Positive electrode material and preparation method thereof, positive plate and lithium ion battery
By loading nanoparticles into lithium iron phosphate cathode materials and forming a three-dimensional conductive network, the problems of insufficient conductivity and transmission rate of traditional materials are solved, and lithium-ion batteries with high rate performance and long life are realized.
Patent Information
- Application Number
- CN202410894793.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional lithium iron phosphate cathode materials have poor conductivity and lithium-ion transport rate, making it difficult to meet the requirements of high rate and long cycle life in new power batteries and power systems.
LiFePO4 nanoparticles are uniformly loaded onto the surface of flower-shaped carbon. The flower-shaped carbon provides a fast electron transport channel and is embedded into the flower-shaped carbon structure through CO-Fe chemical bonding to form a three-dimensional conductive network. This controls the particle distribution to prevent aggregation.
It significantly improves electron transport capability and lithium-ion transport rate, enhances battery rate performance and electrode energy density, and ensures high material utilization and stability.
Smart Images

Figure HDA0004928602260000011 
Figure HDA0004928602260000012 
Figure HDA0004928602260000013
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a positive electrode material and a preparation method thereof, a positive electrode sheet and a lithium ion battery. Background Art
[0002] Lithium-ion batteries (LIBs) have been widely used in portable electronic devices, electric vehicles (EVs), smart grids and other fields. Lithium iron phosphate, as a cathode material with the advantages of good high-temperature stability, wide operating temperature range, environmental friendliness, low cost and high safety, has been widely used in new power batteries and power systems. At present, the "fast charging anxiety" of electric vehicles and the "high power" working conditions of energy storage have put forward higher requirements on the charging speed of LIBs systems. However, due to its poor intrinsic conductivity and slow lithium ion transfer rate, traditional lithium iron phosphate cathode materials cannot meet the requirements of high rate and long cycle life in new power batteries and power systems. Therefore, the modification of lithium iron phosphate cathode materials has become a research hotspot.
[0003] A Chinese patent (CN114715870A) discloses a method for preparing a porous carbon layer coated lithium iron phosphate material, wherein an Fe-MOFs nanomaterial containing an ionic liquid is used as an iron source and a carbon source, and the Fe-MOFs nanomaterial containing an ionic liquid is mixed with a phosphorus source and a lithium source, and then solid-phase sintered in an inert atmosphere to obtain a porous carbon layer coated lithium iron phosphate material. However, the porous carbon as a coating layer has limited performance improvement on lithium iron phosphate. A Chinese patent (CN112397698A) discloses a composite conductive agent coated lithium iron phosphate material and a preparation method thereof, wherein an anion exchange resin is used to adsorb potassium ferrate, and then porous carbon / iron oxide is prepared by wrapping and sintering with activated carbon, a portion of the carbon source is added to the iron source in advance, and a liquid phase mixing method is adopted to prepare a lithium iron phosphate precursor, and a polymer conductive compound polyaniline is added at the same time. The preparation process is relatively complicated, and polyaniline is not easy to be evenly dispersed in the composite material, and it is difficult to form a complete and effective three-dimensional conductive network structure, and the cycle performance is poor at high rates.
[0004] At present, the rate performance of lithium iron phosphate positive electrode materials needs to be further improved. Summary of the invention
[0005] The main purpose of the present invention is to provide a positive electrode material and a preparation method thereof, a positive electrode sheet and a lithium ion battery in view of the problems and shortcomings of the prior art. In the positive electrode material, LiFePO4 nanoparticles are uniformly loaded on the surface of flower-like carbon, and the flower-like carbon provides a fast electron transmission channel and can effectively inhibit the agglomeration of LiFePO4 nanoparticles during the sintering process, thereby showing large capacity, long life and excellent high rate performance.
[0006] In order to solve the above technical problems, the technical solution of the present invention is as follows:
[0007] A positive electrode material comprises three-dimensional flower-shaped carbon and nano lithium iron phosphate particles filled between the three-dimensional flower-shaped carbon skeletons.
[0008] Preferably, the flower-shaped carbon is a spherical particle with a diameter of 1-3 μm and a petal thickness of 5-10 nm, and the lithium iron phosphate particle size is 20-70 nm.
[0009] Preferably, the specific surface area of the flower-like carbon is 1500-2000m 2 / g, pore volume is 0.9-1.2cm 3 / g.
[0010] The method for preparing the positive electrode material comprises the following steps:
[0011] 1) Mixing the flower-shaped carbon and the iron source in a mass ratio of 1:10-20, calcining at 500-700° C. for 1-5 h under protective atmosphere to obtain a flower-shaped carbon material loaded with iron salt;
[0012] 2) dispersing the flower-shaped carbon material loaded with iron salt in ethylene glycol, adding a lithium source and a phosphorus source respectively, wherein the molar ratio of the lithium source, the iron source and the phosphorus source is 1:0.95 to 1:0.95 to 1, mixing evenly and transferring to a hydrothermal reactor, keeping warm at 120 to 200° C. for 15 to 24 hours, washing, filtering and drying to obtain a flower-shaped carbon material loaded with lithium iron phosphate precursor;
[0013] 3) heat-treating the flower-shaped carbon material loaded with a lithium iron phosphate precursor in an argon-hydrogen atmosphere to obtain the positive electrode material.
[0014] Preferably, the preparation method of the flower-like carbon is: coal tar powder, a mixture of K2CO3 and Na2CO3, and KOH are uniformly mixed, transferred into a tubular furnace, activated under a nitrogen atmosphere, and the flower-like carbon is obtained after washing, filtering, and drying.
[0015] Preferably, the sintering conditions in step 3) are 500-700° C. and the reaction time is 1-5 hours.
[0016] Preferably, the volume fraction of hydrogen gas in the argon hydrogen atmosphere in step 3) is 5%-10%.
[0017] Preferably, the lithium source is at least one of lithium hydroxide and lithium carbonate; the phosphorus source is at least one of phosphoric acid, ammonium dihydrogen phosphate and diammonium hydrogen phosphate.
[0018] Preferably, the protective atmosphere in step 1) is one of argon or nitrogen.
[0019] A positive electrode sheet, wherein the slurry for preparing the positive electrode sheet contains the positive electrode material.
[0020] A lithium ion battery comprises the positive electrode sheet.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The unpassivated iron atoms on the surface of LiFePO4 particles undergo electron transfer with the flower-like carbon sheets and are embedded into the flower-like carbon structure through CO-Fe chemical bonding. They are bridged by the three-dimensional carbon network with excellent conductive properties, which can significantly improve the electron transmission capacity between LiFePO4 particles. The highly graphitized three-dimensional carbon skeleton structure can act as a conductive additive, thereby improving the electrode energy density.
[0023] (2) The flower-like carbon skeleton structure can effectively control the distribution of LiFePO4 particles and prevent their harmful agglomeration during material synthesis, electrode preparation and battery reaction, thereby greatly improving the utilization rate of the positive electrode material.
[0024] (3) The three-dimensional flower-like carbon structure with high specific surface area is conducive to the penetration and retention of electrolyte, so that LiFePO4 particles can fully contact with the electrolyte, effectively improving Li + The transfer rate in the electrode enhances the rate performance of the battery.
[0025] (4) During the preparation process, the flower-like carbon skeleton can effectively limit the growth of LiFePO4 grains, making it easy to obtain nano-lithium iron phosphate particles. The high-density distribution of nano-sized LiFePO4 particles in the flower-like carbon skeleton can ensure the volume density and tap density of the composite material.
[0026] (5) The prepared LiFePO4 / CF composite material has high electrical conductivity, high specific surface area and a stable three-dimensional carbon conductive network, which can achieve rapid charging and discharging while ensuring that the electrode has a high energy density. It is an ideal positive electrode material for high-performance batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A schematic diagram of a method for preparing a composite material of flower-like carbon (hereinafter referred to as CF) loaded with nano lithium iron phosphate (hereinafter referred to as LFP) provided in an embodiment of the present invention;
[0028] Figure 2 XRD diffraction patterns of the composite positive electrode materials of Example 1 and Comparative Examples 3 and 5.
[0029] Figure 3 Raman spectra of CF, FeCl3 / CF and LFP / CF.
[0030] Figure 4 SEM images of CF, LFP / CF and LFP of Comparative Example 6.
[0031] Figure 5 TEM image of LFP / CF composite cathode material.
[0032] Figure 6 The rate performance of the LFP / CF composite positive electrode material and comparative example 6 and comparative examples 1, 2, and 3.
[0033] Figure 7 1C cycle performance of LFP / CF composite positive electrode material and comparative example 6.
[0034] Figure 8 The cycling performance of the LFP / CF composite positive electrode material and comparative example 6 at 80% DOD at 6C rate.
[0035] Fig. 9 This is the SEM image of Comparative Example 2.
[0036] Fig.10 This is the SEM image of Comparative Example 5. DETAILED DESCRIPTION
[0037] The principles and features of the present invention are described below in conjunction with examples, which are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, it is worth noting that the raw materials involved in the present invention are all common commercial products unless otherwise specified.
[0038] In the following examples, the preparation methods of flower-like carbon are all prepared by the following method:
[0039] Coal tar powder was mixed with K2CO3 / Na2CO3 (molar ratio of 0.45:0.55) and KOH in a mass ratio of 1:2:2, transferred into a tube furnace, and activated at 750°C in a nitrogen atmosphere. The activation time was 5 hours. After washing, filtering and drying, flower-like carbon was obtained with a diameter of 1-3 μm, a petal thickness of 5-10 nm, and a specific surface area of 1500-2000 m 2 / g, pore volume 0.9~1.2cm 3 / g.
[0040] Example 1
[0041] A method for preparing a positive electrode material, comprising the following steps:
[0042] (1) Weighing 0.5 g of flower-like carbon and 6.5 g of anhydrous ferric chloride, grinding until mixed evenly, heating to 650° C. at a heating rate of 5° C. / min under an argon atmosphere, and keeping the temperature for 5 h to obtain a flower-like carbon material loaded with ferric chloride;
[0043] (2) The flower-shaped carbon material loaded with ferric chloride in step (1) was dispersed in 50 mL of ethylene glycol, and 1.6 g of LiOH·H2O (dissolved in 10 mL of ethylene glycol) and 2.6 mL of 85 wt% H3PO4 solution were added respectively. After stirring evenly, the mixture was transferred to a high-temperature reactor and kept at 180° C. for 20 hours. After washing, filtering and drying, a flower-shaped carbon material loaded with a lithium iron phosphate precursor was obtained;
[0044] (3) The flower-shaped carbon material loaded with lithium iron phosphate precursor in step (2) is heated to 600° C. at a heating rate of 5° C. / min in an argon-hydrogen atmosphere (10 vol-% hydrogen), and kept warm for 2 h to obtain the target product, i.e., the flower-shaped carbon loaded with nano-lithium iron phosphate composite positive electrode material.
[0045] Comparative Example 1
[0046] A method for preparing a positive electrode material, comprising the following steps:
[0047] (1) Weighing 1.0 g of flower-like carbon and 6.5 g of anhydrous ferric chloride, grinding until mixed evenly, heating to 650° C. at a heating rate of 5° C. / min under an argon atmosphere, and keeping the temperature for 5 h to obtain a flower-like carbon material loaded with ferric chloride;
[0048] (2) The flower-shaped carbon material loaded with ferric chloride in step (1) was dispersed in 50 mL of ethylene glycol, and 1.6 g of LiOH·H2O (dissolved in 10 mL of ethylene glycol) and 2.6 mL of 85 wt% H3PO4 solution were added respectively. After stirring evenly, the mixture was transferred to a high-temperature reactor and kept at 180° C. for 20 hours. After washing, filtering and drying, a flower-shaped carbon material loaded with a lithium iron phosphate precursor was obtained;
[0049] (3) The flower-shaped carbon material loaded with lithium iron phosphate precursor in step (2) is heated to 600° C. at a heating rate of 5° C. / min in an argon-hydrogen atmosphere (10 vol-% hydrogen), and kept warm for 2 h to obtain the target product, i.e., the flower-shaped carbon loaded with nano-lithium iron phosphate composite positive electrode material.
[0050] Comparative Example 2
[0051] A method for preparing a positive electrode material, comprising the following steps:
[0052] (1) Weighing 0.2 g of flower-like carbon and 6.5 g of anhydrous ferric chloride, grinding until mixed evenly, heating to 650° C. at a heating rate of 5° C. / min under an argon atmosphere, and keeping the temperature for 5 h to obtain a flower-like carbon material loaded with ferric chloride;
[0053] (2) The flower-shaped carbon material loaded with ferric chloride in step (1) was dispersed in 50 mL of ethylene glycol, and 1.6 g of LiOH·H2O (dissolved in 10 mL of ethylene glycol) and 2.6 mL of 85 wt% H3PO4 solution were added respectively. After stirring evenly, the mixture was transferred to a high-temperature reactor and kept at 180° C. for 20 hours. After washing, filtering and drying, a flower-shaped carbon material loaded with a lithium iron phosphate precursor was obtained;
[0054] (3) The flower-shaped carbon material loaded with lithium iron phosphate precursor in step (2) is heated to 600° C. at a heating rate of 5° C. / min in an argon-hydrogen atmosphere (10 vol-% hydrogen), and kept warm for 2 h to obtain the target product, i.e., the flower-shaped carbon loaded with nano-lithium iron phosphate composite positive electrode material.
[0055] Comparative Example 3
[0056] A method for preparing a positive electrode material, comprising the following steps:
[0057] (1) Weighing 0.5 g of flower-like carbon and 6.5 g of anhydrous ferric chloride, grinding until mixed evenly, heating to 650° C. at a heating rate of 5° C. / min under an argon atmosphere, and keeping the temperature for 5 h to obtain a flower-like carbon material loaded with ferric chloride;
[0058] (2) The flower-shaped carbon material loaded with ferric chloride in step (1) was dispersed in 50 mL of ethylene glycol, and 1.6 g of LiOH·H2O (dissolved in 10 mL of ethylene glycol) and 2.6 mL of 85 wt% H3PO4 solution were added respectively. After stirring evenly, the mixture was transferred to a high-temperature reactor and kept at 180° C. for 10 hours. After washing, filtering and drying, a flower-shaped carbon material loaded with a lithium iron phosphate precursor was obtained;
[0059] (3) The flower-shaped carbon material loaded with lithium iron phosphate precursor in step (2) is heated to 600° C. at a heating rate of 5° C. / min in an argon-hydrogen atmosphere (10 vol-% hydrogen), and kept warm for 2 h to obtain the target product, i.e., the flower-shaped carbon loaded with nano-lithium iron phosphate composite positive electrode material.
[0060] Comparative Example 4
[0061] A method for preparing a positive electrode material, comprising the following steps:
[0062] (1) Weighing 0.5 g of flower-like carbon and 6.5 g of anhydrous ferric chloride, grinding until mixed evenly, heating to 650° C. at a heating rate of 5° C. / min under an argon atmosphere, and keeping the temperature for 5 h to obtain a flower-like carbon material loaded with ferric chloride;
[0063] (2) The flower-shaped carbon material loaded with ferric chloride in step (1) was dispersed in 50 mL of ethylene glycol, and 1.6 g of LiOH·H2O (dissolved in 10 mL of ethylene glycol) and 2.6 mL of 85 wt% H3PO4 solution were added respectively. After stirring evenly, the mixture was transferred to a high-temperature reactor and kept at 180° C. for 20 hours. After washing, filtering and drying, a flower-shaped carbon material loaded with a lithium iron phosphate precursor was obtained;
[0064] (3) The flower-like carbon material loaded with lithium iron phosphate precursor in step (2) is heated to 800° C. at a heating rate of 5° C. / min in an argon-hydrogen atmosphere (10 vol-% hydrogen), and kept warm for 2 h to obtain the target product, i.e., the flower-like carbon loaded nano-lithium iron phosphate composite positive electrode material.
[0065] Comparative Example 5
[0066] A method for preparing a positive electrode material, comprising the following steps:
[0067] (1) Weighing 0.5 g of activated carbon and 6.5 g of anhydrous ferric chloride, grinding until mixed evenly, heating to 650° C. at a heating rate of 5° C. / min under an argon atmosphere, and keeping the temperature for 5 h to obtain an activated carbon / ferric chloride material;
[0068] (2) The activated carbon / ferric chloride material in step (1) was dispersed in 50 mL of ethylene glycol, and 1.6 g of LiOH·H2O (dissolved in 10 mL of ethylene glycol) and 2.6 mL of 85 wt% H3PO4 solution were added respectively. After stirring evenly, the mixture was transferred to a high-temperature reactor and kept at 180° C. for 20 hours. After washing, filtering and drying, a lithium iron phosphate precursor was obtained;
[0069] (3) The lithium iron phosphate precursor in step (2) is heated to 600° C. at a heating rate of 5° C. / min in an argon hydrogen atmosphere (10 vol-% hydrogen), and kept at this temperature for 2 h to obtain an activated carbon-supported nano-lithium iron phosphate composite positive electrode material.
[0070] Comparative Example 6
[0071] This comparative example is substantially the same as Example 1, except that there is no flower-like carbon in step 1).
[0072] Figure 1 The reaction process of Example 1 is demonstrated: first, flower-like carbon and anhydrous ferric chloride are mixed in a certain mass ratio, and a flower-like carbon / ferric chloride material is obtained after calcination; then, the material is evenly mixed with a lithium source and a phosphorus source, and a flower-like carbon material loaded with a lithium iron phosphate precursor is obtained through a solvent thermal reaction; finally, a flower-like carbon-loaded nano-lithium iron phosphate composite positive electrode material is obtained after sintering.
[0073] Figure 2It is the XRD diffraction analysis diagram of the flower-shaped carbon-supported nano-lithium iron phosphate composite positive electrode material of Example 1, Comparative Example 3 and Comparative Example 5. The composite positive electrode material corresponds to the lithium iron phosphate standard card (#81-1173).
[0074] Figure 3 The Raman spectra of CF, FeCl3 / CF and LFP / CF of Example 1 show that the carbon peak is blue-shifted due to the doping of FeCl3. The higher D / G ratio (0.3) of LFP / CF indicates that it has better conductivity.
[0075] Figure 4 The SEM images of CF (a), LFP / CF of Example 1 (b) and Comparative Example 6 (c) show that nanometer (20-70 nm) lithium iron phosphate particles are uniformly loaded in the flower-like carbon sheets. Wherein, def is a partial enlarged view of abc, respectively.
[0076] Figure 5 This is a TEM image of the LFP / CF composite positive electrode material of Example 1, where it can be observed that the nano-lithium iron phosphate particles and the flower-like carbon skeleton are tightly combined. abc are transmission photos, high-resolution transmission photos, and selected area electron diffraction photos, respectively.
[0077] Figure 6 The rate performance of the LFP / CF composite positive electrode materials of Example 1, Comparative Examples 1-3 and Comparative Example 6. Since CO-Fe bonding provides more lithium insertion sites, the LFP / CF composite positive electrode material exhibits better capacity, and the three-dimensional conductive network drives efficient charge transfer at high rates, showing excellent rate performance, with a 10C capacity of 138.2 mAh / g.
[0078] Figure 7 The 1C cycle performance of the LFP / CF composite positive electrode material of Example 1 and Comparative Example 6. After 300 cycles, the reversible capacity of the LFP / CF composite positive electrode material is 155.5 mAh / g, and the capacity retention rate is 97%.
[0079] Figure 8 The 80% DOD cycle performance at 6C rate of the LFP / CF composite positive electrode material of Example 1 and Comparative Example 6. After 100 cycles, the capacity at 90% SOC is 115.4 mAh / g, and the capacity retention rate is 96%.
[0080] In Comparative Example 1, due to the excessive content of flower-like carbon in the preparation process, the lithium iron phosphate particles cannot completely fill the flower-like carbon voids and are unevenly distributed, which increases the ion transmission path, resulting in low specific capacity and poor rate performance of the composite positive electrode material (such as Figure 6 shown).
[0081] In Comparative Example 2, due to the low content of flower-like carbon in the preparation process, the flower-like carbon voids could not support all lithium iron phosphate particles, and some lithium iron phosphate was separated from the conductive network, and agglomeration was observed (e.g. Fig. 9 As shown), the conductivity of the composite positive electrode material is reduced and the utilization rate of lithium iron phosphate is low.
[0082] In Comparative Example 3, due to the short solvent thermal reaction time, the product showed Li3PO4 impurity phase (such as Figure 2 As shown in the figure), the purity of lithium iron phosphate is reduced, resulting in low specific capacity and poor cycle performance of the composite positive electrode material (as shown in the figure). Figure 6 shown).
[0083] In Comparative Example 4, due to the high sintering temperature, Fe +3 Reduced to Fe 2+ , and continues to be reduced to elemental iron, the magnetism of the product is enhanced, the purity of lithium iron phosphate is reduced, and the electrochemical properties of the composite positive electrode material are affected.
[0084] In Comparative Example 5, due to the large pore size and uneven distribution of activated carbon, the nano-lithium iron phosphate particles are locally agglomerated (e.g. Fig.10 As shown), the product has impurities such as Fe2P and Li3PO4 (as shown Figure 2 As shown in the figure, the purity of lithium iron phosphate is reduced, which significantly affects the electrochemical performance of the composite cathode material.
[0085] In Comparative Example 6, although the capacity of lithium iron phosphate can reach 150 mAh / g at a current density of 0.5 C after activation, due to the lack of a reliable conductive network, the capacity quickly decays to 40 mAh / g at a high rate of 10 C, and the material rate performance is poor.
[0086] It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A positive electrode material, characterized in that: The positive electrode material includes three-dimensional flower-shaped carbon and nano-lithium iron phosphate particles filled between the three-dimensional flower-shaped carbon skeletons.
2. The positive electrode material according to claim 1, characterized in that The flower-like carbon is a spherical particle with a diameter of 1-3 µm and a petal thickness of 5-10 nm, and the lithium iron phosphate particle size is 20-70 nm.
3. The positive electrode material according to claim 1, characterized in that The specific surface area of the flower-like carbon is 1500-2000m 2 / g, pore volume of 0.9-1.2 cm 3 / g.
4. The method for preparing a positive electrode material according to any one of claims 1 to 3, characterized in that: The steps include: 1) Mixing the flower-like carbon and the iron source in a mass ratio of 1:10-20, calcining at 500-700 °C for 1-5 h under protective atmosphere to obtain a flower-like carbon material loaded with iron salt; 2) dispersing the flower-shaped carbon material loaded with iron salt in ethylene glycol, adding a lithium source and a phosphorus source respectively, wherein the molar ratio of the lithium source, the iron source and the phosphorus source is 1:0.95-1:0.95-1, mixing evenly and transferring to a reaction kettle, keeping the mixture at 120-200° C. for 15-24 hours, washing, filtering and drying to obtain a flower-shaped carbon material loaded with lithium iron phosphate precursor; 3) heat-treating the flower-shaped carbon material loaded with a lithium iron phosphate precursor in an argon-hydrogen atmosphere to obtain the positive electrode material.
5. The preparation method according to claim 4, characterized in that: The preparation method of the flower-like carbon is as follows: coal tar powder, a mixture of K2CO3 and Na2CO3, and KOH are uniformly mixed, transferred into a tubular furnace, activated under a nitrogen atmosphere, and the flower-like carbon is obtained after washing, filtering, and drying.
6. The preparation method according to claim 4, characterized in that The sintering conditions in step 3) are 500-700° C. and the reaction time is 1-5 h.
7. The preparation method according to claim 4, characterized in that: The volume fraction of hydrogen gas in the argon hydrogen atmosphere in step 3) is 5%-10%.
8. The preparation method according to claim 4, characterized in that: The lithium source is at least one of lithium hydroxide and lithium carbonate; the phosphorus source is at least one of phosphoric acid, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate.
9. The preparation method according to claim 4, characterized in that: The protective atmosphere in step 1) is one of argon or nitrogen.
10. A positive electrode sheet, characterized in that: The slurry for preparing the positive electrode sheet contains the positive electrode material according to any one of claims 1 to 3.
11. A lithium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 10.