Method for producing exhaust gas purification catalyst

In the manufacturing method of the catalyst for exhaust gas purification, the design of the substrate and ventilation and drying technology are used to ensure that the catalyst layer is evenly distributed inside the partition wall, solving the problem of easy occlusion of the catalyst layer and increasing pressure loss, and achieving efficient exhaust gas purification.

CN118973709APending Publication Date: 2024-11-15CATALER CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202380024633.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-01
Filing Date
2023-02-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The catalyst layer of the existing wall flow type exhaust gas purification catalyst is easily blocked or narrowed inside the partition wall, resulting in an increase in pressure loss and difficult to evenly distribute, affecting purification performance.

Method used

A manufacturing method is adopted in which the base material has a first chamber with only one end opening and a second chamber with another end opening, and the catalyst layer forming material is ventilated and dried by an uncoated portion to ensure that the catalyst layer is inside the partition wall. The uniform distribution is reduced, and the viscosity and particle size of the material for forming the catalyst layer are preferred, as well as the ventilation speed and coating ratio are controlled to achieve uniformity of the catalyst layer.

Benefits of technology

Through this method, a catalyst layer with high thickness direction uniformity and efficient purification performance is produced, which reduces pressure loss and improves the exhaust gas purification efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973709A_ABST
    Figure CN118973709A_ABST
Patent Text Reader

Abstract

Provided is a method for producing an exhaust gas purification catalyst having a catalyst layer having high uniformity in the thickness direction of partition walls. This method for producing an exhaust gas purification catalyst comprises: a step for preparing a base material (10) having a wall flow structure, the base material (10) having a first cell having only one end open, a second cell having only the other end open, and a porous partition wall that partitions the first cell and the second cell; a catalyst layer forming material is supplied to the end of the first cell opening of the base material, and an uncoated portion of the catalyst layer forming material is formed on the end side of the second cell opening in the range of the partition wall facing the first cell in the direction of extension of the partition wall, and the catalyst layer is formed in the direction of extension of the partition wall such that the uncoated portion of the catalyst layer forming material is formed on the end side of the second cell opening in the range of the partition wall facing the first cell in the direction of extension of the partition wall. Coating the inside of the partition wall with a catalyst layer-forming material from the end of the first cell opening of the base material to a predetermined length; and drying the coated material for forming the catalyst layer by ventilating from the end of the second cell opening of the base material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a catalyst for purifying exhaust gas. In addition, this application claims priority based on Japanese Patent Application No. 2022-031196 filed on March 1, 2022, the entire contents of which are incorporated herein by reference. Background Art

[0002] Exhaust gas from internal combustion engines such as vehicle engines contains hydrocarbons (HC), carbon monoxide (CO), nitrogen oxides (NO x ) and other toxic exhaust gas components, particulate matter (PM: Particulate Matter), etc. In order to efficiently remove these exhaust gas components, a wall-flow type exhaust gas purification catalyst has been used.

[0003] The wall-flow type exhaust gas purification catalyst typically includes a substrate and a catalyst layer containing a catalyst capable of purifying exhaust gas components, wherein the substrate includes: an inlet chamber with only an end opening on the exhaust gas inlet side, an outlet chamber adjacent to the inlet chamber and only an end opening on the exhaust gas outlet side, and a porous partition wall (rib wall) separating the two chambers. The exhaust gas discharged from the internal combustion engine flows into the inlet chamber from the end of the exhaust gas inlet side, and flows out from the end of the exhaust gas outlet side of the adjacent outlet chamber through the pores of the porous partition wall. During this period, the exhaust gas can be purified (detoxified) by contacting the catalyst layer (such as catalyst metal).

[0004] The catalyst layer contributes to improving the exhaust gas purification performance and suppressing the increase of pressure loss by its composition and the location of the catalyst layer. For example, Patent Documents 1 and 2 disclose exhaust gas purification catalysts in which a catalyst layer is formed inside the partition wall (specifically, the wall surface of the pores of the partition wall), and the catalyst layer is segregated toward the specified small chamber side in the thickness direction of the partition wall. In addition, Patent Document 3 discloses a manufacturing technology for segregating the catalyst layer inside the partition wall toward the specified small chamber side.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2019 / 221214

[0008] Patent Document 2: International Publication No. 2019 / 221217

[0009] Patent Document 3: Japanese Patent Application Publication No. 2019-198837 Summary of the invention

[0010] However, when the catalyst layer is formed by segregating inside the partition wall, the pores of the partition wall of the catalyst layer are easily blocked or narrowed, so there is a tendency that the pressure loss is easy to increase. Therefore, from the viewpoint of suppressing the increase of the pressure loss, it is desired that the catalyst layer is formed more uniformly inside the partition wall.

[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing an exhaust gas-purifying catalyst having a catalyst layer having high uniformity in the thickness direction of the partition walls.

[0012] The present disclosure provides a method for manufacturing an exhaust gas purification catalyst that is disposed in an exhaust path of an internal combustion engine and purifies exhaust gas discharged from the internal combustion engine. The method for manufacturing an exhaust gas purification catalyst comprises: preparing a substrate having a wall flow structure having a first chamber with only one end opening, a second chamber with only the other end opening, and a porous partition wall separating the first chamber and the second chamber; supplying a catalyst layer forming material to the end of the opening of the first chamber of the substrate, so that an uncoated portion of the catalyst layer forming material is formed on the end side of the opening of the second chamber in the extension direction of the partition wall facing the first chamber, and applying the catalyst layer forming material to the inside of the partition wall from the end of the opening of the first chamber of the substrate to a predetermined length along the extension direction of the partition wall; and ventilating from the end of the opening of the second chamber of the substrate to dry the applied catalyst layer forming material.

[0013] According to the manufacturing method, ventilation is conducted from the end portion (opening portion of the second chamber) on the side of the uncoated portion where the catalyst layer forming material is not coated, and the coated catalyst layer forming material is dried. The dry wind introduced into the second chamber is branched into a flow path toward the inner side of the second chamber and a flow path through the uncoated portion and flowing into the first chamber. Thus, the coated catalyst layer forming material can be dried simultaneously from the surface connected to the first chamber and the surface connected to the second chamber. As a result, the segregation of the coated catalyst layer forming material can be suppressed, and an exhaust gas purification catalyst having a catalyst layer with high uniformity in the thickness direction of the partition wall can be manufactured.

[0014] In addition, in a preferred embodiment of the method for producing an exhaust gas purification catalyst disclosed herein, in the extension direction of the partition wall, the ratio of the length of the catalyst layer forming material applied to the partition wall is less than 90% of the total length of the partition wall. With this structure, the ratio of the length of the uncoated portion is high, so that the drying air can easily pass through the uncoated portion, and the coated catalyst layer forming material can be dried more uniformly. As a result, an exhaust gas purification catalyst having a catalyst layer with higher uniformity in the thickness direction of the partition wall can be manufactured.

[0015] In a preferred embodiment of the method for producing an exhaust gas purifying catalyst disclosed herein, the measurement temperature is 25° C. and the shear rate is 4 s -1 The viscosity of the catalyst layer forming material is less than 1500 mPa·s. This makes it easy to apply the catalyst layer forming material.

[0016] In addition, in a preferred embodiment of the exhaust gas purification catalyst manufacturing method disclosed herein, when the average pore size of the partition wall is set to X μm, the average particle size of the particles contained in the catalyst layer forming material based on the laser diffraction scattering method is 0.15X μm or less. Thus, it is easy to apply the catalyst layer forming material to the inside of the partition wall.

[0017] In a preferred embodiment of the exhaust gas purifying catalyst production method disclosed herein, the ventilation velocity is 10 m / s or less. This makes it possible to produce an exhaust gas purifying catalyst having a catalyst layer with higher uniformity in the thickness direction of the partition walls.

[0018] Furthermore, in one embodiment of the exhaust gas-purifying catalyst production method disclosed herein, the catalyst layer-forming material contains a catalyst metal, and the catalyst metal may contain at least any one of Pt, Pd, and Rh. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram showing the structure of an exhaust gas purification device and its surroundings.

[0020] Figure 2 It is a perspective view schematically showing an exhaust gas-purifying catalyst according to an embodiment.

[0021] Figure 3 It is a diagram schematically showing a cross section of an exhaust gas purifying catalyst according to an embodiment along the extending direction of the partition walls.

[0022] Figure 4 This is a schematic diagram for explaining an example of a conventional exhaust gas purifying catalyst production technology.

[0023] Figure 5 This is a schematic diagram for explaining the production technology of the exhaust gas-purifying catalyst disclosed herein.

[0024] Figure 6 It is a diagram schematically showing a cross section of an exhaust gas purifying catalyst according to a second embodiment, taken along the extending direction of the partition walls.

[0025] Figure 7 It is a diagram schematically showing a cross section of an exhaust gas purifying catalyst according to a third embodiment, taken along the extending direction of the partition walls.

[0026] Figure 8 This is a SEM image of the partition wall of the exhaust gas-purifying catalyst in Example 1.

[0027] Fig. 9 This is a SEM image of the partition wall of the exhaust gas-purifying catalyst in Example 2.

[0028] Fig.10 This is a graph showing the average neck diameter of the partition walls of the exhaust gas purifying catalysts in Examples 1 and 2.

[0029] Fig.11 This is a graph showing the pressure loss increase rate of the exhaust gas purifying catalyst in Examples 1 and 2. DETAILED DESCRIPTION

[0030] Hereinafter, the technology disclosed herein will be described with appropriate reference to the accompanying drawings. In addition, matters necessary for the implementation of the present technology other than those specifically mentioned in this specification can be grasped as design matters based on the prior art in the field by those skilled in the art. The present technology can be implemented based on the contents disclosed in this specification and the technical knowledge in the field. In addition, in this specification, when it comes to a numerical range recorded as A to B (here, A and B are arbitrary numerical values), it means above A and below B, including a range larger than A and smaller than B.

[0031] Figure 1 Schematic diagram showing the structure of an exhaust gas purification device 1 and its periphery. The exhaust gas purification device 1 is arranged in the exhaust system of an internal combustion engine (engine) 2. A mixed gas containing oxygen and fuel gas is supplied to the internal combustion engine 2. The internal combustion engine 2 burns the mixed gas, and the combustion energy is converted into mechanical energy. At this time, the burned mixed gas becomes exhaust gas and is discharged to the exhaust system. The internal combustion engine 2 of the present embodiment is mainly composed of a gasoline engine of an automobile. However, the internal combustion engine 2 may also be an engine other than a gasoline engine (for example, a diesel engine, etc.).

[0032] The exhaust gas purification device 1 purifies harmful components contained in the exhaust gas discharged from the internal combustion engine 2, such as hydrocarbons (HC), carbon monoxide (CO), nitrogen oxides (NO x ), and captures particulate matter (PM) contained in the exhaust gas. The exhaust gas purification device 1 includes an exhaust path (exhaust manifold 3 and exhaust pipe 4) connecting the internal combustion engine 2 and the exhaust system, an engine control unit (ECU) 7, a catalyst unit 5 and a filter unit 6. In addition, the arrows in the figure indicate the flow direction of the exhaust gas.

[0033] The exhaust path of this embodiment is composed of an exhaust manifold 3 and an exhaust pipe 4. An exhaust port (not shown) communicating with the exhaust system of the internal combustion engine 2 is connected to one end of the exhaust manifold 3. The other end of the exhaust manifold 3 is connected to the exhaust pipe 4.

[0034] A catalyst unit 5 and a filter unit 6 are arranged in the middle of the exhaust pipe 4. In the present embodiment, a gasoline particulate filter (GPF) is arranged in the filter unit 6. However, the filter unit 6 can adopt a filter other than the GPF according to the structure of the internal combustion engine 2, for example, a diesel particulate filter (DPF). The exhaust gas purification catalyst disclosed herein can be used as the filter unit 6, for example. The structure of the catalyst unit 5 can be the same as in the past and is not particularly limited. The catalyst unit 5 can be, for example, a conventionally known oxidation catalyst (oxidation catalyst DOC), a three-way catalyst, a NO x Adsorption reduction catalyst (LNT), etc. The catalyst unit 5 may include, for example, a carrier and a precious metal supported by the carrier, such as rhodium (Rh), palladium (Pd), platinum (Pt), etc. In addition, the catalyst unit 5 is not necessary and can be omitted. In addition, other catalysts can also be further configured on the downstream side of the filter unit 6.

[0035] ECU7 controls the exhaust gas purification device 1 and the internal combustion engine 2. The structure of ECU7 can be the same as before and is not particularly limited. ECU7 is, for example, a digital computer. An input port (not shown) is provided in ECU7. ECU7 is electrically connected to sensors (for example, pressure sensor 8) provided in various parts of the exhaust gas purification device 1 and the internal combustion engine 2. Thus, the information detected by each sensor is transmitted to ECU7 via the above-mentioned input port as an electrical signal. In addition, an output port (not shown) is provided in ECU7. ECU7 sends a control signal via the output port. ECU7 controls the start and stop of the exhaust gas purification device 1, for example, according to the amount of exhaust gas discharged from the internal combustion engine 2.

[0036] Hereinafter, one embodiment of the exhaust gas-purifying catalyst disclosed herein will be described in detail. Figure 2 It is a perspective view schematically showing an exhaust gas-purifying catalyst according to an embodiment. Figure 3 The figure schematically shows a cross section of an exhaust gas purification catalyst according to one embodiment along the extension direction of the partition wall. In addition, the symbol A in each figure referred to in this specification represents the "flow direction of the exhaust gas". In addition, the symbol X represents the "extension direction of the partition wall", and the symbol Y represents the "thickness direction of the partition wall".

[0037] like Figure 2 and 3 As shown, in this embodiment, the exhaust gas purifying catalyst 100 includes a substrate 10, a first catalyst layer 20, and a second catalyst layer 30. The exhaust gas purifying catalyst 100 has a function of purifying exhaust gas components contained in the exhaust gas and also has a function of capturing particulate matter (PM) contained in the exhaust gas.

[0038] The substrate 10 constitutes the skeleton of the exhaust gas purifying catalyst 100. Figure 2As shown, in this embodiment, a cylindrical substrate 10 extending along the exhaust gas flow direction A is used. In addition, the outer shape of the substrate is not limited to a cylindrical shape, and may be an elliptical cylindrical shape, a polygonal cylindrical shape, etc. In addition, the total length and capacity of the substrate 10 are not particularly limited, and can be adjusted according to the internal combustion engine 2 (see Figure 1 ) performance, the size of the exhaust pipe 4, etc. The substrate 10 can be appropriately changed according to the performance of the exhaust gas purifying catalyst, the size of the exhaust pipe 4, etc. In addition, the substrate 10 can use a conventionally known material that can be used for the substrate of the exhaust gas purifying catalyst without particular limitation. As an example of the material of the substrate 10, a highly heat-resistant material represented by ceramics such as cordierite, silicon carbide (SiC), and aluminum titanate, and alloys such as stainless steel can be cited. For example, cordierite has excellent durability against thermal shock, and therefore, it can be particularly suitably used as a material for the substrate of a particulate filter (GPF) for a gasoline engine that is easily supplied with high-temperature exhaust gas.

[0039] The substrate 10 in this embodiment is a wall flow type honeycomb substrate. In this specification, the honeycomb structure refers to a structure composed of a plurality of small chambers (hollow parts (cells)) that serve as flow paths for fluids (such as exhaust gas). Figure 2 and 3 As shown, the substrate 10 includes a first chamber 12 having only one end 10b open, a second chamber 14 having only the other end 10a open, and a porous partition wall 16 separating the first chamber 12 and the second chamber 14. In the present embodiment, the first chamber 12 is an outlet chamber having only the end 10b on the exhaust gas outflow side open. In addition, the second chamber 14 is an inlet chamber having only the end 10a on the exhaust gas inflow side open. The first chamber 12 is a gas flow path in which the end 10a on the exhaust gas inflow side is closed by a sealing portion 12a, and the end 10b on the exhaust gas outflow side is open. The second chamber 14 is a gas flow path in which the end 10a on the exhaust gas inflow side is open, and the end 10b on the exhaust gas outflow side is closed by a sealing portion 14a. In addition, the partition wall 16 is a partition having a plurality of pores through which the exhaust gas can pass. The partition wall 16 has a plurality of pores that connect the first chamber 12 and the second chamber 14. In the exhaust gas purifying catalyst 100 according to the present embodiment, the shape of the first cell 12 (the second cell 14) in the cross section of the partition wall 16 perpendicular to the extending direction X is a square (see Figure 2 ). However, the shape of the inlet chamber (outlet chamber) of the cross section of the partition wall 16 perpendicular to the extension direction X is not limited to a square, and various shapes can be adopted. For example, it can also be a rectangular shape such as a parallelogram, a rectangle, a trapezoid, a triangle, other polygonal shapes (such as a hexagon, an octagon), a circle, and other various geometric shapes.

[0040] The partition wall 16 of the substrate 10 is preferably formed in consideration of PM collection performance, pressure loss suppression performance, etc. For example, the thickness of the partition wall 16 is preferably about 100 μm to 350 μm. Furthermore, the porosity of the partition wall 16 is preferably about 20 volume % to 70 volume %, more preferably 50 volume % to 70 volume %. The porosity can be measured by mercury penetration.

[0041] From the perspective of fully ensuring the air permeability of the partition wall 16 and suppressing the increase in pressure loss, the average pore diameter of the pores of the partition wall 16 is preferably 8 μm or more, more preferably 12 μm or more, and further preferably 15 μm or more. On the other hand, from the perspective of ensuring appropriate PM capture performance, the upper limit of the average pore diameter of the pores of the partition wall 16 is preferably 30 μm or less, more preferably 25 μm or less, and further preferably 20 μm or less. In addition, the average pore diameter is a numerical range at the portion of the partition wall 16 that does not have a catalyst layer (including the case of the partition wall before the catalyst layer is formed). In addition, the average pore diameter is a value measured by the bubble point method using a micropore analyzer, which refers to the average pore diameter of the through holes.

[0042] like Figure 3 As shown, the first catalyst layer 20 is formed with a predetermined length in the area inside the partition wall 16 that is at least connected to the second chamber 14, from the end 10b on the exhaust gas outflow side along the extension direction of the partition wall 16. In addition, in this specification, "the catalyst layer is formed inside the partition wall" means that the catalyst layer mainly exists inside the partition wall (specifically, the wall surface of the pores of the partition wall can be listed), rather than outside the partition wall (typically, the surface can be listed). More specifically, for example, it refers to the overall length L of the partition wall 16 in the extension direction X in the cross section of the partition wall 16 where the first catalyst layer 20 is to be formed. w When the coating amount within the range of 1 / 10 of the length is taken as 100%, the coating amount present in the interior of the partition wall is typically 80% or more, for example, 85% or more, preferably 90% or more, further 95% or more, and especially substantially 100%. Therefore, it is obviously different from the situation that, for example, when a catalyst layer is to be arranged on the surface of the partition wall, a part of the catalyst layer accidentally penetrates into the interior of the partition wall.

[0043] The distribution of the amount of the catalyst layer applied (the ratio of the amount of the catalyst layer applied in a predetermined area) can be measured by using the number of pixels of the catalyst layer forming portion in an electron microscope observation image of a cross section of the partition wall 16. Specifically, the measurement can be performed according to the following procedure.

[0044] (a) An exhaust gas purification catalyst to be inspected is decomposed, and a sample sheet in which a partition wall of a substrate is embedded with a resin is prepared.

[0045] (b) The sample piece is cut to expose the cross section of the partition wall. The exposed cross section of the partition wall is then observed using a scanning electron microscope (SEM) to obtain a cross-sectional SEM observation image (eg, a reflected electron image obtained at an observation magnification of 150 times).

[0046] (c) The cross-sectional SEM observation image is automatically binarized using two-dimensional image analysis software (eg, product name: ImageJ (registered trademark)) to obtain a binary image reflecting only the catalyst layer.

[0047] (d) Counting the "total number of pixels of the catalyst layer" in a predetermined area confirmed in the binary image. Then, the distribution of the catalyst layer can be measured based on the counted number of pixels.

[0048] In the thickness direction Y of the next door 16 perpendicular to the extension direction X of the next door 16, the first catalyst layer 20 is formed throughout the thickness of the next door 16. In addition, the first catalyst layer 20 is formed with high uniformity along the thickness direction of the next door 16. Specifically, when the two regions obtained when the next door 16 is divided into two equal parts along the thickness direction Y are respectively used as the first region (for example, the region on the side of the first chamber 12 in the figure) and the second region (for example, the region on the side of the second chamber 14 in the figure), the coating amount of the first catalyst layer 20 contained in the first region is divided by the coating amount of the first catalyst layer 20 contained in the second region. The value obtained is, for example, 0.33 or more and 3 or less, preferably 0.33 or more and 0.5 or less, or more than 2 and less than 3, and more preferably 0.5 or more and less than 2. Thus, it is possible to prevent the pores of the next door 16 from being locally narrowed or blocked due to the catalyst layer, and thus it is possible to suppress the increase in pressure loss. In the present specification, the value obtained by dividing the coating amount of the first catalyst layer 20 contained in the first region by the coating amount of the first catalyst layer 20 contained in the second region is calculated using the number of pixels of the catalyst layer formation portion in the cross-sectional SEM observation image of the partition wall (refer to the above method).

[0049] The first catalyst layer 20 is formed from the end portion 10b of the substrate 10 in the extending direction X of the partition walls 16. w From the viewpoint of reducing pressure loss, the length (average length) L1 of the first catalyst layer 20 in the extension direction X is, for example, the total length L of the partition wall 16. w Less than 95% (i.e. L1≤0.95L w ), can be 90% or less, 80% or less, 70% or less, or 60% or less. In addition, from the perspective of improving purification performance, the length L1 of the first catalyst layer 20 is, for example, the total length L1 of the partition wall 16. w More than 10% (i.e. L1 ≥ 0.1L w), more preferably 30% or more, further preferably 50% or more.

[0050] Furthermore, the first catalyst layer 20 may contain a catalyst that functions as a catalyst capable of oxidizing or reducing at least one exhaust gas component. Examples of the catalyst include a three-way catalyst and an SCR catalyst.

[0051] As the catalyst metal used in the three-way catalyst, for example, metals belonging to the platinum group such as palladium (Pd), rhodium (Rh), platinum (Pt), ruthenium (Ru), osmium (Os), iridium (Ir) or other metals that act as oxidation or reduction catalysts can be listed. Among them, Pd and Pt have excellent purification performance (oxidation purification ability) of carbon monoxide and hydrocarbons, and Rh has excellent purification performance (reduction purification ability) of NOx, so they are particularly preferred catalyst metals as three-way catalysts. In addition, metals composed of barium (Ba), strontium (Sr) and other alkaline earth metals, alkali metals, transition metals, etc. can also be used as co-catalyst components. The average particle size of the catalyst metal based on electron microscope observation is preferably 0.5nm to 50nm, and can be more preferably 1nm to 20nm, but it is not particularly limited. The average particle size is the arithmetic average of the particle size (equivalent circle diameter) of at least 100 catalyst metal particles measured in the image observed by electron microscope observation.

[0052] In the first catalyst layer 20, the catalyst metal may be supported on a carrier. Examples of the carrier include aluminum oxide (Al2O3), cerium oxide (CeO2), zirconium dioxide (ZrO2), silicon dioxide (SiO2), titanium dioxide (TiO2), etc. In addition, rare earth metal oxides such as yttrium oxide (Y2O3), alkali metal oxides, alkaline earth metal oxides, etc. may be used. In addition, inorganic oxides (so-called OSC materials) having an oxygen storage capacity (OSC: oxygen storage capacity) that can absorb and release oxygen may be used. Examples of OSC materials include ceria-zirconium dioxide composite oxides (CZ or ZC composite oxides), etc. In addition, from the perspective of improving heat resistance, OSC materials such as ceria, ceria-zirconium dioxide composite oxides, etc., to which oxides containing, for example, yttrium (Y), lanthanum (La), niobium (Nb), praseodymium (Pr) or other rare earth elements are added in trace amounts, can be preferably used. In addition, one carrier may be used, or two or more carriers may be used in combination.

[0053] The shape (outer shape) of the above-mentioned carrier is not particularly limited, but from the viewpoint of being able to ensure a larger specific surface area, it is preferred to use a powdered material. For example, the average particle size of the carrier (average particle size based on the laser diffraction scattering method) is preferably, for example, less than 20 μm, typically less than 10 μm, for example, less than 7 μm. When the average particle size of the above-mentioned carrier is too large, there is a tendency for the dispersibility of the precious metal supported by the carrier to decrease, and the purification performance of the catalyst decreases, so it is not preferred. The above-mentioned average particle size can also be, for example, less than 5 μm, typically less than 3 μm. On the other hand, the smaller the average particle size of the carrier, the lower the heat resistance of the carrier itself composed of the carrier, and therefore, the heat resistance characteristics of the catalyst decrease, which is not preferred. Therefore, it is generally preferred to use a carrier with an average particle size of approximately 0.1 μm or more, for example, more than 0.5 μm. The amount of catalyst metal supported in the carrier is not particularly limited, but the amount of catalyst metal supported in the first catalyst layer 20 is preferably in the range of 0.01% to 10% by mass (e.g., 0.1% to 8% by mass, typically 0.2% to 5% by mass) relative to the total mass. When the amount of catalyst metal supported is too small, the catalyst activity obtained from the catalyst metal may not be sufficient. On the other hand, when the amount of catalyst metal supported is too large, the catalyst metal is prone to particle growth, which is also disadvantageous in terms of cost.

[0054] In this specification, the average particle size based on the laser diffraction and scattering method refers to the particle size (D) corresponding to 50% of the cumulative total from the microparticle side in the volume-based particle size distribution obtained by the particle size distribution measurement based on the laser diffraction and light scattering method. 50 Particle size, also called median particle size).

[0055] The method for supporting the catalyst metal particles on the carrier is not particularly limited, and can be prepared, for example, by impregnating the carrier with an aqueous solution containing a catalyst metal salt (eg, nitrate) or a catalyst metal complex (eg, tetraamine complex), followed by drying and calcining.

[0056] In addition, as the SCR catalyst exemplified as the catalyst that can be included in the first catalyst layer 20, for example, a zeolite catalyst and a vanadium catalyst can be listed. The SCR catalyst can purify nitrogen oxides (NOx) in the exhaust gas. As the zeolite catalyst, there is no particular limitation, and examples include β-type zeolite, silicoaluminophosphate (SAPO) zeolite, ZSM-5 zeolite, Cu-Y zeolite, etc. loaded with metal elements. For example, if the structure of the preferred zeolite is represented by the code specified by the International Zeolite Association (IZA: International Zeolite Association), AEI, AFT, AFX, AST, BEA, BEC, CHA, EAB, ETR, GME, ITE, KFI, LEV, THO, PAU, UFI, SAS, SAT, SAV can be listed. One of them can be used or two or more can be used in combination. As the metal element loaded by the above-mentioned zeolite, copper, iron, silver, etc. are exemplified. For example, it is particularly preferred to use SAPO zeolite loaded with copper and β-type zeolite loaded with iron.

[0057] The first catalyst layer 20 is formed inside the partition wall 16, and therefore, the average particle size of the particles (e.g., carrier particles of the supported catalyst) contained in the first catalyst layer 20 is smaller than the average pore size of the partition wall 16. When the average pore size of the partition wall 16 is X μm, the average particle size of the particles contained in the first catalyst layer 20 based on the laser diffraction scattering method is, for example, 0.15X μm or less, and can be preferably 0.10X μm or less, 0.07X μm or less. In addition, although not particularly limited, the average particle size can be, for example, 0.01X μm or more.

[0058] The coating density of the first catalyst layer 20 (i.e., the value obtained by dividing the mass of the first catalyst layer 20 by the volume of the length L1 portion of the substrate (including the overall gross volume of the volume of the cell passage)) is not particularly limited, but it is more appropriate to be approximately 350 g / L or less. From the viewpoint of reducing pressure loss, etc., the coating density of the first catalyst layer 20 is preferably 300 g / L or less, more preferably 250 g / L or less, and further preferably 200 g / L or less. In addition, the coating density of the first catalyst layer 20 can be, for example, 180 g / L or less, or 160 g / L or less. In addition, the lower limit of the coating density of the first catalyst layer 20 is not particularly limited, but from the viewpoint of improving purification performance, etc., it is preferably 30 g / L or more, more preferably 50 g / L or more, and further preferably 75 g / L or more. For example, the coating density of the first catalyst layer 20 is 90 g / L or more, and typically can be 100 g / L or more.

[0059] The average pore diameter (neck diameter) of the pores of the partition wall 16 at the portion where the first catalyst layer 20 is formed is not particularly limited, but from the viewpoint of reducing the increase in pressure loss, it is preferably 12 μm or more, and more preferably 13 μm or more. On the other hand, from the viewpoint of ensuring appropriate PM capture performance, the upper limit of the average pore diameter of the partition wall 16 at the portion where the first catalyst layer 20 is formed is preferably 20 μm or less, and more preferably 15 μm or less. In addition, the average pore diameter is a value measured by a bubble point method using a micropore analyzer, and refers to the average pore diameter of the through-holes.

[0060] In this embodiment, the second catalyst layer 30 is formed on the surface of the partition wall 16 on the side in contact with the second cell 14, extending from the end 10a of the substrate 10 along the extension direction X by a length L greater than the total length L of the partition wall 16. w However, the length (average length) L2 of the second catalyst layer 30 in the extension direction is not particularly limited. From the viewpoint of improving purification performance, the length L2 of the second catalyst layer 30 may be L w More than 10% (i.e. L2 ≥ 0.1L w ), 15% or more, 20% or more, 25% or more. In addition, from the viewpoint of reducing pressure loss, the length L2 of the second catalyst layer 30 may be, for example, the above L w Less than 60% (i.e. L2≤0.6L w ), 55% or less, 50% or less, 40% or less. In addition, the second catalyst layer 30 is a catalyst layer formed arbitrarily for the purpose of improving the exhaust gas purification performance, etc., and is not an essential structure.

[0061] The second catalyst layer 30 may have a portion (overlap portion) overlapping with the first catalyst layer 20 in the extending direction X of the partition walls 16. In other words, the following conditions may be met: w <L1+L2<2L w This can prevent the exhaust gas flowing into the exhaust gas purifying catalyst 100 from passing through the portion where the catalyst layer is not formed and being discharged in an unpurified state. The length of the overlapping portion is not particularly limited, but is, for example, the entire length L of the partition wall 16. w 2% to 60%, preferably 5% to 40%, more preferably 10% to 20%.

[0062] In the thickness direction Y orthogonal to the extension direction X, the thickness (average thickness) of the second catalyst layer 30 is not particularly limited, but is, for example, 5% or more of the thickness of the partition wall 16, preferably 8% or more, more preferably 10% or more, and further preferably 15% or more. When the thickness of the second catalyst layer 30 is within such a range, when the opening of the second chamber 14 is used as the exhaust gas inflow side, the intrusion of the exhaust gas into the partition wall 16 on the upstream side (or even the exhaust gas flow only through the second catalyst layer 30) can be suppressed, and the exhaust gas purification performance is improved. The upper limit of the thickness of the second catalyst layer 30 is not particularly limited, but from the viewpoint of reducing pressure loss, etc., it can be preferably 50% or less of the thickness of the partition wall 16, more preferably 30% or less, further preferably 25% or less, and particularly preferably 20% or less.

[0063] The components that the second catalyst layer 30 may contain (e.g., catalysts, co-catalysts, carriers, etc.) may be selected from the components exemplified as the components that the first catalyst layer 20 may contain. However, in order to form the second catalyst layer 30 on the surface of the partition wall 16, when the average pore size of the partition wall 16 is X μm, the average particle size of the particles contained in the second catalyst layer 30 based on the laser diffraction scattering method may be 0.3X μm or more, preferably 0.5X μm or more. In addition, the coating density of the second catalyst layer 30 is not particularly limited, and for example, it may be the same as the range exemplified as the coating density of the first catalyst layer 20.

[0064] The present disclosure provides a method for producing a catalyst for purifying exhaust gas. One embodiment of the method for producing a catalyst for purifying exhaust gas disclosed herein includes: a substrate preparation step of preparing a substrate; a coating step of coating a catalyst layer forming material on the substrate; and a drying step of drying the coated catalyst layer forming material. In addition, the method for producing a catalyst for purifying exhaust gas disclosed herein may include a firing step of firing the dried catalyst layer forming material to form a catalyst layer. In addition, the method for producing a catalyst for purifying exhaust gas disclosed herein may include a second catalyst layer forming step of forming another catalyst layer. Figure 4 This is a schematic diagram for explaining an example of a conventional exhaust gas purifying catalyst production technology. Figure 5 This is a schematic diagram for explaining the production technology of the exhaust gas-purifying catalyst disclosed herein.

[0065] In the substrate preparation step, the substrate 10 of the exhaust gas purifying catalyst 100 is prepared. That is, a substrate 10 of a wall flow structure is prepared, which has a first cell 12 opened only at one end 10b, a second cell 14 opened only at the other end 10a, and a porous partition wall 16 that separates the first cell 12 and the second cell 14. The details of the structure of the substrate 10 prepared here may be the same as the structure of the substrate 10 of the exhaust gas purifying catalyst 100 described above.

[0066] The coating process may include preparing a catalyst layer forming material. The catalyst layer forming material is a material for forming a catalyst layer inside the partition wall 16 of the substrate 10, and here, it is a material for forming the above-mentioned first catalyst layer 20. The catalyst layer forming material can typically be a slurry (including a paste or ink. The same below) that can be coated on the partition wall 16. The catalyst layer forming material at least includes a catalyst and a dispersion medium for dispersing the catalyst. As a catalyst, it can be the same as the catalyst that can be contained in the above-mentioned first catalyst layer 20, for example, it can be a catalyst metal.

[0067] As the dispersion medium, any dispersion medium used for the catalyst layer forming material can be used without particular limitation. For example, an aqueous solvent (for example, water, deionized water, pure water, etc.) can be preferably used.

[0068] Furthermore, the catalyst layer forming material may contain a thickener for adjusting the viscosity. Examples of the thickener include water-soluble organic polymers.

[0069] From the viewpoint of making it easy to apply the catalyst layer forming material to the inside of the partition wall, the viscosity of the catalyst layer forming material is, for example, less than 2000 mPa·s, preferably less than 1500 mPa·s, and more preferably less than 1000 mPa·s (for example, less than 1000 mPa·s). In addition, although not particularly limited, the viscosity of the catalyst layer forming material can be, for example, greater than 1 mPa·s, greater than 10 mPa·s, or greater than 50 mPa·s. In addition, in this specification, the viscosity of the catalyst layer forming material refers to the viscosity of the catalyst layer formed using an E-type viscometer (produced by Toki Sangyo Co., Ltd., TVE-35H), using a rotor type 1°34'×R24, at a measurement temperature of 25°C and a shear rate of 4s -1 The viscosity of the test piece is shown in Table 1.

[0070] From the viewpoint of making it easy to apply the catalyst layer forming material to the inside of the partition wall 16, when the average pore size of the partition wall 16 of the substrate 10 is set to Xμm, the average particle size of the particles contained in the catalyst layer forming material is, for example, less than 0.5Xμm, preferably less than 0.15Xμm, and more preferably less than 0.1Xμm. Thus, the particles contained in the catalyst layer forming material invade the pores of the partition wall 16, and a catalyst layer can be formed inside the partition wall 16. In addition, although not particularly limited, the average particle size of the particles contained in the catalyst layer forming material is, for example, more than 0.01Xμm, preferably more than 0.05Xμm, and more preferably more than 0.07Xμm. In addition, the average particle size refers to a value measured based on a laser diffraction scattering method.

[0071] As a coating method for the catalyst layer forming material, for example, a suction coating method can be cited. In the suction coating method, first, the catalyst layer forming material is supplied to the end 10b side of the opening of the first chamber 12 of the substrate 10. Then, suction is performed from the opposite side of the end 10b (that is, the end 10a of the opening of the second chamber 14) to suck the supplied catalyst forming material into the interior of the substrate 10. Thus, along the extension direction X of the partition wall 16, the catalyst layer forming material is coated on the interior of the partition wall 16 from the end 10b of the opening of the first chamber 12 of the substrate 10 to a prescribed length. At this time, it is adjusted so that the catalyst layer forming material is not coated to the entire length of the extension direction X of the partition wall 16. Thus, as Figure 4 and Figure 5 As shown, a coating portion 120 coated with a catalyst layer forming material and an uncoated portion 160 not coated with a catalyst layer forming material can be formed on the partition wall 16. In addition, at this time, the coating portion 120 is formed in a manner that at least a portion of the uncoated portion 160 is formed to exist in the range of the partition wall 16 facing the first chamber 12 in the extension direction X of the partition wall 16, that is. In other words, the coating portion 120 is formed in a manner that the uncoated portion 160 is formed to be longer than the sealing portion 12a in the extension direction X of the partition wall 16. In addition, the coating portion 120 is formed throughout the entire thickness direction Y of the partition wall 16.

[0072] In the drying step, the coated catalyst layer forming material is dried by ventilation from the end 10a of the second chamber 14 of the substrate 10. In other words, the coated portion 120 is dried by ventilation from the end of the substrate 10 where the uncoated portion 160 is formed.

[0073] like Figure 4As shown, in an example of the conventional manufacturing technology, the drying air F is ventilated from the opening of the first chamber 12 located at the end 10b of the substrate 10 to the interior of the first chamber 12. In other words, the drying air F is introduced from the end 10b of the substrate 10 on the side where the coating portion 120 is formed. Since the drying air F cannot pass through most of the wet portion (coating portion 120) of the partition wall 16, most of the drying air F introduced into the first chamber 12 flows toward the inner side (sealed portion 12a side) of the first chamber 12, passes through the uncoated portion 160 of the partition wall 16, and flows out from the opening of the second chamber 14. When the coating portion is dried by such a flow path of the drying air F, the drying of the surface of the coating portion 120 in contact with the first chamber 12 is significantly promoted. Thus, in the coating portion 120, the catalyst moves from the second chamber 14 side to the first chamber 12 side, and a catalyst unevenly existing portion 21 where the catalyst is unevenly existing is formed on the first chamber 12 side where drying is promoted, and a catalyst sparse portion 22 where the amount of catalyst is less than that of the catalyst unevenly existing portion 21 is formed on the second chamber 14 side. Although not particularly limited, the mechanism of such uneven existence of the catalyst is considered to be that the drying of the surface of the coating portion 120 on the first chamber 12 side is promoted, so that the catalyst on the second chamber 14 side is aggregated on the first chamber 12 side due to the capillary phenomenon.

[0074] On the other hand, Figure 5 As shown, in the technology disclosed herein, the drying wind F is ventilated from the opening of the second chamber 14 located at the end 10a of the substrate 10 (i.e., the side where the uncoated portion 160 is formed) to the interior of the second chamber 14. The drying wind F introduced into the second chamber 14 is branched into a flow path flowing to the inner side (sealed portion 14a side) of the second chamber 14 and a flow path flowing to the first chamber 12 through the uncoated portion 160 of the partition 16. Thus, the surface of the coating portion 120 in contact with the first chamber 12 and the surface in contact with the second chamber 14 can be efficiently dried at the same time. As a result, the entire coating portion 120 can be dried with high uniformity, so that the segregation of the catalyst contained in the coated catalyst layer forming material can be suppressed, and the first catalyst layer 20 with high uniformity in the thickness direction of the partition 16 can be formed.

[0075] The wind speed of the drying wind F is not particularly limited, but from the viewpoint of further suppressing the segregation of the catalyst, it is preferably 10 m / s or less, more preferably 8 m / s or less, and further preferably 6 m / s or less. In addition, from the viewpoint of increasing the drying speed, the wind speed of the drying wind F is, for example, 1 m / s or more, preferably 2 m / s or more. In addition, "m / s" means "m / second".

[0076] The temperature of the drying air F is not particularly limited, and is, for example, 50° C. to 200° C., and preferably 90° C. to 150° C. The drying time is not particularly limited, and drying can be performed in, for example, about 1 minute to 30 minutes.

[0077] The length of the coating portion 120 in the extension direction X of the partition wall 16 is equal to the length L1 of the first catalyst layer 20. That is, the length (average length) of the coating portion 120 in the extension direction X is, for example, the total length L1 of the partition wall 16. w The length of the coating portion 120 is preferably less than 95%, and may be preferably less than 90%, less than 80%, less than 70%, or less than 60%. The lower the length ratio of the coating portion 120, the higher the length ratio of the uncoated portion 160. Therefore, the drying air F is easy to pass through the uncoated portion 160, and the coating portion 120 can be dried more evenly. In addition, the length of the coating portion 120 is not particularly limited, and may be, for example, the total length L of the partition wall 16. w The content of the organic solvent is 10% or more, more preferably 30% or more, and further preferably 50% or more.

[0078] In the firing step, the dried coated catalyst layer forming material is fired to form a catalyst layer. The firing temperature is not particularly limited, and is, for example, 400° C. or higher, preferably 450° C. or higher, and more preferably 500° C. or higher. The upper limit of the firing temperature is not particularly limited, and is, for example, 1000° C. or lower, 800° C. or lower, or 600° C. or lower. The firing time is not particularly limited, and is, for example, 30 seconds to 5 hours, and is preferably 1 minute to 1 hour.

[0079] In the second catalyst layer forming step, the second catalyst layer 30 is formed at a position different from the first catalyst layer 20. The position where the second catalyst layer 30 is formed is not particularly limited, and can be appropriately changed according to the purpose and type of the exhaust gas purification catalyst to be manufactured. The method for forming the second catalyst layer 30 can be the same as the conventionally known method, and can be an air blowing method, a suction coating method, etc. In addition, the second catalyst layer forming step can be performed, for example, after the drying step, after the firing step, etc.

[0080] The production method disclosed herein may further include any other steps, for example, a third catalyst layer forming step, etc. The third catalyst layer may be formed, for example, at a position different from the first catalyst layer and the second catalyst layer.

[0081] In addition, Figure 3 In the illustrated embodiment, the second catalyst layer 30 is formed on the surface of the partition wall 16 , but the second catalyst layer may be formed inside the partition wall 16 , for example. Figure 6 FIG. 2 is a diagram schematically showing a cross section of an exhaust gas purifying catalyst according to a second embodiment along the extending direction of the partition walls. Figure 6 In the exhaust gas purifying catalyst 100A shown in FIG. 1 , the second catalyst layer 30A is formed inside the partition wall 16 by segregating toward the surface side of the partition wall 16 in contact with the second cell 14. Such a second catalyst layer 30A can be used, for example. Figure 4 It is formed by the conventional drying method described in .

[0082] In addition, the second catalyst layer can also be formed in the same manner as the first catalyst layer 20 by following the order of the above-mentioned coating step and drying step. Figure 7 FIG. 2 is a diagram schematically showing a cross section of an exhaust gas purifying catalyst according to a third embodiment along the extending direction of the partition walls. Figure 7 In the exhaust gas purification catalyst 100B shown, the second catalyst layer 30B is formed as a catalyst layer with high uniformity in the thickness direction Y relative to the partition wall 16, as in the first catalyst layer 20. As a method for forming such a second catalyst layer 30B, for example, first, from the opposite side of the side where the first catalyst layer 20 is formed (the end 10a of the substrate 10), the second catalyst layer forming material is applied to the inside of the partition wall 16 along the extension direction X of the partition wall 16 to a predetermined length. As a result, an uncoated portion on which the second catalyst layer forming material is not applied is formed on the side where the first catalyst layer 20 is formed (the end 10b side of the substrate 10). At this time, the uncoated portion may overlap with the position of the first catalyst layer 20. Next, a drying wind F is introduced from the uncoated portion side (the end 10b side of the substrate 10) to dry the portion coated with the second catalyst layer forming material. The drying air F can easily pass through the dry portion of the partition wall 16, so even if the uncoated portion overlaps with the first catalyst layer 20, the drying air F can easily pass through the partition wall 16. As a result, the surface of the coated portion of the second catalyst layer forming material that is in contact with the first cell 12 and the surface that is in contact with the second cell 14 are efficiently dried at the same time, and a second catalyst layer 30 with high uniformity in the thickness direction Y of the partition wall 16 can be formed.

[0083] As mentioned above, several embodiments of the technology disclosed herein have been described. However, the above embodiments are merely examples of the technology, and the technology is not limited to the above embodiments.

[0084] The exhaust gas purification catalyst disclosed herein can be used as a gasoline particulate filter (GPF), a diesel particulate filter (DPF), or the like.

[0085] Several embodiments related to the technology disclosed herein will be described below, but the technology disclosed herein is not intended to be limited to the technology described in these embodiments.

[0086] [Test 1]

[0087] <Preparation of base material>

[0088] As a substrate, a cylindrical honeycomb substrate of a wall-flow type with a substrate volume of 1.314 L and a length of 122 mm (made of cordierite, number of cells 300 cpsi, partition thickness 8 mils (1 mil is 1 / 1000 inch), average pore size of the partition 15 μm) was prepared. This substrate was used as the substrate of the exhaust gas purification catalyst in Examples 1 to 12. In addition, in order to illustrate the relationship between the average pore size of the substrate and the average particle size of the powder contained in the catalyst slurry, in the following description, the average pore size of the partition of the substrate is recorded as X μm.

[0089] <Manufacturing of Exhaust Gas Purifying Catalyst>

[0090] (Example 1)

[0091] A catalyst slurry as a material for forming a catalyst layer is prepared by mixing Rh nitrate solution, alumina powder and ion exchange water. The average particle size (D 50 The average particle size of the particles contained in the catalyst slurry was measured using a particle size distribution measuring device based on a laser diffraction scattering method. In addition, the viscosity of the catalyst slurry was 50 mPa·s. The viscosity of the catalyst slurry was measured at a temperature of 25°C and a shear rate of 4 s -1 Measured under the conditions of .

[0092] Next, the prepared catalyst slurry is supplied to the end of the outlet chamber side of the substrate, and the catalyst slurry is introduced into the interior of the partition wall by suction from the inlet chamber side. At this time, the entire length of the partition wall is taken as 100%, and the coating length of the catalyst slurry is made into an area from the end of the outlet chamber side to 60% of the length. Then, a 90°C wind is introduced from the inlet chamber (i.e., the side where the catalyst slurry is not coated) at a wind speed of 4m / s to dry the introduced catalyst slurry. Then, the exhaust gas purification catalyst of Example 1 is prepared by calcining at 500°C for 1 hour.

[0093] (Example 2)

[0094] An exhaust gas purifying catalyst of Example 2 was prepared in the same manner as in Example 1, except that the drying after the catalyst slurry was introduced was performed from the outlet-side chamber (ie, the catalyst slurry coating portion side).

[0095] <Evaluation of Catalyst Layer Distribution>

[0096] After the exhaust gas purifying catalyst was decomposed and the partition walls were taken out, the partition walls were embedded with a resin, and then the cross section of the partition walls was exposed and observed using a scanning electron microscope (TM4000Plus manufactured by Hitachi High-Tech Fielding) to obtain a SEM image. Figure 8 The SEM image of the partition wall of the exhaust gas purifying catalyst in Example 1 is shown. Fig. 9 FIG. 4 shows a SEM image of the partition wall of the exhaust gas purifying catalyst in Comparative Example 1. Figure 8 and 9 In the embodiment, the upper part of the next door is the outlet chamber side, and the lower part of the next door is the inlet chamber side. The upper and lower ends of the thickness direction of the next door are observed from the obtained SEM image to confirm the thickness of the next door. Further using two-dimensional image analysis software (product name: ImageJ (registered trademark)), the obtained SEM image is automatically binarized to obtain a binary image of only the reaction catalyst layer. In this binary image, the number of pixels of the catalyst layer in the region of the upper half of the thickness of the next door (the first region in the figure) and the number of pixels of the catalyst layer in the region of the lower half of the thickness of the next door (the second region in the figure) are measured. Then, the value (uniformity evaluation value) of "the number of pixels of the catalyst layer in the first region" divided by "the number of pixels of the catalyst layer in the second region" is obtained. If the value is 0.5 or more and 2 or less, it is judged as "◎ (Excellent)", if it is 0.33 or more and less than 0.5 or 2 or more and less than 3, it is judged as "○ (Good)", and if it is less than 0.33 or greater than 3, it is judged as "× (Not good)". The results are shown in Table 1.

[0097] <Pressure loss measurement>

[0098] The pressure loss of the exhaust gas purifying catalyst was measured using a pressure loss measuring device (manufactured by TSUKUBARIKASEIKI). Specifically, air was introduced into the inlet chamber of the exhaust gas purifying catalyst, and the exhaust volume of the air discharged from the outlet chamber was measured. 3 / s, the pressure difference between the air inlet side (inlet side) and the exhaust side (exit side) of the exhaust gas purification catalyst. In addition, for the substrate not coated with the catalyst slurry, the pressure difference between the air inlet side and the exhaust side is measured in the same way, and the pressure difference is taken as the pressure loss (pressure loss). Then, the pressure loss increase rate (%) caused by the formation of the catalyst layer is calculated by the following formula:

[0099] Pressure loss increase rate (%) = Pressure loss of exhaust gas purification catalyst (kPa) ÷ Pressure loss of substrate (kPa) × 100 - 100. Display the result in Fig.10 middle.

[0100] <Neck diameter measurement>

[0101] The catalyst layer forming part of the partition wall of the exhaust gas purification catalyst was taken out and the through pore diameter of the partition wall was measured. The measurement was carried out using a micropore analyzer (manufactured by PMI) based on the bubble point method. The through pore diameter measured in this way was taken as the average neck diameter. The results were displayed in Fig.11 middle.

[0102] [Table 1]

[0103] Table 1

[0104]

[0105] like Figure 8 As shown in Table 1, it can be seen that by introducing drying air from the uncoated portion side where the catalyst slurry is not applied to dry the portion as in Example 1, a catalyst layer with high uniformity in the thickness direction of the partition wall can be formed. Fig. 9 As shown in Table 1, it can be seen that when the drying air is introduced from the side where the catalyst slurry is applied (the side where the catalyst slurry is introduced) as in Example 2, the catalyst layer is moved toward the partition wall on the side of the small chamber where the drying air is introduced (at Fig. 9 The first zone in the middle) segregation.

[0106] In addition, if Fig.10 As shown in FIG. 1 , it was confirmed that the exhaust gas purifying catalyst of Example 1, in which a highly uniform catalyst layer was formed in the thickness direction of the partition wall, had a larger average neck diameter than the exhaust gas purifying catalyst of Example 2, in which segregation of the catalyst layer occurred. Fig.11 As shown, it was confirmed that the pressure loss increase rate of the exhaust gas purifying catalyst of Example 1 was lower than that of the exhaust gas purifying catalyst of Example 2. Based on these facts, it is believed that in the exhaust gas purifying catalyst having a catalyst layer with high uniformity in the thickness direction of the partition wall, the introduced exhaust gas can easily pass through the partition wall by suppressing the narrowness of the neck diameter of the partition wall, and as a result, the increase in pressure loss can be suppressed.

[0107] [Test 2]

[0108] In Experiment 2, the ratio of the coating length of the catalyst slurry was investigated.

[0109] (Example 3)

[0110] An exhaust gas purifying catalyst of Example 3 was prepared in the same manner as in Example 1 except that the entire length of the partition wall was taken as 100% and the coating length of the catalyst slurry was set to a region from the end portion on the inlet cell side to 30% of the length.

[0111] (Example 4)

[0112] An exhaust gas purifying catalyst of Example 4 was prepared in the same manner as in Example 1 except that the entire length of the partition wall was taken as 100% and the coating length of the catalyst slurry was the region from the end portion on the inlet cell side to 90% of the length.

[0113] (Example 5)

[0114] An exhaust gas purifying catalyst of Example 5 was prepared in the same manner as in Example 1 except that the entire length of the partition wall was taken as 100% and the coating length of the catalyst slurry was the region from the end portion on the inlet cell side to 95% of the length.

[0115] (Example 6)

[0116] The exhaust gas purification catalyst of Example 6 was prepared in the same manner except that the total length of the partition wall was taken as 100% in Example 1, and the coating length of the catalyst slurry was made to be the region from the end of the inlet chamber side to 100% of the length (i.e., the entire surface). In addition, in Example 6, dry ventilation was performed from the outlet chamber side, but the ratio of the coating length of the catalyst slurry was 100%, so in Table 2, it is shown as the case of ventilation from the slurry coating part side.

[0117] The exhaust gas purifying catalysts of Examples 3 to 6 were evaluated for catalyst layer distribution in the same manner as in Test 1. Table 2 shows the results.

[0118] [Table 2]

[0119] Table 2

[0120]

[0121] As shown in Table 2, it is known that when the ratio of the coating length of the catalyst slurry is less than 95% of the total length of the next wall, a catalyst layer with high uniformity in the thickness direction of the next wall can be formed. In addition, it is known that especially when the ratio of the coating length of the catalyst slurry is less than 90% of the total length of the next wall, a catalyst layer with more excellent uniformity in the thickness direction of the next wall can be formed. This is considered to be due to the fact that the lower the ratio of the coating length of the catalyst slurry, the larger the range of the uncoated part that the drying wind can easily pass through, and thus it is easy to make the catalyst slurry coating part more uniformly dried from both the inlet chamber and the outlet chamber.

[0122] [Test 3]

[0123] In Experiment 3, the viscosity of the catalyst slurry was investigated.

[0124] (Example 7)

[0125] The exhaust gas-purifying catalyst of Example 7 was prepared in the same manner as in Example 1, except that the viscosity of the catalyst slurry was adjusted to 1 mPa·s. In addition, the viscosity of the catalyst slurry was adjusted by the ratio of ion-exchanged water.

[0126] (Example 8)

[0127] The exhaust gas purifying catalyst of Example 8 was prepared in the same manner as in Example 1, except that the viscosity of the catalyst slurry was adjusted to 1000 mPa·s. In addition, the viscosity of the catalyst slurry was adjusted by the ratio of ion exchange water and the mixing of the thickener.

[0128] (Example 9)

[0129] The exhaust gas purifying catalyst of Example 9 was prepared in the same manner as in Example 1, except that the viscosity of the catalyst slurry was adjusted to 2000 mPa·s. The viscosity of the catalyst slurry was adjusted by the ratio of ion exchange water and the mixing of the thickener.

[0130] The exhaust gas purifying catalysts of Examples 7 to 9 were evaluated for catalyst layer distribution in the same manner as in Test 1. Table 3 shows the results.

[0131] [Table 3]

[0132] Table 3

[0133]

[0134] As shown in Table 3, it can be seen that when the viscosity of the catalyst slurry shown in Example 9 is 2000 mPa·s or more, the catalyst layer distribution becomes non-uniform.

[0135] [Test 4]

[0136] In Experiment 4, the D 50 The particle size was investigated.

[0137] (Example 10)

[0138] In addition to changing the size of the alumina powder in Example 1 so that the particle size D of the catalyst slurry is 50 The exhaust gas purifying catalyst of Example 10 was prepared in the same manner except that the particle diameter was changed to 0.10X μm.

[0139] (Example 11)

[0140] In addition to changing the size of the alumina powder in Example 1 so that the particle size D of the catalyst slurry is 50 The exhaust gas purifying catalyst of Example 11 was prepared in the same manner except that the particle size was changed to 0.15X μm.

[0141] (Example 12)

[0142] In addition to changing the size of the alumina powder in Example 1 so that the particle size D of the catalyst slurry is 50 The exhaust gas purifying catalyst of Example 12 was prepared in the same manner except that the particle size was changed to 0.5X μm.

[0143] The catalyst layer distribution of the exhaust gas-purifying catalysts of Examples 10 to 12 was evaluated in the same manner as in Test 1. Table 4 shows the results.

[0144] [Table 4]

[0145] Table 4

[0146]

[0147] As shown in Table 4, it can be seen that when the average pore diameter of the partition wall is set to X μm, the D 50 The particle size is 0.15X μm or less, and a catalyst layer with high uniformity in the thickness direction of the partition wall can be formed. In addition, it is found that the D of the particles contained in the catalyst slurry is 50 When the particle size is 0.10X μm or less, a catalyst layer with higher uniformity in the thickness direction of the partition wall can be formed. This is considered to be because 50 When the particle size is too small, the particles contained in the catalyst slurry can easily penetrate into the pores of the cell walls.

[0148] The test examples of the technology disclosed herein have been described in detail above, but these are merely examples and are not intended to limit the claims. The technology described in the claims includes various modifications and changes to the specific examples described above.

Claims

1. A method for producing an exhaust gas purifying catalyst, which is arranged in an exhaust passage of an internal combustion engine and purifies exhaust gas discharged from the internal combustion engine, comprising the following steps: Preparing a substrate having a wall flow structure including a first cell with only one end open, a second cell with only the other end open, and a porous partition wall separating the first cell from the second cell; Supplying a catalyst layer forming material to the end of the first cell opening of the substrate, so that an uncoated portion not coated with the catalyst layer forming material is formed on the end side of the second cell opening in the range of the partition wall facing the first cell in the extension direction of the partition wall, the catalyst layer forming material is applied to the interior of the partition wall from the end of the first cell opening of the substrate to a predetermined length along the extension direction of the partition wall; and The applied catalyst layer forming material is dried by ventilation from the end of the second cell opening of the substrate.

2. The manufacturing method according to claim 1, wherein: In the extending direction of the partition walls, the ratio of the length of the partition walls coated with the catalyst layer forming material is 90% or less of the entire length of the partition walls.

3. The manufacturing method according to claim 1 or 2, wherein: Measurement temperature 25°C, shear rate 4s -1 The viscosity of the catalyst layer forming material is less than 1500 mPa·s.

4. The production method according to any one of claims 1 to 3, wherein: When the average pore size of the partition walls is X μm, the average particle size of particles contained in the catalyst layer forming material measured by a laser diffraction scattering method is 0.15X μm or less.

5. The production method according to any one of claims 1 to 4, wherein: The ventilation speed is below 10 m / s.

6. The production method according to any one of claims 1 to 5, wherein: The catalyst layer forming material contains a catalyst metal, The catalyst metal includes at least any one of Pt, Pd, and Rh.

Citation Information

Patent Citations

  • Method for producing exhaust gas purification catalyst

    JP2019198837A

  • Noise removal method and device

    JP2022031196A

  • Exhaust gas purifying catalyst

    WO2019221214A1

  • Exhaust gas purification catalyst