanted into the first epitaxial layer 103 for the first time to form a vertical region of the L-shaped structure region;
[0059] 2-7) depositing and growing a fourth dielectric film layer on the surface of the etched ion implantation mask layer, the dielectric film layer being silicon nitride, silicon oxide or polysilicon, with a thickness of 0.8 um (which can be set to 0.2-1.0 um according to requirements), and being used to form an ion implantation mask layer for ion implantation in the lateral region of the L-shaped structure region;
[0060] 2-8) etching the fourth dielectric film layer using an etching process to form an ion implantation window in a lateral region of the L-shaped structure region;
[0061] 2-9) Based on the ion implantation window of the lateral region of the formed L-shaped structure region, the first epitaxial layer 103 is implanted with aluminum ions for a second time to form the lateral region of the L-shaped structure region;
[0062] 2-10) forming two layers of ion implantation mask layers of the current extension region on the surface of the first epitaxial layer 103 formed in step 2-9): the first dielectric film layer is silicon oxide with a thickness of 0.3 um (can be set to 0.2-1.0 um as required), serving as an etching stop layer of the etching process in step 2-12); the second dielectric film layer is polysilicon with a thickness of 1.5 um (can be set to 1.0-2.0 um as required), serving as an etching layer of the etching process in step 2-12);
[0063] 2-11) coating a photoresist on the upper surface of the ion implantation mask layer, and performing patterning by a photolithography process to form a patterned photoresist;
[0064] 2-12) etching the ion implantation mask layer using an etching process according to the patterned photoresist to form an ion implantation window;
[0065] 2-13) removing the patterned photoresist and retaining the ion implantation mask layer after etching;
[0066] 2-14) Based on the etched ion implantation mask layer, nitrogen ions are implanted into the first epitaxial layer 103 to form a current extension region;
[0067] 3) forming a lightly doped second epitaxial layer 106 of the first doping type on the upper surface of the first epitaxial layer 103;
[0068] 4) forming a well region 107 of the second doping type in the second epitaxial layer 106, and forming a contact region 108 of the second doping type and a source region 109 of the first doping type in the well region 107;
[0069] 5) A gate trench 110 is opened between the first epitaxial layer 103 and the second epitaxial layer 106, a gate dielectric layer 111 is disposed in the trench, and then a polysilicon layer 112 of a first doping type is filled in the gate trench 110, wherein the gate dielectric layer 111 is formed by the following steps:
[0070] 5-1) A silicon oxide layer is grown on the surface of the gate trench 110 by dry oxidation process, with a thickness of 15 um (which can be set to 10-20 nm according to requirements);
[0071] 5-2) Annealing the silicon oxide layer in a gas atmosphere of NO or N 2 A mixed gas of O and Ar, the gas flow rate is 100-200 sccm, the annealing temperature is 1100-1400°C, and the annealing time is 60-120 min;
[0072] 5-3) After annealing, a silicon oxide layer is grown on the surface of the silicon oxide layer formed by the thermal oxidation process by using a thermal growth atomic layer deposition process at a growth temperature of 300 to 500° C. using bis(diethylamino)silane, and the thickness of the oxide layer is 40 to 80 nm;
[0073] 5-4) Annealing the oxide layer formed in step 5-3) to form a gate dielectric layer 111, the gas atmosphere is an inert gas Ar or N 2 , gas flow rate is 50-100 sccm, annealing temperature is 600-900°C, and annealing time is 10-30 min;
[0074] 6) forming a passivation layer 113 on the surface of the second epitaxial layer 106;
[0075] 7) forming source windows 114 at both ends of the passivation layer 113, forming a source ohmic contact layer 115 therein, and forming a source electrode 118 on the surface of the source ohmic contact layer 115;
[0076] 8) A gate window 116 is formed above the middle polysilicon layer 112 of the passivation layer 113, and a gate electrode 117 is formed in the gate window 116;
[0077] 9) Thinning the bottom of the substrate 101;
[0078] 10) After thinning, a drain ohmic contact layer 119 and a drain electrode 120 are formed on the bottom surface of the substrate 101 .
[0079] Example 2
[0080] The difference from Embodiment 1 is that the first doping type is P type and the second doping type is N type.
[0081] In the preparation method, the gate dielectric layer 111 is formed in step 5) including the following steps:
[0082] 5-1) A silicon oxide layer with a thickness of 10 to 20 nm is grown on the surface of the gate trench 110 by a wet thermal oxidation process;
[0083] 5-2) Annealing the silicon oxide layer in a gas atmosphere of NO or N 2 A mixed gas of O and Ar, the gas flow rate is 100-200 sccm, the annealing temperature is 1100-1400°C, and the annealing time is 60-120 min;
[0084] 5-3) After annealing, a plasma enhanced atomic layer deposition process is used on the surface of the silicon oxide layer formed by the thermal oxidation process, and the plasma driving power is 150 to 350 W, and then a layer of aluminum oxide layer is grown using trimethylaluminum, and the thickness of the oxide layer is 40 to 80 nm;
[0085] 5-4) Annealing the oxide layer formed in step 5-3) to form a gate dielectric layer 111, the gas atmosphere is an inert gas Ar or N 2 , gas flow rate is 50-100 sccm, annealing temperature is 600-900°C, and annealing time is 10-30 min;
[0086] Example 3
[0087] Different from Example 2, in the preparation method, after annealing in step 5-3), a plasma-enhanced atomic layer deposition process is used on the surface of the silicon oxide layer formed by the thermal oxidation process, and the plasma driving power is 150 to 350 W. Then, a layer of hafnium oxide is grown using tetrakis(diethylamino)hafnium, and the thickness of the oxide layer is 40 to 80 nm.
Claims
1. A trench MOSFET device, comprising, arranged in sequence from bottom to top, a drain electrode (120), a drain ohmic contact layer (119), a heavily doped substrate (101) of a first doping type, a lightly doped first epitaxial layer (103) of the first doping type, a lightly doped second epitaxial layer (106) of the first doping type, and a passivation layer (113); a well region (107) of a second doping type is arranged in the second epitaxial layer (106); a group of contact regions (108) of a second doping type are symmetrically arranged on the top of the well region (107) of the second doping type; a source region (109) of a first doping type is arranged between the two groups of contact regions (108) of the second doping type; and A gate trench (110) is provided between the first epitaxial layer (103) and the second epitaxial layer (106), penetrating the second epitaxial layer (106); a gate dielectric layer (111) is provided in the trench; a polysilicon layer (112) of a first doping type is filled in the gate trench (110); source windows (114) are provided at both ends of the passivation layer (113); a source ohmic contact layer (115) is provided on the surface of the source window (114); a source electrode (118) is provided on the source ohmic contact layer (115); a gate window (116) is provided in the middle of the passivation layer (113) and above the polysilicon layer (112); and a gate electrode (117) is provided in the gate window (116); It is characterized in that A group of L-shaped structural regions (104) of the second doping type are symmetrically arranged on the top of the first epitaxial layer (103), and a current extension region (105) of the first doping type is arranged between two L-shaped structural regions (104).
2. The trench MOSFET device according to claim 1, It is characterized in that A buffer layer (102) is provided between the substrate (101) and the first epitaxial layer (103) for transition of doping concentration and preventing abnormal growth caused by concentration gradient changes.
3. The trench MOSFET device according to claim 1, It is characterized in that The vertical region in the L-shaped structural region (104) has a depth of 0.8 to 2.0 um, a width of 0.3 to 1.0 um, and a doping concentration of 1e17 to 1e19 cm -3 The distance between the vertical region and the gate trench (110) is 0.2 to 1.0 um; the depth of the lateral region is 0.2 to 1.0 um, and the doping concentration is 1e17 to 1e19 cm -3 , the distance between the boundary of the horizontal area and the vertical area is 0.2~0.6um.
4. The trench MOSFET device according to claim 1, It is characterized in that The distance between the upper boundary of the current extension region (105) and the lower boundary of the well region (107) is 0-0.5 um, the depth of the current extension region (105) is 0.2-0.6 um, and the doping concentration is 1e16-1e17 cm -3 .
5. The trench MOSFET device according to claim 1, It is characterized in that The width of the gate trench (110) is 0.5-2.0 um, and the aspect ratio of the depth to the width is 0.8-2 um; the bottom corner of the gate trench (110) is in an arc shape, and the curvature radius of the arc shape is 0.1-0.5 um.
6. The trench MOSFET device according to claim 1, It is characterized in that The doping type is N-type or P-type, and the first doping type and the second doping type are different doping types.
7. A method for preparing a trench MOSFET device, It is characterized in that The steps include: 1) preparing a heavily doped substrate (101) of a first doping type, and forming a lightly doped first epitaxial layer (103) of the first doping type on its upper surface; 2) forming an L-shaped structure region (104) of the second doping type and a current extension region (105) of the first doping type in the first epitaxial layer (103); 3) forming a lightly doped second epitaxial layer (106) of a first doping type on the upper surface of the first epitaxial layer (103); 4) forming a well region (107) of the second doping type in the second epitaxial layer (106), and forming a contact region (108) of the second doping type and a source region (109) of the first doping type in the well region (107); 5) a gate trench (110) is opened between the first epitaxial layer (103) and the second epitaxial layer (106), a gate dielectric layer (111) is disposed in the trench, and then a polysilicon layer (112) of a first doping type is filled in the gate trench (110); 6) forming a passivation layer (113) on the surface of the second epitaxial layer (106); 7) forming source windows (114) at both ends of the passivation layer (113), forming a source ohmic contact layer (115) therein, and forming a source electrode (118) on the surface of the source ohmic contact layer (115); 8) forming a gate window (116) above the middle polysilicon layer (112) of the passivation layer (113), and forming a gate electrode (117) in the gate window (116); 9) Thinning the bottom of the substrate (101); 10) After thinning, a drain ohmic contact layer (119) and a drain electrode (120) are formed on the bottom surface of the substrate (101).
8. The method for preparing a trench MOSFET device according to claim 7, It is characterized in that A buffer layer (102) is provided between the substrate (101) and the first epitaxial layer (103) for transition of doping concentration and preventing abnormal growth caused by concentration gradient changes.
9. The method for preparing a trench MOSFET device according to claim 7, It is characterized in that The step 2) comprises the following steps: 2-1) forming three ion implantation mask layers on the surface of the first epitaxial layer (103), wherein the first dielectric film layer is silicon oxide or silicon nitride with a thickness of 0.2 to 1.0 um, the second dielectric film layer is polysilicon with a thickness of 1.5 to 3 um, and the third dielectric film layer is silicon oxide or silicon nitride with a thickness of 0.2 to 1.0 um; 2-2) coating a photoresist on the upper surface of the mask layer, and performing patterning by a photolithography process to form a patterned photoresist; 2-3) etching the third dielectric film layer of the ion implantation mask layer using an etching process according to the patterned photoresist to form an etching window for etching the second dielectric film layer; 2-4) removing the patterned photoresist; 2-5) etching the second dielectric film layer using an etching process according to the etching window formed in step 2-3) to form an ion implantation window; 2-6) According to the ion implantation window formed in step 2-5), aluminum ions are implanted into the first epitaxial layer (103) for the first time to form a vertical region of the L-shaped structure region; 2-7) depositing and growing a fourth dielectric film layer on the surface of the etched ion implantation mask layer, the dielectric film layer being silicon nitride, silicon oxide or polysilicon with a thickness of 0.2 to 1.0 um; 2-8) etching the fourth dielectric film layer using an etching process to form an ion implantation window in the lateral region of the L-shaped structure region; 2-9) Based on the ion implantation window in the lateral region of the L-shaped structure region, the first epitaxial layer (103) is implanted with aluminum ions for a second time to form the lateral region of the L-shaped structure region; 2-10) forming two ion implantation mask layers of the first doping type current extension region on the surface of the first epitaxial layer (103) formed in step 2-9): the first dielectric film layer is silicon oxide with a thickness of 0.2 to 1.0 um, and the second dielectric film layer is polysilicon with a thickness of 1.0 to 2.0 um; 2-11) coating a photoresist on the upper surface of the ion implantation mask layer, and performing patterning by a photolithography process to form a patterned photoresist; 2-12) etching the ion implantation mask layer using an etching process according to the patterned photoresist to form an ion implantation window; 2-13) removing the patterned photoresist and retaining the ion implantation mask layer after etching; 2-14) Based on the etched ion implantation mask layer, nitrogen ions are implanted into the first epitaxial layer (103) to form a current expansion region.
10. The method for preparing a trench MOSFET device according to claim 7, It is characterized in that The step 5) of forming the gate dielectric layer comprises the following steps: 5-1) growing a silicon oxide layer with a thickness of 10 to 20 nm on the surface of the gate trench (110) by using a dry or wet thermal oxidation process; 5-2) annealing the silicon oxide layer; 5-3) After annealing, a silicon oxide layer, an aluminum oxide layer or a hafnium oxide layer is grown on the surface of the silicon oxide layer formed by the thermal oxidation process by an atomic layer deposition process, wherein the thickness of the oxide layer is 40 to 80 nm; 5-4) Annealing the oxide layer formed in step 5-3) to form a gate dielectric layer (111).
Citation Information
Patent Citations
SiC MOSFET device and preparation method thereof
CN113571584A