Method for producing slurry and method for producing catalyst for exhaust gas purification

Through the two-stage grinding and reasonable selection of media particle size, the problems of long crushing time of the catalyst slurry and particle blockage are solved, and efficient powder microscopy and production efficiency are achieved.

CN118973713AActive Publication Date: 2024-11-15CATALER CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380029871.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-02
Publication Date
2024-11-15
Estimated Expiration
2043-03-02

AI Technical Summary

Technical Problem

In the preparation of catalyst slurry, it takes a long time to crush the powder to below 1 μm, resulting in worse productivity, and coarse particles may clog the slits of the grinding device, affecting the grinding efficiency.

Method used

Using a two-stage grinding method, firstly, the powder is finely refined to a particle size of more than 5 μm or less than 13 μm using a first grinding device of a larger medium, and then further grinding to less than 1 μm using a second grinding device of a smaller medium, combining wet crushing and circulation Grinding device is designed to monitor the powder particle size to appropriately switch the grinding process.

Benefits of technology

It significantly shortens the total grinding time, improves the grinding efficiency, avoids the problem of slit blockage, and enhances the powder's fineness efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973713A_ABST
    Figure CN118973713A_ABST
Patent Text Reader

Abstract

Provided is a method for producing a slurry in which the polishing time is shortened. The disclosed production method comprises: a material preparation step for preparing a slurry production material containing a first inorganic oxide powder; a first polishing step for polishing the slurry production material using a first polishing device having a first medium until the average particle diameter of the powder contained in the slurry production material by the laser diffraction / scattering method reaches 5 [mu] m or more and 13 [mu] m or less; and a second polishing step in which, after the first polishing step, a second polishing device having a second medium having an average particle diameter smaller than that of the first medium is used to polish the slurry production material until the average particle diameter of the powder contained in the slurry production material by the laser diffraction / scattering method is 1 [mu] m or less. The method further includes a step of mixing the second inorganic oxide powder with the slurry production material before the first polishing step or after the first polishing step and before the second polishing step.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a slurry and a method for producing a catalyst for purifying exhaust gas. The present application claims priority based on Japanese Patent Application No. 2022-048385 filed on March 24, 2022, the entire contents of which are incorporated herein by reference. Background Art

[0002] The exhaust gas emitted from internal combustion engines such as vehicle engines contains hydrocarbons (HC), carbon monoxide (CO), nitrogen oxides (NO x Therefore, an exhaust gas purification catalyst having a catalytic metal capable of purifying exhaust gas components by oxidation or reduction reaction is arranged in the exhaust gas path from the internal combustion engine.

[0003] The catalyst for exhaust purification typically comprises: a honeycomb substrate having a plurality of small chambers as flow paths for exhaust gas; and a catalyst layer having a catalyst metal formed in the small chambers. In general, the catalyst layer is formed by applying a slurry containing a catalyst metal and an inorganic oxide supporting the catalyst metal to a substrate, followed by drying and firing. For example, Patent Document 1 discloses a method for manufacturing a catalyst for exhaust purification, wherein in the step of manufacturing a washcoat slurry, a catalyst metal powder and γ-Al2O3 as a washcoat material are ground, and during such grinding, a step of adding a mixture (CeO2 and ZrO2-CeO2) is included. In addition, Patent Document 2 discloses a technique for preparing a catalyst slurry containing a catalyst powder having a specified particle size distribution by wet grinding, dry grinding, or a combination of wet grinding and dry grinding in the process of preparing a catalyst slurry.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 7-88384

[0007] Patent Document 2: International Publication No. 2018-159214 Summary of the invention

[0008] However, in the preparation of catalyst slurry, it takes a long time to grind the powder contained in the catalyst slurry to about 1 μm or less. Since the grinding time is long, the productivity is poor, so a technology to shorten the grinding time is expected. In order to shorten the grinding time, there is a method of reducing the diameter of the medium (such as beads) used for grinding, thereby increasing the contact frequency between the powder and the medium, but according to the research of the inventor of the present invention, the following technical problem was found: due to the presence of coarse particles in the powder, the slit used to separate the medium and the powder of the grinding device is sometimes blocked.

[0009] Therefore, the present invention is made in view of the above circumstances, and one of its objects is to provide a method for producing a slurry with a shortened grinding time. Another object is to provide a method for producing an exhaust gas purifying catalyst using such a method for producing a slurry.

[0010] The slurry manufacturing method disclosed in the present invention is used to manufacture a slurry containing a first inorganic oxide powder, a second inorganic oxide powder having an average particle size smaller than that of the first inorganic oxide powder, and a dispersion medium. The method includes: a material preparation step, which prepares a slurry manufacturing material containing the first inorganic oxide powder; a first grinding step, which uses a first grinding device having a first medium to grind the slurry manufacturing material until the average particle size of the powder contained in the slurry manufacturing material based on the laser diffraction / scattering method reaches 5 μm or more and 13 μm or less; and a second grinding step, which after the first grinding step, uses a second grinding device having a second medium having an average particle size smaller than that of the first medium to grind the slurry manufacturing material until the average particle size of the powder contained in the slurry manufacturing material based on the laser diffraction / scattering method reaches 1 μm or less. In addition, it is also characterized in that it includes a step of mixing the second inorganic oxide powder in the slurry manufacturing material before the first grinding step or after the first grinding step and before the second grinding step.

[0011] With this configuration, the second grinding is performed after the powder is finely ground to a size that is unlikely to clog the slit for separating the media and powder of the second grinding device by the first grinding, thereby improving the grinding efficiency and shortening the total grinding time.

[0012] In a preferred embodiment of the method for producing the slurry disclosed in the present invention, the average particle size of the first medium is 1 mm to 10 mm. With such a configuration, the powder contained in the slurry production material can be efficiently refined to an average particle size of 5 μm to 13 μm, thereby further shortening the grinding time.

[0013] In a preferred embodiment of the slurry manufacturing method disclosed in the present invention, the average particle size of the second medium is 0.1 mm to 0.5 mm. With such a configuration, the average particle size of the powder contained in the slurry manufacturing material can be easily refined to 1 μm or less, thereby further shortening the grinding time.

[0014] In a preferred embodiment of the method for producing the slurry disclosed in the present invention, before the second inorganic oxide powder is mixed, the average particle size of the second inorganic oxide powder based on the laser diffraction / scattering method is 5 μm or more and 13 μm or less. With such a configuration, the slit of the second polishing device can be prevented from being clogged by the second inorganic oxide powder.

[0015] In addition, in a preferred embodiment of the method for producing the slurry disclosed in the present invention, the pulverization method implemented in the first grinding step and the second grinding step is wet pulverization. With such a configuration, the powder agglomeration in the slurry manufacturing material can be suppressed, the powder refinement efficiency is improved, and the grinding time can be further shortened.

[0016] In a preferred embodiment of the method for producing the slurry disclosed in the present invention, the second inorganic oxide powder is mixed before the first grinding step. With such a configuration, the first grinding and the second grinding can be performed continuously, and thus the grinding time can be further shortened.

[0017] In addition, in a preferred embodiment of the method for manufacturing the slurry disclosed in the present invention, a slurry tank connected to the first grinding device in a cyclic manner is further prepared, and the slurry manufacturing material is circulated between the first grinding device and the slurry tank while the slurry manufacturing material is ground. With such a configuration, the average particle size of the powder contained in the slurry manufacturing material can be monitored while the first grinding is performed, so that the first grinding can be switched to the second grinding at an appropriate time point. Thus, the grinding time can be further shortened.

[0018] In addition, in a preferred embodiment of the method for manufacturing the slurry disclosed in the present invention, the slurry tank and the second grinding device are connected in a cyclic manner, and the slurry manufacturing material is circulated between the second grinding device and the slurry tank while the slurry manufacturing material is ground. With such a configuration, the average particle size of the powder contained in the slurry manufacturing material can be monitored while continuously grinding. Thus, excessive grinding can be prevented, and thus the grinding time can be further shortened.

[0019] In one embodiment of the method for producing slurry disclosed in the present invention, the slurry producing material contains at least one catalyst metal that functions as a catalyst capable of oxidizing or reducing exhaust gas components. Thus, slurry for forming a catalyst layer of an exhaust gas purification catalyst can be produced.

[0020] The present invention can also provide a method for manufacturing an exhaust gas purification catalyst. The method for manufacturing an exhaust gas purification catalyst disclosed in the present invention is used to manufacture an exhaust gas purification catalyst for purifying exhaust gas discharged from an internal combustion engine, and the manufacturing method includes: a step of preparing a catalyst layer forming slurry using the slurry manufacturing method disclosed in the present invention; a step of coating the catalyst layer forming slurry on a substrate; and a step of firing the substrate coated with the catalyst layer forming slurry. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a flowchart showing a schematic process of the method for producing the slurry according to the first embodiment.

[0022] Figure 2 It is a schematic diagram which shows the structure of the manufacturing apparatus of the slurry which concerns on one Embodiment.

[0023] Figure 3 It is a flowchart showing the schematic process of the method for producing the slurry according to the second embodiment.

[0024] Figure 4 It is a flowchart showing the schematic steps of a method for producing an exhaust gas purifying catalyst according to an embodiment.

[0025] Figure 5 It is a perspective view schematically showing the structure of an exhaust gas purification catalyst according to an embodiment.

[0026] Figure 6 It is a diagram schematically showing a cross section of an exhaust gas purification catalyst according to an embodiment, taken along the cylinder axis direction.

[0027] Figure 7 The average particle size (D 50 ) versus grinding time.

[0028] Figure 8 The average particle size (D 50 ) versus grinding time. DETAILED DESCRIPTION

[0029] Hereinafter, the technology disclosed in the present invention will be described with appropriate reference to the accompanying drawings. Among them, matters other than those specifically mentioned in this specification and matters required for implementing this technology can be grasped as design matters for those skilled in the art based on the prior art in this field. This technology can be implemented based on the contents disclosed in this specification and the technical knowledge in this field. In addition, in this specification, when the numerical range is recorded as "A to B (wherein A and B are arbitrary numerical values)", it refers to "Above A and Below B", and also includes the meaning of "greater than A and less than B", "greater than A and below B" and "Above A and Less than B".

[0030] The method for manufacturing a slurry disclosed in the present invention is a method for manufacturing a slurry containing a first inorganic oxide powder, a second inorganic oxide powder having an average particle size smaller than that of the first inorganic oxide powder, and a dispersion medium. In one embodiment of the method for manufacturing a slurry disclosed in the present invention, the method comprises: a material preparation step, which prepares a slurry manufacturing material containing a first inorganic oxide powder; a first grinding step, which uses a first grinding device having a first medium to grind the slurry manufacturing material until the average particle size of the powder contained in the slurry manufacturing material based on a laser diffraction / scattering method reaches 5 μm or more and 13 μm or less; and a second grinding step, which after the first grinding step, uses a second grinding device having a second medium having an average particle size smaller than that of the first medium to grind the above-mentioned slurry manufacturing material until the average particle size of the powder contained in the slurry manufacturing material based on a laser diffraction / scattering method reaches 1 μm or less. It is also characterized in that the second inorganic oxide powder is mixed in the slurry manufacturing material before the first grinding step or after the first grinding step and before the second grinding.

[0031] By using this technology, the second grinding is performed after the powder is refined to a size that is difficult to clog the slit used to separate the medium and powder of the second grinding device through the first grinding, thereby improving the grinding efficiency and shortening the total grinding time. In addition, by setting the time point of ending the first grinding to when the average particle size of the powder contained in the slurry manufacturing material based on the laser diffraction / scattering method reaches 5 μm or more and 13 μm or less, it is possible to switch to the second grinding before the grinding efficiency of the first grinding decreases significantly, thereby shortening the total grinding time.

[0032] (First Embodiment)

[0033] Figure 1 1 is a flowchart showing a schematic process of the method for producing slurry according to the first embodiment. This embodiment includes a material preparation step S11 , a first polishing step S12 , and a second polishing step S13 .

[0034] In the material preparation step S11, a material for slurry production containing at least a first inorganic oxide powder is prepared. In the first embodiment, a material for slurry production containing a first inorganic oxide powder and a second inorganic oxide powder is prepared. The first inorganic oxide powder and the second inorganic oxide powder prepared in the present invention are raw materials for the powder components contained in the manufactured slurry.

[0035] The first inorganic oxide powder (i.e., before grinding) prepared in the present invention uses a powder having an average particle size larger than that of the second inorganic oxide powder (before grinding) prepared. The average particle size of such a first inorganic oxide powder is not particularly limited, and is, for example, 15 μm to 150 μm, 20 μm to 80 μm, or 30 μm to 60 μm. In this specification, unless otherwise specified, "average particle size" refers to the cumulative 50% particle size (D ) of the volume-based particle size distribution obtained by measuring using a particle size distribution measuring device based on a laser diffraction / scattering method. 50 ).

[0036] The type of the first inorganic oxide powder is not particularly limited and can be appropriately changed according to the intended use of the slurry. For example, in the case of a slurry for forming a catalyst layer of an exhaust gas purification catalyst, it is suitable to use an inorganic oxide capable of supporting a catalyst metal, an inorganic oxide having an oxygen storage capacity (OSC: oxygen storage capacity) capable of absorbing / releasing oxygen (so-called OSC material), etc. As inorganic oxides capable of supporting a catalyst metal, for example, aluminum oxide (Al2O3), ceria (CeO2), zirconium oxide (ZrO2), silicon dioxide (SiO2), titanium dioxide (TiO2), etc. can be listed. It can also be a rare earth metal oxide such as yttrium oxide (Y2O3), an alkali metal oxide, an alkaline earth metal oxide, etc. As an OSC material, for example, a ceria-zirconia composite oxide (CZ or ZC composite oxide) can be listed. In addition, it is preferable to use OSC materials such as ceria and ceria-zirconia composite oxides to which trace amounts of oxides containing other rare earth elements such as yttrium (Y), lanthanum (La), niobium (Nb), and praseodymium (Pr) are added.

[0037] The average particle size of the prepared second inorganic oxide powder (i.e. before grinding) can be smaller than the average particle size of the prepared first inorganic oxide powder. The average particle size of such a second inorganic oxide powder is not particularly limited, and can be, for example, 1 μm to 50 μm, 3 μm to 30 μm, or 5 μm to 13 μm.

[0038] The type of the second inorganic oxide powder can be appropriately changed according to the use of the slurry. For example, in the case of a slurry for forming a catalyst layer of an exhaust gas purification catalyst, it can be any of the powders exemplified in the above-mentioned first inorganic oxide powder. In a preferred example of a slurry for forming a catalyst layer of an exhaust gas purification catalyst, as the first inorganic oxide powder, an inorganic oxide (such as alumina) capable of supporting a catalyst metal can be used, and as the second inorganic oxide powder, an OSC material (such as a CZ composite oxide) can be used.

[0039] The material for making a slurry typically contains a dispersion medium. By containing a dispersion medium, wet grinding can be performed as grinding. As such a dispersion medium, for example, an aqueous solvent such as water or deionized water is preferably used. The proportion of the dispersion medium in the entire material for making a slurry can be, for example, 10wt% to 90wt% of the material for making a slurry, preferably 25wt% to 75wt%, and more preferably 40wt% to 60wt%.

[0040] In addition, when the dispersion medium is set to 100wt%, the proportion of the first inorganic oxide powder is not particularly limited, and can be, for example, 10wt% to 90wt%, 20wt% to 70wt%, or 30wt% to 50wt%. In addition, when the dispersion medium is set to 100wt%, the proportion of the second inorganic oxide powder is not particularly limited, and can be, for example, 10wt% to 90wt%, 20wt% to 70wt%, or 30wt% to 50wt%.

[0041] The material for making the slurry may also contain other components. For example, in the case of a slurry for forming a catalyst layer of an exhaust gas purification catalyst, as other components, at least one catalyst metal, a promoter, a binder, a dispersant, a thickener, etc., which can function as a catalyst capable of oxidizing or reducing exhaust gas components, can be listed. As catalyst metals, for example, metals belonging to the platinum group such as palladium (Pd), rhodium (Rh), and platinum (Pt) or other metals that function as oxidation or reduction catalysts can be listed. Pd and Pt have excellent purification performance (oxidation purification ability) for carbon monoxide and hydrocarbons, and Rh has excellent purification performance (reduction purification ability) for NOx, so these are particularly preferred catalyst metals as three-way catalysts. The catalyst metals can be mixed in the form of powders, or they can be mixed in the form of raw material compounds (such as water-soluble metal salts such as Pd nitrate and Rh nitrate) that generate catalyst metal particles after sintering. As a promoter component, for example, barium sulfate can be exemplified. As a binder, aluminum sol and silica sol can be exemplified.

[0042] In the first grinding step S12, a first grinding device having a first medium is used to perform grinding until the average particle size of the powder contained in the slurry manufacturing material reaches a specified range. As such a specified range, it is preferably 5 μm or more and 13 μm or less, and more preferably 10 μm or more and 13 μm or less. When the average particle size of such a powder is 13 μm or less, it is difficult for the slit of the second grinding device used in the second grinding step S13 to be clogged. In addition, from the perspective of performing grinding at an earlier time point using a medium with a smaller average particle size, thereby shortening the total grinding time, the average particle size of such a powder is preferably 5 μm or more, and more preferably 10 μm or more.

[0043] As the first grinding device, a ball mill, a bead mill, etc. can be exemplified, and a bead mill is preferably used. A bead mill has a stronger pulverizing force than a ball mill, and thus the grinding time can be further shortened.

[0044] The average particle size of the first medium of the first grinding device is preferably 1 mm to 10 mm, more preferably 1 mm to 3 mm, and further preferably 1 mm to 2 mm. With such an average particle size, the powder contained in the slurry manufacturing material can be efficiently refined to a predetermined average particle size. The average particle size of the first medium can also be a value of the diameter of a commercially available medium.

[0045] The material of the first medium is not particularly limited, and examples thereof include glass, alumina, zircon, zirconia, and steel.

[0046] The pulverization method of the first grinding device is not particularly limited, and examples thereof include dry pulverization and wet pulverization, and wet pulverization is preferred. In the case of wet pulverization, powder agglomeration can be suppressed, and the powder refinement efficiency is improved, so the grinding time can be further shortened.

[0047] When the first grinding device is a bead mill, the type of the stirring structure (agitator) of the bead mill is not particularly limited, and examples thereof include a disc type, a needle type, a ring type, etc. In addition, the direction of the grinding chamber (container) of the bead mill is not particularly limited, and for example, it may be vertical or horizontal.

[0048] As the operation mode of the first grinding device, a cycle operation, a single path operation, a batch operation, etc. can be exemplified, and a cycle operation is preferably adopted. In the case of a cycle operation, the average particle size of the powder contained in the slurry manufacturing material can be monitored while the first grinding is performed, so that the first grinding can be switched to the second grinding at an appropriate time point. Thus, the grinding time can be further shortened.

[0049] In the second grinding step S13, grinding is performed using a second grinding device having a second medium until the average particle size of the powder contained in the slurry manufacturing material reaches 1 μm or less (for example, 0.1 μm to 0.6 μm). The powder contained in the slurry manufacturing material supplied to the second grinding device is refined to a predetermined average particle size range by the first grinding. Therefore, clogging of the slit of the second grinding device can be suppressed.

[0050] As the second grinding device, a ball mill, a bead mill, etc. can be exemplified, and a bead mill is preferably used. A bead mill has a stronger pulverizing force than a ball mill, and thus the grinding time can be further shortened.

[0051] The average particle size of the second medium of the second grinding device is preferably 0.1 mm to 0.5 mm, for example. With such an average particle size, it is easy to refine the average particle size of the powder contained in the slurry manufacturing material to less than 1 μm. The average particle size of the second medium can also be the value of the diameter of a commercially available medium.

[0052] The material of the second medium is not particularly limited, and examples thereof include glass, alumina, zircon, zirconia, steel, and the like.

[0053] The pulverization method of the second grinding device is not particularly limited, and examples thereof include dry pulverization, wet pulverization, etc., preferably wet pulverization. When wet pulverization is used, powder agglomeration can be suppressed, and the efficiency of powder miniaturization is improved, so the grinding time can be further shortened. In addition, by making the pulverization methods of the first grinding device and the second grinding device both wet pulverization, the first grinding and the second grinding can be continuously implemented, so the slurry manufacturing time can be shortened.

[0054] When the second grinding device is a bead mill, the type of the stirring structure (agitator) of the bead mill is not particularly limited, and examples thereof include a disc type, a needle type, a ring type, etc. In addition, the direction of the grinding chamber (container) of the bead mill is not particularly limited, and for example, it may be a vertical type or a horizontal type.

[0055] As the operation mode of the second grinding device, a circulation operation, a single path operation, a batch operation, etc. can be exemplified, and a circulation operation is preferably adopted. In the case of a circulation operation, the average particle size of the powder contained in the slurry manufacturing material can be monitored while continuously grinding. Thus, excessive grinding can be prevented, and thus the grinding time can be further shortened.

[0056] The above is a description of a manufacturing method according to one embodiment. The manufacturing method disclosed in the present invention may further include other steps at any stage. For example, any component may be mixed into the manufactured slurry after the second grinding step S13. As the arbitrary component, for example, a binder, an antioxidant, a dispersant, a thickener, etc. may be exemplified. In addition, in the case of a slurry for forming a catalyst layer of an exhaust gas purification catalyst, a raw material compound, a promoter, etc. for generating catalyst metal particles may also be mixed after firing.

[0057] Figure 2 Schematic diagram showing the structure of a slurry manufacturing device involved in one embodiment. The present technology can be implemented using the illustrated slurry manufacturing device 100, for example. In the present embodiment, the slurry manufacturing device 100 has a slurry tank 110, a pump 120, a first grinding device 140, and a second grinding device 150. The slurry manufacturing device 100 of the present embodiment also has a switching component 130. The slurry tank 110 is connected to the pump 120 via a pipeline 131. The pump 120 is connected to the switching component 130 via a pipeline 132. The switching component 130 is connected to the first grinding device 140 via a pipeline 133, and the first grinding device 140 is connected to the slurry tank 110 via a pipeline 134. In this way, the slurry tank 110 and the first grinding device 140 are connected in a cyclic manner to realize the cyclic operation of the first grinding device 140. In addition, as shown in the figure, the switching component 130 is connected to the second grinding device 150 via a pipeline 135, and the second grinding device 150 is connected to the slurry tank 110 via a pipeline 136. In this way, the slurry tank 110 and the second grinding device 150 are connected in a cyclic manner to realize the cyclic operation of the second grinding device 150. The switching assembly 130 is configured to switch the connection with the pipeline 133 and the connection with the pipeline 135, and can switch the connection between the slurry tank 110 and any one of the first grinding device 140 and the second grinding device 150. Figure 2 The arrows in denoted the directions in which the slurry manufacturing material 30 can flow.

[0058] The slurry tank 110 is a tank for storing the slurry manufacturing material 30. The slurry tank 110 has a stirring blade 112, and can stir the slurry manufacturing material in the slurry tank 110.

[0059] The pump 120 functions as a power source for circulating the slurry manufacturing material 30, and can realize the circulation operation of the slurry tank 110 and the first polishing device 140 or the second polishing device 150. In the present embodiment, one pump 120 is provided before the switching assembly 130, but, for example, one pump 120 may be provided between the switching assembly 130 and the first polishing device 140, and one pump 120 may be provided between the switching assembly 130 and the second polishing device 150.

[0060] The switching assembly 130 is an element that is arbitrarily set and is not a necessary structure. By having the switching assembly 130, the switching between the first grinding and the second grinding becomes smooth, and as a result, the grinding time can be shortened. As the switching assembly 130, for example, a switching valve can be used. In addition, the connection of the pipeline can also be changed manually, and the circulation path between the slurry tank 110 and the first grinding device 140 is changed to the circulation path with the second grinding device 150, thereby replacing the setting of the switching assembly 130.

[0061] In this embodiment, a total of two first grinding devices 140 and second grinding devices 150 are provided in series. Thus, the first grinding step S12 and the second grinding step 13 can be continuously implemented, which can help shorten the slurry manufacturing time. Among them, the first grinding device 140 is a device used in the first grinding step S12, as long as it is the same as the aforementioned device. In addition, the second grinding device 150 is a device used in the second grinding step S13, as long as it is the same as the aforementioned device.

[0062] In the slurry manufacturing apparatus 100 , the average particle size of the powder contained in the slurry manufacturing material can be monitored while performing the first polishing step S12 or the second polishing step S13 . For example, part of the slurry manufacturing material in the slurry tank 110 can be appropriately collected, and the particle size can be monitored online.

[0063] (Second Embodiment)

[0064] Figure 3 It is a flowchart showing the general process of the method for manufacturing the slurry involved in the second embodiment. The second embodiment includes a material preparation step S21, a first grinding step S22, a second inorganic oxide powder adding step S23 and a second grinding step S24. In the above-mentioned first embodiment, in the material preparation step S11 before the first grinding step S12, a slurry manufacturing material containing a first inorganic oxide powder and a second inorganic oxide powder is prepared. In the second embodiment, a slurry manufacturing material containing a first inorganic oxide powder is prepared in the material preparation step S21, and the second inorganic oxide powder is mixed in the slurry manufacturing material after the first grinding step S22 and before the second grinding step S24. Thus, it is possible to suppress the excessive refinement of the second inorganic oxide powder having an average particle size smaller than that of the first inorganic oxide powder. Among them, the matters other than the second inorganic oxide powder in the material preparation step S21 of the second embodiment can be the same as the above-mentioned material preparation step S11. In addition, the first grinding step S22 can be the same as the above-mentioned first grinding step S12, and the second grinding step S24 can be the same as the above-mentioned second grinding step S13.

[0065] In the second embodiment, since the second inorganic oxide powder is not subjected to the first grinding, the average particle size of the second inorganic oxide powder is preferably 5 μm to 13 μm from the viewpoint of preventing clogging of the slit of the second grinding device during the second grinding.

[0066] The method for producing the slurry disclosed in the present invention is suitable for use as a method for producing a slurry for forming a catalyst layer of an exhaust gas purification catalyst for purifying exhaust gas discharged from an internal combustion engine. Therefore, in the present invention, a method for producing an exhaust gas purification catalyst including the method for producing the slurry disclosed in the present invention is provided.

[0067] Figure 4 It is a flow chart showing the general process of a method for manufacturing an exhaust gas purification catalyst involved in one embodiment. The method for manufacturing an exhaust gas purification catalyst disclosed in the present invention includes a process of preparing a slurry for forming a catalyst layer (hereinafter also referred to as "slurry preparation process S31"), a process of coating the slurry for forming a catalyst layer on a substrate (hereinafter also referred to as "coating process S32"), and a process of firing the substrate coated with the slurry for forming a catalyst layer (hereinafter also referred to as "firing process S34"). In addition, as Figure 4 As shown, a drying step S33 of drying the substrate coated with the catalyst layer forming slurry may be included. In addition, the exhaust gas purification catalyst disclosed in the present invention may further include other steps at any stage.

[0068] The slurry preparation step S31 is to prepare a catalyst layer forming slurry using the slurry manufacturing method disclosed in the present invention. The catalyst layer forming slurry contains powder with an average particle size of 1 μm or less, and is typically suitable for forming a catalyst layer inside a porous partition wall, and can also be used to form a catalyst layer on the surface of the partition wall.

[0069] In the coating step S32 , the catalyst layer forming slurry is coated on the substrate constituting the skeleton of the exhaust gas purifying catalyst. Figure 5 It is a perspective view schematically showing the structure of an exhaust gas purification catalyst according to an embodiment. Figure 6 The figure schematically shows a cross section of an exhaust gas purification catalyst 1 according to one embodiment along the cylinder axis direction. The symbol A in the figure represents the exhaust gas flow direction A. The substrate prepared in the present invention may be as follows: Figure 5The cylindrical substrate 10 is elongated along the flow direction A of the exhaust gas as shown. The substrate 10 can have a honeycomb structure that gathers a plurality of small chambers as flow paths of a fluid (such as exhaust gas). Among them, the shape of the substrate is not limited to a cylindrical shape, and can also be an elliptical cylindrical shape, a polygonal cylindrical shape, etc. In addition, the total length and capacity of the substrate 10 are not particularly limited, and can be appropriately changed according to the performance and size of the internal combustion engine. In addition, the substrate 10 is not particularly limited, and the existing known raw materials that can be used for the substrate of the exhaust gas purification catalyst can be used. As an example of the raw material of such a substrate 10, high heat-resistant raw materials represented by ceramics such as cordierite, silicon carbide (SiC), aluminum titanate, and alloys such as stainless steel can be cited. For example, cordierite is excellent in durability to thermal shock, and can be particularly suitably used as a raw material for the substrate of an exhaust gas purification catalyst for a gasoline engine that is easy to supply high-temperature exhaust.

[0070] The substrate 10 may be Figure 6 The wall flow type substrate is as shown. Figure 5 and 6 As shown, the substrate 10 has an inlet chamber 12 that is open only at the end on the exhaust gas inlet side, an outlet chamber 14 that is open only at the end on the exhaust gas outlet side, and a porous partition wall 16 that separates the inlet chamber 12 from the outlet chamber 14. Specifically, the inlet chamber 12 is a gas flow path that is open at the end on the exhaust gas inlet side and is blocked by a sealing portion 12a at the end on the exhaust gas outlet side. On the other hand, the outlet chamber 14 is a gas flow path that is blocked by a sealing portion 14a at the end on the exhaust gas inlet side and is open at the end on the exhaust gas outlet side. In addition, the partition wall 16 is a partition material formed with a plurality of pores through which exhaust gas can pass. The partition wall 16 has a plurality of pores that connect the inlet chamber 12 and the outlet chamber 14. Among them, in Figure 5 In the exhaust gas purification catalyst 1 shown, the shape of the inlet chamber 12 (outlet chamber 14) of the cross section perpendicular to the extension direction (cylinder axis direction X) of the partition wall 16 is a square. However, the shape of the inlet chamber (outlet chamber) of the cross section perpendicular to the extension direction is not limited to a square, and various shapes can be adopted. For example, it can be a parallelogram, a rectangle, a trapezoid or other quadrilateral, a triangle, other polygons (for example, a hexagon, an octagon), a circle or other various geometric shapes.

[0071] The partition wall 16 of the substrate 10 is preferably formed in consideration of the capture performance of particulate matter (PM: Particulate Matter) and the pressure loss suppression performance. For example, the thickness of the partition wall 16 is preferably about 100μm to 350μm. In addition, the porosity of the partition wall 16 is preferably about 20% by volume to 70% by volume, and more preferably 50% by volume to 70% by volume. In addition, from the perspective of fully ensuring the air permeability of the partition wall 16 and suppressing the increase in pressure loss, the average pore diameter of the pores is preferably 8μm or more, more preferably 12μm or more, and further preferably 15μm or more. On the other hand, from the perspective of ensuring appropriate PM capture performance, the upper limit of the average pore diameter of the pores is preferably 30μm or less, more preferably 25μm or less, and further preferably 20μm or less. Among them, the porosity and average pore diameter of the partition wall 16 refer to the values ​​measured by mercury intrusion.

[0072] In addition, the substrate is not limited to the wall flow type, and may be a so-called linear flow type substrate in which a plurality of through holes are gathered.

[0073] The coating method of the catalyst layer forming slurry to the substrate 10 can be the same as the coating implemented by the existing technology, for example, a wash coating method, a suction coating method, etc. can be cited. In the wash coating method, after the substrate 10 is immersed in the catalyst layer forming slurry, the substrate 10 is taken out, and the excess slurry is removed by blowing, thereby the catalyst layer forming slurry can be coated. In addition, in the suction coating method, the catalyst layer forming slurry is supplied to the end of the substrate 10, and the slurry is introduced into the interior of the substrate 10 by suction from the other end, so that the catalyst layer forming slurry can be coated. Among them, at this time, by adjusting the range of the impregnation catalyst layer forming slurry and adjusting the suction time, the configuration of the formed catalyst layer 20 can be adjusted.

[0074] In addition, the thickness of the catalyst layer can be appropriately adjusted according to the viscosity of the slurry for forming the catalyst layer. For example, a commercially available cone plate viscometer is used to measure the viscosity of the catalyst layer at a rotation speed of 1 to 100 rpm, room temperature (25° C.), and a shear rate of 380 s. -1 The viscosity measured under the conditions is appropriately about 10 mPa to 1000 mPa.

[0075] The drying step S33 can be performed under the same conditions as those of the drying performed by the conventional technique, and is not particularly limited. For example, the drying can be performed at a temperature of 50° C. to 200° C. for about 1 minute to 30 minutes.

[0076] The firing step S34 can be performed under the same conditions as those of the firing performed by the conventional technique, and is not particularly limited. For example, the firing can be performed at a temperature of 400° C. to 1000° C. for about 30 seconds to 5 hours.

[0077] In this way, it is possible to produce, for example Figure 6 The exhaust gas purification catalyst 1 shown in FIG. Figure 6 In the exhaust gas purification catalyst 1 shown, a catalyst layer 20 is formed inside the partition wall 16, and the catalyst layer 20 is formed throughout the entire length of the partition wall 16 in the cylindrical axis direction X and the thickness of the partition wall 16 orthogonal to the cylindrical axis direction X. However, this is only an example, and the manufactured exhaust gas purification catalyst is not limited to this. For example, the catalyst layer 20 can also be formed on the surface of the partition wall 16. In addition, the catalyst layer 20 can also be formed at a predetermined ratio (for example, 10% to 90%) relative to the total length of the partition wall 16 in the cylindrical axis direction X. Furthermore, the exhaust gas purification catalyst 1 can also be provided with a second catalyst layer having a composition different from that of the catalyst layer 20 at a position different from the catalyst layer 20.

[0078] The exhaust gas purification catalyst 1 can be used in various applications depending on the composition of the catalyst layer 20 , and can be used, for example, as a three-way catalyst, a NOx catalyst, an oxidation catalyst, a reduction (SCR) catalyst, or an ammonia slip catalyst (ASC).

[0079] Hereinafter, several embodiments of the technology disclosed in the present invention will be described, but the technology disclosed in the present invention is not intended to be limited to the technology described in these embodiments.

[0080] (Test 1)

[0081] [Preparation of materials for slurry production]

[0082] Alumina powder (average particle size: about 32 μm), ceria-zirconia composite oxide (CZ composite oxide) powder (average particle size: about 12.8 μm), Pd nitrate and water are mixed to prepare a slurry manufacturing material. Such a slurry manufacturing material is prepared in a mass ratio of alumina powder: CZ composite oxide powder: Rh nitrate: water = 20:23:2:55. The average particle size (D 50 ), and the obtained results are shown in Table 1 as the initial particle size. Using such slurry manufacturing materials, the grinding of the following Examples 1, 2, Comparative Example 1, and Reference Example was carried out. Among them, the manufactured slurry has an average particle size (D 50 ) is a slurry of powder with a size of less than 0.6 μm.

[0083] <Example 1>

[0084] As a grinding device for the first grinding, a first bead mill having zirconium oxide beads (first medium) with a diameter of 1 mm is prepared. In addition, as a grinding device for the second grinding, a second bead mill having zirconium oxide beads (second medium) with a diameter of 0.5 mm is prepared. Then, a slurry tank filled with the slurry manufacturing material prepared above is prepared. The slurry tank is connected to the first bead mill in a manner that the filled slurry manufacturing material can be circulated. In addition, the slurry tank is similarly connected to the second bead mill in a manner that the filled slurry manufacturing material can be circulated. In addition, a switching valve is configured in a manner that the circulation path between the slurry tank and the first bead mill and the circulation path between the slurry tank and the second bead mill can be switched. First, the slurry manufacturing material is supplied from the slurry tank to the first bead mill, and the first grinding is performed. The first grinding is performed until the average particle size (D 50 ) reached 12.88 μm, the circulation path was switched to the second bead mill to perform the second grinding. The second grinding was performed until the average particle size (D 50 ) reaches 0.6 μm. In this way, a slurry is prepared. Part of the slurry manufacturing material is recovered during grinding, and the average particle size of the powder contained in the slurry manufacturing material is measured using a particle size distribution measuring device based on a laser diffraction / scattering method. 50 The relationship between ) and grinding time is shown in the curve diagram Figure 7 . For each of the examples described below, the results are also shown in Figure 7 In addition, the grinding conditions, the particle size of the powder contained in the slurry manufacturing material based on the particle size distribution at the end of the first grinding, and the average particle size (D 50 ) are shown in Table 1. In addition, for each example described later, the polishing conditions and results are also shown in Table 1.

[0085] <Example 2>

[0086] In Example 1, the time point of switching from the first grinding to the second grinding was changed to the average particle size (D 50 ) reached 5 μm, the same operation was carried out except for the above to prepare a slurry.

[0087] <Comparative Example 1>

[0088] In Example 1, the time point of switching from the first grinding to the second grinding was changed to the average particle size (D 50 ) reached 15.12 μm, and the same procedure was repeated except for this. However, the slit of the second bead mill was clogged, so the second grinding was interrupted during the process.

[0089] <Reference example>

[0090] The first bead mill was used to grind the powder contained in the slurry production material until the average particle size (D 50 ) reached 0.5 μm, and the slurry was prepared. That is, in the reference example, the slurry was prepared using a bead mill having zirconia beads with a diameter of 1 mm.

[0091] [Table 1]

[0092]

[0093] like Figure 7 As shown in Table 1, it can be seen that compared with the reference example in which a bead mill with 1 mm beads is used to grind until the specified average particle size (here 0.5 mm), Examples 1 and 2 using a first bead mill with 1 mm beads and a second bead mill with 0.5 mm beads can significantly shorten the total grinding time. However, as in Comparative Example 1, when switching from the first grinding to the second grinding, when the average particle size of the powder in the slurry manufacturing material is too large, the second bead mill has slit clogging. Therefore, as shown in Examples 1 and 2, it can be seen that the time point of switching from the first grinding to the second grinding is appropriate when the first grinding is used to grind until the average particle size of the powder in the slurry manufacturing material reaches 5 μm to 13 μm.

[0094] (Test 2)

[0095] [Preparation of materials for slurry production]

[0096] Alumina powder (average particle size: about 32 μm) and water were mixed to prepare a slurry material. The slurry material was prepared at a mass ratio of alumina powder: water = 20:55. The average particle size (D 50 ), and the obtained results are shown in Table 2 as the initial particle size. Using such slurry manufacturing materials, the grinding of the following Example 3 and Comparative Example 2 was carried out. Among them, the manufactured slurry contains an average particle size (D 50 ) is a slurry of powder with a size of less than 0.6 μm.

[0097] <Example 3>

[0098] Prepare the same first bead mill and second bead mill as in Example 1, and a slurry tank filled with the slurry manufacturing material prepared above. Connect the slurry tank to the first bead mill in a manner that the slurry manufacturing material can circulate. In addition, similarly connect the slurry tank to the second bead mill in a manner that the filled slurry manufacturing material can circulate. The slurry tank is configured to switch the circulation path with the first bead mill and the circulation path with the second bead mill at a desired time point. First, the slurry manufacturing material is supplied from the slurry tank to the first bead mill, and the first grinding is performed. The first grinding is performed until the average particle size (D 50 ) reached 10.40 μm. Then, CZ composite oxide powder (average particle size: about 12.8 μm) was added to the slurry manufacturing material after the first grinding, so that the mass ratio of alumina powder: CZ composite oxide powder: water = 20:25:55. The average particle size (D 50 ) was 11.76 μm. Next, the circulation path with the second bead mill was switched to perform the second grinding. The second grinding was performed until the average particle size (D 50 ) reaches 0.6 μm. In this way, a slurry is prepared. Part of the slurry manufacturing material is recovered during grinding, and the average particle size of the powder contained in the slurry manufacturing material is measured using a particle size distribution measuring device based on a laser diffraction / scattering method. 50 The relationship between ) and grinding time is shown in the curve diagram Figure 8 In addition, Figure 8 In the graph, two points are plotted at a grinding time of 34 minutes, which indicates that before and after the mixing of the CZ composite oxide, the point after the mixing of the CZ composite oxide shows that the average particle size has increased. In addition, the grinding conditions, the particle size of the powder contained in the slurry manufacturing material based on the particle size distribution at the end of the first grinding (before the mixing of the CZ composite oxide), and the average particle size (D 50 ) are shown in Table 2.

[0099] <Comparative Example 2>

[0100] The grinding was performed using only the first bead mill in the same manner as in the reference example. The grinding was performed until the average particle size (D 50 ) reached 9.8 μm, CZ composite oxide was added to the slurry manufacturing material so that the mass ratio of alumina powder: CZ composite oxide: water = 20:25:55. Then, grinding using the first bead mill was continued until the average particle size (D 50 ) reached 0.58 μm. The results are shown in Figure 8and Table 2. In Comparative Example 2, the grinding by the first bead mill after mixing the CZ composite oxide powder is referred to as the second grinding.

[0101] [Table 2]

[0102]

[0103] From Table 2 and Figure 8 It is found that even when a CZ composite oxide having an average particle size smaller than that of the alumina powder is mixed after the first milling, the total milling time is shortened by using beads smaller than those used in the first milling in the second milling.

[0104] The specific examples of the technology disclosed in the present invention have been described in detail above, but these are only examples and do not limit the scope of the claims. The technology described in the scope of the claims includes various modifications and changes to the specific examples described above.

Claims

1. A method for producing a slurry, characterized in that: The slurry contains a first inorganic oxide powder, a second inorganic oxide powder having an average particle size smaller than that of the first inorganic oxide powder, and a dispersion medium. The manufacturing method include: a material preparation step of preparing a material for slurry production containing the first inorganic oxide powder; a first grinding step of grinding the slurry-making material using a first grinding device having a first medium until the average particle size of the powder contained in the slurry-making material reaches 5 μm or more and 13 μm or less based on a laser diffraction / scattering method; and a second grinding step, after the first grinding step, grinding the slurry-making material using a second grinding device having a second medium having an average particle size smaller than that of the first medium until the average particle size of the powder contained in the slurry-making material reaches 1 μm or less based on a laser diffraction / scattering method, The production method further includes the step of mixing the second inorganic oxide powder with the slurry production material before the first grinding step or after the first grinding step and before the second grinding step.

2. The manufacturing method according to claim 1, Features: The average particle size of the first medium is greater than or equal to 1 mm and less than or equal to 10 mm.

3. The manufacturing method according to claim 1 or 2, Features: The average particle size of the second medium is greater than or equal to 0.1 mm and less than or equal to 0.5 mm.

4. The production method according to any one of claims 1 to 3, Features: Before the second inorganic oxide powder is mixed, the average particle size of the second inorganic oxide powder based on a laser diffraction / scattering method is 5 μm or more and 13 μm or less.

5. The production method according to any one of claims 1 to 4, Features: The pulverization method performed in the first grinding step and the second grinding step is wet pulverization.

6. The production method according to any one of claims 1 to 5, Features: The second inorganic oxide powder is mixed before the first grinding step.

7. The production method according to any one of claims 1 to 6, Features: A slurry tank circulatably connected to the first polishing device is further prepared, and the slurry-producing material is polished while circulating the slurry-producing material between the first polishing device and the slurry tank.

8. The manufacturing method according to claim 7, Features: The slurry tank and the second polishing device are connected to each other in a circulation manner, and the slurry-producing material is polished while circulating the slurry-producing material between the second polishing device and the slurry tank.

9. The production method according to any one of claims 1 to 8, Features: The slurry manufacturing material contains at least one catalyst metal that functions as a catalyst capable of oxidizing or reducing exhaust gas components.

10. A method for producing an exhaust gas purification catalyst for purifying exhaust gas discharged from an internal combustion engine, the method comprising: include: A step of preparing a slurry for forming a catalyst layer using the manufacturing method according to claim 9; The step of coating the catalyst layer forming slurry on a substrate; and A step of firing the substrate coated with the catalyst layer forming slurry.

Citation Information

Patent Citations

  • Pneumatic transmitting and fine grinding system for producing vanadium-free rare earth based titanium-tungsten powder

    CN105149070A

  • Method for preparing spheroidic powder through mechanical crushing method and spheroidic powder

    CN113399093A

  • Vibration mill, grinding set and grinding media for such

    DE102018103013A1

  • Manufacture of slurry and device therefor

    JP1997150072A

  • Wet grinding process and slurry composition produced by the same process