Thermoplastic resin and optical lens comprising same
The existing optical lenses are solved by introducing specific structural monomers into 1,3-bis(1-methyl-1-phenethyl)benzene compounds, and a thermoplastic resin with excellent refractive index, Abbe number and photoelastic coefficient have been developed, which has led to the development of existing optical lenses. The problem of insufficient heat resistance and optical performance of the material achieves an optical lens with high refractive index and high heat resistance.
Patent Information
- Application Number
- CN202380031795.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-02-03
- Filing Date
- 2023-04-06
- Publication Date
- 2024-11-15
AI Technical Summary
Existing optical lens materials have shortcomings in heat resistance, transparency, low water absorption, chemical resistance and low birefringence, and it is difficult to meet the needs of high refractive index and high heat resistance.
Thermoplastic resins with excellent refractive index, Abbe number and photoelastic coefficient were developed by introducing specific aryl or aralkyl structural monomers into 1,3-bis(1-methyl-1-phenethyl)benzene compounds. and used to prepare optical lenses.
Achieving durable heat resistance and excellent optical properties, providing a solution for high refractive index and high heat resistance optical lenses.
Smart Images

Figure CN118974141A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a thermoplastic resin and an optical lens comprising the same, and more particularly to a polycarbonate resin, a polyester carbonate resin, a polyester resin and an optical lens comprising the same. Background Art
[0002] Optical glass or optical resin has been used as the material of optical lenses used in the optical systems of various cameras such as cameras, film cameras, and video cameras. Although optical glass has excellent heat resistance, transparency, dimensional stability, and chemical resistance, it has problems such as high material cost, poor molding processability, and low productivity.
[0003] On the other hand, optical lenses made of optical resins have the advantage of being able to be mass-produced by injection molding, and polycarbonate, polyester carbonate, polyester resin, etc. have been used as high-refractive index materials for camera lenses.
[0004] When optical resins are used as optical lenses, in addition to optical properties such as refractive index and Abbe number, they are also required to have heat resistance, transparency, low water absorption, chemical resistance, low birefringence, resistance to moisture and heat, etc. In recent years, in particular, due to the need for optical lenses with high refractive index and high heat resistance, various resins have been developed (Patent Documents 1 to 5).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-2893
[0008] Patent Document 2: Japanese Patent Application Publication No. 2018-2894
[0009] Patent Document 3: Japanese Patent Application Publication No. 2018-2895
[0010] Patent Document 4: Japanese Patent Application Publication No. 2018-59074
[0011] Patent Document 5: WO2017 / 078073 Summary of the invention
[0012] Problems to be solved by the invention
[0013] An object of the present invention is to provide a thermoplastic resin which maintains durable heat resistance and has excellent optical properties such as refractive index, Abbe number and photoelastic coefficient, and an optical lens using the same.
[0014] Methods for solving problems
[0015] The inventors of the present invention have repeatedly conducted intensive studies in order to solve the conventional problems, and as a result, have found that a thermoplastic resin having excellent optical properties such as refractive index, Abbe number and photoelastic coefficient and also excellent heat resistance can be obtained by using a monomer having a specific structure in which a specific aryl group or arylalkyl group is introduced into a 1,3-bis(1-methyl-1-phenylethyl)benzene compound as a raw material, thereby completing the present invention.
[0016] That is, the present invention includes the following aspects.
[0017] <1> A thermoplastic resin comprising a structural unit (A) derived from a monomer represented by the following general formula (1).
[0018]
[0019] (wherein, R1 independently represents an aryl group having 6 to 14 carbon atoms or an aralkyl group having 7 to 17 carbon atoms, R2 independently represents a hydrogen atom, an aryl group having 6 to 14 carbon atoms or an aralkyl group having 7 to 17 carbon atoms, a independently represents 0 or an integer of 1 to 3, and R3 independently represents -OH or -O-(CH2) n -OH, n represents an integer of 1 to 4. )
[0020] <2> The thermoplastic resin according to <1> above, wherein the monomer represented by the general formula (1) is a monomer represented by the following formula (1A).
[0021]
[0022] (In the formula, R1, R2 and a are the same as defined in the general formula (1).)
[0023] <3> The thermoplastic resin according to <1> above, wherein the monomer represented by the general formula (1) is a monomer represented by the following formula (5).
[0024]
[0025] <4> The thermoplastic resin according to <1> above, wherein the monomer represented by the general formula (1) is a monomer represented by the following formula (1B).
[0026]
[0027] (In the formula, R1, R2 and a are the same as defined in the general formula (1), and n independently represents an integer of 1 to 4.)
[0028] <5> The thermoplastic resin according to the above <1>, wherein the monomer represented by the general formula (1) is a monomer represented by the following formula (15).
[0029]
[0030] <6> The thermoplastic resin according to any one of <1> to <5>, wherein the thermoplastic resin is a polycarbonate resin, a polyester carbonate resin, or a polyester resin.
[0031] <7> The thermoplastic resin according to any one of <1> to <6>, wherein the thermoplastic resin comprises a structural unit (B) derived from a monomer represented by the following general formula (6) and / or a structural unit (C) derived from a monomer represented by the following general formula (7).
[0032]
[0033] (In general formula (6),
[0034] R a and R b each independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxy group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxy group having 5 to 20 carbon atoms which may have a substituent, an aryl group having 6 to 20 carbon atoms which may have a substituent, a heteroaryl group having 6 to 20 carbon atoms which may have a substituent and containing one or more heteroatoms selected from O, N and S, an aryloxy group having 6 to 20 carbon atoms which may have a substituent, and -C≡C-R h ,
[0035] R h represents an aryl group having 6 to 20 carbon atoms which may have a substituent, or a heteroaryl group having 6 to 20 carbon atoms which may have a substituent and contains one or more heteroatoms selected from O, N and S,
[0036] X represents a single bond or a fluorenyl group which may have a substituent,
[0037] A and B each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent,
[0038] m and n each independently represent an integer of 0 to 6,
[0039] a and b each independently represent an integer of 0 to 10. )
[0040]
[0041] (In general formula (7),
[0042] R c and R deach independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxy group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxy group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent,
[0043] Y1 is a single bond, a fluorenyl group which may have a substituent, or any one of the structural formulae (8) to (14) below,
[0044]
[0045] (In formulas (8) to (14),
[0046] R 61 , R 62 , R 71 and R 72 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or R 61 With R 62 Mutually bonded, or R 71 With R 72 are bonded to each other to form a carbon ring or heterocyclic ring having 1 to 20 carbon atoms which may have a substituent,
[0047] r and s each independently represent an integer from 0 to 5000. )
[0048] A and B each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent,
[0049] p and q each independently represent an integer of 0 to 4,
[0050] a and b each independently represent an integer of 0 to 10. )
[0051] <8> The thermoplastic resin according to <7> above, wherein in the general formula (6) and the general formula (7), A and B each independently represent an alkylene group having 2 or 3 carbon atoms.
[0052] <9> The thermoplastic resin according to <7> or <8>, wherein the thermoplastic resin contains at least a structural unit derived from any one of BPEF, BNE, BNEF and DPBHBNA.
[0053] <10> The thermoplastic resin according to any one of <1> to <9>, further comprising a structural unit derived from at least one monomer selected from the following monomer group.
[0054]
[0055] (In the above formula, R1 and R2 each independently represent a hydrogen atom, a methyl group or an ethyl group, and R3 and R4 each independently represent a hydrogen atom, a methyl group, an ethyl group or an alkylene glycol having 2 to 5 carbon atoms.)
[0056] <11> The thermoplastic resin according to any one of <1> to <10>, wherein the thermoplastic resin has a polystyrene-equivalent weight average molecular weight (Mw) of 10,000 to 100,000.
[0057] <12> The thermoplastic resin according to any one of <1> to <11>, wherein the refractive index (nD) of the thermoplastic resin is 1.600 to 1.700.
[0058] <13> The thermoplastic resin according to any one of <1> to <12>, wherein the thermoplastic resin has an Abbe number (ν) of 22.0 to 26.0.
[0059] <14> The thermoplastic resin according to any one of <1> to <13>, wherein the thermoplastic resin has a glass transition temperature of 70 to 200°C.
[0060] <15> The thermoplastic resin according to any one of <1> to <14>, wherein the photoelastic coefficient of the thermoplastic resin is 25 to 45.
[0061] <16> An optical lens comprising the thermoplastic resin according to any one of <1> to <15> above.
[0062] Effects of the Invention
[0063] According to the present invention, it is possible to provide a thermoplastic resin which maintains durable heat resistance and is excellent in optical properties such as refractive index, Abbe number and photoelastic coefficient, and an optical lens including the resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Figure 1 This is a diagram showing a statistical graph of differential scanning calorimetry (DSC) data of the crystals of the compound obtained in Synthesis Example 2.
[0065] Figure 2 This is a diagram showing a statistical graph of powder X-ray diffraction (PXRD) measurement of crystals of the compound obtained in Synthesis Example 2. DETAILED DESCRIPTION
[0066] Hereinafter, the present invention will be described in detail with reference to synthesis examples and examples, but the present invention is not limited to the synthesis examples and examples, and any method can be changed within the scope not greatly exceeding the scope of the present invention.
[0067] <Thermoplastic resin>
[0068] One embodiment of the present invention is a thermoplastic resin containing a structural unit (A) derived from a monomer represented by the following general formula (1).
[0069]
[0070] In the formula, R1 independently represents an aryl group having 6 to 14 carbon atoms or an aralkyl group having 7 to 17 carbon atoms, R2 independently represents a hydrogen atom, an aryl group having 6 to 14 carbon atoms or an aralkyl group having 7 to 17 carbon atoms, a independently represents 0 or an integer of 1 to 3, and R3 independently represents -OH or -O-(CH2) n -OH, n represents an integer of 1 to 4.
[0071] (R1 in the general formula (1))
[0072] R1 in the general formula (1) each independently represents an aryl group having 6 to 14 carbon atoms or an aralkyl group having 7 to 17 carbon atoms, wherein each independently preferably represents an aryl group having 6 to 14 carbon atoms or an aralkyl group having 7 to 13 carbon atoms, each independently more preferably represents an aryl group having 6 to 14 carbon atoms or an aralkyl group having 7 to 11 carbon atoms, each independently further preferably represents an aryl group having 6 to 14 carbon atoms, and each independently particularly preferably represents an aryl group having 6 to 10 carbon atoms.
[0073] Examples of the aryl group having 6 to 14 carbon atoms include phenyl, naphthyl, anthryl, and phenanthryl. Among them, phenyl and naphthyl are preferred, and phenyl is more preferred.
[0074] Examples of the aralkyl group having 7 to 17 carbon atoms include benzyl, phenethyl, 1-methyl-1-phenethyl, 1-methylnaphthyl, 2-methylnaphthyl, 1-methyl-1-(1-naphthyl)ethyl, 1-methyl-1-(2-naphthyl)ethyl, 9-methylanthracenyl, 9-methylphenanthrenyl, and the like. Among them, benzyl, 1-methyl-1-phenethyl, 1-methylnaphthyl, and 2-methylnaphthyl are preferred; benzyl, 1-methylnaphthyl, and 2-methylnaphthyl are more preferred; and benzyl is further preferred.
[0075] As R1 in the general formula (1), it is particularly preferred that both R1 are phenyl groups.
[0076] (R2 in the general formula (1))
[0077] R2 in the general formula (1) each independently represents a hydrogen atom, an aryl group having 6 to 14 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms, among which each independently preferably represents a hydrogen atom, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 13 carbon atoms, and each independently more preferably represents a hydrogen atom, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 11 carbon atoms.
[0078] Examples of the aryl group having 6 to 14 carbon atoms include phenyl, naphthyl, anthryl, and phenanthryl. Among them, phenyl and naphthyl are preferred, and phenyl is more preferred.
[0079] Examples of the aralkyl group having 7 to 17 carbon atoms include benzyl, phenethyl, 1-methyl-1-phenethyl, 1-methylnaphthyl, 2-methylnaphthyl, 1-methyl-1-(1-naphthyl)ethyl, 1-methyl-1-(2-naphthyl)ethyl, 9-methylanthracenyl, 9-methylphenanthrenyl, and the like. Among them, benzyl, 1-methyl-1-phenethyl, 1-methylnaphthyl, and 2-methylnaphthyl are preferred; benzyl, 1-methylnaphthyl, and 2-methylnaphthyl are more preferred; and benzyl is further preferred.
[0080] a in the general formula (1) each independently represents 0 or an integer of 1 to 3, each independently preferably is 0, 1 or 2, each independently more preferably is 0 or 1, and further preferably is 0. When a in the general formula (1) represents an integer of 1 to 3, it is preferred that at least one R2 and R3 are bonded at the ortho position.
[0081] (R3 in the general formula (1))
[0082] R3 in the general formula (1) independently represents -OH or -O-(CH2) n -OH.
[0083] The compound in which R3 in the general formula (1) is -OH is a compound represented by the general formula (1A) (Compound 1A).
[0084]
[0085] In the formula, R1, R2 and a are the same as defined in the general formula (1).
[0086] R3 in the general formula (1) is -O-(CH2) n The compound in the case of -OH is a compound represented by the general formula (1B) (Compound 1B).
[0087]
[0088] In the formula, R1, R2, a and n are the same as defined in the general formula (1).
[0089] n in the general formula (1B) each independently represents an integer of 1 to 4, and among them, an integer of 2 to 4 is preferred, 2 or 3 is more preferred, and 2 is particularly preferred.
[0090] Specific examples of compound 1A among the 1,3-bis(1-methyl-1-phenylethyl)benzene compounds represented by the general formula (1) in the present invention are shown below.
[0091]
[0092]
[0093]
[0094] [Method for producing monomer-1]
[0095] Regarding the 1,3-bis(1-methyl-1-phenylethyl)benzene compound represented by the general formula (1) in the present invention, the starting material and the production method in the production thereof are not particularly limited.
[0096] The method for producing compound 1A is exemplified by the following reaction formula, and an example of a method for producing compound 1A is a method of reacting a phenol compound represented by general formula (2) with α,α,α',α'-tetramethyl-1,3-benzenedimethanol.
[0097]
[0098] In the formula, R1, R2 and a are the same as defined in the general formula (1).
[0099] Specific examples of the phenol compound represented by the general formula (2) include 2-phenylphenol, 2-(1-naphthyl)phenol, 2-(2-naphthyl)phenol, 2-(9-anthryl)phenol, 2-(9-phenanthryl)phenol, 2,6-diphenylphenol, 2-benzylphenol, 2-(1-methyl-1-phenethyl)phenol, 2-(1-naphthylmethyl)phenol, 2-(2-naphthylmethyl)phenol, 2-(9-anthrylmethyl)phenol, 2-(9-phenanthrylmethyl)phenol, 2-phenyl-6-benzylphenol, 2-phenyl-6-(1-methyl-1-phenethyl)phenol, 2-phenyl-6-(1-naphthylmethyl)phenol, 2-phenyl-6-( phenol, 2-(1-naphthyl)-6-benzylphenol, 2-(1-naphthyl)-6-(1-benzyl)phenol, 2-(1-naphthyl)-6-(1-benzyl)phenol, 2-(1-naphthyl)-6-(1-methyl-1-phenylethyl)phenol, 2-(1-naphthyl)-6-(1-naphthylmethyl)phenol, 2-(1-naphthyl)-6-(2-naphthylmethyl)phenol, 2-(2-naphthyl)-6-benzylphenol, 2-(2-naphthyl)-6-(1-methyl-1-phenylethyl)phenol, 2-(2-naphthyl)-6-(1-naphthylmethyl)phenol, 2-(2-naphthyl)-6-(2-naphthylmethyl)phenol, etc.
[0100] In the production method, the amount of the phenol compound represented by the general formula (2) used is preferably 5 to 12 mol, more preferably 7 to 10 mol, and even more preferably 8 mol per mol of α,α,α',α'-tetramethyl-1,3-benzenedimethanol.
[0101] The above production method is preferably carried out in the presence of an acidic catalyst. Preferred acid catalysts include concentrated hydrochloric acid, sulfuric acid, and hydrogen chloride gas. Among them, it is more preferred to use hydrogen chloride gas until it reaches saturation in the reaction solution.
[0102] The reaction is usually carried out in the presence of a solvent. As a solvent, there is no particular limitation as long as it does not inhibit the reaction. Since compound 1A is easily soluble in various solvents, various solvents can be used. Among them, alcohols with good solubility in the phenolic compound represented by general formula (2) are preferred, and alcohols with 1 to 10 carbon atoms are more preferred, and methanol, ethanol, propanol, isopropanol are further preferred, and methanol is particularly preferred. These solvents can be used alone or in combination.
[0103] The amount of the solvent used is not particularly limited as long as it does not interfere with the reaction, but is usually preferably used in an amount within a range of 1 to 5 times by weight, more preferably 1 to 3 times by weight, and even more preferably 1 to 2 times by weight relative to α,α,α',α'-tetramethyl-1,3-benzenedimethanol.
[0104] The above-mentioned production method may be carried out in either an air atmosphere or an inert gas atmosphere, but is preferably carried out in an inert gas atmosphere such as nitrogen or argon in order to suppress coloration of the reaction product.
[0105] The reaction temperature is usually in the range of 20 to 40°C, preferably in the range of 25 to 30°C.
[0106] The reaction may be carried out under normal pressure, under increased pressure or under reduced pressure, but is preferably carried out under normal pressure.
[0107] The obtained reaction-finished mixture can be separated and purified according to conventional methods to obtain compound 1A from the reaction mixture. For example, in order to neutralize the acid catalyst, an alkaline aqueous solution such as an aqueous sodium hydroxide solution and an aqueous ammonia solution is added to the reaction-finished solution to neutralize the acid catalyst. The neutralized reaction mixture is allowed to stand, and a solvent separated from water is added as needed to separate and remove the water layer. As needed, the operation of adding distilled water to the obtained oil layer, stirring and washing with water, and then separating and removing the water layer is performed once or repeatedly to remove the neutralization salt. By distilling and removing the residual raw materials, solvents, etc. from the obtained oil layer, the target product compound 1A can be obtained as a residual liquid.
[0108] Specific examples of compound 1B of the 1,3-bis(1-methyl-1-phenylethyl)benzene compound represented by general formula (1) in the present invention are shown below.
[0109]
[0110]
[0111]
[0112] <Method for producing monomer-2>
[0113] As a method for producing compound 1B, there can be mentioned a method of reacting a compound represented by general formula (1A) with an oxyalkylene agent. As the oxyalkylene agent, a reaction formula in the case of using a carbonate represented by general formula (3) is exemplified.
[0114]
[0115] In the formula, R1, R2, a and n are the same as defined in the general formula (1).
[0116] In the above production method, the compound 1A represented by the general formula (1A) can be the compound obtained by the above production method-1. As the oxyalkylene agent, for example, carbonates represented by the general formula (3) such as ethylene carbonate, 2-chloroethanol, 3-chloro-1-propanol and other halogenated alcohols can be used depending on the target compound.
[0117] The following describes the case where the carbonate represented by the general formula (3) is used as the oxyalkylenating agent in the above production method.
[0118] The raw material molar ratio of compound 1A to carbonate ester is generally in the range of about 1 / 2 to 1 / 5, preferably in the range of about 1 / 2 to 1 / 4, and more preferably in the range of about 1 / 2 to 1 / 3.
[0119] In the above-mentioned production method, it is preferred to use a basic catalyst during the reaction. As the basic catalyst, a commonly known catalyst can be used. Specifically, quaternary ammonium salts such as tetraethylammonium bromide and tetramethylammonium chloride, alkali metal halide salts such as potassium hydroxide, potassium iodide and sodium bromide, triphenylphosphine, tributylphosphine and other triorganophosphine compounds, amine catalysts such as 1-methylimidazole, potassium carbonate, calcium carbonate, magnesium carbonate, magnesium hydroxide, calcium hydroxide, sodium hydroxide, sodium bicarbonate, sodium methoxide and sodium phenolate can be listed. These basic catalysts can be used alone or in combination of two or more.
[0120] The amount of the basic catalyst used is 0.001 to 10% by weight, preferably 0.01 to 1% by weight, based on the compound 1A represented by the general formula (1A).
[0121] Although the reaction can be carried out in the absence of a solvent by using an excess of carbonate, it is generally preferred to use an organic solvent from the viewpoint of economic efficiency and operability.
[0122] When a reaction solvent is used, various known solvents that are inert to the reaction can be used. Examples of such reaction solvents include aromatic hydrocarbons such as toluene and xylene, ether solvents such as tetrahydrofuran, dioxane, and 1,2-dimethoxyethane, ketone solvents such as acetone and methyl isobutyl ketone, halogenated hydrocarbons such as chloroform and 1,2-dichloroethane, aliphatic alcohols such as butanol and ethylene glycol, and polar solvents such as dimethylformamide and dimethyl sulfoxide.
[0123] The amount of the reaction solvent used is not particularly limited, but is preferably in the range of 0.5 to 10 times by weight, more preferably 0.5 to 5 times by weight, relative to Compound 1A.
[0124] The above-mentioned production method may be carried out in either an air atmosphere or an inert gas atmosphere. However, in order to suppress coloration of the reaction product, it is preferably carried out in an inert gas atmosphere such as nitrogen or argon.
[0125] The reaction temperature is not particularly limited as long as the reaction proceeds, and the reaction is usually carried out under heating, for example, at a temperature of 100° C. to 250° C., preferably under reflux of the solvent.
[0126] The reaction time depends on the reaction temperature, the amount and type of carbonates and basic catalysts used, and is usually about 3 to 24 hours. In this reaction, the moment when the generation of carbon dioxide gas is suppressed is regarded as the sign of the completion of the reaction.
[0127] The obtained reaction-completed mixture can be separated and purified according to a conventional method to obtain Compound 1B from the reaction mixture.
[0128] When a basic catalyst is used, acidic water (for example, hydrochloric acid, sulfuric acid), acetic acid, propionic acid, etc. are added thereto for neutralization. This neutralization step may be performed after the hydrolysis step described later.
[0129] In this reaction, due to the addition of excessive carbonates, even after the reaction is completed, carbonates will remain in the reaction solution. Once heated in this state, side reactions will occur, and the purity and yield of the target compound compound 1B may be reduced. Therefore, it is preferred to add water to carry out the hydrolysis step of carbonates. The amount of water used is in the range of 1 to 10 molar times relative to the amount of carbonates used in the above reaction.
[0130] The temperature may be lower than the boiling point of the reaction solution, and is usually in the range of room temperature to lower than the boiling point of the reaction solution. Specifically, the lower limit is 10° C. or higher, more preferably 20° C. or higher. The upper limit depends on the boiling point of the solvent used, but is preferably 150° C. or lower.
[0131] Then, as needed, after adding a solvent that separates from water, the oil layer can be washed with water several times, the water layer can be separated and removed, and low-boiling substances such as the solvent can be distilled off from the obtained oil layer under reduced pressure, and then washed with water, crystallized, filtered, distilled, column chromatographed, etc., to perform post-treatment operations such as separation and drying. In order to further improve the purity, further purification such as distillation, recrystallization, column chromatography, etc. can be performed according to conventional methods.
[0132] Since the crystals of 1,3-bis[1-methyl-1-(4-(2-hydroxyethoxy)-3-phenylphenyl)ethyl]benzene represented by the following formula (15) in the compound 1B of the present invention can be handled as a crystalline solid, it is very useful in the industrial production of thermoplastic resins due to its excellent handleability and transportability.
[0133]
[0134] The peak top temperature of the endothermic peak of the crystals of 1,3-bis[1-methyl-1-(4-(2-hydroxyethoxy)-3-phenylphenyl)ethyl]benzene represented by the above formula (15) obtained by differential scanning calorimetry is in the range of 134 to 140°C, more preferably in the range of 135 to 139°C, and particularly preferably in the range of 136 to 139°C.
[0135] In addition, the crystal of 1,3-bis[1-methyl-1-(4-(2-hydroxyethoxy)-3-phenylphenyl)ethyl]benzene represented by the above formula (15) has diffraction peaks at diffraction angles 2θ of 7.9±0.2°, 10.8±0.2°, 16.3±0.2°, and 18.6±0.2° in the powder X-ray diffraction peak pattern of Cu-Kα rays. In addition, it may also have peaks at diffraction angles 2θ of 12.8±0.2°, 14.9±0.2°, 20.2±0.2°, and 24.1±0.2°.
[0136] The crystalline purity of 1,3-bis[1-methyl-1-(4-(2-hydroxyethoxy)-3-phenylphenyl)ethyl]benzene represented by the above formula (15) is preferably 90% or more in area percentage as determined by liquid chromatography analysis, more preferably 93% or more, further preferably 95% or more, and particularly preferably 98% or more.
[0137] The crystals of the compound represented by the above formula (15) can be obtained by precipitating the compound from a solution dissolved in a chain aliphatic ketone solvent having 5 to 8 carbon atoms. The compound used here can be a compound obtained by the above method. When the compound represented by the above formula (15) is precipitated from a solution dissolved in a chain aliphatic ketone solvent having 5 to 8 carbon atoms, the precipitation can be carried out by cooling the solution and removing the solvent of the solution by distillation. The solution obtained by mixing a chain or cyclic aliphatic hydrocarbon solvent having 5 to 10 carbon atoms into a solution of the compound dissolved in a chain aliphatic ketone solvent having 5 to 8 carbon atoms is preferably cooled to precipitate the compound in order to further reduce the solubility of the solution.
[0138] As the chain aliphatic ketone solvent having 5 to 8 carbon atoms, diethyl ketone (carbon number 5), methyl isobutyl ketone (carbon number 6), methyl amyl ketone (carbon number 7), methyl hexyl ketone (carbon number 8) and the like can be used, among which methyl isobutyl ketone and methyl amyl ketone are preferred. By using such an organic solvent, the solution can be washed with water before crystallization, and water-soluble impurities such as salts can also be removed.
[0139] The amount of the chain aliphatic ketone solvent used is preferably in the range of 1 to 7 times by weight, more preferably 1.5 to 6 times by weight, and further preferably 2 to 5 times by weight, relative to the weight of the compound represented by the above formula (15).
[0140] As the linear or cyclic aliphatic hydrocarbon solvent having 5 to 10 carbon atoms, pentane, hexane, heptane, octane, isooctane, cyclopentane, cyclohexane and the like can be used. Among them, cyclic aliphatic hydrocarbon solvent having 5 to 10 carbon atoms is preferred, and cyclopentane or cyclohexane is more preferred.
[0141] The amount of the aliphatic hydrocarbon solvent used is preferably in the range of 1 to 10 times by weight, more preferably 1 to 7 times by weight, and even more preferably 1 to 5 times by weight, relative to the amount of the compound represented by the above formula (15).
[0142] The temperature of mixing the chain or cyclic aliphatic hydrocarbon solvent having 5 to 10 carbon atoms with the chain aliphatic ketone solution having 5 to 8 carbon atoms of the compound represented by the above formula (15) depends on the chain aliphatic ketone solution used, and is preferably in the range of 60 to 120°C, more preferably in the range of 60 to 100°C, and further preferably in the range of 60 to 90°C.
[0143] The temperature at which the crystals of the compound represented by the above formula (15) begin to precipitate is preferably in the range of 10 to 50°C, more preferably in the range of 15 to 40°C.
[0144] The separation of the crystals obtained by the above method can be carried out according to conventional methods, for example, the crystals can be separated by centrifugal filtration, etc. In addition, it is preferred to further wash the crystals with a solvent. The solvent used can be removed by drying the obtained crystals.
[0145] The thermoplastic resin of one embodiment of the present invention is not particularly limited to polyester resin, polycarbonate resin, polyester carbonate resin, epoxy resin, polyurethane resin, polyacrylate resin, polymethacrylate resin, etc., preferably a polycarbonate resin, polyester carbonate resin or polyester resin, and more preferably contains a structural unit (A) represented by the following formula.
[0146]
[0147] In the formula, R1, R2 and a are the same as defined in the general formula (1).
[0148] In the thermoplastic resin of one embodiment of the present invention, the ratio of the structural unit (A) represented by the above formula in all structural units is not particularly limited, but is preferably 1 to 80 mol %, more preferably 1 to 60 mol %, and particularly preferably 5 to 50 mol % in all structural units.
[0149] That is, the thermoplastic resin according to one embodiment of the present invention may contain, in addition to the structural unit (A) represented by the above formula, structural units derived from aliphatic dihydroxy compounds and structural units derived from aromatic dihydroxy compounds, which are generally used as structural units of polycarbonate resins, polyester carbonate resins, etc.
[0150] Specifically, various compounds can be mentioned as the aliphatic dihydroxy compound, and in particular, 1,4-cyclohexanedimethanol, tricyclodecanedimethanol, 1,3-adamantanedimethanol, 2,2-bis(4-hydroxycyclohexyl)-propane, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 2-(5-ethyl-5-hydroxymethyl-1,3-dioxane-2-yl)-2-methylpropane-1-ol, isosorbide, 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, and the like can be mentioned.
[0151] Examples of the aromatic dihydroxy compound include various compounds, and in particular, examples include 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 4,4'-dihydroxybiphenyl, bis(4-hydroxyphenyl)cycloalkane, bis(4-hydroxyphenyl)oxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)ketone, and bisphenoxyethanolfluorene.
[0152] Furthermore, the thermoplastic resin according to one embodiment of the present invention preferably includes a structural unit (B) derived from a monomer represented by the following general formula (6).
[0153]
[0154] In the general formula (6), R a and R b each independently selected from a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxy group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxy group having 5 to 20 carbon atoms which may have a substituent, an aryl group having 6 to 20 carbon atoms which may have a substituent, a heteroaryl group having 6 to 20 carbon atoms which may have a substituent and containing one or more heteroatoms selected from O, N and S, an aryloxy group having 6 to 20 carbon atoms which may have a substituent, and -C≡C-R h . R h The aryl group represents an optionally substituted aryl group having 6 to 20 carbon atoms or an optionally substituted heteroaryl group having 6 to 20 carbon atoms containing one or more heteroatoms selected from O, N and S.
[0155] R a and R b Preferred are a hydrogen atom, an aryl group having 6 to 20 carbon atoms which may have a substituent, and a heteroaryl group having 6 to 20 carbon atoms which may have a substituent and contains one or more heterocyclic atoms selected from O, N and S. More preferred are a hydrogen atom and an aryl group having 6 to 20 carbon atoms which may have a substituent, and further preferred are a hydrogen atom and an aryl group having 6 to 12 carbon atoms which may have a substituent.
[0156] In the general formula (6), X represents a single bond or a fluorenyl group which may have a substituent. X is preferably a single bond or a fluorenyl group which may have a substituent having 12 to 20 carbon atoms in total.
[0157] In the general formula (6), A and B are each independently an alkylene group having 1 to 5 carbon atoms which may have a substituent, and preferably an alkylene group having 2 or 3 carbon atoms.
[0158] In the general formula (6), m and n are each independently an integer of 0 to 6, preferably an integer of 0 to 3, and more preferably 0 or 1.
[0159] In the general formula (6), a and b are each independently an integer of 0 to 10, preferably an integer of 1 to 3, and more preferably 1 or 2.
[0160] Specific examples of the structural unit (B) include structural units derived from 2,2′-bis(2-hydroxyethoxy)-1,1′-binaphthyl (BNE), DPBHBNA, and the like.
[0161]
[0162] Furthermore, the thermoplastic resin according to one embodiment of the present invention preferably has a structural unit (C) derived from a monomer represented by the following general formula (7).
[0163]
[0164] In the general formula (7), R c and R d Each is independently selected from a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxy group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxy group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent.
[0165] In the general formula (7), R c and R dPreferred are a hydrogen atom, an aryl group having 6 to 20 carbon atoms which may have a substituent, and a heteroaryl group having 6 to 20 carbon atoms which may have a substituent and contains one or more heterocyclic atoms selected from O, N and S. More preferred are a hydrogen atom and an aryl group having 6 to 20 carbon atoms which may have a substituent, and further preferred are a hydrogen atom and an aryl group having 6 to 12 carbon atoms which may have a substituent.
[0166] In the general formula (7), Y1 is a single bond, a fluorenyl group which may have a substituent, or any of the structural formulae (8) to (14) below, and is preferably a single bond or the structural formula (8) below.
[0167]
[0168] In formulas (8) to (14), R 61 , R 62 , R 71 and R 72 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or represents R 61 With R 62 Mutually bonded, or R 71 With R 72 are bonded to each other to form a carbon ring or heterocyclic ring having 1 to 20 carbon atoms which may have a substituent,
[0169] In formulae (8) to (14), r and s each independently represent an integer of 0 to 5000.
[0170] In the above general formula (7), A and B are each independently an alkylene group having 1 to 5 carbon atoms which may have a substituent, and preferably an alkylene group having 2 or 3 carbon atoms. In the above general formula (7), p and q are each independently an integer of 0 to 4, and preferably 0 or 1. In addition, in the above general formula (7), a and b are each independently an integer of 0 to 10, and preferably an integer of 0 to 5, and more preferably an integer of 0 to 2, for example, 0 or 1.
[0171] Specific examples of the structural unit (C) include bisphenols derived from BPEF (9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene), BPPEF (9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene), 9,9-bis[6-(2-hydroxyethoxy)naphth-2-yl]fluorene (BNEF), bisphenol A, bisphenol AP, bisphenol AF, bisphenol B, bisphenol BP, bisphenol C, bis(4-hydroxyphenyl)-2,2-dichloroethylene, bisphenol E, bisphenol F, bisphenol G, bisphenol B, bisphenol C, bisphenol E, bisphenol F, bisphenol G, bisphenol A, bisphenol A, bisphenol A, bisphenol A, bisphenol B, bisphenol B, bisphenol C, bis(4-hydroxyphenyl)-2,2-dichloroethylene, bisphenol E, bisphenol F, bisphenol G, bisphenol B, bisphenol A, bisphenol A, bisphenol A, bisphenol A, bisphenol A, bisphenol A, bisphenol A, bisphenol B, bisphenol B, bisphenol C, bis(4-hydroxyphenyl)-2,2-dichloroethylene, bisphenol E, bisphenol F, bisphenol G, bisphenol A ... Bisphenol M, bisphenol S, bisphenol P, bisphenol PH, bisphenol TMC, bisphenol P-AP (4,4'-(1-phenylethylidene) bisphenol), bisphenol P-CDE (4,4'-cyclododecylidene bisphenol), bisphenol P-HTG (4,4'-(3,3,5-trimethylcyclohexylidene) bisphenol), bisphenol P-MIBK (4,4'-(1,3-dimethylbutylidene) bisphenol), bisphenol PEO-FL (bisphenoxyethanol fluorene), bisphenol P-3MZ (4-[1-(4-hydroxyphenyl)-3-methylcyclohexylidene) bisphenol bisphenol Z, BP-2EO (2,2'-[[1,1'-biphenyl]-4,4'-diylbis(oxy)diethanol), S-BOC (4,4'-(1-methylethylidene)bis(2-methylphenol)), TrisP-HAP (4,4',4"-ethylenetriphenol), 1,1-bis(4-hydroxyphenyl)-1-phenyl Structural units such as ethane (BPAP), 1,1-bis(4-hydroxyphenyl)cyclododecane (HPCD), 1,1-bis(4-hydroxyphenyl)cyclohexane (BPZ), 9,9-bis(4-hydroxy-3-methylphenyl)fluorene (BCFL), bis(4-hydroxyphenyl)diphenylmethane (BPBP), and 1,3-bis(1-methyl-1-phenylethyl)benzene (BPM). Among these, the structural unit (C) preferably includes a structural unit derived from BPEF, BNEF, or BCFL.
[0172]
[0173] In the thermoplastic resin of one embodiment of the present invention, the structural unit (A) is essential, and in addition to a polymer containing the structural unit (B) but not containing the structural unit (C), a polymer containing the structural unit (C) but not containing the structural unit (B), a copolymer having the structural unit (B) and the structural unit (C), a mixture of a polymer having the structural unit (B) and a polymer having the structural unit (C), and a combination thereof. As the polymer containing the structural unit (C) but not containing the structural unit (B), for example, a polymer having the structural unit of the following formula (I-1) to (I-3) can be cited, and as the copolymer having the structural unit (B) and the structural unit (C), for example, a copolymer having the structural unit of the following formula (II-1) to (II-4) can be cited.
[0174]
[0175] (In formula (I-1), m and n are each an integer of 1 to 10, preferably an integer of 1 to 5, and more preferably 1.
[0176] The number of repeating units in formula (I-3) is an integer of 1 to 10, preferably an integer of 1 to 5, and more preferably 1.)
[0177] Furthermore, as the polymer having multiple structural units, any of block copolymers and random copolymers having m and n values as large as 100 or more can be used, and a random copolymer is preferred, and a random copolymer having m and n values of 1 is more preferred.
[0178]
[0179] (In formulae (II-1) to (II-4), m and n are each independently an integer of 1 to 10, preferably an integer of 1 to 5, and more preferably 1.)
[0180] In addition, as a polymer having multiple structural units, any block copolymer and random copolymer in which the values of m and n (or m, n and l) are large, for example, 100 or more can be used, preferably a random copolymer, and more preferably a random copolymer in which the values of m and n (or m, n and l) are 1.
[0181] In the copolymer, the molar ratio of the structural unit (B) to the structural unit (C) is preferably 1:99 to 99:1, more preferably 10:90 to 90:10, further preferably 15:85 to 85:15, and particularly preferably 30:70 to 70:30. In addition, in the mixture, the mass ratio of the polymer having the structural unit (B) to the polymer having the structural unit (C) is preferably 1:99 to 99:1, more preferably 10:90 to 90:10, further preferably 15:85 to 85:15, and particularly preferably 30:70 to 70:30.
[0182] The thermoplastic resin according to one embodiment of the present invention preferably further includes a structural unit derived from at least one monomer selected from the following monomer group.
[0183]
[0184] (In the above formula, R1 and R2 each independently represent a hydrogen atom, a methyl group or an ethyl group, and R3 and R4 each independently represent a hydrogen atom, a methyl group, an ethyl group or an alkylene glycol having 2 to 5 carbon atoms.)
[0185] In addition, the thermoplastic resin of one embodiment of the present invention preferably has a structural unit (D) derived from a monomer represented by the following general formula (16). In this case, the content of the structural unit (D) derived from the monomer represented by the general formula (16) is preferably 1 to 50 mol%, more preferably 1 to 30 mol% in all structural units.
[0186]
[0187] In general formula (16),
[0188] L 1 Each independently represents a divalent linking group; R 3 and R 4 j3 and j4 each independently represent an integer of 0 to 4; and t represents an integer of 0 or 1.
[0189] In the above general formula (16), L 1 Each independently represents a divalent linking group. 1 It is preferably an alkylene group having 1 to 12 carbon atoms which may have a substituent, more preferably an alkylene group having 1 to 5 carbon atoms, further preferably an alkylene group having 2 or 3 carbon atoms, and particularly preferably an ethylene group. 1 The substituent of the alkylene group includes an alkyl group, a cycloalkyl group, an aryl group, an alkoxy group and a combination thereof. Specific examples of these groups include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a phenyl group, a methoxy group, an ethoxy group and the like.
[0190] In the presence of R 3 and R 4In the case of , each independently represents a halogen atom or a substituent having 1 to 20 carbon atoms which may contain an aromatic group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and the like. Examples of the substituent having 1 to 20 carbon atoms which may contain an aromatic group include a methyl group, a phenyl group, a naphthyl group, a thienyl group, and a benzothienyl group. Examples of the naphthyl group include 1-naphthyl and 2-naphthyl group. Examples of the thienyl group include 2-thienyl and 3-thienyl group. In addition, examples of the benzothienyl group include 2-benzo[b]thienyl and 3-benzo[b]thienyl. These groups may further have a substituent, and examples of such a substituent include the above-mentioned L 1 The substituents of the alkylene group are described in the foregoing, but are not limited thereto.
[0191] j3 and j4 each independently represent an integer of 0 to 4. j3 and j4 are preferably integers of 0 to 2, more preferably 0 or 1, and particularly preferably 0.
[0192] t represents an integer of 0 or 1, and is preferably 1.
[0193] The monomer represented by the general formula (16) preferably has a structure represented by the following formula (16').
[0194]
[0195] In the polycarbonate resin of a preferred embodiment of the present invention, alcohol compounds such as phenolic compounds which may be produced as by-products during the production process, diol components which remain without participating in the reaction, and carbonic acid diesters may exist as impurities.
[0196] Since alcohol compounds such as phenolic compounds and carbonic acid diesters as impurities may cause a decrease in the strength of a molded body and generate odorous gas, their content is preferably as small as possible.
[0197] The content of the residual phenolic compound is preferably 3000 ppm by mass or less, more preferably 1000 ppm by mass or less, and particularly preferably 300 ppm by mass or less, based on 100% by mass of the polycarbonate resin.
[0198] The content of the remaining diol component relative to 100 mass % of the polycarbonate resin is preferably 1000 mass ppm or less, more preferably 100 mass ppm or less, particularly preferably 10 mass ppm or less.
[0199] The content of the residual carbonic acid diester relative to 100 mass % of the polycarbonate resin is preferably 1000 mass ppm or less, more preferably 100 mass ppm or less, particularly preferably 10 mass ppm or less.
[0200] In particular, the content of compounds such as phenol and tert-butylphenol is preferably small, and the content of these compounds is preferably within the above range.
[0201] The content of the phenolic compound remaining in the polycarbonate resin can be measured by a method of analyzing the phenolic compound extracted from the polycarbonate resin using gas chromatography.
[0202] The content of the alcohol compound remaining in the polycarbonate resin can also be measured by analyzing the alcohol compound extracted from the polycarbonate resin using gas chromatography.
[0203] The contents of the diol component and the carbonic acid diester remaining in the polycarbonate resin can also be measured by extracting these compounds from the polycarbonate resin and analyzing them using gas chromatography.
[0204] The content of alcohol compound byproducts such as phenolic compounds, diol components and carbonic acid diesters can be reduced to an undetectable level, but from the perspective of productivity, they can also be contained in trace amounts within a range that does not impair the effect. In addition, if they are in trace amounts, plasticity can also be improved during the resin melting period.
[0205] The content of each of the remaining phenolic compound, the diol component, and the carbonic acid diester relative to 100 mass % of the polycarbonate resin may be, for example, 0.01 mass ppm or more, 0.1 mass ppm or more, or 1 mass ppm or more.
[0206] The content of the residual alcohol compound relative to 100 mass % of the polycarbonate resin may be, for example, 0.01 mass ppm or more, 0.1 mass ppm or more, or 1 mass ppm or more.
[0207] It should be noted that the content of alcohol compound byproducts such as phenolic compounds, diol components and carbonic acid diesters in the polycarbonate resin can be adjusted to the above range by appropriately adjusting the polycondensation conditions and device settings, etc. In addition, it can also be adjusted by the conditions of the extrusion process after polycondensation.
[0208] For example, the residual amount of alcohol byproducts such as phenolic compounds is related to the type of carbonic acid diester used in the polymerization of polycarbonate resin, polymerization reaction temperature and polymerization pressure, etc. By adjusting these conditions, the residual amount of alcohol byproducts such as phenolic compounds can be reduced.
[0209] For example, when using dialkyl carbonates such as diethyl carbonate to make polycarbonate resin, there is a trend that the molecular weight is difficult to increase, becomes low-molecular-weight polycarbonate, and the content of the byproduct alkyl alcohol compounds increases. The volatility of such alkyl alcohol is high, and when remaining in polycarbonate resin, there is a trend that the moldability of resin deteriorates. In addition, when the residual amount of alcohol compound byproducts such as phenolic compounds is many, the problem of generating odorous gas may occur when resin is molded, or the cracking reaction of resin skeleton may occur when blending, so that the molecular weight is reduced. Therefore, relative to polycarbonate resin (100 mass %), the content of the alcohol compound byproduct remaining in the obtained polycarbonate resin is preferably below 3000 mass ppm. Relative to polycarbonate resin 100 mass %, the content of the alcohol compound remaining is preferably below 3000 mass ppm, more preferably below 1000 mass ppm, and particularly preferably below 300 mass ppm.
[0210] <Physical properties of thermoplastic resin>
[0211] (1) Refractive index (nD)
[0212] In one embodiment of the present invention, one of the characteristics of the thermoplastic resin is a high refractive index, and the refractive index is preferably 1.600 to 1.700, more preferably 1.626 to 1.700, and particularly preferably 1.630 to 1.650. In the present invention, the refractive index can be measured by the method described in the Examples below.
[0213] (2) Abbe number (ν)
[0214] In one embodiment of the present invention, the Abbe number of the thermoplastic resin is preferably 22.0 to 26.0, more preferably 23.0 to 26.0, and particularly preferably 23.0 to 24.7. In the present invention, the Abbe number can be measured by the method described in the Examples described below.
[0215] (3) Glass transition temperature (Tg)
[0216] In one embodiment of the present invention, one of the characteristics of the thermoplastic resin is high heat resistance, and the glass transition temperature (Tg) is preferably 70 to 200° C., more preferably 100 to 200° C., further preferably 100 to 150° C., further preferably 125 to 150° C., further preferably 125 to 145° C., and particularly preferably 125 to 140° C. In the present invention, the glass transition temperature can be measured by the method described in the Examples described below.
[0217] (4) Weight average molecular weight (Mw) calculated as polystyrene
[0218] In one embodiment of the present invention, the polystyrene-equivalent weight average molecular weight of the thermoplastic resin is preferably 10,000 to 100,000, more preferably 10,000 to 80,000, and particularly preferably 10,000 to 60,000.
[0219] (5) Photoelastic coefficient
[0220] In one embodiment of the present invention, one of the characteristics of the thermoplastic resin is that the photoelastic coefficient is low, and the photoelastic coefficient is preferably 25 to 45, more preferably 25 to 38, and particularly preferably 30 to 38. In the present invention, the photoelastic coefficient can be measured by the method described in the Examples described below.
[0221] <Thermoplastic resin composition>
[0222] Another embodiment of the present invention is a thermoplastic resin composition comprising the above-mentioned thermoplastic resin and an additive. The thermoplastic resin composition of this embodiment can be used in combination with a resin other than the thermoplastic resin of the present invention comprising the above-mentioned structural unit (A) within the range that does not impair the expected effect of the present embodiment. Such a resin is not particularly limited, and examples thereof include at least one resin selected from polycarbonate resins, polyester resins, polyester carbonate resins, (meth) acrylic resins, polyamide resins, polystyrene resins, cycloolefin resins, acrylonitrile-butadiene-styrene copolymer resins, vinyl chloride resins, polyphenylene ether resins, polysulfone resins, polyacetal resins, and methyl methacrylate-styrene copolymer resins. These resins can use various known resins, and can be used alone or in combination of two or more and added to the thermoplastic resin composition.
[0223] [Antioxidant]
[0224] The thermoplastic resin composition preferably contains an antioxidant as the above-mentioned additive.
[0225] As the antioxidant, at least one of a phenolic antioxidant and a phosphite antioxidant is preferably contained.
[0226] Examples of phenolic antioxidants include 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-2,4,6-trimethylbenzene, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 4,4',4"-(1-methylpropyl-3-ylidene)tris(6-tert-butyl-m-cresol), 6,6'-di-tert-butyl-4,4'-butylene-m-cresol, 3-(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione,
[0063] octadecyl tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxospiro[5.5]undecane, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] are preferred.
[0227] Examples of the phosphite antioxidant include 2-ethylhexyl diphenyl phosphite, isodecyl diphenyl phosphite, triisodecyl phosphite, triphenyl phosphite, 3,9-bis(octadecanoyloxy)-2,4,8,10-tetraoxo-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 2,2'-methylenebis(4,6-di-tert-butylphenyl)-2-ethylhexyl diphenyl phosphite, and 1,2-diisodecyl diphenyl phosphite. Phosphate, tris(2,4-di-tert-butylphenyl)phosphite, tris(nonylphenyl)phosphite, tetra-C12-15 alkyl (propane-2,2-diylbis(4,1-phenylene))bisphosphite, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, etc., preferably 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane.
[0228] As the antioxidant, any one of the above may be used alone, or a mixture of two or more may be used.
[0229] The thermoplastic resin composition preferably contains 1 wtppm to 3000 wtppm of an antioxidant based on the total weight of the resin composition. The content of the antioxidant in the thermoplastic resin composition is more preferably 50 wtppm to 2500 wtppm, further preferably 100 wtppm to 2000 wtppm, particularly preferably 150 wtppm to 1500 wtppm, and further preferably 200 wtppm to 1200 wtppm.
[0230] [Release agent]
[0231] The thermoplastic resin composition preferably contains a release agent as the above-mentioned additive.
[0232] Examples of the release agent include ester compounds, such as fatty acid glycerol esters such as monoglycerol and diglycerol of glycerol fatty acid, glycol fatty acid esters such as propylene glycol fatty acid ester and sorbitan fatty acid ester, higher alcohol fatty acid ester, full ester or mono fatty acid ester of aliphatic polyol and aliphatic carboxylic acid, etc. When an ester of aliphatic polyol and aliphatic carboxylic acid is used as the release agent, any of monoester and full ester may be used, and esters other than full esters such as monoester may also be used.
[0233] Specific examples of the release agent include the following compounds.
[0234] That is, sorbitan fatty acid esters such as sorbitan stearate, sorbitan laurate, sorbitan oleate, sorbitan trioleate, sorbitan tribehenate, sorbitan stearate, sorbitan tristearate, and sorbitan caprylate can be cited;
[0235] Propylene glycol fatty acid esters such as propylene glycol monostearate, propylene glycol monooleate, propylene glycol monobehenate, propylene glycol monolaurate, and propylene glycol monopalmitate;
[0236] Higher alcohol fatty acid esters such as stearyl stearate;
[0237] Glycerol fatty acid esters Monoglycerides, including: glycerol monostearate and glycerol mono-12-hydroxystearate, glycerol monohydroxystearate, glycerol monooleate, glycerol monobehenate, glycerol monocaprylate, glycerol monocaprate, glycerol monolaurate, etc.; glycerol mono / diester of glycerol mono / distearate, glycerol mono / distearate, glycerol mono / dibehenate, glycerol mono / dioleate, etc.;
[0238] Glycerol fatty acid esters such as glyceryl diacetyl monolaurate, acetylated monoglycerides;
[0239] Glycerol fatty acid ester organic acid monoglyceride such as citric acid fatty acid monoglyceride, succinic acid fatty acid monoglyceride, diacetyltartaric acid fatty acid monoglyceride;
[0240] Stearic acid diglyceride, lauric acid diglyceride, oleic acid diglyceride, monostearic acid diglyceride, monolauric acid diglyceride, monomyristic acid diglyceride, monooleic acid diglyceride, stearic acid tetraglyceride, lauric acid decaglyceride, oleic acid decaglyceride, polyglycerol polyricin esters and other polyglycerol fatty acid esters, etc.
[0241] The thermoplastic resin composition preferably contains 1 wtppm to 5000 wtppm of a release agent based on the total weight of the resin composition. The content of the release agent in the thermoplastic resin composition is more preferably 50 wtppm to 4000 wtppm, further preferably 100 wtppm to 3500 wtppm, particularly preferably 500 wtppm to 13000 wtppm, and further preferably 1000 wtppm to 2500 wtppm.
[0242] [Other additives]
[0243] In addition to the above-mentioned antioxidant and release agent, other additives may be added to the thermoplastic resin composition. For example, additives that may be included in the thermoplastic resin composition include compounding agents, catalyst deactivators, heat stabilizers, plasticizers, fillers, ultraviolet absorbers, rust inhibitors, dispersants, defoamers, leveling agents, flame retardants, lubricants, dyes, pigments, bluing agents, nucleating agents, clarifiers, and the like.
[0244] The content of additives other than the antioxidant and the release agent in the thermoplastic resin composition is preferably 10 ppm to 5.0 wt%, more preferably 100 ppm to 2.0 wt%, further preferably 1000 ppm to 1.0 wt%, but is not limited thereto.
[0245] The above-mentioned additives may have an adverse effect on light transmittance, and therefore, are preferably not added in excess. For example, the total amount added is within the above-mentioned range.
[0246] <Optical Components>
[0247] The thermoplastic resin or thermoplastic resin composition of the present invention (hereinafter abbreviated as "resin composition") can be applied to optical elements. In one embodiment of the present invention, an optical element comprising the resin composition of the present invention is provided. In one embodiment of the present invention, the optical element includes an optical disc, a transparent conductive substrate, an optical card, a sheet, a film, an optical fiber, a lens, a prism, an optical film, a substrate, an optical filter, a hard coating, etc., but is not limited thereto. Since the resin composition of the present invention has high fluidity and can be formed by a casting method, it is particularly suitable for the manufacture of thin optical elements. In a preferred embodiment of the present invention, the optical element material manufactured using the resin composition of the present invention can be an optical lens. In another preferred embodiment of the present invention, the optical element material manufactured using the resin composition of the present invention can be an optical film.
[0248] When an optical element comprising the resin composition of the present invention is manufactured by injection molding, it is preferably molded under the conditions of a barrel temperature of 260 to 350°C and a mold temperature of 90 to 170°C. More preferably, it is molded under the conditions of a barrel temperature of 270 to 320°C and a mold temperature of 100 to 160°C. When the barrel temperature is higher than 350°C, the resin composition will decompose and color, and when it is lower than 260°C, the melt viscosity is high, making molding difficult. In addition, when the mold temperature is higher than 170°C, it becomes difficult to remove the molded piece made of the resin composition from the mold. On the other hand, when the mold temperature is lower than 90°C, during the molding process, the resin solidifies prematurely in the mold, and it becomes difficult to control the shape of the molded piece, or it becomes difficult to fully transfer the shaping attached to the mold.
[0249] <Optical lens>
[0250] In one embodiment of the present invention, the resin composition can be applied to an optical lens. Since the optical lens manufactured using the resin composition of the present invention has a high refractive index and good heat resistance, it can be used in fields such as telescopes, binoculars, and television projectors that have previously used expensive high-refractive-index glass lenses, which is extremely useful.
[0251] For example, in a smartphone lens, a lens molded from a thermoplastic resin containing the above-mentioned structural unit (A) can be superimposed on a resin containing a structural unit of any one of formulas (II-1) to (II-4) or a lens molded from a resin containing a structural unit derived from a monomer of any of the following formulas and used as a lens unit.
[0252]
[0253] (In the above formula, R1 and R2 each independently represent a hydrogen atom, a methyl group or an ethyl group, and R3 and R4 each independently represent a hydrogen atom, a methyl group, an ethyl group or an alkylene glycol having 2 to 5 carbon atoms.)
[0254] The optical lens of the present invention can be appropriately implemented using the form of an aspherical lens as needed. Since the aspherical lens can achieve substantially zero spherical aberration with a single lens, there is no need to eliminate spherical aberration by combining multiple spherical lenses, which can achieve lightweighting and reduced molding costs. Therefore, the aspherical lens is particularly useful as a camera lens among optical lenses.
[0255] In addition, since the optical lens of the present invention has high molding fluidity, it is particularly useful as a material for a thin, small and complex-shaped optical lens. As a specific lens size, the thickness of the center portion is preferably 0.05 to 3.0 mm, more preferably 0.05 to 2.0 mm, and further preferably 0.1 to 2.0 mm. In addition, the diameter is preferably 1.0 mm to 20.0 mm, more preferably 1.0 to 10.0 mm, and further preferably 3.0 to 10.0 mm. In addition, as its shape, a meniscus lens with one convex side and one concave side is preferred.
[0256] The optical lens of the present invention can be formed by any method such as mold forming, cutting, grinding, laser processing, electrical discharge machining, etching, etc. Among them, mold forming is more preferred from the perspective of manufacturing cost.
[0257] <Optical films>
[0258] In one embodiment of the present invention, the resin composition can be applied to an optical film. In particular, since an optical film produced using the polycarbonate resin of the present invention has excellent transparency and heat resistance, it is suitable for a liquid crystal substrate film, an optical memory card, and the like.
[0259] In order to avoid foreign matter from mixing into the optical film as much as possible, the molding environment must naturally be a low-dust environment, preferably below level 6, and more preferably below level 5.
[0260] Example
[0261] The following examples and comparative examples of the present invention are shown together to illustrate the contents of the present invention in detail, but the present invention is not limited to these examples. The physical properties of the obtained resin were measured based on the following methods and devices.
[0262] 1) NMR analysis
[0263] Measurement device: Fourier transform nuclear magnetic resonance AVANCE III HD 400 (BRUKER)
[0264] The sample was dissolved in deuterated chloroform (CDCl3) and the 13 C-NMR and 1 H-NMR spectrum.
[0265] 2) Refractive index
[0266] Measuring device: Refractometer (RA-500 manufactured by Kyoto Electronics Co., Ltd.)
[0267] Tetrahydrofuran solutions of the measurement samples (30%, 20%, and 10% solutions) were prepared, and the refractive index was measured using a refractometer. Based on the results obtained, the relationship between concentration and refractive index was deduced, and the value at a concentration of 100% was calculated using the extrapolation method, and this value was used as the refractive index of the measurement sample.
[0268] 3) Thermal analysis
[0269] 3 mg of the crystals obtained in Synthesis Example were weighed in an aluminum pan, and thermal analysis of the crystals was performed using a differential scanning calorimeter (DSC7020, manufactured by Hitachi High-Tech Sciences, Ltd.) under the following operating conditions with alumina as a reference.
[0270] (Operation Conditions)
[0271] Heating rate: 10℃ / min
[0272] Measuring temperature range: 30~400℃
[0273] Measurement environment: open, nitrogen 50mL / min
[0274] 4) Powder X-ray Diffraction (PXRD)
[0275] 0.1 g of the compound obtained in Synthesis Example was filled in the sample filling portion of a glass test plate, and measurement was performed using the following apparatus and conditions.
[0276] [Measurement device]
[0277] MiniFlex600-C / manufactured by Rigaku Co., Ltd.
[0278] [Measurement conditions]
[0279] X-ray source: CuKα
[0280] Tube voltage: 40kV
[0281] Tube current: 15mA
[0282] Scan axis: 2θ / θ
[0283] Mode: Continuous
[0284] Measuring range: 2θ=5°~90°
[0285] Step size: 0.02°
[0286] Speed measurement time: 10° / min
[0287] Entrance slit: 0.25°
[0288] Photosensitive slit: 13.00mm
[0289] 5) Weight average molecular weight (Mw)
[0290] The weight average molecular weight of the obtained resin was measured by gel permeation chromatography (GPC) and calculated in terms of standard polystyrene. The apparatus, column and measurement conditions used were as follows.
[0291] ·GPC device: HLC-8420GPC manufactured by Tosoh Corporation
[0292] ·Column: TSKgel SuperHM-M manufactured by Tosoh Corporation × 3 columns, TSKgel Guard Column SuperH-H manufactured by Tosoh Corporation
[0293] Detector: RI detector
[0294] · Standard polystyrene: Made by Tosoh Corporation, Standard polystyrene kit PStQuick C
[0295] Sample solution: 0.2 mass% tetrahydrofuran solution
[0296] ·Eluent: Tetrahydrofuran
[0297] Eluent flow rate: 0.6mL / min
[0298] Column temperature: 40℃
[0299] 6) Glass transition temperature (Tg)
[0300] According to JIS K7121-1987, the measurement was performed using a differential scanning calorimeter at a temperature increase program of 10° C. / min.
[0301] Differential scanning calorimeter: DSC2500 manufactured by TA Instruments
[0302] 7) Refractive index (nD)
[0303] The polycarbonate resin was molded into a V-shaped block according to JIS B 7071-2: 2018, and the test piece was used as the refractive index at a temperature of 23° C. using a refractometer (KPR-3000 manufactured by Shimadzu Corporation).
[0304] 8) Abbe number (ν)
[0305] The refractive index at wavelengths of 486 nm, 589 nm, and 656 nm at 23° C. was measured using a refractometer using the same test piece (V-shaped block) as used for the refractive index measurement, and the Abbe number was calculated using the following formula.
[0306] Refractometer: KPR-3000 manufactured by Shimadzu Corporation
[0307] ν=(nD-1) / (nF-nC)
[0308] nD: refractive index at a wavelength of 589nm
[0309] nC: refractive index at a wavelength of 656nm
[0310] nF: refractive index at a wavelength of 486nm
[0311] 9) Photoelastic coefficient
[0312] The obtained resin was dissolved in dichloromethane to obtain a resin solution, which was spread on a pad and the solvent was evaporated to obtain a film with a thickness of 0.1 mm, which was used as a test piece.
[0313] The photoelastic coefficients were measured using ellipsometer.
[0314] Measurement Method: The photoelastic coefficient is calculated by measuring the change in birefringence relative to a change in load at a wavelength of 633 nm.
[0315] Ellipsometer: Ellipsometer M-220 manufactured by JASCO Corporation
[0316] [Synthesis example 1]
[0317] Production of 1,3-bis[1-methyl-1-(4-hydroxy-3-phenylphenyl)ethyl]benzene
[0318]
[0319] 157.7 g (0.93 mol) of 2-phenylphenol and 21.0 g of methanol were placed in a 1000 mL four-necked flask equipped with a reflux device, and the interior of the flask was completely replaced with nitrogen gas and then completely replaced with hydrogen chloride gas at an internal temperature of 35°C.
[0320] On the other hand, 30.0 g (0.15 mol) of α,α,α',α'-tetramethyl-1,3-benzenedimethanol, 53.0 g (0.31 mol) of 2-phenylphenol, and 37.5 g of methanol were placed in another glass container and heated to 65° C. to prepare a solution A.
[0321] Hydrogen chloride gas was blown into the four-necked flask while maintaining the internal temperature at 30° C., and solution A was added dropwise over 2 hours using a dropping funnel. After the addition was completed, the internal temperature was lowered to 25° C., and stirring was continued overnight.
[0322] After the reaction was completed, the reaction solution was neutralized with an aqueous sodium hydroxide solution, and the separated water layer was removed. 192.5 g of toluene and 45.0 g of water were added, and the mixture was stirred at an internal temperature of 65° C. for 30 minutes and then allowed to stand to remove the separated water layer. The obtained oil layer was then repeatedly washed with water twice at an internal temperature of 75° C. to remove the sodium chloride generated by the neutralization.
[0323] Then, toluene and 2-phenylphenol in the flask were distilled off by distillation under heating and reduced pressure (final internal temperature of the flask was 270° C. and internal pressure was 0.6 kPa). Thereafter, the residue in the flask was taken out. The solid obtained by cooling was colorless and transparent.
[0324] The obtained solid was confirmed to be the target product by the above-mentioned NMR analysis.
[0325] 1 H-NMR (400 MHz, solvent: CDCl3) δ<ppm>: 1.75 (s, 6H), 5.32 (s, 1H), 7.10-7.55 (m, 9H).
[0326] 13 C-NMR (400 MHz, solvent: CDCl3) δ<ppm>: 31.09, 42.60, 115.43, 123.97, 127.39, 127.69, 127.75, 127.85, 128.48, 129.23, 129.26, 137.73, 148.29, 150.19, 150.37.
[0327] The yield of the obtained solid was 89 mol % of the target product based on the raw material of α,α,α',α'-tetramethyl-1,3-benzenedimethanol. The purity measured by high performance liquid chromatography was 91.9%.
[0328] [Synthesis example 2]
[0329] Production of 1,3-bis[1-methyl-1-(4-(2-hydroxyethoxy)-3-phenylphenyl)ethyl]benzene
[0330]
[0331] 52.6 g (0.31 mol) of 3-phenylphenol and 11.8 g of methanol were placed in a 500 mL four-necked flask equipped with a reflux device, and the interior of the flask was completely replaced with nitrogen gas and then completely replaced with hydrogen chloride gas at an internal temperature of 35°C.
[0332] On the other hand, 15.0 g (0.08 mol) of α,α,α',α'-tetramethyl-1,3-benzenedimethanol, 26.0 g (0.15 mol) of 3-phenylphenol, and 18.8 g of methanol were placed in another glass container and heated to 65° C. to prepare a solution A.
[0333] Hydrogen chloride gas was blown into the four-necked flask while maintaining the internal temperature at 30° C., and solution A was added dropwise over 1.5 hours using a dropping funnel. After the addition was completed, the internal temperature was lowered to 25° C., and stirring was continued overnight.
[0334] After the reaction was completed, the inside of the flask was replaced with nitrogen, and the reaction solution was neutralized with an aqueous sodium hydroxide solution, and the separated water layer was removed. 96.2 g of toluene and 22.5 g of water were added, and the mixture was stirred at an internal temperature of 65°C for 30 minutes and then allowed to stand, and the separated water layer was removed. The obtained oil layer was then washed with water twice at an internal temperature of 75°C to remove the sodium chloride generated by the neutralization. Then, the toluene and 3-phenylphenol in the flask were distilled off by distillation under heating and reduced pressure conditions (the final internal temperature of the flask was 220°C and the internal pressure was 0.5 kPa). It was confirmed that the obtained distillation residue 36.9 g contained 1,3-bis[1-methyl-1-(4-hydroxy-3-phenylphenyl)ethyl]benzene (hereinafter referred to as "Compound A") synthesized in Synthesis Example 1. The crude yield of Compound A relative to α,α,α',α'-tetramethyl-1,3-benzenedimethanol was 94 mol%
[0335] Then, 15.3 g (0.17 mol) of ethylene carbonate, 1.6 g (0.03 mol) of potassium hydroxide, 1.2 g (0.004 mol) of tetrabutylammonium bromide and 110.7 g of methyl isobutyl ketone were added to the flask. After replacing the interior of the flask with nitrogen, the liquid temperature in the flask was raised to 115°C and maintained at 115°C to 116°C, and stirred for 5 hours.
[0336] After the reaction, the liquid temperature in the flask was lowered to 85°C, and 22.9 g of pure water was added to the reaction solution to hydrolyze the remaining ethylene carbonate. Then, 8.8 g of 12% hydrochloric acid aqueous solution was added to neutralize the mixture, and the water layer was separated. Pure water was added to the obtained oil layer and stirred, and the water layer was washed with water 5 times to remove potassium chloride generated by neutralization.
[0337] Then, 73.6 g of cyclohexane was added, and the liquid in the flask was cooled to 25°C to precipitate crystals. The precipitated crystals were filtered to obtain 44.6 g of crystals containing the solvent. By NMR analysis, it was confirmed that the obtained crystals were 1,3-bis[1-methyl-1-(4-(2-hydroxyethoxy)-3-phenylphenyl)ethyl]benzene (hereinafter abbreviated as "Compound B"). The yield of Compound B relative to the content of Compound A was 77 mol%.
[0338] Next, 44.3 g of the obtained crystals of compound B (34.0 g based on compound B) and 132.9 g of methyl isobutyl ketone were added to a 500 ml four-necked flask with a reflux, and the liquid temperature in the flask was heated to 75° C., and the solid was completely dissolved by stirring. Then 88.6 g of cyclohexane was added, and the liquid in the flask was cooled to 25° C. to precipitate crystals. The precipitated crystals were filtered and dried by heating under reduced pressure to obtain white crystals of compound B.
[0339] 1H-NMR (400 MHz, solvent: CDCl3) δ<ppm>: 1.75 (s, 6H), 2.22 (t, 1H), 3.80-3.83 (q, 2H), 4.03-4.05 (t, 2H), 6.87-6.89 (d, 1H), 7.12-7.55 (m, 10H).
[0340] 13 C-NMR (400 MHz, solvent: CDCl3) δ<ppm>: 30.99, 42.59, 61.41, 70.32, 112.94, 123.78, 126.22, 126.97, 127.19, 127.63, 128.12, 129.31, 129.56, 1, 30.47, 138.88, 143.94, 150.30, 153.25.
[0341] The purity determined by HPLC was 98.8%.
[0342] The obtained compound was used as a measurement sample, and the refractive index measured by the above-mentioned analysis method was 1.611.
[0343] The crystals of the obtained compound were subjected to differential scanning calorimetry analysis. As a result, the peak top temperature of the endothermic peak was 137.3° C. The differential scanning calorimetry (DSC) data are shown in Figure 1 .
[0344] The diffraction angle 2θ (°) of the diffraction peaks shown by X-ray diffraction (PXRD) measurement of the obtained compound crystal powder and the diffraction peaks with a relative integrated intensity of 30 or more based on the peak with the strongest integrated intensity are shown in Table 1. The PXRD measurement statistical graph is shown in Figure 2 .
[0345] [Table 1]
[0346] 2θ / θ(°) Relative integrated intensity 2θ / θ(°) Relative integrated intensity 7.88 73 17.01 34 10.79 93 18.00 33 12.79 60 18.62 71 14.86 100 20.19 63 15.07 57 21.33 31 16.33 90 24.14 42
[0347] (Example 1)
[0348] As raw materials, 16.694 g (0.0381 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (BPEF), 8.1361 g (0.0163 mol) of 4-(1-{3-[1-(4-hydroxy-3-phenylphenyl)-isopropyl]phenyl}-isopropyl)-2-phenylphenol (also known as 1,3-bis[1-methyl-1-(4-hydroxy-3-phenylphenyl)ethyl]benzene, abbreviation: BisOPP-M) obtained in Synthesis Example 1, 12.000 g (0.0560 mol) of diphenyl carbonate (DPC) and 2.5×10 ﹣220 μl of sodium bicarbonate aqueous solution (5.0×10 ﹣7 mole, that is, the total amount of dihydroxy compounds relative to 1 mole is 9.2×10 ﹣6 mol) was added to a 300mL reactor with a stirrer and a distillation apparatus, and the system was set to a nitrogen flow condition. The reactor was immersed in an oil bath heated to 200°C to start the transesterification reaction. The temperature was raised to 240°C over 140 minutes, and the pressure was reduced to 0 kPa. After maintaining it for 30 minutes, nitrogen was introduced into the reaction system and restored to 101.3 kPa to obtain a polycarbonate resin. The physical properties of the obtained resin are shown in Table 1.
[0349] (Example 2)
[0350] A polycarbonate resin was obtained in the same manner as in Example 1 except that the amounts of raw materials added were as shown in Table 2. Table 1 shows the physical properties of the obtained resin.
[0351] (Comparative Example 1)
[0352] A polycarbonate resin was obtained in the same manner as in Example 1 except that 5.6527 g (0.0163 mol) of 1,3-bis(1-methyl-1-phenylethyl)benzene (abbreviation: BPM) was used instead of 8.1361 g (0.0163 mol) of 1,3-bis[1-methyl-1-(4-hydroxy-3-phenylphenyl)ethyl]benzene (abbreviation: BisOPP-M) obtained in Synthesis Example 1. The physical properties of the obtained resin are shown in Table 1.
[0353] [Table 2]
[0354]
[0355] [Table 3]
[0356]
[0357] (Examples 3 to 4, Comparative Example 2)
[0358] A polycarbonate resin was obtained in the same manner as in Example 1 except that the amounts of raw materials added were as shown in Table 4. Table 3 shows the physical properties of the obtained resin.
[0359] [Table 4]
[0360]
[0361] [Table 5]
[0362]
[0363]
[0364] (Example 5)
[0365] (Process 1)
[0366] 36.1 g of BisOPP-M obtained in Synthesis Example 1 and 63.9 g of 9,9-bis(4-hydroxy-3-methylphenyl)fluorene (abbreviated as BCFL) were added to 500 ml of 9 w / w% sodium hydroxide aqueous solution, i.e., BisOPP-M:BCFL=30:70 (mol%), and 0.5 g of sulfite was added and dissolved. 300 ml of dichloromethane and 0.1 g of triethylbenzylammonium chloride (TEBAC: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to the solution, and the solution temperature was set to 20° C. while stirring, and 47.8 g of phosgene was blown in over 30 minutes.
[0367] (Process 2)
[0368] After the phosgene blowing was completed, 1.45 g of p-tert-butylphenol (PTBP) dissolved in 50 ml of dichloromethane was added, and after vigorous stirring for 7 minutes to emulsify, 0.5 ml of triethylamine as a polymerization catalyst was added and polymerization was carried out for 30 minutes.
[0369] (Post-processing process)
[0370] The polymer solution was separated into an aqueous layer and an organic layer, and the organic layer was neutralized with phosphoric acid and repeatedly washed with pure water until the pH value of the washing liquid reached pH = 7.0. The organic solvent was distilled off from the purified polycarbonate resin to obtain a polycarbonate resin powder. The polycarbonate resin powder was dried at 120° C. for 24 hours to completely distill off the solvent. The physical properties of the obtained resin are shown in Table 5.
[0371] (Comparative Example 3)
[0372] A polycarbonate resin was obtained in the same manner as in Example 5 except that BisOPP-M was replaced by 28.2 g of BPM, 71.8 g of BCFL (i.e., BPM:BCFL=30:70 (mol%), 37.6 g of phosgene, and 2.04 g of PTBT. The physical properties of the obtained resin are shown in Table 5.
[0373] [Table 6]
[0374]
Claims
1. A thermoplastic resin, characterized in that: It contains a structural unit (A) derived from a monomer represented by the following general formula (1), In formula (1), R1 each independently represents an aryl group having 6 to 14 carbon atoms or an aralkyl group having 7 to 17 carbon atoms, R2 each independently represents a hydrogen atom, an aryl group having 6 to 14 carbon atoms or an aralkyl group having 7 to 17 carbon atoms, a each independently represents 0 or an integer from 1 to 3, and R3 each independently represents -OH or -O-(CH2) n -OH, n represents an integer of 1 to 4.
2. The thermoplastic resin according to claim 1, characterized in that: The monomer represented by the general formula (1) is a monomer represented by the following formula (1A), In formula (1A), R1, R2 and a are the same as defined in general formula (1).
3. The thermoplastic resin according to claim 1, characterized in that: The monomer represented by the general formula (1) is a monomer represented by the following formula (5), 4. The thermoplastic resin according to claim 1, characterized in that: The monomer represented by the general formula (1) is a monomer represented by the following formula (1B), In the formula (1B), R1, R2 and a are the same as defined in the general formula (1), and n independently represents an integer of 1 to 4.
5. The thermoplastic resin according to claim 1, characterized in that: The monomer represented by the general formula (1) is a monomer represented by the following formula (15), 6. The thermoplastic resin according to any one of claims 1 to 6, characterized in that: The thermoplastic resin is a polycarbonate resin, a polyester carbonate resin or a polyester resin.
7. The thermoplastic resin according to any one of claims 1 to 6, characterized in that: The thermoplastic resin comprises a structural unit (B) derived from a monomer represented by the following general formula (6) and / or a structural unit (C) derived from a monomer represented by the following general formula (7), In the general formula (6), R a and R b each independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may be substituted, an alkoxy group having 1 to 20 carbon atoms which may be substituted, a cycloalkyl group having 5 to 20 carbon atoms which may be substituted, a cycloalkoxy group having 5 to 20 carbon atoms which may be substituted, an aryl group having 6 to 20 carbon atoms which may be substituted, a heteroaryl group having 6 to 20 carbon atoms which may be substituted and containing one or more heteroatoms selected from O, N and S, an aryloxy group having 6 to 20 carbon atoms which may be substituted, and -C≡C-R h , R h represents an aryl group having 6 to 20 carbon atoms which may have a substituent, or a heteroaryl group having 6 to 20 carbon atoms which may have a substituent and contains one or more heteroatoms selected from O, N and S, X represents a single bond or a fluorenyl group which may have a substituent, A and B each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, m and n each independently represent an integer of 0 to 6, a and b each independently represent an integer from 0 to 10, In the general formula (7), R c and R d are each independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxy group having 1 to 20 carbon atoms which may have a substituent, a cycloalkyl group having 5 to 20 carbon atoms which may have a substituent, a cycloalkoxy group having 5 to 20 carbon atoms which may have a substituent, and an aryl group having 6 to 20 carbon atoms which may have a substituent, Y1 is a single bond, a fluorenyl group which may have a substituent, or any one of the structural formulae (8) to (14) below, A and B each independently represent an alkylene group having 1 to 5 carbon atoms which may have a substituent, p and q each independently represent an integer of 0 to 4, a and b each independently represent an integer from 0 to 10, In formulas (8) to (14), R 61 , R 62 , R 71 and R 72 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 30 carbon atoms which may have a substituent, or represents R 61 With R 62 Mutually bonded, or R 71 With R 72 are bonded to each other to form a carbon ring or heterocyclic ring having 1 to 20 carbon atoms and optionally having a substituent, r and s each independently represent an integer of 0 to 5000.
8. The thermoplastic resin according to claim 7, characterized in that: In the general formula (6) and the general formula (7), A and B each independently represent an alkylene group having 2 or 3 carbon atoms.
9. The thermoplastic resin according to claim 7 or 8, characterized in that: The thermoplastic resin includes at least a structural unit derived from any one of BPEF, BNE, BNEF, and DPBHBNA.
10. The thermoplastic resin according to any one of claims 1 to 9, characterized in that: The thermoplastic resin further comprises a structural unit derived from at least one monomer selected from the following monomer group, In the above formula, R1 and R2 each independently represent a hydrogen atom, a methyl group or an ethyl group, and R3 and R4 each independently represent a hydrogen atom, a methyl group, an ethyl group or an alkylene glycol having 2 to 5 carbon atoms.
11. The thermoplastic resin according to any one of claims 1 to 10, characterized in that: The thermoplastic resin has a polystyrene-equivalent weight average molecular weight Mw of 10,000 to 100,000.
12. The thermoplastic resin according to any one of claims 1 to 11, characterized in that: The refractive index nD of the thermoplastic resin is 1.600 to 1.
700.
13. The thermoplastic resin according to any one of claims 1 to 12, characterized in that: The Abbe number ν of the thermoplastic resin is 22.0 to 26.
0.
14. The thermoplastic resin according to any one of claims 1 to 13, characterized in that: The glass transition temperature of the thermoplastic resin is 70 to 200°C.
15. The thermoplastic resin according to any one of claims 1 to 14, characterized in that: The photoelastic coefficient of the thermoplastic resin is 25-45.
16. An optical lens, characterized in that: The thermoplastic resin according to any one of claims 1 to 15 is included.