Battery module and preparation method thereof
By using lithium-rich manganese-based and silicon-carbon composite materials in the battery module, combined with fluorine-containing additive modified electrolyte and cast coating technology, the problem of short cycle life of the battery module is solved and higher battery performance is achieved and safety, extending battery life.
Patent Information
- Application Number
- CN202411019383.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
At this stage, the cycle life of the battery module is relatively short, mainly due to material and process factors, the activity of positive and negative electrode materials is reduced, the side reactions are generated, and the exfoliation of positive electrode materials is limited, which makes lithium ions move limited and it is difficult to meet the long-term use needs. .
Lithium-rich manganese-based materials and silicon-carbon composite materials are used as the positive and negative electrode materials, combined with fluorine-containing additives to modify the electrolyte, and through Kechen superconducting carbon black and casting coating technology, a stable interface mask is formed to reduce side reactions and The electrolyte decomposes, improves interface stability and mechanical strength, and ensures close bonding between the battery cells through hot pressing.
It significantly improves the cycle life and safety of the battery module, reduces internal resistance, improves energy density and power density, extends the service life of the battery and reduces the risk of electrolyte overflow.
Smart Images

Figure CN118970144A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery modules, and in particular to a battery module and a preparation method thereof. Background Art
[0002] With the advancement of science and technology and the rapid development of new energy technologies, battery modules, as key components for energy storage and conversion, are playing an increasingly important role in fields such as renewable energy storage systems. Battery modules refer to a battery pack with a certain voltage and capacity formed by combining multiple single cells in a certain way. The combination method can improve the efficiency of battery use, reduce costs, and facilitate integration and management. With the rapid development of renewable energy and policy support, the market scale of renewable energy storage systems continues to expand. As one of the core components of renewable energy storage systems, the market demand for battery modules will continue to grow. Therefore, battery modules have broad market prospects and huge economic potential in the field of renewable energy storage systems.
[0003] At present, the cycle life of battery modules is relatively short. Due to the influence of many factors such as materials and processes, from a molecular level, the hole structure that accommodates lithium ions on the positive and negative electrodes will gradually collapse and become blocked. From a chemical point of view, the activity of the positive and negative electrode materials will be passivated, and side reactions will occur to generate other stable compounds. Physically, the positive electrode material will gradually peel off, reducing the number of lithium ions that can move freely in the battery module during the charging and discharging process. The capacity of the battery module decays rapidly after hundreds of cycles, making it difficult to meet the needs of long-term use. Summary of the invention
[0004] The object of the present invention is to provide a battery module and a method for preparing the same, so as to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A battery module, comprising:
[0007] A plurality of battery cells, each of which is composed of a positive electrode, a negative electrode, a separator and an electrolyte;
[0008] The positive electrode is made of lithium-rich manganese (xLi 2 MnO 3 ·(1-x)LiMO 2 ), conductive agent (Carbon EPC), adhesive (PVDF); the conductive agent is Ketjen superconducting carbon black; the adhesive is PVDF 761;
[0009] The negative electrode material comprises a silicon-carbon composite material, a conductive agent (Carbon EPC), a thickener (CMC), and a binder (SBR); the conductive agent is Ketjen superconducting carbon black; the SBR is styrene-butadiene rubber latex; and the CMC is sodium carboxymethyl cellulose;
[0010] The diaphragm is a PP / PE / PP three-layer composite diaphragm;
[0011] The electrolyte is modified by a fluorine-containing additive, and the fluorine-containing additive is fluoroethylene carbonate (FEC);
[0012] Preferably, the mass ratio of each component in the positive electrode material is: lithium-rich manganese base (μm) 96%, n-electrolyte (CarbonEPC) 2%, binder (PVDF 761) 2%, and the weight ratio of NMP: solid matter is about 810:1496;
[0013] The mass ratio of each component in the negative electrode material is: silicon-carbon composite material 94.5%, conductive agent (Carbon EPC) 1%, thickener (CMC) 2.25%, binder (SBR) 2.25%, and the weight ratio of water: solid matter is: 1600:1417.5.
[0014] Preferably, the silicon-carbon composite material is made of nano-silicon powder, graphite and petroleum asphalt powder as raw materials, which are mixed and ball-milled, and heat-treated at a specific temperature to prepare the silicon / carbon composite material, and the heat treatment is performed under an inert atmosphere, such as argon.
[0015] Preferably, the lithium-rich manganese-based material is composed of layered manganese salt Li 2 MnO 3 and lithium salt LiMO 2 It is composed of two components.
[0016] Preferably, the preparation method of the PP / PE / PP three-layer composite diaphragm is as follows: homopolypropylene and atactic polypropylene are blended and melt-extruded on a single screw extruder, and high-density polyethylene is melt-extruded on another single screw extruder;
[0017] Composite cast film: The molten material is transported to the co-extrusion die, and the distributor at the die inlet divides the homopolypropylene and atactic polypropylene blended molten material into two PP layers as the surface layer and the PE layer as the middle layer; the molten material converges at the co-extrusion die outlet, and then is stretched and cooled by the casting roller to form a film, so as to obtain a hard elastic PP / PE / PP composite cast base film; an air knife can be installed between the casting roller and the co-extrusion die outlet to quickly cool the surface of the melt film;
[0018] Heat treatment: The base film is heat treated, and the composite film is heat treated in a hot air circulation furnace at 125°C for 6 hours;
[0019] Stretching treatment: low temperature stretching between two rollers at 45°C, with a stretching rate of 20%, the two rollers are 350mm apart, and the roller speed on the supply side is 1.6m / min;
[0020] Heat setting: heat setting treatment is performed on the stretched composite film;
[0021] Cutting and inspection: Cut the prepared PP / PE / PP three-layer composite diaphragm according to size to ensure that each diaphragm is perfectly covered between two adjacent pole pieces, and carry out necessary performance tests such as peel strength, ion permeability, etc.
[0022] Preferably, the fluorine-containing additive modified electrolyte is prepared by:
[0023] Additive synthesis: Through the nucleophilic substitution reaction between the fluorinating agent and ethylene carbonate, one hydrogen atom in ethylene carbonate is replaced by a fluorine atom to generate FEC;
[0024] Basic electrolyte solvent composition: ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), etc. are used as solvents;
[0025] The fluorinating agent and ethylene carbonate are mixed in a basic electrolyte solvent, and stirred to react at room temperature to 80° C. for 2 hours;
[0026] The fluoride ions in the fluorinating agent react with the hydroxyl groups in the ethylene carbonate to form fluoroethylene carbonate (FEC) and corresponding by-products (such as water and hydrofluoric acid);
[0027] The unreacted fluorinating agent, solvent and by-products are removed by filtration and distillation to obtain fluoroethylene carbonate (FEC) with high purity.
[0028] A battery module and a method for preparing the same, comprising the following steps:
[0029] Step 1: Pretreatment of positive electrode raw materials: dehydrate the lithium-rich manganese base, conductive agent, binder, and NMP respectively, pour the dehydrated lithium cobalt oxide and conductive agent into the ball mill barrel, add grinding balls, dry material: grinding balls = 1:1, the speed of the ball mill barrel is controlled at more than 60rmp, and the ball milling time is 2h;
[0030] Pretreatment of negative electrode raw materials:
[0031] 1) Silicon-carbon composite material: baked at 300-400℃ under normal pressure to remove surface oily substances;
[0032] 2) Water-based adhesive: Dilute the adhesive appropriately with deionized water to improve the dispersibility;
[0033] Pour the silicon-carbon composite material and the conductive agent into the material barrel and add them to the ball mill at the same time, with the ratio of dry material to grinding ball being 1:1.2, and the speed being controlled at above 60rmp, and the ball mill is separated after 4 hours through a sieve;
[0034] Step 2: Preparation of positive electrode raw materials:
[0035] a) Pour NMP into a power mixer (100L) to 80°C, weigh PVDF and add it, start the machine; set parameters: speed 25±2 rpm, stir for 115 to 125 minutes:
[0036] b) Turn on the cooling system, add the ground positive electrode dry material in four equal portions, with an interval of 28-32 minutes between each addition. NMP needs to be added during the third addition, and NMP is added after the fourth addition. Power mixer parameter setting: speed is 20±2 rpm;
[0037] c) 30±2 minutes after the fourth addition, high-speed stirring is performed for 480±10 minutes: the parameters of the power mixer are set as follows: revolution is 30±2 rpm, rotation is 25±2 rpm;
[0038] d) Vacuum mixing: Connect the power mixer to vacuum, maintain the vacuum degree at -0.09Mpa, and stir for 30±2 minutes: Power mixer parameter settings: revolution for 10±2 minutes, rotation for 8±2 rpm;
[0039] e) Take 250-300 ml of slurry and measure the viscosity using a viscometer; test conditions: rotor number 5, speed 12 or 30 rpm, temperature range 25°C;
[0040] f) taking the positive electrode material out of the power mixer and subjecting it to colloid milling and sieving;
[0041] Negative electrode raw material preparation:
[0042] 1) Heat deionized water to 80℃ and pour into a power mixer (2L). Disperse and dissolve CMC in deionized water at high speed. The concentration of CMC is about 1.5%. Stir for 60±2 minutes. The parameters of the power mixer are: revolution for 25±2 minutes and rotation for 15±2 rpm.
[0043] 2) Add SBR and deionized water, stir for 60±2 minutes, and set the parameters of the power mixer: revolution for 30±2 minutes, rotation for 20±2 rpm;
[0044] 3) The negative electrode dry material is added in four equal batches, and deionized water is added at the same time. The viscosity is adjusted to 2000-5000 cP. The interval between each batch is 28-32 minutes. The parameters of the power mixer are set as follows: revolution is 20±2 rpm, rotation is 15±2 rpm;
[0045] 4) 30±2 minutes after the fourth addition, high-speed stirring is performed for 480±10 minutes; the parameters of the power mixer are set as follows: revolution is 30±2 rpm, rotation is 25±2 rpm;
[0046] 5) Vacuum mixing: Connect the power mixer to vacuum, maintain the vacuum degree at -0.09 to 0.10Mpa, stir for 30±2 minutes, set the power mixer parameters as follows: revolution at 10±2 rpm, rotation at 8±2 rpm, slow stirring for vacuum degassing;
[0047] 6) Take 500 ml of slurry and use a viscometer to measure the viscosity: Test conditions: rotor number 5, speed 30 rpm, temperature range 25 °C;
[0048] 7) Taking the negative electrode material out of the power mixer for grinding and sieving;
[0049] Step 3: Coat the positive electrode material and the negative electrode material on the current collector respectively. The positive electrode current collector is aluminum foil and the negative electrode current collector is copper foil to form positive and negative electrode sheets. The specific steps are as follows:
[0050] 1) Coating:
[0051] Positive electrode coating: Use a coating machine to evenly coat the positive electrode coating solution on the aluminum foil. The thickness of the positive electrode coating is controlled between 10 and 20 μm.
[0052] Negative electrode coating: Use a coating machine to evenly coat the negative electrode coating solution on the copper foil. The thickness of the negative electrode coating is controlled between 8 and 15 μm.
[0053] 2) Casting:
[0054] The coated positive and negative electrode sheets are sent to a tape casting machine for tape casting treatment to achieve a thin and uniform thickness;
[0055] 3) Drying and curing:
[0056] After cutting, the current collector coated with active material is sent to the oven for drying and curing. By adjusting the temperature and ventilation conditions of the oven, the solvent and volatiles in the coating layer are removed to ensure the close bonding between the coating and the current collector.
[0057] Step 4: stack the cured positive and negative electrode sheets and the diaphragm sheet in a certain order, and stack them in the order of positive electrode sheet-diaphragm sheet-negative electrode sheet. Place the materials between the heating plates of the hot press and apply constant pressure to make the materials of the positive electrode sheet-diaphragm sheet-negative electrode sheet in the battery module tightly combined to form a battery cell unit.
[0058] Multiple battery cells are stacked together to form a battery module. After the stacking is completed, the multiple battery cells are placed between the heating plates of the hot press by hot pressing, and constant pressure is applied to make the multiple battery cells tightly combined to form a battery module. The hot pressing temperature range is controlled at 65°C to 85°C, and the hot pressing pressure range is 1T to 6T;
[0059] After the battery module is hot-pressed, copper-cobalt welding is performed on the positive and negative electrodes of the battery cell unit to form a complete current path inside to ensure uniform current transmission;
[0060] Step 5: Test the battery module for charging and discharging.
[0061] The specific steps of the charging test are as follows: connect the battery module to a dedicated charging device and set the constant current constant voltage (CC-CV) charging mode; monitor and record the changes in the battery module's charging current, voltage, temperature and other parameters over time; when the battery module reaches a fully charged state, calculate and record its charging capacity, charging efficiency and charging time;
[0062] Evaluation criteria: Charging rate: The battery module should reach the predetermined charging capacity within the specified time; Charging efficiency: The charging efficiency of the battery module should meet the design standard to reduce energy loss; Safety: During the charging process, the battery module should not have safety hazards such as overheating and short circuit;
[0063] The specific steps of the discharge test are as follows: connect the battery module to a dedicated discharge device and set the constant current discharge mode; monitor and record the changes of the battery module's discharge current, voltage, temperature and other parameters over time; when the battery module reaches the discharge termination voltage, calculate and record its discharge capacity and discharge time;
[0064] Evaluation criteria: Discharge capacity: The discharge capacity of the battery module should meet the design standard and meet the actual use requirements; Discharge rate: Within the specified time, the battery module should be able to discharge stably without a sharp drop; Discharge voltage: The discharge voltage of the battery module should remain stable and meet the design requirements;
[0065] Cycle life test: Perform cycle charge and discharge test on battery modules. After each cycle, record the battery's charge and discharge capacity and internal resistance and other parameters. Based on the test data, draw the charge and discharge capacity retention rate and internal resistance change curves, and evaluate the battery's cycle life through data analysis.
[0066] Safety testing: Test battery modules under extreme conditions such as overcharge, over discharge, short circuit, high temperature, and low temperature; monitor and record key parameters such as temperature changes, voltage changes, and gas emissions during the test; check whether the battery modules have thermal runaway, combustion, explosion, and other safety hazards under extreme conditions;
[0067] Evaluation criteria: Safety: The battery module should maintain good safety performance under extreme conditions, without thermal runaway, combustion, explosion and other safety hazards; Protection performance: The battery module should be equipped with a complete protection mechanism, such as overcharge and over-discharge protection, short-circuit protection, etc., to ensure that the battery module can operate safely under various conditions;
[0068] Step 6: Place the battery module in a square aluminum shell, and use the liquid injection equipment to inject the fluorine-containing additive-modified electrolyte into the battery module in the aluminum shell. After the electrolyte injection is completed, add an appropriate amount of degassing agent to the electrolyte to reduce the gas generation in the electrolyte, thereby reducing the risk of electrolyte overflow. Finally, use the welding sealing process and equipment to seal the aluminum shell.
[0069] Compared with the prior art, the present invention has the following beneficial effects: by modifying the electrolyte with a fluorine-containing additive, a stable SEI film is formed on the electrode surface, side reactions are reduced, and decomposition of the electrolyte under high voltage is inhibited; the fluorine-containing additive can generate a LiF-rich interface film on the surface of the negative electrode, and the interface film has higher stability and mechanical strength. By improving the stability of the interface film, the fluorine-containing additive can significantly improve the cycle life and safety of the battery module; the negative electrode adopts a silicon-carbon composite material and the positive electrode adopts a lithium-rich manganese-based material to improve the specific capacity and initial efficiency of the negative electrode and reduce lithium loss during the cycle;
[0070] The use of advanced pole piece tape coating technology can achieve precise control of pole piece thickness, surface density and size by precisely controlling the parameters in the coating process, such as coating speed and coating amount, to ensure that the performance parameters of each pole piece are basically consistent, thereby improving the consistency and overall performance of the battery module. The tape coating process is used to ensure the uniform distribution of positive and negative electrode materials on the current collector, avoiding excessively thick or thin coatings, thereby improving the uniformity and consistency of the pole piece. The uniform pole piece coating helps to reduce the non-uniformity of the electrochemical reaction inside the battery, reduce the internal resistance of the battery, and thus improve the efficiency and safety of the battery. The tape coating technology can significantly increase the capacity and cycle life of the battery, while reducing the internal resistance and improving the energy density and power density of the battery.
[0071] Hot pressing can ensure close bonding between the layers of the battery cell, ensure a stable and reliable connection between the battery cell and the module, improve the capacity, cycle life and safety performance of the battery cell, add an appropriate amount of degasser to the electrolyte to reduce gas generation in the electrolyte, thereby reducing the risk of electrolyte overflow and preventing performance degradation caused by electrolyte leakage. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] Figure 1 This is a flow chart of the method for preparing a battery module of the present invention;
[0073] Figure 2The present invention is a flow chart for preparing the silicon-carbon composite material;
[0074] Figure 3 This is a flow chart for preparing the lithium-rich manganese-based material of the present invention;
[0075] Figure 4 The figure is a flow chart of the preparation of the PP / PE / PP three-layer composite diaphragm of the present invention;
[0076] Figure 5 The present invention is a flow chart for preparing a fluorine-containing additive modified electrolyte;
[0077] Figure 6 The present invention is a flow chart for preparing the positive electrode raw material;
[0078] Figure 7 The figure is a flow chart of the preparation of negative electrode raw materials of the present invention.
[0079] In the figure: 1. Dilution water pipe; 101. Manual butterfly valve A; 102. Electric butterfly valve; 103. Pressure transmitter A; 104. Electromagnetic flowmeter A; 2. Clarification tank; 201. Guardrail; 202. Manhole; 203. Dilution water inlet A; 204. Lime milk inlet A; 205. Ultrasonic level meter A; 206. Overflow weir; 207. Mixing barrel; 208. Waveguide; 3. Slag discharge valve pipe; 301. Pneumatic butterfly valve; 302. Manual butterfly valve B; 303. Air compression system; 304. Backwashing Valve A; 4. Mixer; 401. Mounting rod; 402. Mounting sleeve; 403. Spoiler; 404. Agitator; 5. Storage tank; 501. Dilution water inlet B; 502. Ultrasonic level meter B; 503. Overflow connecting pipe; 504. Ladder; 505. Overflow pipe; 506. Drug outlet; 507. Lime milk inlet B; 508. Drain port; 6. Dosing pipe; 601. Booster pump; 602. Electromagnetic flowmeter B; 603. Pressure transmitter B; 604. Backwash valve B; 7. Base. DETAILED DESCRIPTION
[0080] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0081] Example
[0082] See also Figure 1-7 , an embodiment of the present invention provides: a battery module, comprising:
[0083] Multiple battery cells, each battery cell is composed of a positive electrode, a negative electrode, a separator and an electrolyte;
[0084] The positive electrode is made of lithium-rich manganese-based (xLi 2 MnO 3 ·(1-x)LiMO 2 ), conductive agent (Carbon EPC), adhesive (PVDF); the conductive agent is Ketjen superconducting carbon black; the adhesive is PVDF 761;
[0085] The negative electrode material includes silicon-carbon composite material, conductive agent (Carbon EPC), thickener (CMC), and adhesive (SBR); the conductive agent is Ketjen superconducting carbon black; SBR is styrene-butadiene rubber latex; CMC is sodium carboxymethyl cellulose;
[0086] The diaphragm adopts PP / PE / PP three-layer composite diaphragm;
[0087] The electrolyte adopts a fluorine-containing additive modified electrolyte, and the fluorine-containing additive adopts fluoroethylene carbonate (FEC);
[0088] Furthermore, the mass ratio of each component in the positive electrode material is: lithium-rich manganese base (μm) 96%, conductive agent (CarbonEPC) 2%, binder (PVDF 761) 2%, and the weight ratio of NMP: solid matter is about 810:1496;
[0089] The mass ratio of each component in the negative electrode material is: silicon-carbon composite material 94.5%, conductive agent (Carbon EPC) 1%, thickener (CMC) 2.25%, binder (SBR) 2.25%, and the weight ratio of water: solid matter is: 1600:1417.5.
[0090] Furthermore, the silicon-carbon composite material is prepared by mixing nano silicon powder, graphite and petroleum asphalt powder as raw materials, ball milling, and heat treating at a specific temperature to prepare a silicon / carbon composite material. The heat treatment is performed in an inert atmosphere, such as argon, to prevent the material from being oxidized during the heat treatment. The specific steps are as follows:
[0091] The silicon-carbon composite material is prepared by mechanical ball milling: silicon powder, graphite and conductive agent are mixed and then mechanically ground in a ball mill. The silicon powder and graphite particles are crushed and mixed under the impact and shearing action of the ball milling medium, and finally a silicon-carbon composite material is formed;
[0092] The ball-milled silicon-carbon composite material was heat treated at different temperatures and times, and the specific parameters were set as follows:
[0093] Heat treatment temperature: divided into several temperature ranges, including 50-350℃, 350℃-600℃, and specific temperature points such as 810℃, 830℃, and 850℃;
[0094] 50~350℃ temperature range: In this temperature range, the silicon-carbon composite material mainly undergoes physical mixing and preliminary chemical bonding to form a relatively loose silicon-carbon composite;
[0095] As the temperature increases, the interaction between silicon and carbon gradually increases, but too high a temperature may cause some carbon materials to oxidize, affecting the performance of the composite material;
[0096] 350℃~600℃ temperature range: In this temperature range, the silicon-carbon composite material undergoes a deeper chemical bond, and the carbon layer gradually forms and stabilizes;
[0097] Appropriate temperature helps to improve the conductivity and structural stability of silicon-carbon composites, thereby improving their electrochemical performance;
[0098] Specific temperature points such as 810℃, 830℃, and 850℃: At higher temperatures, the silicon-carbon composite material may undergo graphitization, further improving its conductivity and stability;
[0099] However, too high a temperature may cause excessive expansion or structural damage of the silicon material, affecting the performance of the composite material;
[0100] Heat treatment time: different time points within 6 to 12 hours, including 6.5 hours, 7 hours, 7.5 hours, etc.
[0101] Furthermore, the lithium-rich manganese-based material is composed of layered manganese salts Li 2 MnO 3 and lithium salt LiMO 2 It is composed of two components;
[0102] Preparation of lithium-rich manganese-based materials by gel method: Li 2 MnO 3 and LiMO 2 Adding an appropriate amount of complexing agent (polyethylene glycol) to an appropriate amount of solvent can effectively control the hydrolysis and condensation reactions of metal ions in the solution, thereby forming a stable sol system.
[0103] The solution is heated under stirring conditions to make the metal ions evenly distributed in the solution to form a uniform sol;
[0104] Sol transformation: As the solvent gradually evaporates, the particles in the sol begin to connect with each other to form a three-dimensional network structure, namely gel;
[0105] Aging treatment: The formed wet gel is aged to make the small colloidal particles gradually connect and grow, thus enhancing the stability and strength of the gel;
[0106] Drying treatment: Through drying treatment, the solvent in the wet gel is removed to obtain a dry gel with uniform spatial distribution of metal ions;
[0107] High temperature calcination: The dry gel is calcined at a high temperature to remove organic impurities and promote the full reaction of manganese salt and lithium salt. This is carried out in an air or oxygen atmosphere, which helps to maintain the oxygen content and structural stability of the material.
[0108] Grinding and screening: Grinding and screening the calcined product to obtain a lithium-rich manganese-based material with uniform particle size and high purity;
[0109] Furthermore, the preparation method of the PP / PE / PP three-layer composite diaphragm is as follows: a liquid hydrocarbon is mixed with homopolypropylene (PP) and then heated to melt, the mixture is cooled to separate phases, the mixture is pressed into a membrane, the pressed membrane is heated to a temperature close to the melting point, and biaxially stretched, after the stretching is completed, the membrane is kept warm for a certain period of time, and then the residual solvent and other impurities are eluted with a volatile substance (such as a solvent), and a homopolypropylene (PP) microporous membrane is prepared through the steps of stretching and elution;
[0110] According to the above method, an atactic polypropylene (PP) microporous membrane and a high-density polyethylene (PE) microporous membrane are prepared, homopolypropylene (PP) and atactic polypropylene (PP) are used as outer layer materials, and high-density polyethylene (PE) is used as an intermediate layer material;
[0111] Melt extrusion: Blend homopolypropylene and atactic polypropylene and melt extrude them on a single screw extruder. Melt extrude high-density polyethylene on another single screw extruder. The temperature settings of each zone of the twin-screw extruder are: Zone I Zone II Zone III Zone IV Zone V Machine head
[0112] Composite cast film: The molten material is transported to the co-extrusion die, and the distributor at the die inlet divides the homopolypropylene and atactic polypropylene blended molten material into two PP layers as the surface layer and the PE layer as the middle layer; the molten material converges at the co-extrusion die outlet, and then is stretched and cooled by the casting roller to form a film, so as to obtain a hard elastic PP / PE / PP composite cast base film; an air knife can be installed between the casting roller and the co-extrusion die outlet to quickly cool the surface of the melt film;
[0113] Heat treatment: Heat treat the base film and use a hot air circulation furnace at 125°C for 6 hours to ensure that the inside of the core reaches the same temperature;
[0114] Stretching treatment: low temperature stretching between two rollers at 45°C, with a stretching rate of 20%, the two rollers are 350mm apart, and the roller speed on the supply side is 1.6m / min;
[0115] Heat setting: The stretched composite film is heat-set, and the composite film is placed in a heat processing device, such as an oven or a heat setting machine, and heated to 280°C to make the composite film reach a softening temperature. In the softened state of the composite film, an external force (such as a mold or vacuum adsorption) can be applied to change its shape. When the composite film reaches the desired shape, it is taken out of the heating device and placed in a cooling device for cooling to ensure that the composite film can maintain the plastic shape and solidify. The composite film is heat-set to obtain a more stable structure and performance;
[0116] Cutting and inspection: Cut the prepared PP / PE / PP three-layer composite diaphragm according to size to ensure that each diaphragm is perfectly covered between two adjacent pole pieces, and carry out necessary performance tests such as peel strength, ion permeability, etc.
[0117] Further, the fluorine-containing additive modified electrolyte is prepared:
[0118] Additive synthesis: Through the nucleophilic substitution reaction between the fluorinating agent and ethylene carbonate, one hydrogen atom in ethylene carbonate is replaced by a fluorine atom to generate FEC;
[0119] The fluorinating agent is one of hydrogen fluoride (HF), potassium fluoride and sodium fluoride;
[0120] Basic electrolyte solvent composition: ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), etc. are used as solvents;
[0121] The fluorinating agent and ethylene carbonate are mixed in a basic electrolyte solvent, and stirred to react at room temperature to 80°C for 2 hours;
[0122] The fluoride ions in the fluorinating agent react with the hydroxyl groups in the ethylene carbonate to form fluoroethylene carbonate (FEC) and corresponding by-products, such as water and hydrofluoric acid;
[0123] The unreacted fluorinating agent, solvent and by-products are removed by filtration and distillation to obtain fluoroethylene carbonate (FEC) with high purity.
[0124] A battery module and a method for preparing the same, characterized in that the steps include:
[0125] Step 1: Pretreatment of the positive electrode raw materials, respectively dehydration treatment of the lithium-rich manganese base, conductive agent, binder, and NMP: lithium-rich manganese base: dehydrated by baking at 120°C and normal pressure for 2 hours; conductive agent: dehydrated by baking at 200°C and normal pressure for 2 hours; binder: dehydrated by baking at 120-140°C and normal pressure for 2 hours; NMP: dehydrated by using a dry molecular sieve for dehydration;
[0126] Pour the dehydrated lithium cobalt oxide and conductive agent into the ball mill barrel, add grinding balls, dry material: grinding balls = 1:1, control the speed of the ball mill barrel at more than 60rmp, and the ball milling time is 2h;
[0127] Pretreatment of negative electrode raw materials:
[0128] 1) Silicon-carbon composite materials: baked at 300-400°C under normal pressure to remove surface oily substances and improve compatibility with water-based adhesives;
[0129] 2) Water-based adhesive: Dilute the adhesive appropriately with deionized water to improve the dispersibility;
[0130] Pour the silicon-carbon composite material and the conductive agent into the material barrel and add them to the ball mill at the same time, with the ratio of dry material to grinding ball being 1:1.2, and the speed being controlled at above 60rmp, and the ball mill is separated after 4 hours through a sieve;
[0131] Step 2: Preparation of positive electrode raw materials:
[0132] a) Pour NMP into a power mixer (100L) to 80°C, weigh PVDF and add it, start the machine; set parameters: speed 25±2 rpm, stir for 115 to 125 minutes:
[0133] b) Turn on the cooling system, add the ground positive electrode dry material in four equal portions, with an interval of 28-32 minutes between each addition. NMP needs to be added during the third addition, and NMP is added after the fourth addition. Power mixer parameter setting: speed is 20±2 rpm;
[0134] c) 30±2 minutes after the fourth addition, high-speed stirring is performed for 480±10 minutes: the parameters of the power mixer are set as follows: revolution is 30±2 rpm, rotation is 25±2 rpm;
[0135] d) Vacuum mixing: Connect the power mixer to vacuum, maintain the vacuum degree at -0.09Mpa, and stir for 30±2 minutes: Power mixer parameter settings: revolution for 10±2 minutes, rotation for 8±2 rpm;
[0136] e) Take 250-300 ml of slurry and measure the viscosity using a viscometer; test conditions: rotor number 5, speed 12 or 30 rpm, temperature range 25°C;
[0137] f) taking the positive electrode material out of the power mixer and subjecting it to colloid milling and sieving;
[0138] Negative electrode raw material preparation:
[0139] 1) Heat deionized water to 80℃ and pour into a power mixer (2L). Disperse and dissolve CMC in deionized water at high speed. The concentration of CMC is about 1.5%. Stir for 60±2 minutes. The parameters of the power mixer are: revolution for 25±2 minutes and rotation for 15±2 rpm.
[0140] 2) Add SBR and deionized water, stir for 60±2 minutes, and set the parameters of the power mixer: revolution for 30±2 minutes, rotation for 20±2 rpm;
[0141] 3) The negative electrode dry material is added in four equal batches, and deionized water is added at the same time. The viscosity is adjusted to 2000-5000 cP. The interval between each batch is 28-32 minutes. The parameters of the power mixer are set as follows: revolution is 20±2 rpm, rotation is 15±2 rpm;
[0142] 4) 30±2 minutes after the fourth addition, high-speed stirring is performed for 480±10 minutes; the parameters of the power mixer are set as follows: revolution is 30±2 rpm, rotation is 25±2 rpm;
[0143] 5) Vacuum mixing: Connect the power mixer to vacuum, maintain the vacuum degree at -0.09 to 0.10Mpa, stir for 30±2 minutes, set the power mixer parameters as follows: revolution at 10±2 rpm, rotation at 8±2 rpm, slow stirring for vacuum degassing;
[0144] 6) Take 500 ml of slurry and use a viscometer to measure the viscosity: Test conditions: rotor number 5, speed 30 rpm, temperature range 25 °C;
[0145] 7) Taking the negative electrode material out of the power mixer for grinding and sieving;
[0146] Step 3: Coat the positive electrode material and the negative electrode material on the current collector respectively. The positive electrode current collector is aluminum foil and the negative electrode current collector is copper foil to form positive and negative electrode sheets. The specific steps are as follows:
[0147] 1) Coating:
[0148] Positive electrode coating: Use a coating machine to evenly coat the positive electrode coating solution on the aluminum foil. The thickness of the positive electrode coating is controlled between 10 and 20 μm.
[0149] Negative electrode coating: Use a coating machine to evenly coat the negative electrode coating solution on the copper foil. The thickness of the negative electrode coating is controlled between 8 and 15 μm.
[0150] 2) Casting:
[0151] The coated positive and negative electrode sheets are sent to the tape casting machine for tape casting treatment to achieve a thin and uniform thickness. The specific steps are as follows:
[0152] Stretching: The positive and negative electrodes are stretched to a predetermined size and shape at a stretching speed of 5 to 10 m / min by the stretching device of the tape casting machine. The temperature of the lower layer of the tape casting machine is controlled at about 130°C, and the temperature of the upper layer is controlled at 150°C to 190°C to ensure the uniformity and dimensional stability of the material.
[0153] Cooling: The stretched positive and negative electrodes are quickly cooled by a cooling device to keep the shape and size of the material unchanged. The cooling water temperature is controlled at 20-30°C.
[0154] Cutting: After stretching and cooling, the positive and negative electrode sheets are cut into predetermined sizes by the cutting device of the tape casting machine. The cutting process needs to be precisely controlled to ensure the dimensional accuracy and edge quality of the positive and negative electrode sheets;
[0155] 3) Drying and curing:
[0156] After cutting, the current collector coated with active material is sent to the oven for drying and curing. The drying stage is between 60℃ and 80℃, and the duration is 1 to 2 hours; the curing stage is between 100℃ and 150℃, and the duration is 2 to 4 hours. By adjusting the temperature and ventilation conditions of the oven, the solvent and volatiles in the coating layer are removed to ensure the close bonding between the coating and the current collector.
[0157] Step 4: stack the cured positive and negative electrode sheets and the diaphragm sheet in a certain order, and stack them in the order of positive electrode sheet-diaphragm sheet-negative electrode sheet. Place the materials between the heating plates of the hot press and apply constant pressure to make the materials of the positive electrode sheet-diaphragm sheet-negative electrode sheet in the battery module tightly combined to form a battery cell unit.
[0158] Multiple battery cells are stacked together to form a battery module. After the stacking is completed, the multiple battery cells are placed between the heating plates of the hot press by hot pressing, and constant pressure is applied to make the multiple battery cells tightly combined to form a battery module. The hot pressing temperature range is controlled at 65°C to 85°C, and the hot pressing pressure range is 1T to 6T. The hot pressing method is used to ensure close contact between the battery cells and reduce resistance;
[0159] After the battery module is hot-pressed, copper-cobalt welding is performed on the positive and negative electrodes of the battery cell unit to form a complete current path inside to ensure uniform current transmission. The specific steps are as follows:
[0160] The copper-cobalt welding material is welded to the positive and negative electrodes of the battery cell by welding equipment to form a battery module connected in series or in parallel. The current during welding is between 40-120 amperes (A), and the pressure during welding is controlled between 5-10 MPa;
[0161] Step 5: Test the battery module for charging and discharging.
[0162] The specific steps of the charging test are as follows: connect the battery module to a dedicated charging device and set the constant current constant voltage (CC-CV) charging mode; monitor and record the changes in the battery module's charging current, voltage, temperature and other parameters over time; when the battery module reaches a fully charged state, calculate and record its charging capacity, charging efficiency and charging time;
[0163] Evaluation criteria: Charging rate: The battery module should reach the predetermined charging capacity within the specified time; Charging efficiency: The charging efficiency of the battery module should meet the design standard to reduce energy loss; Safety: During the charging process, the battery module should not have safety hazards such as overheating and short circuit;
[0164] The specific steps of the discharge test are as follows: connect the battery module to a dedicated discharge device and set the constant current discharge mode; monitor and record the changes of the battery module's discharge current, voltage, temperature and other parameters over time; when the battery module reaches the discharge termination voltage, calculate and record its discharge capacity and discharge time;
[0165] Evaluation criteria: Discharge capacity: The discharge capacity of the battery module should meet the design standard and meet the actual use requirements; Discharge rate: Within the specified time, the battery module should be able to discharge stably without a sharp drop; Discharge voltage: The discharge voltage of the battery module should remain stable and meet the design requirements;
[0166] Cycle life test: The battery module is subjected to cycle charge and discharge test. The battery module is charged at 0.2C and discharged at 0.5C for cycles. The test is stopped when the discharge capacity is less than 72min (60%) for two consecutive times. The cycle life of the battery module is not less than 500 times. After each cycle, the battery charge and discharge capacity and internal resistance and other parameters are recorded. Based on the test data, the charge and discharge capacity retention rate and internal resistance change curves are drawn, and the battery cycle life is evaluated through data analysis.
[0167] Safety testing: Test battery modules under extreme conditions such as overcharge, over discharge, short circuit, high temperature, and low temperature; monitor and record key parameters such as temperature changes, voltage changes, and gas emissions during the test; check whether the battery modules have thermal runaway, combustion, explosion, and other safety hazards under extreme conditions;
[0168] Evaluation criteria: Safety: The battery module should maintain good safety performance under extreme conditions, without thermal runaway, combustion, explosion and other safety hazards; Protection performance: The battery module should be equipped with a complete protection mechanism, such as overcharge and over-discharge protection, short-circuit protection, etc., to ensure that the battery module can operate safely under various conditions;
[0169] Step 6: Place the battery module in a square aluminum shell, and use the liquid injection equipment to inject the fluorine-containing additive-modified electrolyte into the battery module in the aluminum shell. After the electrolyte injection is completed, add an appropriate amount of degassing agent to the electrolyte to reduce the gas generation in the electrolyte. Finally, use the welding sealing process and equipment to seal the aluminum shell.
[0170] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A battery module, characterized in that: include: A plurality of battery cells, each of which is composed of a positive electrode, a negative electrode, a separator and an electrolyte; The positive electrode is composed of lithium-rich manganese-based xLi2 MnO3·(1-x)LiMO2, conductive agent Carbon EPC, and adhesive PVDF; the conductive agent is Ketjen superconducting carbon black; the adhesive is PVDF 761; The negative electrode material comprises a silicon-carbon composite material, a conductive agent Carbon EPC, a thickener CMC, and a binder SBR; the conductive agent is Ketjen superconducting carbon black; the SBR is styrene-butadiene rubber latex; and the CMC is sodium carboxymethyl cellulose; The diaphragm is a PP / PE / PP three-layer composite diaphragm; The electrolyte adopts a fluorine-containing additive to modify the electrolyte, and the fluorine-containing additive adopts fluoroethylene carbonate FEC.
2. A battery module according to claim 1, characterized in that: The mass ratio of each component in the positive electrode material is: lithium-rich manganese base (μm) 96%, conductive agent (Carbon EPC) 2%, binder (PVDF 761) 2%, and the weight ratio of NMP: solid matter is about 810:1496; The mass ratio of each component in the negative electrode material is: silicon-carbon composite material 94.5%, conductive agent (Carbon EPC) 1%, thickener (CMC) 2.25%, binder (SBR) 2.25%, and the weight ratio of water: solid matter is: 1600:1417.
5.
3. A battery module according to claim 1, characterized in that: The silicon-carbon composite material is prepared by mixing nano silicon powder, graphite and petroleum asphalt powder, ball milling and heat treatment at a specific temperature to prepare the silicon / carbon composite material, and the heat treatment is carried out in an inert atmosphere, such as argon.
4. A battery module according to claim 1, characterized in that: The lithium-rich manganese-based material is composited from two components: layered manganese salt Li2MnO3 and lithium salt LiMO2.
5. A battery module according to claim 1, characterized in that: The preparation method of the PP / PE / PP three-layer composite diaphragm comprises: blending homopolypropylene and atactic polypropylene, and melt-extruding them on a single screw extruder, and melt-extruding high-density polyethylene on another single screw extruder; Composite cast film: The molten material is transported to the co-extrusion die, and the distributor at the die inlet divides the homopolypropylene and atactic polypropylene blended molten material into two PP layers as the surface layer and the PE layer as the middle layer; the molten material converges at the co-extrusion die outlet, and then is stretched and cooled by the casting roller to form a film, so as to obtain a hard elastic PP / PE / PP composite cast base film; an air knife can be installed between the casting roller and the co-extrusion die outlet to quickly cool the surface of the melt film; Heat treatment: The base film is heat treated, and the composite film is heat treated in a hot air circulation furnace at 125°C for 6 hours; Stretching treatment: low temperature stretching between two rollers at 45°C, with a stretching rate of 20%, the two rollers are 350mm apart, and the roller speed on the supply side is 1.6m / min; Heat setting: heat setting treatment is performed on the stretched composite film; Cutting and inspection: Cut the prepared PP / PE / PP three-layer composite diaphragm according to size to ensure that each diaphragm is perfectly covered between two adjacent pole pieces, and carry out necessary performance tests such as peel strength and ion permeability.
6. The method for preparing a battery module according to claim 1, characterized in that: The preparation of the fluorine-containing additive modified electrolyte is as follows: Additive synthesis: Through the nucleophilic substitution reaction between the fluorinating agent and ethylene carbonate, one hydrogen atom in ethylene carbonate is replaced by a fluorine atom to generate FEC; Basic electrolyte solvent composition: ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) are used as solvents; The fluorinating agent and ethylene carbonate are mixed in a basic electrolyte solvent, and stirred to react at room temperature to 80° C. for 2 hours; The fluoride ions in the fluorinating agent react with the hydroxyl groups in the ethylene carbonate to form fluoroethylene carbonate (FEC) and corresponding by-products; The unreacted fluorinating agent, solvent and by-products are removed by filtration and distillation to obtain fluoroethylene carbonate (FEC) with high purity.
7. A method for preparing a battery module, characterized in that: The following steps are involved: Step 1: Pretreatment of positive electrode raw materials: dehydrate the lithium-rich manganese base, conductive agent, binder, and NMP respectively, pour the dehydrated lithium cobalt oxide and conductive agent into the ball mill barrel, add grinding balls, dry material: grinding balls = 1:1, the speed of the ball mill barrel is controlled at more than 60rmp, and the ball milling time is 2h; Pretreatment of negative electrode raw materials: 1) Silicon-carbon composite material: baked at 300-400℃ under normal pressure to remove surface oily substances; 2) Water-based adhesive: Dilute the adhesive appropriately with deionized water to improve the dispersibility; Pour the silicon-carbon composite material and the conductive agent into the material barrel and add them to the ball mill at the same time, with the ratio of dry material to grinding ball being 1:1.2, and the speed being controlled at above 60rmp, and the ball mill is separated after 4 hours through a sieve; Step 2: Preparation of positive electrode raw materials: a) Pour NMP into a power mixer and heat it to 80°C, weigh PVDF and add it, then start the machine; set the parameters: speed 25±2 rpm, stir for 115 to 125 minutes: b) Turn on the cooling system, add the ground positive electrode dry material in four equal portions, with an interval of 28-32 minutes between each addition. NMP needs to be added during the third addition, and NMP is added after the fourth addition. Power mixer parameter setting: speed is 20±2 rpm; c) 30±2 minutes after the fourth addition, high-speed stirring is performed for 480±10 minutes: the parameters of the power mixer are set as follows: revolution is 30±2 rpm, rotation is 25±2 rpm; d) Vacuum mixing: Connect the power mixer to vacuum, maintain the vacuum degree at -0.09Mpa, and stir for 30±2 minutes: Power mixer parameter settings: revolution for 10±2 minutes, rotation for 8±2 rpm; e) Take 250-300 ml of slurry and measure the viscosity using a viscometer; test conditions: rotor number 5, speed 12 or 30 rpm, temperature range 25°C; f) taking the positive electrode material out of the power mixer for colloid milling and sieving; Negative electrode raw material preparation: 1) Heat deionized water to 80℃ and pour it into a power mixer. Disperse and dissolve CMC in deionized water at high speed. The concentration of CMC is about 1.5%. Stir for 60±2 minutes. The parameters of the power mixer are: revolution for 25±2 minutes and rotation for 15±2 rpm. 2) Add SBR and deionized water, stir for 60±2 minutes, and set the parameters of the power mixer: revolution for 30±2 minutes, rotation for 20±2 rpm; 3) The negative electrode dry material is added in four equal batches, and deionized water is added at the same time. The viscosity is adjusted to 2000-5000 cP. The interval between each batch is 28-32 minutes. The parameters of the power mixer are set as follows: revolution is 20±2 rpm, rotation is 15±2 rpm; 4) 30±2 minutes after the fourth addition, high-speed stirring is performed for 480±10 minutes; the parameters of the power mixer are set as follows: revolution is 30±2 rpm, rotation is 25±2 rpm; 5) Vacuum mixing: Connect the power mixer to vacuum, maintain the vacuum degree at -0.09 to 0.10Mpa, stir for 30±2 minutes, set the power mixer parameters as follows: revolution at 10±2 rpm, rotation at 8±2 rpm, slow stirring for vacuum degassing; 6) Take 500 ml of slurry and use a viscometer to measure the viscosity: Test conditions: rotor number 5, speed 30 rpm, temperature range 25 °C; 7) Taking the negative electrode material out of the power mixer for grinding and sieving; Step 3: Coat the positive electrode material and the negative electrode material on the current collector respectively. The positive electrode current collector is aluminum foil and the negative electrode current collector is copper foil to form positive and negative electrode sheets. The specific steps are as follows: 1) Coating: Positive electrode coating: Use a coating machine to evenly coat the positive electrode coating solution on the aluminum foil, and the thickness of the positive electrode coating is controlled between 10 and 20 μm; Negative electrode coating: Use a coating machine to evenly coat the negative electrode coating solution on the copper foil, and the thickness of the negative electrode coating is controlled between 8 and 15 μm; 2) Casting: The coated positive and negative electrode sheets are sent to a tape casting machine for tape casting treatment to achieve a thin and uniform thickness; 3) Drying and curing: After cutting, the current collector coated with active material is sent to the oven for drying and curing. By adjusting the temperature and ventilation conditions of the oven, the solvent and volatiles in the coating layer are removed to ensure the close bonding between the coating and the current collector. Step 4: stack the cured positive and negative electrode sheets and the diaphragm sheet in a certain order, and stack them in the order of positive electrode sheet-diaphragm sheet-negative electrode sheet. Place the materials between the heating plates of the hot press and apply constant pressure to make the materials of the positive electrode sheet-diaphragm sheet-negative electrode sheet in the battery module tightly combined to form a battery cell unit. Multiple battery cells are stacked together to form a battery module. After the stacking is completed, the multiple battery cells are placed between the heating plates of the hot press by hot pressing, and constant pressure is applied to make the multiple battery cells tightly combined to form a battery module. The hot pressing temperature range is controlled at 65°C to 85°C, and the hot pressing pressure range is 1T to 6T; After the battery module is hot-pressed, copper-cobalt welding is performed on the positive and negative electrodes of the battery cell unit to form a complete current path inside to ensure uniform current transmission; Step 5: Test the battery module for charging and discharging. The specific steps of the charging test are as follows: connect the battery module to a dedicated charging device and set the constant current and constant voltage charging mode; monitor and record the changes in the charging current, voltage, and temperature parameters of the battery module over time; when the battery module reaches a fully charged state, calculate and record its charging capacity, charging efficiency, and charging time; Evaluation criteria: Charging rate: The battery module should reach the predetermined charging capacity within the specified time; Charging efficiency: The charging efficiency of the battery module should meet the design standard to reduce energy loss; Safety: During the charging process, the battery module should not have safety hazards such as overheating and short circuit; The specific steps of the discharge test are as follows: connect the battery module to a dedicated discharge device and set the constant current discharge mode; monitor and record the changes in the discharge current, voltage, and temperature parameters of the battery module over time; when the battery module reaches the discharge termination voltage, calculate and record its discharge capacity and discharge time; Evaluation criteria: Discharge capacity: The discharge capacity of the battery module should meet the design standard and meet the actual use requirements; Discharge rate: Within the specified time, the battery module should be able to discharge stably without a sharp drop; Discharge voltage: The discharge voltage of the battery module should remain stable and meet the design requirements; Cycle life test: Perform cycle charge and discharge test on battery modules. After each cycle, record the charge and discharge capacity and internal resistance parameters of the battery. Based on the test data, draw the charge and discharge capacity retention rate and internal resistance change curve, and evaluate the cycle life of the battery through data analysis. Safety testing: Test the battery modules under extreme conditions of overcharge, over discharge, short circuit, high temperature and low temperature; monitor and record the temperature change, voltage change and key gas emission parameters of the battery modules during the test; check whether the battery modules have thermal runaway, combustion and explosion safety hazards under extreme conditions; Evaluation criteria: Safety: The battery module should maintain good safety performance under extreme conditions, without thermal runaway, combustion, or explosion hazards; Protection performance: The battery module should be equipped with a complete protection mechanism to ensure that the battery module can operate safely under various conditions; Step 6: Place the battery module in a square aluminum shell, and use the liquid injection equipment to inject the fluorine-containing additive-modified electrolyte into the battery module in the aluminum shell. After the electrolyte injection is completed, add an appropriate amount of degassing agent to the electrolyte to reduce the gas generation in the electrolyte, thereby reducing the risk of electrolyte overflow. Finally, use the welding sealing process and equipment to seal the aluminum shell.
Citation Information
Patent Citations
Method for synthesizing fluorinated ethylene carbonate
CN101676282A
Lithium ion battery adopting lithium-rich manganese-based material as positive electrode and preparation method of lithium ion battery
CN103560250A
Method for producing silicon-carbon composite negative electrode material of lithium ion battery
CN103633307A
Porous state polymer lithium-ion battery and preparing method thereof
CN106410211A
Preparation method of fluoroethylene carbonate
CN108033943A