Battery separator filling conditioner and preparation method thereof
By using a combination of base oil composition, polymethacrylate PMA and antioxidant in the battery separator fill oil, the dark color of the separator oil, insufficient antioxidant performance and other performance problems in the prior art were solved, and the separator oil in the prior art was prepared. The battery separator filled with conditioner with excellent performance can meet the color, porosity, pore size and resistivity requirements of the separator and reduce production costs.
Patent Information
- Application Number
- CN202410866811.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-01
AI Technical Summary
The existing battery separator filling oil has dark color, insufficient antioxidant performance, many low components, large high temperature performance, poor operating environment, difficult bubble extrusion, high sulfur content, and poor material compatibility, resulting in the color of the separator , porosity, pore size, and resistance performance do not meet the requirements, and the motor discharge during use causes the formation of flocs on the surface of the electrolyte.
Adsorption by stirring, molecular distillation and activated carbon by using base oil composition, decoagulant (polymethacrylate PMA) and antioxidant (3,5-di-tert-butyl-4-hydroxyphenylpropionate). The battery separator filling conditioning agent is prepared through precision filtration process, and the composition ratio is 98-100 parts of base oil composition, 0.5-1.0 parts of polymethacrylate PMA, 1-2 parts of antioxidants, and 80 parts of paraffin-based neutral oil 90 parts, 10-20 parts of cycloalkyl neutral oil.
The prepared fill conditioner has a light appearance, moderate viscosity, high flash point, low sulfur content, good oxidation resistance and compatibility to ensure the color, porosity, pore size, resistivity and sealability of the partition. , reducing volatile losses and floc formation, improving the aging resistance and operating safety of the partition, and high recycling rate, reducing production costs.
Smart Images

Figure CN118970370A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal cutting, and in particular to a battery separator filling conditioner and a preparation method thereof. Background Art
[0002] In recent years, the battery manufacturing industry has developed rapidly, the manufacturing level and production efficiency have been greatly improved and broken through, production automation has replaced traditional manufacturing processes, and product adaptability has gradually increased. With the rapid development of modern industry, especially the rapid development and application of automobiles, high-speed railways, aviation, medical equipment, etc., higher requirements are placed on the performance of batteries. At the same time, there are higher requirements and expectations for the technological development and innovation of the battery industry, as well as product iteration. The separator, known as the "third electrode", plays a vital role in the high performance of the battery. As a filling conditioner, one of the raw materials for manufacturing battery separators, it is mainly used in the processing of uniform mixing and extrusion molding. It plays a key role in the key properties of the separator material, such as color, porosity, puncture, lateral elongation, and anti-aging.
[0003] However, the ordinary separator filling oil and the separators produced in the prior art still generally have the following problems: (1) The separator oil is dark in color and cannot fully guarantee the color requirements of the separator; (2) The antioxidant performance is insufficient, which seriously affects the elongation and ductility of the separator; (3) The separator oil has too many low-component components, a large amount of high-temperature performance, a poor operating environment, and difficulty in squeezing out the bubbles of the separator; (4) The sulfur content of the separator oil is high, which not only cannot meet the requirements of the acid corrosion test, but also, during the use of the separator, the motor discharge causes the formation of flocs on the electrolyte surface; (5) The material compatibility is poor, and the solvent cannot wash out the excess filling oil, resulting in the porosity, pore size and resistance performance of the separator failing to meet the requirements. Summary of the invention
[0004] In view of the above technical problems in the related art, the present invention proposes a battery separator filling conditioner and a preparation method thereof, which can solve the above problems.
[0005] To achieve the above technical objectives, the technical solution of the present invention is implemented as follows: A battery separator filling conditioner and a preparation method thereof, wherein the main components include a base oil composition, a pour point depressant (polymethacrylate PMA) and an antioxidant (3,5-di-tert-butyl-4-hydroxybenzene propionate isooctyl ester); the base oil composition includes a paraffin-based neutral oil (SN-1) and a cycloalkyl neutral oil (DN-2); the components in the battery separator filling conditioner are calculated by mass as follows: 98-100 parts of the base oil composition, 0.5-1.0 parts of polymethacrylate PMA, and 1-2 parts of the antioxidant (3,5-di-tert-butyl-4-hydroxybenzene propionate); the components in the base oil composition are calculated by mass as follows: 80-90 parts of the paraffin-based neutral oil (SN-1), 10-20 parts of the cycloalkyl neutral oil (DN-2), and the sum of the two parts is 98-100 parts.
[0006] Furthermore, the preparation method comprises the following steps: S1: preparing a base oil composition A: placing a paraffin-based neutral oil (SN-1) and a cycloalkyl neutral oil (DN-2) in a container, and stirring the container until the temperature rises to a temperature range, thereby obtaining a base oil composition A; S2: preparing base oil composition B: subjecting base oil composition A to molecular distillation to obtain base oil composition B; S3 cooling: after the S2 process is completed, the base oil composition B is cooled in the container to a temperature range required by the S4 process; S4: preparing base oil composition C: subjecting base oil composition B to an activated carbon adsorption process to obtain base oil composition C; S5: Adding auxiliary materials: adding polymethacrylate PMA and 3,5-di-tert-butyl-4-hydroxyphenylpropionate isooctyl into a container in sequence, and mixing with the base oil composition C to form a final mixture D; S6 Filter out the finished product: Cool at room temperature and perform precision filtration on the final mixture D to obtain the battery separator filling conditioner.
[0007] Furthermore, in step S1, the components of the base oil composition are calculated by mass as follows: 80-90 parts of paraffin-based neutral oil (SN-1), 10-20 parts of cycloalkyl neutral oil (DN-2), and the sum of the two parts is 98-100 parts, the temperature range is 30°C-40°C, and the stirring time is 30 minutes.
[0008] Furthermore, in step S2, the components of the final mixture D are calculated by mass as follows: 98-100 parts of the base oil composition; 0.5-1.0 parts of polymethacrylate PMA; 1-2 parts of antioxidant (3,5-di-tert-butyl-4-hydroxyphenylpropionate), and the temperature of the molecular distillation process equipment is 210°C-220°C.
[0009] Furthermore, in step S3, the base oil composition B is cooled in a range of 45°C to 55°C.
[0010] Furthermore, in step S4, the activated carbon adsorption process processes 5-6 KL / h.
[0011] Furthermore, in step S5, the stirring time is 60 minutes.
[0012] Furthermore, in step S6, the precision of the fine filtration is no more than 1 um.
[0013] Furthermore, the container is a normal pressure blending kettle.
[0014] Furthermore, the cooling temperature ranges from 35°C to 45°C.
[0015] Beneficial effects: The filling conditioner prepared in the present invention has a light appearance color, which meets the color requirements of the partition; the viscosity is moderate, the pour point is low, and it is convenient for mixing materials under low temperature environment conditions; the flash point is high, the volatilization loss is small, and the extrusion molding operation is safe; the sulfur content is extremely low, which largely prevents the formation of flocs due to the freeing of sulfur ions to the surface of the electrolyte during the discharge process; the lower aniline point and reasonable C-type distribution ensure that the filling conditioner has good compatibility and antioxidant ability; the filling conditioner has good antioxidant performance, which enhances the aging resistance of the partition to a certain extent; the appropriate solubility ability, while being washed out by the solvent, well controls the porosity, pore size, resistivity, flexibility, sealability, etc. of the partition; the recycled conditioner has high utilization rate, less waste, and significant cost reduction and efficiency improvement. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] The present invention is further described in detail below with reference to the accompanying drawings.
[0018] Figure 1 This is a data table of various indicators of the battery separator filling conditioner prepared in Example 1; Figure 2 This is a data table of various indicators of the battery separator filling conditioner prepared in Example 2; Figure 3 This is a data table of various indicators of the battery separator filling conditioner prepared in Example 3. DETAILED DESCRIPTION
[0019] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the battery separator filling conditioner and the preparation method thereof will be further described below in conjunction with the accompanying drawings and through specific implementation methods.
[0020] A battery separator filling conditioner and a preparation method thereof, wherein the main components include a base oil composition, a pour point depressant (polymethacrylate PMA) and an antioxidant (3,5-di-tert-butyl-4-hydroxybenzene propionate isooctyl ester); the base oil composition includes a paraffin-based neutral oil (SN-1) and a cycloalkyl neutral oil (DN-2); the components in the battery separator filling conditioner are calculated by mass as follows: 98-100 parts of the base oil composition, 0.5-1.0 parts of polymethacrylate PMA, and 1-2 parts of the antioxidant (3,5-di-tert-butyl-4-hydroxybenzene propionate); the components in the base oil composition are calculated by mass as follows: 80-90 parts of the paraffin-based neutral oil (SN-1), 10-20 parts of the cycloalkyl neutral oil (DN-2), and the sum of the two parts is 98-100 parts.
[0021] The above-mentioned preparation method comprises the following steps: S1: preparing a base oil composition A: placing a paraffin-based neutral oil (SN-1) and a cycloalkyl neutral oil (DN-2) in a container, stirring the container until the temperature rises to a temperature range, and obtaining a base oil composition A; S2: preparing base oil composition B: subjecting base oil composition A to molecular distillation to obtain base oil composition B; S3 cooling: after the S2 process is completed, the base oil composition B is cooled in the container to a temperature range required by the S4 process; S4: preparing base oil composition C: subjecting base oil composition B to an activated carbon adsorption process to obtain base oil composition C; S5: Adding auxiliary materials: adding polymethacrylate PMA and 3,5-di-tert-butyl-4-hydroxyphenylpropionate isooctyl into a container in sequence, and mixing with the base oil composition C to form a final mixture D; S6 Filter out the finished product: cool at room temperature, and perform precision filtration on the final mixture D to obtain the battery separator filling conditioner.
[0022] In the above step S1, the components of the base oil composition are calculated by mass as follows: 80-90 parts of paraffin-based neutral oil (SN-1), 10-20 parts of cycloalkyl neutral oil (DN-2), and the sum of the two parts is 98-100 parts; the temperature range is 30°C-40°C, and the stirring time is 30 minutes.
[0023] In the above step S2, the components of the final mixture D are calculated by mass as follows: 98-100 parts of the base oil composition; 0.5-1.0 parts of polymethacrylate PMA; 1-2 parts of antioxidant (3,5-di-tert-butyl-4-hydroxyphenylpropionate); and the temperature of the molecular distillation process equipment is 210°C-220°C.
[0024] In the above step S3, the base oil composition B is cooled in the range of 45°C to 55°C.
[0025] In the above-mentioned step S4, the activated carbon adsorption process processes 5-6 KL / h.
[0026] In the above step S5, the stirring time is 60 minutes.
[0027] In the above-mentioned step S6, the precision of the fine filtration is no more than 1 um.
[0028] The above-mentioned container is a normal pressure blending kettle.
[0029] The above cooling temperature ranges from 35°C to 45°C.
[0030] The technical solution and technical effects of the present invention will be further described below in conjunction with specific embodiments.
[0031] Example 1 This embodiment provides a method for preparing a battery separator filling conditioner: (1) 85 parts of paraffin-based neutral oil (SN-1) and 10 parts of cycloalkyl neutral oil (DN-2) were placed in a blending kettle, heated to 30°C-40°C with stirring, and stirred for 30 minutes to obtain a base oil composition A; (2) subjecting the base oil composition A to molecular distillation at a process temperature of 210° C. to 220° C. to obtain a base oil composition B; (3) cooling the base oil composition B to 45° C. to 55° C. and treating it with activated carbon adsorption to obtain a base oil composition C; (4) 0.5 parts of polymethacrylate PMA and 1.0 parts of 3,5-di-tert-butyl-4-hydroxyphenylpropionate are added to the final base oil composition C in sequence, and the mixture is stirred for 60 minutes. The mixture is cooled to 35°C-45°C and finely filtered with a filtration accuracy of 1 μm to obtain a battery separator filling conditioner prepared by a special process.
[0032] Example 2 This embodiment provides a method for preparing a battery separator filling conditioner: (1) 88 parts of paraffin-based neutral oil (SN-1) and 15 parts of cycloalkyl neutral oil (DN-2) were placed in a blending kettle, heated to 30°C-40°C with stirring, and stirred for 30 minutes to obtain a base oil composition A; (2) subjecting the base oil composition A to molecular distillation at a process temperature of 210° C. to 220° C. to obtain a base oil composition B; (3) cooling the base oil composition B to 45° C. to 55° C. and treating it with activated carbon adsorption to obtain a base oil composition C; (4) 0.6 parts of polymethacrylate PMA and 1.2 parts of 3,5-di-tert-butyl-4-hydroxyphenylpropionate are added to the final base oil composition C in sequence, and the mixture is stirred for 60 minutes. The mixture is cooled to 35°C-45°C and finely filtered with a filtration accuracy of 1 μm to obtain a battery separator filling conditioner prepared by a special process.
[0033] Example 3 This embodiment provides a method for preparing a battery separator filling conditioner: (1) 90 parts of paraffin-based neutral oil (SN-1) and 18 parts of cycloalkyl neutral oil (DN-2) were placed in a blending kettle, heated to 30°C-40°C with stirring, and stirred for 30 minutes to obtain a base oil composition A; (2) subjecting the base oil composition A to molecular distillation at a process temperature of 210° C. to 220° C. to obtain a base oil composition B; (3) cooling the base oil composition B to 45° C. to 55° C. and treating it with activated carbon adsorption to obtain a base oil composition C; (4) 0.5 parts of polymethacrylate PMA and 1.3 parts of 3,5-di-tert-butyl-4-hydroxyphenylpropionate are added to the final base oil composition C in sequence, and the mixture is stirred for 60 minutes. The mixture is cooled to 35°C-45°C and finely filtered with a filtration accuracy of 1 μm to obtain a battery separator filling conditioner prepared by a special process.
[0034] The detection of various indicators of the product of the embodiment is shown in the figure. Combining the above embodiments and test results, it can be seen that through the above technical scheme of the present invention, compared with the prior art, the battery separator filling conditioner prepared by the special process provided by the present invention and the battery separator material processed and manufactured using the same have the following characteristics and performance advantages: the filling conditioner has a light appearance color to ensure the color requirements of the separator; moderate viscosity and low pour point are convenient for mixing materials under low temperature conditions; high flash point, less volatilization loss, and safe extrusion molding operation; extremely low sulfur content, to a large extent, prevents the formation of flocs due to the freeing of sulfur ions to the surface of the electrolyte during the discharge process; low aniline point and reasonable C-type distribution ensure that the filling conditioner has good compatibility and antioxidant ability; the filling conditioner has good antioxidant performance, which enhances the aging resistance of the separator to a certain extent; suitable solubility, while being washed out by the solvent, it well controls the porosity, pore size, resistivity, flexibility, sealability, etc. of the separator; the recycled conditioner has high utilization rate, less waste, and significant cost reduction and efficiency improvement. This will overcome the shortcomings of traditional technology, achieve product iteration, replace imported products of the same type, and fill the gap in special conditioners for battery separators in China.
[0035] Obviously, the above-described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments, and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field should be included in the protection scope of the present invention.
Claims
1. A battery separator filling conditioner and a preparation method thereof, characterized in that: Its main components include a base oil composition, a pour point depressant (polymethacrylate PMA) and an antioxidant (3,5-di-tert-butyl-4-hydroxybenzene propionate 2-octyl ester); the base oil composition includes a paraffin-based neutral oil (SN-1) and a cycloalkyl neutral oil (DN-2); the components of the battery separator filling conditioner are calculated by weight as follows: 98-100 parts of the base oil composition, 0.5-1.0 parts of polymethacrylate PMA, and 1-2 parts of the antioxidant (3,5-di-tert-butyl-4-hydroxybenzene propionate); the components of the base oil composition are calculated by weight as follows: 80-90 parts of the paraffin-based neutral oil (SN-1), 10-20 parts of the cycloalkyl neutral oil (DN-2), and the total of the two parts is 98-100 parts.
2. A battery separator filling conditioner and a preparation method thereof according to claim 1, characterized in that: The preparation method comprises the following steps: S1: preparing a base oil composition A: placing a paraffin-based neutral oil (SN-1) and a cycloalkyl neutral oil (DN-2) in a container, stirring the container until the temperature rises to a temperature range, and obtaining a base oil composition A; S2: preparing base oil composition B: subjecting base oil composition A to molecular distillation to obtain base oil composition B; S3 cooling: after the S2 process is completed, the base oil composition B is cooled in the container to a temperature range required by the S4 process; S4: preparing base oil composition C: subjecting base oil composition B to an activated carbon adsorption process to obtain base oil composition C; S5: Adding auxiliary materials: adding polymethacrylate PMA and 3,5-di-tert-butyl-4-hydroxyphenylpropionate isooctyl into a container in sequence, and mixing with the base oil composition C to form a final mixture D; S6 Filter out the finished product: cool at room temperature, and perform precision filtration on the final mixture D to obtain the battery separator filling conditioner.
3. A battery separator filling conditioner and a preparation method thereof according to claim 2, characterized in that: In the step S1, the components of the base oil composition are calculated by mass as follows: 80-90 parts of paraffin-based neutral oil (SN-1), 10-20 parts of cycloalkyl neutral oil (DN-2), and the sum of the two parts is 98-100 parts. The temperature range is 30°C-40°C, and the stirring time is 30 minutes.
4. A battery separator filling conditioner and a preparation method thereof according to claim 2, characterized in that: In the step S2, the components of the final mixture D are calculated by mass as follows: 98-100 parts of the base oil composition; 0.5-1.0 parts of polymethacrylate PMA; 1-2 parts of antioxidant (3,5-di-tert-butyl-4-hydroxyphenylpropionate), and the temperature of the molecular distillation process equipment is 210° C.-220° C.
5. A battery separator filling conditioner and a preparation method thereof according to claim 2, characterized in that: In the step S3, the base oil composition B is cooled in a range of 45°C to 55°C.
6. A battery separator filling conditioner and a preparation method thereof according to claim 2, characterized in that: In step S4, the activated carbon adsorption process processes 5-6 KL / h.
7. A battery separator filling conditioner and a preparation method thereof according to claim 2, characterized in that: In step S5, the stirring time is 60 minutes.
8. A battery separator filling conditioner and a preparation method thereof according to claim 2, characterized in that: In step S6, the precision of the fine filtration is no more than 1 um.
9. A battery separator filling conditioner and a preparation method thereof according to claim 2, characterized in that: The container is a normal pressure blending kettle.
10. A battery separator filling conditioner and a preparation method thereof according to claim 2, characterized in that: The cooling temperature ranges from 35°C to 45°C.
Citation Information
Patent Citations
PE separator plate for lead acid battery and preparation method thereof
CN102244219A
High-porosity battery diaphragm and preparation method thereof
CN114069157A
PE partition plate of gel battery and preparation method of PE partition plate
CN117810645A
Separator for lead storage battery and lead storage battery comprising the same
JP2024080355A
Cited By
Filling conditioner for battery separator and preparation method thereof
CN120810179A