Open cell polymer foam compositions with adjustable tortuosity and methods of making same
By using a polymer composition with crosslinkable thermoplastic matrix and a pore opener, combined with specific heating and cooling processes, polymer foams with high pore content and adjustable tortuosity are prepared, which solves the low tortuosity in the prior art and poor thermal dimensional stability, suitable for a variety of applications.
Patent Information
- Application Number
- CN202380031583.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-28
- Publication Date
- 2024-11-15
AI Technical Summary
When existing thermoplastic-based open-cell foams are prepared by mechanical deformation, they have low tortuosity and poor thermal dimensional stability, making it difficult to meet the needs of various applications.
Using a polymer composition containing a crosslinkable thermoplastic matrix, a crosslinking agent, a foaming agent and a pore opening agent, a high pore opening content polymer foam is prepared under positive pressure by a specific heating and cooling process, so as to achieve adjustable tone. and improved thermal stability.
It realizes polymer foam with high opening content and adjustable tortuosity, avoids mechanical deformation steps, improves the thermal dimensional stability and sound absorption ability of the foam, and is suitable for a variety of applications.
Smart Images

Figure BDA0005065127230000161 
Figure BDA0005065127230000171 
Figure BDA0005065127230000181
Abstract
Description
Background Art
[0001] Polymer foams with an open-cell structure, such as polyurethane foams, are useful in a wide range of applications, including insulation, sound and vibration absorption, cushioning, furniture, and packaging. For open-cell foams based on thermoplastics, high open-cell content is typically achieved using mechanical deformation after the closed-cell or partially closed-cell foam is prepared. However, open-cell foams prepared using mechanical deformation techniques typically have low tortuosity and have poor thermal dimensional stability. Summary of the invention
[0002] This Summary is provided to introduce a series of concepts that are further described in the Detailed Description below. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used as an aid in limiting the scope of the claimed subject matter.
[0003] In one aspect, embodiments disclosed herein relate to a polymer composition comprising a cross-linkable thermoplastic matrix, a cross-linking agent, a blowing agent, and at least one cell opening agent.
[0004] In another aspect, the embodiments disclosed herein relate to an open-cell polymer foam comprising a thermoplastic polymer foam. The foam has an open-cell content of at least 80% and a viscosity of 13 kg / m 3 Up to 60kg / m 3 density.
[0005] On the other hand, embodiments disclosed in the present specification relate to a method for adjusting the tortuosity of an open-cell polymer foam. The method includes: selecting a target tortuosity range; selecting a polymer composition based on the target tortuosity range; blending the polymer composition to form a foamable precursor; heating the foamable precursor to a temperature higher than the decomposition temperature of a cross-linking agent and lower than the decomposition temperature of a chemical foaming agent under positive pressure to produce a primary foam; heating the primary foam to a temperature higher than the decomposition temperature of the chemical foaming agent; and cooling the primary foam to a temperature lower than the softening temperature of a cross-linkable thermoplastic polymer to form an open-cell polymer foam having the target tortuosity range. The polymer composition includes a cross-linkable thermoplastic polymer, a cross-linking agent, a chemical foaming agent, and at least one cell opener.
[0006] On the other hand, embodiments disclosed in the present specification relate to a method for producing an open-cell polymer foam. The method includes heating a foamable precursor, wherein the foamable precursor comprises a cross-linkable thermoplastic polymer, a cross-linking agent, a chemical foaming agent and at least one cell opening agent. The heating of the foamable precursor is carried out under positive pressure to a temperature higher than the decomposition temperature of the cross-linking agent and lower than the decomposition temperature of the chemical foaming agent to produce a primary foam. Then, the method includes heating the primary foam to a temperature higher than the decomposition temperature of the chemical foaming agent, and then cooling the primary foam to a temperature lower than the softening temperature of the cross-linkable thermoplastic polymer to form the open-cell polymer foam. After the step of cooling the primary foam, the resulting open-cell polymer foam has an open-cell content of at least 80%.
[0007] In another aspect, embodiments disclosed herein relate to a cell opener masterbatch composition comprising a carrier polymer and 10 wt % to about 75 wt % of at least one cell opener.
[0008] Other aspects and advantages of the claimed subject matter will become apparent from the following description and appended claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a schematic diagram of a foaming step of a method according to one or more embodiments.
[0010] Figure 2 is a schematic diagram of a foaming step of a method according to one or more embodiments.
[0011] Figure 3 is a schematic diagram showing tortuosity. DETAILED DESCRIPTION
[0012] In one aspect, embodiments disclosed herein relate to open-cell polymer foams having adjustable tortuosity and high open-cell content. Open-cell polymer foams are foams that are particularly useful due to the interconnection of the cells that make up the foam. Foams according to the present disclosure have unique adjustable properties because high open-cell content can be achieved directly through the foam production process without mechanical deformation. High open-cell content is achieved through a combination of a base polymer composition and a method for preparing the foam. In addition, embodiments also relate to such polymer compositions and cell opener masterbatch compositions that can be combined with other components to obtain polymer compositions and foams described herein.
[0013] Polymer composition
[0014] One or more embodiments of the present disclosure are directed to a polymer composition comprising a cross-linkable thermoplastic matrix, a cross-linking agent, a blowing agent, and at least one cell opening agent.
[0015] The polymer composition according to the present disclosure comprises 100 parts by weight of a crosslinkable thermoplastic matrix suitable as a base material for an open-cell polymer foam. In a specific embodiment, the crosslinkable thermoplastic matrix may include different types of polyolefin polymers. In one or more embodiments, the crosslinkable thermoplastic matrix may be selected from polyolefins, ethylene-based polymers, propylene-based polymers, and combinations thereof. In one or more embodiments, the crosslinkable thermoplastic matrix may be selected from the group consisting of low-density polyethylene, high-density polyethylene, linear low-density polyethylene, copolymers of ethylene and one or more C3 to C20 alpha-olefins, polypropylene, ethylene-vinyl acetate copolymers, ethylene methyl acrylate copolymers, ethylene butyl acrylate copolymers, ethylene-propylene copolymers, ethylene-propylene diene copolymers, thermoplastic ethylene elastomers, metallocene polymers, polyether amide block copolymers, polyvinylidene fluoride, copolyesters, polyolefin elastomers, vulcanized thermoplastic elastomers or styrene block copolymers, chlorinated derivatives of the above substances, and combinations thereof. In a specific embodiment, the thermoplastic matrix is selected from ethylene-vinyl acetate copolymers, low-density polyethylene, and combinations thereof. In some embodiments, the thermoplastic matrix may include polymers produced from petroleum-based monomers and / or bio-based monomers (e.g., ethylene obtained from ethanol derived from sugar cane). Commercial examples of bio-based polymers include "I'm Green" bio-polyethylene and bio-ethylene vinyl acetate copolymers from Braskem Corporation. TM series.
[0016] In one or more embodiments, the thermoplastic matrix according to the present disclosure may include ethylene vinyl acetate copolymers (EVA polymers) having various ethylene and vinyl acetate ratios, and may also include one or more optional additional comonomers. For example, the thermoplastic matrix according to the present disclosure may include ethylene vinyl acetate copolymers, as determined by ASTM D5594, the ethylene vinyl acetate copolymers contain a weight percentage range of vinyl acetate content relative to the weight of the ethylene vinyl acetate copolymer from a lower limit selected from 5wt%, 8wt%, 12wt%, 15wt%, 20wt% to an upper limit selected from 25wt%, 30wt%, 35wt%, 40wt%, 60wt%, 75wt% or 95wt%, wherein any lower limit can be paired with any upper limit. In addition, in the total amount of vinyl acetate, it should be understood that at least a portion of the vinyl acetate may be optionally based on a renewable carbon source.
[0017] The thermoplastic matrix according to the present disclosure may include an EVA polymer, wherein the EVA polymer exhibits a melt index ranging from a lower limit selected from one of 0.1 g / 10 min, 1 g / 10 min, 2 g / 10 min, 5 g / 10 min, 10 g / 10 min, 20 g / 10 min, 50 g / 10 min to an upper limit selected from one of 50 g / 10 min, 100 g / 10 min, 200 g / 10 min, 300 g / 10 min or 400 g / 10 min, as determined by ASTM D1238, measured at 190° C. with a load of 2.16 kg, wherein any lower limit may be paired with any upper limit.
[0018] The thermoplastic matrix according to the present disclosure may include an EVA polymer, wherein the density of the EVA polymer may range from 0.91 g / cm 3 , 0.95g / cm 3 , 0.97g / cm 3 or 1.1 g / cm 3 The lower limit of one is selected from 1.1 g / cm 3 , 1.5g / cm 3 , 1.9g / cm 3 , 1.21g / cm 3 or 1.25g / cm 3 Any lower bound can be paired with any upper bound.
[0019] The polymer composition disclosed in this specification includes a crosslinking agent suitable for crosslinking a crosslinkable thermoplastic matrix. The crosslinking agent can be selected based on the type of crosslinkable thermoplastic matrix used. In one or more embodiments, the crosslinking agent can be a peroxide. In other embodiments, the crosslinking agent can be a silane. In one or more embodiments, the crosslinking agent is selected from the group consisting of: 1,1-bis (tert-butyl peroxy) -3,3,5-trimethylcyclohexane, tert-butyl peroxybenzoate, 2,2-bis (tert-butyl peroxy) butane, diisopropyl benzene peroxide, di-tert-amyl peroxide, di-tert-butyl peroxide, 1,2-bis (tert-butyl) -isopropyl benzene, 2,5-bis (tert-butyl peroxy) -2-5-dimethylhexane, 2,5-dimethyl-2,5-di (tert-Butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 4,4-bis(tert-butylperoxy)butyl valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl perbenzoate, tert-butyl peroxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, tert-butyl isopropyl peroxide, and combinations thereof.
[0020] Crosslinking agents may also include peroxides such as: benzoyl peroxide; dicumyl peroxide; di-tert-butyl peroxide; tert-amyl-O-2-ethylhexylmonoperoxycarbonate; tert-butyl cumyl peroxide; tert-butyl 3,5,5-trimethylhexanoate peroxide; tert-butyl peroxybenzoate; tert-butyl peroxycarbonate-2-ethylhexyl ester; tert-butyl 2-hydroxy- ... peroxide); 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane; 1,1-di(tert-butylperoxide)-3,3,5-trimethylcyclohexane; 2,5-dimethyl-2,5-di(tert-butylperoxide)hexyne-3; 3,3,5,7,7-pentamethyl-1,2,4-trioxepane; 4,4-di(tert-butylperoxide)butyl valerate; di(2,4-dichlorobenzoyl)peroxide; di(4-methylbenzoyl)peroxide; di(tert-butylperoxyisopropyl)benzene peroxide, etc.
[0021] Crosslinking agents may also include benzoyl peroxide, 2,5-di(isopropylphenylperoxy)-2,5-dimethylhexane, 2,5-di(isopropylphenylperoxy)-2,5-dimethylhexyne-3,4-methyl-4-(tert-butylperoxy)-2-pentanol, butyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, tert-butyl peroxyneodecanoate, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, 4-methyl-4-(tert-amylperoxy)-2-pentanol, 4-methyl-4-(isopropylphenylperoxy)-2-pentanol, 4-methyl-4-(tert-butylperoxy)-2-pentanone, 4-methyl-4-(tert-amylperoxy)-2-pentanone ...tert-amylperoxy)-2-pentanone, 4-methyl-4-(tert-amylperoxy)-2-pentanone, 4-methyl-4-(tert-amylperoxy)-2-pentanone, 4-methyl-4-(tert-butylperoxy)-2-pentanone, 4-methyl-4-(tert-butylperoxy)-2-pentanone, 4-methyl-4-(tert-butylperoxy)-2-pentanone, 4-methyl-4- )-2-pentanone, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-amylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(tert-amylperoxy)hexyne-3, 2,5-dimethyl-2-tert-butylperoxy-5-hydroperoxyhexane, 2,5-dimethyl-2-isopropylphenylperoxy-5-hydroperoxyhexane, 2,5-dimethyl-2-tert-amylperoxy-5-hydroperoxyhexane, m / p-α,α -bis[(tert-butylperoxy)isopropyl]benzene, 1,3,5-tri(tert-butylperoxyisopropyl)benzene, 1,3,5-tri(tert-amylperoxyisopropyl)benzene, 1,3,5-tri(cumylperoxyisopropyl)benzene, bis[1,3-dimethyl-3-(tert-butylperoxy)butyl]carbonate, bis[1,3-dimethyl-3-(tert-amylperoxy)butyl]carbonate, bis[1,3-dimethyl-3-(isopropylphenylperoxy)butyl]carbonate, di-tert-amyl peroxide, tert-amyl isopropylphenyl peroxide, tert-butyl isopropenyl peroxide, 2,4,6-tri(butylperoxy)-s-triazine, 1,3,5-tri[1-(tert-butylperoxy)-1-methylethyl]benzene, 1,3,5 -Tris[(tert-butylperoxy)-isopropyl]benzene, 1,3-dimethyl-3-(tert-butylperoxy)butanol, 1,3-dimethyl-3-(tert-amylperoxy)butanol, di(2-phenoxyethyl)peroxydicarbonate, di(4-tert-butylcyclohexyl)peroxydicarbonate, dimyristylperoxydicarbonate, dibenzylperoxydicarbonate, di(isobonyl)peroxydicarbonate, 3-isopropylphenylperoxy-1,3-dimethylbutyl methacrylate, 3-tert-butylperoxy-1,3-dimethylbutyl methacrylate, 3-tert-amylperoxy-1,3-dimethylbutyl methacrylate, tris(1,3-Dimethyl-3-tert-butylperoxybutoxy)vinylsilane, 1,3-dimethyl-3-(t-butylperoxy)butyl N-[1-{3-(1-methylethenyl)-phenyl)1-methylethyl]carbamate, 1,3-dimethyl-3-(t-butylperoxy)butyl N-[1-{3-(1-methylethenyl)-phenyl)1-methylethyl]carbamate, 1,3-dimethyl-3-(t-amylperoxy)butyl N-[1-{3-(1-methylethenyl)-phenyl}-1-methylethyl]carbamate, 1,3-dimethyl-3-(t-amylperoxy)butyl N-[1-{3-(1-methylethenyl)-phenyl}-1-methylethyl]carbamate, 1,3-dimethyl-3-(isopropylphenylperoxy)butyl N-[1-{3-(1-methylvinyl)-phenyl}-1-methylethyl]carbamate, 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-butylperoxy) 4,4-di(tert-butylperoxy) pentanoic acid butyl ester, 3,3-di(tert-butylperoxy)butyric acid ethyl ester, 2,2-di(tert-butylperoxy)propane, 3,6,6,9,9-pentamethyl-3-ethoxycabonylmethyl-1,2,4,5-tetraoxacyclononane, 1-4,4-bis(tert-butylperoxy) pentanoic acid butyl ester 1-4,4-bis(t-butylperoxy)valerate), ethyl-3,3-di(tert-amylperoxy)butyrate, benzoyl peroxide, OO-tert-butyl-O-hydrogen-monoperoxy-succinate, OO-tert-amyl-O-hydrogen-monoperoxy-succinate, 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (or methylethyl ketone peroxide cyclic trimer), methylethyl ketone peroxide cyclic dimer, 3,3,6,6,9,9-hexamethyl-1,2,4,5-tetraoxacyclononane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-butyl perbenzoate, tert-butyl peroxy acetate, tert-butyl peroxy-2-ethyl hexanoate), tert-amyl perbenzoate, tert-amyl peracetate, tert-butyl peroxyisobutyrate, 3-hydroxy-1-hexanoate,1-dimethyl tert-butyl ester, OO-t-amyl-O-hydrogen-monoperoxy succinate, OO-t-butyl-O-hydrogen-monoperoxy succinate, di-t-butyl phthalate diperoxyphthalate), tert-butyl peroxy (3,3,5-trimethylhexanoate), 1,4-bis (t-butylperoxycarbo) cyclohexane, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxy-(cis-3-carboxy) propionate, 3-methyl-3-tert-butylperoxybutyrate, OO-t-butyl-O-isopropylmonoperoxy carbonate, OO-t-butyl-O-(2-ethylhexyl)monoperoxy carbonate carbonate), 1,1,1-tris[2-(tert-butylperoxycarbonyloxy)ethoxymethyl]propane, 1,1,1-tris[2-(tert-amylperoxycarbonyloxy)ethoxymethyl]propane, 1,1,1-tris[2-(isopropylphenylperoxycarbonyloxy)ethoxymethyl]propane, OO-t-amyl-O-isopropylmonoperoxy carbonate, di(4-methylbenzoyl)peroxide, di(3-methylbenzoyl)peroxide, di(2-methylbenzoyl)peroxide, didecanoyl peroxide, dilauroyl peroxide, 2,4-dibromo-benzoyl peroxide, peroxysuccinic acid, dibenzoyl peroxide, di(2,4-dichloro-benzoyl)peroxide, and combinations thereof.
[0022] In one or more embodiments, the crosslinking agent can be included in the polymer composition in an amount of from 0.1 phr (parts by weight per 100 parts by weight of the crosslinkable thermoplastic matrix) to 4.0 phr. For example, the content of the crosslinking agent can have a lower limit of one of 0.1 phr, 0.2 phr, 0.3 phr, 0.5 phr, 0.7 phr, 1.0 phr, 1.2 phr, 1.4 phr, 1.5 phr, 1.7 phr and 2.0 phr and an upper limit of one of 2.2 phr, 2.4 phr, 2.5 phr, 2.7 phr, 3.0 phr, 3.2 phr, 3.5 phr, 3.7 phr and 4.0 phr, wherein any lower limit can be paired with any mathematically compatible upper limit.
[0023] The polymer composition of one or more embodiments includes one or more blowing agents. The blowing agent may include a solid, liquid or gaseous blowing agent. Physical blowing agents may include: volatile organic solvents, such as hydrocarbons (e.g., propane, n-butane, isobutane, n-pentane, isopentane, cyclopentane, n-hexane, isohexane, cyclohexane), alcohols (e.g., ethanol and methanol); gases, such as nitrogen, carbon dioxide, carbon monoxide, hydrofluoroolefins (HFO), hydrofluorocarbons (HFC); and other physical blowing agents. The blowing agent may be a chemical blowing agent. In embodiments where the blowing agent is a chemical blowing agent, the chemical blowing agent can be selected from the group consisting of azodicarbonamide, azobisisobutyronitrile, oxybisbenzenesulfonyl hydrazide, 5-phenyltetrazole, sodium bicarbonate, citric acid, citrate, urea, N,N'-dinitrosopentamethylenetetramine, N,N'-dimethyl-N,N'-dinitrosoterephthalamidetrinitrotimethyltriamine, 4,4'-oxybis(benzenesulfonylhydrazide), p-toluenesulfonylhydrazide, diphenylsulfone-3,3'-disulfonylhydrazide, allylbis(sulfonylhydrazide), p-toluenesulfonylsemicarbazide, 4,4'-oxybis(benzenesulfonylsemicarbazide), trichloromonofluoromethane, dichloromonofluoromethane, 5-morpholino-1,2,3,4-thiatriazole, and combinations thereof. In one or more embodiments, the polymer composition may include a physical blowing agent and a chemical blowing agent.
[0024] In one or more embodiments, the blowing agent is included in the polymer composition in an amount of 1 phr to 60 phr. For example, the blowing agent content can have a lower limit of one of 1 phr, 2.5 phr, 5 phr, 10 phr, 15 phr, 20 phr, 25 phr and 30 phr and an upper limit of one of 35 phr, 40 phr, 45 phr, 50 phr, 55 phr and 60 phr, wherein any lower limit can be paired with any mathematically compatible upper limit.
[0025] The polymer composition according to the present disclosure also includes at least one cell opener. The cell opener can be used to open the cells during the foam generation process. Therefore, the cell opener helps to obtain a foam with adjustable tortuosity. Different types of cell openers can be selected based on the desired properties of the foam prepared by the polymer composition. The types of cell openers include surface tension modifiers, rheology modifiers and inorganic compounds. The cell openers can be used alone or in combination.
[0026] In one or more embodiments, the cell opener includes one or more surface tension modifiers. The surface tension modifier can be a polymer matrix that can be blended with the aforementioned cross-linkable polymer matrix. Examples of types of surface tension modifiers include styrene-based materials, polyolefins, polyamides, acrylate-based polymers, polyesters, biodegradable products, rubbers, and thermoplastic elastomers. In a specific embodiment, the surface tension modifier can be selected from the group consisting of: polystyrene, styrene acrylonitrile, polypropylene, polyolefins with a weight average molecular weight higher than the crosslinkable matrix, polymethyl methacrylate, polyethylene terephthalate, ethylene glycol-modified polyethylene terephthalate, polyhydroxyalkanoate (PHA), polylactic acid, starch, polyvinyl alcohol, natural rubber, ethylene-propylene-diene monomer (EPDM), polydimethylsiloxane (PDMS), acrylonitrile butadiene rubber (NBR), polyetheramide block copolymer (PEBA), thermoplastic polyolefin elastomer (TPO), styrene block copolymer (TPS), thermoplastic polyurethane elastomer (TPU), thermoplastic vulcanizate (also known as crosslinked thermoplastic elastomer) and thermoplastic copolyester elastomer.
[0027] In one or more embodiments, the surface tension modifier is present in an amount of 1 phr to 50 phr. For example, the content of the surface tension modifier can have a lower limit of one of 1 phr, 5 phr, 10 phr, 15 phr, 20 phr and 25 phr and an upper limit of one of 25 phr, 30 phr, 35 phr, 40 phr, 45 phr and 50 phr, wherein any lower limit can be paired with any mathematically compatible upper limit.
[0028] In one or more embodiments, the cell opener comprises one or more rheology modifiers. Rheology modifiers are compounds that interfere with the crosslinking process and thus change the rheology of the composition. In one or more specific embodiments, the rheology modifier can be a fatty acid of a primary or secondary amide or a diamide, or an amide or a diamide formed by a primary or secondary fatty acid. For example, the rheology modifier can be erucamide, oleamide, behenamide, stearamide, ethylenebisoleamide, stearyl erucamide or oleyl palmitamide. In one or more embodiments, the rheology modifier is present in an amount of 0.05phr to 7.0phr. For example, the content of the rheology modifier can have a lower limit of one of 0.05, 0.1, 0.2, 0.5, 1.0, 1.5, 2.0, 2.5 and 3.0 and an upper limit of one of 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5 and 7.0, wherein any lower limit can be paired with any upper limit.
[0029] In one or more embodiments, the cell opener includes one or more inorganic compounds. The inorganic compound promotes the rupture of the pore wall during the foaming process. The inorganic compound can be any suitable inorganic compound in the form of particles or microparticles. Examples of types of inorganic compounds include, but are not limited to, talc, carbonates (e.g., calcium carbonate and sodium carbonate), silicates, mica, silicon dioxide, hydroxides (e.g., metal hydroxides (e.g., aluminum hydroxide and magnesium hydroxide)) and clays (e.g., montmorillonite and sepiolite). The inorganic material can have particles with a particle size range from nanometers to micrometers.
[0030] In one or more embodiments, the inorganic compound is present in an amount of 1 phr to 50 phr. For example, the content of the inorganic compound can have a lower limit of one of 1 phr, 5 phr, 10 phr, 15 phr, 20 phr and 25 phr and an upper limit of one of 30 phr, 35 phr, 40 phr, 45 phr and 50 phr, wherein any lower limit can be paired with any upper limit.
[0031] According to the polymer composition of the present disclosure, one or more foaming promoters (also called kickers) may be included, which enhance or initiate the action of the foaming agent by lowering the associated activation temperature. For example, if the selected foaming agent reacts or decomposes at a temperature above 140° C. (e.g., 220° C. or higher), where the surrounding polymer will degrade if heated to the activation temperature, then a foaming promoter may be used. The foaming promoter may include any suitable foaming promoter capable of activating the selected foaming agent. In one or more embodiments, suitable foaming promoters may include cadmium salts, cadmium-zinc salts, lead salts, lead-zinc salts, barium salts, barium-zinc (Ba-Zn) salts, zinc oxide, titanium dioxide, triethanolamine, diphenylamine, sulfonated aromatic acids and salts thereof, and the like.
[0032] In one or more embodiments, the content of the foaming promoter can be in the range of 0.01 phr to 4.00 phr. For example, the content of the foaming promoter can have a lower limit of one of 0.01 phr, 0.05 phr, 0.10 phr, 0.50 phr, 1.00 phr, 1.20 phr, 1.50 phr, 1.70 phr and 2.00 phr and an upper limit of one of 2.20 phr, 2.40 phr, 2.60 phr, 2.80 phr, 3.00 phr, 3.20 phr, 3.40 phr, 3.60 phr, 3.80 phr and 4.00 phr, wherein any lower limit can be paired with any mathematically compatible upper limit.
[0033] The polymer composition disclosed in this specification may include a processing aid. In one or more specific embodiments, the processing aid may be stearic acid, glyceryl monostearate (GMS), a metal stearate (e.g., zinc stearate or magnesium stearate), a wax (e.g., paraffin wax and polyolefin-based wax).
[0034] In one or more embodiments, the content of the processing aid can be in the range of 0.05 phr to 2.0 phr. For example, the content of the processing aid can have a lower limit of one of 0.05 phr, 0.1 phr, 0.2 phr, 0.5 phr, 0.7 phr and 1.0 phr and an upper limit of one of 1.0 phr, 1.2 phr, 1.5 phr, 1.7 phr and 2.0 phr, wherein any lower limit can be paired with any mathematically compatible upper limit.
[0035] The polymer composition of the present disclosure may also include a cell enlarger. The cell enlarger may be a polymer having a linear chain structure of the same nature as the crosslinkable thermoplastic matrix. Regardless of the molecular structure (branched or linear) of the crosslinkable thermoplastic matrix, the cell enlarger will be a polymer exhibiting a linear molecular chain. In one or more specific embodiments, the cell enlarger may be selected from the group consisting of linear low-density polyethylene, linear polypropylene, high-density polyethylene, and combinations thereof.
[0036] In one or more embodiments, the content of the cell enlarger can be in the range of 1 phr to 30 phr. For example, the content of the cell enlarger can have a lower limit of one of 1 phr, 2 phr, 5 phr, 10 phr, 12 phr and 15 phr and an upper limit of one of 15 phr, 22 phr, 25 phr, 27 phr and 30 phr, wherein any lower limit can be paired with any mathematically compatible upper limit.
[0037] The polymer compositions according to the present disclosure may contain one or more property modifiers such as fillers and additives that change various physical and chemical properties when added to the polymer composition during the blending process, including one or more polymer additives such as lubricants, antistatic agents, clarifiers, nucleating agents, β-nucleating agents, antioxidants, compatibilizers, antacids, light stabilizers (e.g., HALS), infrared absorbers, brighteners, inorganic fillers, organic and / or inorganic dyes, antiblocking agents, flame retardants, plasticizers, biocides, adhesion promoters, metal oxides, mineral fillers, flow aids, oils, antioxidants, antiozonants, accelerators, pigments, colorants, and vulcanizing agents.
[0038] The polymer composition according to the present disclosure may contain one or more inorganic fillers as property modifiers, such as talc, glass fiber, marble dust, cement dust, clay, carbon black, graphite, feldspar, silica or glass, fumed silica, silicates, calcium silicate, silicic acid powder, glass microspheres, mica, metal oxide particles and nanoparticles (such as magnesium oxide, antimony oxide, zinc oxide), inorganic salt particles and nanoparticles (such as barium sulfate), wollastonite, aluminum oxide, aluminum silicate, titanium oxide, calcium carbonate, polyhedral oligomeric silsesquioxane (POSS), recycled polymer matrix (such as LDPE (low density polyethylene), EVA (ethylene vinyl acetate), HDPE (high density polyethylene), PP (polypropylene)), etc. As defined in the present disclosure, recycled polyolefins may be derived from regrind materials that have been subjected to at least one processing method (such as molding or extrusion or foaming), and grinding or shredding subsequent sprues, runners, flash, defective parts, etc.
[0039] In one or more embodiments, the content of the property modifier can be in the range of 0.01 phr to 50 phr. For example, the content of the property modifier can have a lower limit of one of 0.01 phr, 0.1 phr, 1.0 phr, 5.0 phr, 10 phr, 15 phr and 20 phr and an upper limit of one of 25 phr, 30 phr, 35 phr, 40 phr, 45 phr and 50 phr, wherein any lower limit can be paired with any mathematically compatible upper limit.
[0040] The polymer compositions described in the present disclosure can be expanded and cured to produce polymer foams. The foams are produced in a process in conjunction with the above polymer compositions that provides high open cell content and adjustable tortuosity of the produced foams.
[0041] Cell opener masterbatch composition
[0042] One or more embodiments of the present disclosure relate to a cell opener masterbatch composition. The cell opener masterbatch composition may include at least one cell opener and a carrier polymer. For example, the cell opener masterbatch raw material may be formulated for storage or transportation, and when necessary, may be combined with a thermoplastic matrix or other materials (such as a crosslinking agent and a foaming agent) to produce a final polymer composition having the above-mentioned composition concentrations, which provides physical and chemical properties suitable for the selected end use. Therefore, the masterbatch composition may be formulated so that the concentration of the cell opener is greater than the final concentration of the cell opener required in the polymer composition as described above. Although the final polymer composition of the present disclosure includes a crosslinking agent and a foaming agent, these components may be omitted from the cell opener masterbatch to prevent premature crosslinking and foaming. The cell opener masterbatch typically includes at least one cell opener and a carrier polymer, which may be the same or different from the thermoplastic matrix, and the cell opener masterbatch may also include additional components, such as a cell enlarger, a filler, a pigment, and the like.
[0043] The carrier polymer contained in the cell opener masterbatch composition can be the same as the thermoplastic matrix used for the final polymer composition, however, other polymers can also be used. In one or more embodiments, the carrier polymer can be selected from the group consisting of low-density polyethylene, high-density polyethylene, linear low-density polyethylene, copolymers of ethylene and one or more C3 to C20 alpha-olefins, polypropylene, ethylene vinyl acetate copolymers, ethylene methyl acrylate copolymers, ethylene butyl acrylate copolymers, ethylene-propylene copolymers, ethylene-propylene diene copolymers, thermoplastic ethylene elastomers, metallocene polymers, polyether amide block copolymers, polyvinylidene fluoride, chlorinated derivatives of the above substances and combinations thereof. Therefore, as described above, the carrier polymer and the thermoplastic matrix can be selected to be the same or different, and even if selected to have the same polymer type, it should be understood that different grades of the same polymer type can be used.
[0044] As described above, the concentration of the cell opener in the masterbatch can be greater than the concentration of the cell opener in the final polymer composition. In one or more embodiments, the masterbatch may include about 10wt% to about 75wt% of the cell opener. The cell opener can be present in the masterbatch in an amount having a lower limit of one of 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 32wt%, 35wt%, 37wt%, 40wt%, 42wt%, 45wt%, 47wt% and 50wt% and an upper limit of one of 25wt%, 30wt%, 32wt%, 35wt%, 37wt%, 40wt%, 42wt%, 45wt%, 47wt%, 50wt%, 52wt%, 55wt%, 57wt%, 60wt%, 62wt%, 65wt%, 67wt%, 70wt% and 75wt%, wherein any lower limit can be paired with any mathematically compatible upper limit. The balance of the weight of the masterbatch composition may be carrier polymer and additives as described above.
[0045] In one or more embodiments, the cell opener masterbatch composition can be blended with a crosslinking agent and a blowing agent (and other optional components described herein) to obtain a polymer composition, or can be blended with a crosslinking agent, a blowing agent, and a crosslinkable thermoplastic matrix (and other optional components described herein) to obtain a final polymer composition. It is foreseeable that in the second case, where the cell opener masterbatch is blended with a crosslinkable thermoplastic matrix, such a blend may contain an amount of the cell opener masterbatch sufficient to achieve a cell opener concentration as described above in the polymer composition. In one or more embodiments, the content of the cell opener masterbatch in the polymer composition can have a lower limit of one of 0.1wt%, 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 10wt%, 15wt%, 20wt% and 25wt% and an upper limit of one of 10wt%, 12wt%, 15wt%, 17wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt% and 50wt%, where any lower limit can be paired with any mathematically compatible upper limit.
[0046] Method for preparing open-cell foam
[0047] In another aspect, one or more embodiments of the present disclosure relate to methods for preparing polymer foams from the compositions described previously. The methods according to one or more embodiments include blending polymer compositions to form a foamable precursor, and then expanding and curing the foamable precursor in a two-step process.
[0048] The polymer composition according to the present disclosure can be blended in any conventional mixing equipment or device to form a foamable precursor. In one or more embodiments, the polymer composition can be blended by mixing in a conventional kneader, a Banbury mixer, a mixing roll, a twin-screw extruder, a press, etc. Blending is generally carried out at a temperature lower than the decomposition temperature of the crosslinking agent and the foaming agent. For example, in one or more embodiments, blending can be carried out at a temperature of about 70°C to 150°C. As will be appreciated by those skilled in the art, the blending temperature will depend on the melting point or softening temperature of the crosslinkable thermoplastic matrix used in the polymer composition, and on the decomposition temperature of the crosslinking agent used.
[0049] In one or more specific embodiments, certain components of the polymer composition may be included in a separately prepared cell opener masterbatch and then blended with additional components to form a foamable precursor. In such an embodiment, the carrier polymer and at least one cell opener are included in the cell opener masterbatch. The cell opener masterbatch may include other components as needed and may be blended with the components described above to form a polymer composition and a foamable precursor. The cell opener masterbatch may help improve the dispersion of the cell opener in the polymer composition and may be used with any composition. However, when a surface tension modifier is used as a cell opener, the cell opener masterbatch may be particularly advantageous, particularly when the cell opener is a polymer having a higher softening temperature than the cross-linkable thermoplastic matrix.
[0050] After the blending step to form the foamable precursor, the foamable precursor is heated in a first heating step. An exemplary embodiment of the first heating step 100 is Figure 1 Shown in. Figure 1 The mold 102 is shown between two hot plates 104 of the press. The foamable precursor 106 is placed in the mold 102 for a first heating step, as shown in the press labeled 108. This first heating step is performed under positive pressure. In one or more embodiments, and as shown in FIG. Figure 1As shown, pressure is applied 110 by pressing the mold in a press. The pressure should be sufficient to maintain the volume of the foamable precursor 106 so that its volume expansion in this step does not exceed 15%, or does not exceed 10%, or does not exceed 5%, or does not exceed 3%, or does not exceed 2%, or does not exceed 1%. When the pressure is applied, the mold in which the foamable precursor is pressed is heated to a temperature higher than the decomposition temperature of the crosslinking agent and lower than the decomposition temperature of the chemical foaming agent. As will be appreciated by those skilled in the art, the temperature will vary depending on the type of crosslinkable thermoplastic polymer, the crosslinking agent used, and the foaming agent. In an exemplary embodiment, the temperature of the first heating step may be in the range of about 130°C to 160°C. The foamable precursor is then kept at an elevated temperature for a sufficient time to ensure that the material reaches the desired crosslinking level. The time at the elevated temperature will vary based on the composition and thickness of the foamable precursor. For example, for a foamable precursor having a thickness of about 25 mm (millimeter), the time at elevated temperature and pressure may be about 40 to 60 minutes. During this step, about 2% to 40% of the foaming agent may be decomposed. As will be appreciated by those skilled in the art, the amount of time at elevated temperatures during this step depends on the thickness of the foamable precursor. A foamable precursor having a thickness of about 25 mm should be heated for about 40 to 60 minutes. However, thicker specimens may require additional heating time, while thinner specimens may require less heating time. Such adjustments may be made as needed, as will be appreciated by those skilled in the art.
[0051] After the first heating step, the pressure is released 112, and the foamable precursor expands to produce a primary foam 114. At this point, the foamable precursor expands into the primary foam at an expansion ratio of about 1.1 to 10.0. For example, the expansion ratio from the foamable precursor to the primary foam can be about 1.1, 1.2, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, or 10.0.
[0052] Then, in Figure 2The primary foam is heated in the second heating step of the method shown. In this step 200, the primary foam 114 is heated using a hot plate 204 similar to those used in the first step. The primary foam 114 is heated to a temperature above the decomposition temperature of the chemical foaming agent in a predetermined volume (e.g., a mold). As will be appreciated by those skilled in the art, the temperature will vary depending on the type of cross-linkable thermoplastic polymer and the foaming agent used. In an exemplary embodiment, the temperature of the second heating step may be in the range of about 160°C to 200°C. Additional external pressure may or may not be applied in this step, including expansion in a reduced pressure environment (i.e., vacuum), however, the volume in which the primary foam is heated is controlled to control the expansion rate of the foam. In an embodiment in which pressure is applied during this step, for example, a movable press with a piston, a sealed mold and pressurized gas may be used, or pressure may be applied by performing this step in a pressure vessel. During this step 200, the foam expands to fill the volume 206, and the expansion rate of the foam is about 10 to 45 compared to the initial volume of the foamable precursor. The expansion ratio during the second step may be about 10, 15, 20, 25, 30, 35, 40, or 45.
[0053] After the primary foam is expanded, it is cooled to a temperature below the softening temperature of the polymer to form an open-cell polymer foam 208 that fills a predetermined volume. Cooling to a temperature below the softening temperature ensures that there is no additional undesired expansion. After the foam is cooled, it can be removed from its expanded volume. Immediately after the cooling step, the open-cell foam can have an open cell content of at least 80%. The foam can also have a tortuosity within a selected tortuosity range.
[0054] No additional mechanical deformation step may be required to achieve the target tortuosity.However, in one or more embodiments, the open-cell polymer foam may be mechanically deformed to change the tortuosity of the open-cell polyolefin foam.
[0055] The method for preparing an open-cell polymer foam described above can be used to change the tortuosity of the foam. In this case, the method includes selecting a target tortuosity range, selecting a polymer composition based on the target tortuosity range, and then continuing to prepare the polymer foam as described above.
[0056] Unlike conventional methods for preparing open-cell polymer foams, the open-cell content and target tortuosity can be achieved directly by the foam synthesis method, which means that mechanical deformation of the foam is not required to obtain high open-cell content and a certain tortuosity. That is, high open-cell content and a certain tortuosity can be achieved by the combination of the polymer composition and the synthesis method described in the present disclosure. In contrast, conventional methods usually have to use mechanical deformation to achieve high open-cell content. According to the method of the present invention, because the high open-cell content is achieved directly by the composition and the synthesis method, when mechanical deformation is used, the mechanical deformation can be for changing the tortuosity of the foam rather than for increasing the open-cell content.
[0057] As described in the present disclosure, tortuosity is a measure of the ease with which a fluid (i.e., gas or liquid) is transported through a foam. Tortuosity is defined as the ratio between the actual distance and the apparent distance that a fluid trapped in a porous structure must cover to move from one side of the foam to the opposite side of the foam. Figure 3 is a diagram used to illustrate how tortuosity is defined.
[0058] The equation used to describe the tortuosity in the present disclosure is shown in formula (I):
[0059]
[0060] Where T is the tortuosity, L is the apparent length, and L0 is the actual length. Figure 3 An article 300 is shown having cells 302 and cell walls 304 defining the cells. Some of the cell walls 304 have holes 306 therein. Figure 3 In the tortuosity diagram, the apparent length (L0) is the length of the article 300 if a straight line is assumed. The actual length (L) is the actual distance that a fluid (e.g., a gas) travels in order to traverse the component (e.g., by passing through a hole in the cell wall). The tortuosity of the foam depends on the characteristics of the foam, such as the open cell content, the number of holes present in the cell wall, and the size of the holes.
[0061] As described in the present disclosure, tortuosity is experimentally determined using electrochemical measurements, as described below.
[0062] A CuSO4·5H2O (0.4 M) solution can be used as an auxiliary liquid. Two copper disks (15 mm in diameter) are used as electrodes. The copper electrodes can be connected to a power supply (EA-3048B Elektro-Automatik GmbH, Germany) that provides alternating current.
[0063] First, measure the conductivity of the solution between the electrodes without the foam sample over a fixed voltage range. Apply Ohm's law to determine the resistance of the solution between the electrodes without the sample (R c). The measurements were performed in a voltage range of 3 to 6 volts in steps of 0.5 volts. An interval of 2 minutes was established between each measurement. During the electrical experiments, conventional ammeters and voltmeters were used to measure voltage and intensity.
[0064] Once the resistance of the solution without the sample has been measured, the conductivity of the solution containing the foam sample placed between two copper electrodes is determined. For this purpose, a cylindrical foam specimen with a thickness of 25 mm and a diameter of 30 mm is immersed in the solution for 14 hours and then measured to assess the proper and complete penetration of the auxiliary liquid inside the porous structure. Thereafter, the sample is placed between two copper electrodes and the conductivity is measured in the same voltage range and under the same conditions and equipment as used for the solution. The resistance of the solution with the sample between the electrodes (R f ).
[0065] Using the equation shown in Equation (III), the tortuosity (T) is defined as the resistance (R) of the foam sample between the copper electrodes. f ) and the resistance of the solution without the foam sample between the electrodes (R c ) ratio:
[0066]
[0067] As described above, methods according to one or more embodiments include selecting a target tortuosity range for an open-cell polymer foam. In one or more embodiments, a low target tortuosity range may be selected. In such embodiments, the target tortuosity is 1.1 to 2.5. For example, the low target tortuosity may be 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, or 2.5. In other embodiments, a high target tortuosity range may be selected. In such embodiments, the target tortuosity is 2.5 to 6.0. For example, the high target tortuosity range may be 2.5, 2.7, 3.0, 3.2, 3.5, 3.7, 4.0, 4.2, 4.5, 4.7, 5.0, 5.2, 5.5, 5.7, or 6.0.
[0068] Once the target tortuosity has been selected, a polymer composition based on the target tortuosity range can be selected. In one or more embodiments, a foam with high tortuosity can be prepared by using a small amount of surface tension modifier. For example, a polystyrene polymer with a content of 5phr to 10phr in an EVA matrix can cause the foam to have a high tortuosity of 2.5 to 6. On the other hand, a foam with a low tortuosity of tortuosity of 1.1 to 2.5 can be produced by a surface tension modifier (e.g., polystyrene) containing a content of 5phr to 15phr and a rheology modifier (e.g., amide of fatty acid) containing a content of 1phr to 3phr. In addition, a combination of a surface tension modifier of 5phr to 15phr and an inorganic filler of 5phr to 20phr in a ratio is a way to reduce the tortuosity of the foam. Once a polymer composition is selected, an open-cell foam can be prepared by the polymer composition as described above.
[0069] As described above, in one or more embodiments, the target tortuosity can be achieved directly by the method of preparing the open-cell foam. However, in one or more other embodiments, an optional mechanical deformation step can be used to change the tortuosity. For example, when preparing an open-cell foam with a higher tortuosity, mechanical deformation can be used to reduce the tortuosity. Mechanical deformation generally includes compressive forces and / or shear forces to destroy additional cell walls in the foam structure. In one or more specific embodiments, the foam can be mechanically deformed using rollers (e.g., a set of two rollers that can be set to different rotation speeds and deformation ratios).
[0070] Open Cell Polymer Foam
[0071] The open-cell polymer foam prepared from the foregoing composition using the foregoing method can provide a unique combination of properties that can be used in a wide range of applications. The open-cell content is a measure of the degree of interconnection of the cells in the polymer foam. For example, a high open-cell content indicates a high level of interconnection of the cells in the polymer foam. As defined in the present disclosure, an open-cell polymer foam is a foam having an open-cell content of at least 80%.
[0072] The open cell content of the polymer foams described in the present disclosure can be determined using gas pycnometer. A gas pycnometer operating under nitrogen or argon can be used, and the equation shown in formula (II) can be used to determine the open cell content:
[0073]
[0074] Where V 样品 is the geometric volume of the foam, measured using conventional methods for measuring the dimensions of materials (e.g., by using calipers), V 比重计 is the volume of the foam measured using a gas pycnometer, ρ 泡沫 is the density of the foam material, ρ 固体is the density of the corresponding solid counterpart. In order to eliminate the potential influence of undesired deformation of the material during the measurement due to the influence of the pressure exerted by the gas introduced into the hydrometer, the volume V given by the hydrometer is measured at different pressures 比重计 The sample volume V measured by the hydrometer 比重计 As a function of pressure, used to provide The obtained curve is fitted to a linear trend to calculate the volume measured by the hydrometer at zero pressure. The value of the volume obtained at zero pressure is used to calculate the open cell content using formula (II). In one or more embodiments, the polymer foam may have an open cell content of at least 80%, at least 82%, at least 85%, at least 87%, at least 90%, at least 92%, at least 95%, at least 98%, or at least 99%.
[0075] The open-cell polymer foam disclosed herein may have a suitable density, and in some cases, may have an ultra-low density. In one or more embodiments, the polymer foam may have a density of 13 kg / m 2 as measured according to ASTM D3575-00 (suffix W-density). 3 Up to 60kg / m 3 In embodiments where the open-cell polymer foam has an ultra-low density, it may have a density of less than 20 kg / m 2 as measured according to ASTM D3575-00 (suffix W-density). 3 Less than 18kg / m 3 or less than 15kg / m 3 density.
[0076] The open-cell polymer foam disclosed in this specification may have a particularly small cell size compared to conventional open-cell foams. In one or more embodiments, when measured using a scanning electron microscope according to ASTM D3576-98, the polymer foam may have an average cell size of 50 microns to 700 microns. In specific embodiments where a smaller cell size is required, when measured using a scanning electron microscope according to ASTM D3576-98, the polymer foam may have an average cell size of 50 microns to 250 microns. The average cell size may have a lower limit of one of 50 microns, 75 microns, 100 microns, 125 microns, 150 microns, 175 microns, and 200 microns and an upper limit of one of 175 microns, 200 microns, 225 microns, 250 microns, 375 microns, 300 microns, 350 microns, 400 microns, 500 microns, 600 microns, and 700 microns, wherein any lower limit may be paired with any mathematically compatible upper limit.
[0077] The open-cell polymer foam disclosed in this specification exhibits unique mechanical properties. For example, when subjected to compressive strain, the response depends on the strain rate. When a polymer foam with high tortuosity is subjected to compressive strain at a low strain rate, it behaves as a typical soft open-cell product, such as a soft polyurethane foam. However, when the same foam product is subjected to a compression test (e.g., an impact test) at a high strain rate, it behaves very similarly to a closed-cell foam, and therefore, is not similar to a soft polyurethane foam at all. Without wishing to be bound by any particular theoretical mechanism, it is believed that the reason for this strain rate-dependent behavior is due to the high tortuosity in the porous structure. In the case of low strain rates, when the material is deformed, the gas enclosed in the porous structure has enough time to leave the material (i.e., the time required for the gas to escape is less than the time scale of the experiment), and therefore (unlike closed-cell foams), the gas phase does not contribute to the stress value obtained. However, in the case of high strain rates, the gas enclosed in the pores comprising the porous structure has no time to escape from the structure because the time required for it to leave the structure is higher than the time scale of the experiment. Therefore, when the product is subjected to an impact test, the gas phase has a positive contribution to the material stress. This dual nature of the foam when it comes to responding to compressive strain makes it an ideal candidate for applications that require both impact protection and comfort.
[0078] The open-cell foam produced by conventional methods that require mechanical deformation for opening cells has reduced thermal stability due to the mechanical opening of the cells. Therefore, compared with conventional open-cell foams, the polymer foam disclosed in this specification provides improved thermal stability. In one or more embodiments, when measured at 70°C according to ASTM D3575 (suffix S-thermal stability), the polymer foam may have an average of ±1% thermal dimensional stability in each direction (length, width and thickness). In one or more embodiments, when measured at 85°C, 90°C or 100°C according to ASTM D3575 (suffix S-thermal stability), the polymer foam may have an average of ±5% thermal dimensional stability in each direction (length, width and thickness). In one or more exemplary embodiments, when measured at 85°C for EVA-based foams with a vinyl acetate content of 19%, or when measured at 100°C for LDPE-based foams, or when measured at 90°C for EBA-based foams with a butyl acrylate content of 17%, the polymer foam may have a thermal stability of ±5%.
[0079] Sound absorption is an important application of flexible polyurethane foams. These materials generally show their maximum absorption at frequencies above 2000 Hz to 2500 Hz. However, for some specific applications, materials with good absorption capabilities below 2000 Hz are required. Compared to conventional foams (such as flexible polyurethane foams), the polymer foams disclosed in this specification provide higher sound absorption capabilities below 2000 Hz. When measured according to ASTM 1050-98 and calculated using the equation shown in formula (IV), the polymer foam can have an average sound absorption capacity of at least 0.50 between f1=500 Hz and f2=2000 Hz.
[0080]
[0081] The polymer foams disclosed in this specification show high oil absorption capacity. Foams with low tortuosity have many characteristics that can be used for oil spill remediation. The extremely low density enables the foam to absorb a high volume of oil per volume of foam. In addition, in one or more embodiments, soft polyolefins (such as LDPE or EVA) can be used as cross-linkable thermoplastics to provide soft foams for oil absorption, which allow the foam to be reusable. Once the oil is absorbed, the soft foam can be squeezed and reused many times. The open cell content and low density of the foams disclosed in this specification also contribute to high and effective oil absorption. Polyolefin-based materials (such as many cross-linkable thermoplastic matrix materials disclosed in this specification) are hydrophobic and oleophilic, which provides oil-water selectivity.
[0082] The oil absorption capacity described in the present disclosure can be measured by placing a foam sample on the surface of the oil. The foam is not immersed or squeezed, but placed on top of the oil sample and left to stand for 10 minutes. The oil absorption is calculated using the equation shown in formula (IV):
[0083]
[0084] Where W 油 / W 泡沫 is the oil absorption capacity, W 10’-油 is the weight of the foam after it has been placed on the oil for 10 minutes, W 初始 is the initial weight of the foam before it is placed on the oil. This test can be repeated any number of times by squeezing the oil out of the foam and testing again. A similar test can also be performed for water absorption using the same equation (all oil values replaced by water). In one or more embodiments, the oil absorption capacity of the open-cell foam of the present disclosure can be per gram of foam W 泡沫 At least 25g oil 油 , or per gram of foam W 泡沫 At least 30g oil 油 , or per gram of foam W 泡沫 At least 35g oil油 , or per gram of foam W 泡沫 At least 40g oil 油 .
[0085] In an exemplary embodiment, for a density of 22 kg / m 3 The open-cell EVA foam (vinyl acetate content of 12%) with a tortuosity of 2.6 can have an oil absorption capacity of W per gram of foam. 泡沫 Up to 25 g oil W 油 In another exemplary embodiment, for a density of 17 kg / m 3 The oil absorption capacity of open-cell EVA foam (vinyl acetate content of 18%) with a tortuosity of 1.9 can be as high as W per gram of foam. 泡沫 43g oil 油 .
[0086] The open-cell foam according to one or more embodiments may have high vibration damping capability. This property can be measured by tan δ, which is the ratio between the storage modulus (E') and the loss modulus (E") in a dynamic thermomechanical analysis (DMA) experiment conducted in compression mode according to ASTM D5024-01. The tan δ value of the open-cell foam at 23°C and 1 Hz frequency may be greater than 0.5, or greater than 0.7, or greater than 0.9. In one or more specific embodiments, for a density of 17 kg / m 3 The open-cell EVA foam (vinyl acetate content 18%) with a tortuosity of 1.9 can have a tan δ value greater than 0.5 at 23°C and 1 Hz frequency. 3 And the open-cell EBA foam (butyl acrylate content of 17%) with a tortuosity of 1.9 can have a tan δ as high as 0.9 at 23°C and 1 Hz frequency.
[0087] The open-cell foams described in the present disclosure can be easily thermoformed into complex shapes using conventional methods involving pressure (or vacuum) and temperature. In addition, the foams can be laminated to other materials (textiles, foams, solid polymers, etc.) using conventional methods (e.g., adhesive bonding or thermal bonding, etc.). In addition, the material can be washed using conventional washing machines including standard temperature programs and laundry detergents. These properties make the foams useful in the manufacture of elements in the apparel industry, such as bras, sports body protection elements, thermal clothing, cups, etc.
[0088] Products
[0089] The open-cell polymer foam according to one or more embodiments of the present disclosure can be used to produce a variety of polymer articles for a variety of end uses. These applications include cushioning materials (e.g., seats, mattresses, cushions, mats), protective elements in the sports field, packaging of different types of goods, sealing applications and gaskets, liquid absorption (water-based or oil-based), filtration, sound absorbing materials, clothing, bras, carpet padding, furniture, shock absorbing elements, automotive related elements (e.g., crash pads, carpet backing, energy management, filters, headliners, headrests, armrests, seats, sound insulation (roof), steering wheels, visors, decoration, shock absorption), bicycle and motorcycle seats, helmets, handicrafts, diapers, earplugs, electronic products, toys, sanitary napkins, sealants in the construction field, thermal insulation materials, cushioning materials for precision instruments or transportation or glass, septic tank carriers, sealing and / or sound absorbing elements for systems including air conditioning systems, refrigeration systems, speakers and personal computers, and sealants for LCD TVs.
[0090] Example
[0091] Sample recipe
[0092] Examples I to VI are open-cell foams prepared from different formulations according to the teachings of the present disclosure. The sample formulations of Examples I to VI are listed in Table 1. Examples I to III are open-cell foams based on a formulation containing EVA (ethylene-vinyl acetate copolymer, wherein the vinyl acetate content is 18 wt%) as a crosslinkable thermoplastic matrix, in which Example IV is an ultra-low density open-cell foam based on EBA (ethylene-butyl acrylate copolymer, wherein the butyl acrylate content is 17%) as a crosslinkable thermoplastic matrix; Example V is a high tortuosity open-cell foam based on LDPE (low-density polyethylene) as a crosslinkable thermoplastic matrix; and Example VI is an ultra-low density foam based on EVA (wherein the vinyl acetate content is 18%) as a crosslinkable thermoplastic matrix.
[0093]
[0094]
[0095] Method for preparing open-cell foam
[0096] The open-cell foam examples presented in this disclosure were prepared using the following process steps.
[0097] 1. Mixing of components
[0098] 1.a. In the case of Examples I and III, a conventional two-roll mill was used to produce the foamable precursor, wherein the two rolls were heated at 118° C. and the mixing time was 15 minutes. The equipment used was DW5110 from Hefei Fanyuan Testing Instrument Co., Ltd.
[0099] 1.b. For those formulations containing polystyrene (PS) (Examples II, IV, V and VI), a cell opener masterbatch was prepared containing the base polymer of each formulation as carrier polymer and PS as cell opener in a weight ratio of 70:30 (carrier:cell opener). The masterbatch was produced in a Dr. Collin twin screw extruder ZK 25T Teachline using a temperature range of 100°C (in the hopper) to 180°C (in the die).
[0100] Then, the masterbatch was added to the formulation by using a conventional two-roll mill, where the two rolls were heated at 118° C. and the mixing time was 15 minutes, so that the material ratios in the foamable precursor were as shown in Table 1. The equipment used was DW5110 from Hefei Fanyuan Testing Instrument Co., Ltd.
[0101] 2. The first heating step to produce primary foam
[0102] This step was carried out in a conventional double hot platen press manufactured by Talleres Remtex (Barcelona, Spain). The mould was made of aluminium. The inner dimensions of the mould were 79 x 79 x 25 mm. 3 The conditions used in each experiment are detailed in Table 2. The mold was completely filled with the foamable precursor produced during the mixing step.
[0103] 3. The second heating step is used to produce open-cell foam
[0104] This step is carried out in a conventional double hot platen press manufactured by Talleres Remtex (Barcelona, Spain). The mould for introducing the primary foam is made of aluminium. The internal dimensions of the mould are 200 x 200 x 100 mm. 3 The conditions used in each experiment are detailed in Table 2.
[0105] 4. Cooling to below softening temperature
[0106] This cooling step is performed by placing the mold used in the second heating step in water for 40 minutes.
[0107] The process conditions used to prepare the foams of Examples I to VI are summarized in Table 2.
[0108]
[0109]
[0110] Open Cell Foam Properties
[0111] The density, open cell content and tortuosity of the open cell foams prepared according to the above formulation and preparation method were evaluated.
[0112] The properties of the foams of Examples I to VI are shown in Table 3.
[0113]
[0114] Although only a few exemplary embodiments are described in detail above, it will be readily appreciated by those skilled in the art that many modifications may be made in the exemplary embodiments without substantially departing from the scope of the invention. Therefore, all such modifications are intended to be included within the scope of the present disclosure as defined by the appended claims. In the claims, functional definitions are intended to cover structures described in this specification as performing the enumerated functions, which not only cover structural equivalents, but also cover equivalent structures. Therefore, although nails and screws may not be structural equivalents because nails use cylindrical surfaces to fix wooden parts together, while screws use helical surfaces, nails and screws may be equivalent structures in the context of fastening wooden parts. It is the applicant's express intention not to invoke Section 112(f) of the United States Patent Act to impose any limitation on any claim in this specification, except for those where the claims explicitly use the wording "device for..." together with associated functions.
Claims
1. A polymer composition comprising: a cross-linkable thermoplastic matrix; Cross-linking agent; Blowing agents; and At least one cell opener.
2. The polymer composition according to claim 1, in, The crosslinkable thermoplastic matrix is selected from the group consisting of low density polyethylene, high density polyethylene, linear low density polyethylene, copolymers of ethylene and one or more C3 to C20 α-olefins, polypropylene, ethylene vinyl acetate copolymers, ethylene methyl acrylate copolymers, ethylene butyl acrylate copolymers, ethylene-propylene copolymers, ethylene-propylene diene copolymers, thermoplastic ethylene elastomers, metallocene polymers, polyether amide block copolymers, polyvinylidene fluoride, copolyesters, polyolefin elastomers, vulcanized thermoplastic elastomers or styrene block copolymers, chlorinated derivatives of the above substances and combinations thereof.
3. The polymer composition according to any one of the preceding claims, in, The crosslinking agent is selected from the group consisting of: 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane; tert-butyl peroxybenzoate; 2,2-bis(tert-butylperoxy)butane; diisopropylbenzene peroxide; di-tert-amyl peroxide; di-tert-butyl peroxide; 1,2-bis(tert-butyl)-isopropylbenzene; 2,5-bis(tert-butylperoxy)-2-5-dimethylhexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3; 1,3-bis(tert-butylperoxyisopropyl)benzene; 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane; n-butyl 4,4-bis(tert-butylperoxy)valerate; benzoyl peroxide; p-chlorobenzoyl peroxide; 2,4-dichlorobenzene Formyl peroxide, tert-butyl peroxybenzoate; tert-butyl peroxyisopropyl carbonate, diacetyl peroxide; lauroyl peroxide, tert-butyl isopropyl peroxide; benzoyl peroxide; diisopropyl peroxide; di-tert-butyl peroxide; tert-amyl peroxy(2-ethylhexyl) carbonate; tert-butyl isopropyl peroxide; tert-butyl peroxide; tert-butyl peroxy-3,5,5-trimethylhexanoate; tert-butyl peroxybenzoate; tert-butyl peroxycarbonate-2-ethylhexyl; 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane; 1,1-di(tert-butyl peroxide)-3,3,5-trimethylcyclohexane; 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexyne-3; 3,3,5,7,7-pentamethyl-1,2,4-trioxy Heterocycloheptane; butyl 4,4-di(tert-butylperoxy)valerate; di(2,4-dichlorobenzoyl) peroxide; di(4-methylbenzoyl) peroxide; di(tert-butylperoxyisopropyl)benzene peroxide benzoyl peroxide; 2,5-di(isopropylphenylperoxy)-2,5-dimethylhexane; 2,5-di(isopropylphenylperoxy)-2,5-dimethylhexyne-3,4-methyl-4-(tert-butylperoxy)-2-pentanol; butyl peroxy 2-ethylhexanoate; tert-butyl peroxypivalate; tert-butyl peroxyneodecanoate; tert-butyl peroxybenzoate; tert-butyl peroxy 2-ethylhexanoate; 4-methyl-4-(tert-amylperoxy)-2-pentanol; 4-methyl-4-(isopropylphenylperoxy)-2 -pentanol; 4-methyl-4-(tert-butylperoxy)-2-pentanone; 4-methyl-4-(tert-amylperoxy)-2-pentanone; 4-methyl-4-(isopropylphenylperoxy)-2-pentanone; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane; 2,5-dimethyl-2,5-di(tert-amylperoxy)hexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3; 2,5-dimethyl-2,5-di(tert-amylperoxy)hexyne-3; 2,5-dimethyl-2-tert-butylperoxy-5-hydroperoxyhexane; 2,5-dimethyl-2-isopropylphenylperoxy-5-hydroperoxyhexane; 2,5-dimethyl-2-tert-amylperoxy-5-hydroperoxyhexane;m / p-α,α-di[(tert-butylperoxy)isopropyl]benzene; 1,3,5-tri(tert-butylperoxyisopropyl)benzene; 1,3,5-tri(tert-amylperoxyisopropyl)benzene; 1,3,5-tri(cumylperoxyisopropyl)benzene; di[1,3-dimethyl-3-(tert-butylperoxy)butyl]carbonate; di[1,3-dimethyl-3-(tert-amylperoxy)butyl]carbonate; di[1,3-dimethyl-3-(isopropylphenylperoxy)butyl]carbonate; di-tert-amyl peroxide, tert-amylisopropylphenyl peroxide; tert-butylisopropylperoxide; 2,4,6-tri(butylperoxy)-s-triazine; 1,3,5-tri[1-(tert-butylperoxy)-1-methylethyl]benzene; 1,3, 5-Tri[(tert-butylperoxy)-isopropyl]benzene; 1,3-dimethyl-3-(tert-butylperoxy)butanol; 1,3-dimethyl-3-(tert-amylperoxy)butanol; di(2-phenoxyethyl)peroxydicarbonate; di(4-tert-butylcyclohexyl)peroxydicarbonate; dimyristylperoxydicarbonate; dibenzylperoxydicarbonate; di(isobornyl)peroxydicarbonate; 3-isopropylphenylperoxy-1,3-dimethylbutyl methacrylate; 3-tert-butylperoxy-1,3-dimethylbutyl methacrylate; 3-tert-amylperoxy-1,3-dimethylbutyl methacrylate; tri(1,3-dimethyl-3-tert-butylperoxybutoxy)vinylsilane; N-[1-{3-(1-methyl)-1,3-dimethylbutyl)-1,3-dimethylbutyl methacrylate] 1,3-dimethyl-3-(tert-butylperoxy)butyl N-[1-{3(1-methylvinyl)-phenyl}-1-methylethyl]carbamate; 1,3-dimethyl-3-(tert-amylperoxy)butyl N-[1-{3(1-methylvinyl)-phenyl}-1-methylethyl]carbamate; 1,3-dimethyl-3-(isopropylphenylperoxy)butyl N-[1-{3-(1-methylvinyl)-phenyl}-1-methylethyl]carbamate; 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane; 1,1-di(tert-butylperoxy)cyclohexane; 4,4-di(tert-amylperoxy)pentanoic acid n-butyl ester; 3,3-di(tert-butylperoxy)butyric acid ethyl ester; 2,2-di(tert-amylperoxy)propane; 3, 6,6,9,9-pentamethyl-3-ethoxycarbonylmethyl-1,2,4,5-tetraoxacyclononane; 1-4,4-bis(tert-butylperoxy)valerate, n-butyl; ethyl-3,3-di(tert-amylperoxy)butyrate; benzoyl peroxide; OO-tert-butyl-O-hydrogen-monoperoxy-succinate; OO-tert-amyl-O-hydrogen-monoperoxy-succinate; 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane (or methyl ethyl ketone peroxide cyclic trimer); methyl ethyl ketone peroxide cyclic dimer; 3,3,6,6,9,9-hexamethyl-1,2,4,5-tetraoxacyclononane; 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; tert-butyl perbenzoate;tert-Butyl peroxyacetate; tert-Butyl peroxy-2-hexanoate; tert-Amyl perbenzoate; tert-Amyl peroxyacetate; tert-Butyl peroxyisobutyrate; tert-3-hydroxy-1,1-dimethyl tert-butyl peroxy-2-hexanoate; OO-tert-Amyl-O-hydrogen-monoperoxysuccinate; OO-tert-Butyl-O-hydrogen-monoperoxysuccinate; di-tert-butyl diperoxyphthalate; tert-Butyl peroxy (3,3,5-trimethylhexanoate), 1,4-di(tert-Butylperoxycarbonyl)cyclohexane; tert-Butyl peroxy-3,5,5-trimethylhexanoate; tert-Butyl peroxy-(cis-3-carboxy)propionate; 3-methyl-3-tert-butylperoxybutyrate; OO-tert-Butyl-O-isopropylmonoperoxycarbonate; OO-tert-Butyl Butyl-O-(2-ethylhexyl) monoperoxycarbonate; 1,1,1-tris[2-(tert-butylperoxycarbonyloxy)ethoxymethyl]propane; 1,1,1-tris[2-(tert-amylperoxycarbonyloxy)ethoxymethyl]propane; 1,1,1-tris[2-(isopropylphenylperoxycarbonyloxy)ethoxymethyl]propane; OO-tert-amyl-O-isopropyl monoperoxycarbonate; di(4-methylbenzoyl) peroxide; di(3-methylbenzoyl) peroxide; di(2-methylbenzoyl) peroxide; didecanoyl peroxide; dilauroyl peroxide; 2,4-dibromo-benzoyl peroxide; peroxysuccinic acid; dibenzoyl peroxide; di(2,4-dichloro-benzoyl) peroxide, and combinations thereof. ; 4. The polymer composition according to any one of the preceding claims, in, The foaming agent is a chemical foaming agent selected from the group consisting of azodicarbonamide, azobisisobutyronitrile, oxybisbenzenesulfonyl hydrazide, 5-phenyltetrazole, sodium bicarbonate, citric acid, citrate, urea, N,N'-dinitrosopentamethylenetetramine, N,N'-dimethyl-N,N'-dinitrosoterephthalamide trinitrotrimethyltriamine, 4,4'-oxybis(benzenesulfonyl hydrazide), p-toluenesulfonyl hydrazide, diphenyl sulfone-3,3'-disulfonylhydrazide, allylbis(sulfonylhydrazide), p-toluenesulfonylsemicarbazide, 4,4'-oxybis(benzenesulfonylsemicarbazide), trichloromonofluoromethane, dichloromonofluoromethane, 5-morpholino-1,2,3,4-thiatriazole and combinations thereof.
5. A polymer composition according to any one of the preceding claims, in, The blowing agent is a physical blowing agent selected from the group consisting of propane, n-butane, isobutane, n-pentane, isopentane, cyclopentane, n-hexane, isohexane, cyclohexane, ethanol, methanol, nitrogen, carbon dioxide gas, carbon monoxide gas, hydrofluoroolefins (HFO), hydrofluorocarbons (HFC) and combinations thereof.
6. A polymer composition according to any one of the preceding claims, in, The at least one cell opener is selected from the group consisting of surface tension modifiers, rheology modifiers, inorganic compounds, and combinations thereof.
7. The polymer composition according to claim 6, in, When the at least one cell opener comprises the surface tension modifier, the surface tension modifier is present in an amount of 1 phr to 50 phr.
8. The polymer composition according to claim 6 or 7, in, The surface tension modifier is selected from the group consisting of polyamide, polystyrene, styrene acrylonitrile, polypropylene, polyolefins having a weight average molecular weight higher than that of the crosslinkable thermoplastic matrix, polymethyl methacrylate, polyethylene terephthalate, glycol-modified polyethylene terephthalate, polyhydroxyalkanoates, polylactic acid, starch, polyvinyl alcohol, natural rubber, ethylene-propylene-diene monomer, polydimethylsiloxane, acrylonitrile butadiene rubber, polyetheramide block copolymers, thermoplastic polyolefin elastomers, styrene block copolymers, thermoplastic polyurethane elastomers, thermoplastic vulcanizates, thermoplastic copolyester elastomers, and combinations thereof.
9. The polymer composition according to any one of claims 6 to 8, in, When the at least one cell opener comprises the rheology modifier, the rheology modifier is present in an amount of 0.05 phr to 7.0 phr.
10. The polymer composition according to any one of claims 6 to 9, in, The rheology modifier is a primary or secondary amide or bisamide fatty acid and a combination thereof.
11. The polymer composition according to any one of claims 6 to 10, in, When the at least one cell opener comprises the inorganic compound, the inorganic compound is present in an amount of 1 phr to 50 phr.
12. The polymer composition according to any one of claims 6 to 11, in, The inorganic compound is selected from the group consisting of talc, calcium carbonate, sodium carbonate, silicate, mica, silicon dioxide, aluminum hydroxide, magnesium hydroxide, montmorillonite, sepiolite, and combinations thereof.
13. The polymer composition according to any one of the preceding claims, further comprising a foaming promoter in an amount of 0.01 phr to 4.00 phr.
14. The polymer composition according to claim 13, in, The foaming promoter is selected from the group consisting of transition metal compounds, zinc oxide, polyols, urea, alkanolamines, organic acids, and combinations thereof.
15. The polymer composition of any of the preceding claims, further comprising a processing aid in an amount of 0.05 to 2.0 phr.
16. The polymer composition according to any one of the preceding claims, further comprising a cell enlarging agent.
17. A polymer composition according to any one of the preceding claims, in, Also included is a property modifier selected from the group consisting of fillers, additives, and combinations thereof.
18. A polymer composition according to any one of the preceding claims, in, The content of the crosslinking agent is 0.1 phr to 2.0 phr.
19. A polymer composition according to any one of the preceding claims, in, The content of the foaming agent is 1 phr to 60 phr.
20. An open-cell polymer foam prepared from the polymer composition of any preceding claim.
21. An open-cell polymer foam comprising: A thermoplastic polymer foam, the foam comprising: At least 80% open cell content; and 13kg / m 3 Up to 60kg / m 3 density.
22. The open-cell polymer foam according to claim 20 or 21, in, The open cell polymer foam has an open cell content of at least 90%.
23. An open-cell polymer foam according to any one of claims 20 to 22, in, The open-cell polymer foam has a thickness of less than 20 kg / m 3 density.
24. The open cell polymer foam of any one of claims 20 to 23, comprising a tortuosity of 1.1 to 2.
5.
25. The open cell polymer foam of any one of claims 20 to 23, comprising a tortuosity of 2.5 to 6.
0.
26. The open cell polymer foam of any one of claims 20 to 25, comprising an average cell size of 50 microns to 700 microns.
27. An open-cell polymer foam according to any one of claims 20 to 26, in, The open cell polymeric foam has a thermal dimensional stability in each direction of length, width and thickness that averages ±1% when measured at 70°C in accordance with ASTM D3575 suffix S - Thermal Stability.
28. An open-cell polymer foam according to any one of claims 20 to 27, in, When measured according to ASTM 1050-98 and calculated using the equation shown below (IV), the open cell polymer foam has a relative humidity of 1.1 % and a relative humidity of 1.1 % at f. 1 =500Hz and f 2 = Average sound absorption capacity of at least 0.50 between 2000Hz 29. An open-cell polymer foam according to any one of claims 20 to 28, in, The open-cell polymer foam has a W per gram of foam 泡沫 At least 25g oil 油 Oil absorption capacity.
30. An article comprising the open-cell polymer foam of any one of claims 20 to 29.
31. The article according to claim 30, in, The article is selected from the group consisting of seats, mattresses, cushions, mats, protective elements in the sports field, packaging, gaskets, liquid absorbing articles, filters, sound absorbing materials, clothing articles, bras, carpet pads, furniture articles, shock absorbing elements, car crash pads, car carpet backings, car energy management, car filters, car roof linings, car headrests, car armrests, car seats, car roof sound insulation, car steering wheels, car visors, car decorations, bicycle seats, motorcycle seats, helmets, handicrafts, diapers, earplugs, electronic products, toys, sanitary napkins, sealants in the construction field, thermal insulation materials, cushioning materials for precision instruments or transportation or glass, septic tank carriers, sealing elements for air conditioning systems, sealing elements for refrigeration systems, sealing elements for speakers, sealing elements for personal computers, sound absorption for air conditioning systems, sound absorption for refrigeration systems, sound absorption for speakers, sound absorption for personal computers, and sealants for LCD TVs.
32. A method for adjusting the tortuosity of an open-cell polymer foam, the method include: Select the target tortuosity range; selecting a polymer composition based on the target tortuosity range; blending the polymer composition to form a foamable precursor, the polymer composition comprising: Cross-linkable thermoplastic polymers; Cross-linking agent; Chemical blowing agents; as well as at least one cell opening agent; heating the foamable precursor under positive pressure to a temperature above the decomposition temperature of the crosslinking agent and below the decomposition temperature of the chemical blowing agent to produce a primary foam; heating the primary foam to a temperature above the decomposition temperature of the chemical blowing agent; and The primary foam is cooled to a temperature below the softening temperature of the cross-linkable thermoplastic polymer to form the open-cell polymer foam having the target tortuosity range.
33. The method according to claim 32, in, The target tortuosity ranges from 1.5 to 2.
5.
34. The method according to claim 32, in, The target tortuosity range is 2.5 to 6.
0.
35. A method of producing an open-cell polymer foam, the method include: heating a foamable precursor, wherein the foamable precursor comprises: Cross-linkable thermoplastic polymers; Cross-linking agent; Chemical blowing agents; as well as at least one cell opening agent; wherein heating the foamable precursor comprises heating under positive pressure to a temperature higher than a decomposition temperature of the cross-linking agent and lower than a decomposition temperature of the chemical foaming agent to produce a primary foam; heating the primary foam to a temperature above the decomposition temperature of the chemical blowing agent, and cooling the primary foam to a temperature below the softening temperature of the cross-linkable thermoplastic polymer to form the open-cell polymer foam; Wherein, after the step of cooling the primary foam, the open-cell polymer foam has an open-cell content of at least 80%.
36. The method of claim 35, further comprising, prior to the heating step, blending the cross-linkable thermoplastic polymer, the cross-linking agent, the chemical blowing agent, and the at least one cell opener to form the foamable precursor.
37. The method of claim 35 or 36, further comprising mechanically deforming the open cell polymer foam to change the tortuosity of the open cell polymer foam.
38. A method according to any one of claims 35 to 37, in, The foamable precursor comprises a composition according to any one of claims 1 to 18.
39. The method according to any one of claims 36 to 38, further comprising, before the blending step, producing a cell opener masterbatch comprising a carrier polymer and the at least one cell opener, wherein the blending step comprises blending the masterbatch with the crosslinking agent and the chemical foaming agent and optionally with the crosslinkable thermoplastic.
40. The method according to any one of claims 35 to 39, in, During heating of the foamable precursor under positive pressure, the foamable precursor expands to an expansion ratio of 1.5 to 10.
0.
41. The method according to any one of claims 35 to 40, in, During heating of the primary foam, the primary foam expands to an expansion ratio of 15 to 45 relative to the initial volume of the foamable precursor.
42. An open cell polymer foam prepared by the method of any one of claims 35 to 41.
43. A cell opener masterbatch composition comprising: a carrier polymer; and 10 wt % to about 75 wt % of at least one cell opener.
44. The masterbatch composition according to claim 43, in, The at least one cell opener is selected from the group consisting of surface tension modifiers, rheology modifiers, inorganic compounds, and combinations thereof.
45. The masterbatch composition according to claim 44, in, The surface tension modifier is selected from the group consisting of polystyrene, styrene acrylonitrile, polypropylene, polyolefins having a weight average molecular weight higher than that of the crosslinkable thermoplastic matrix, polymethyl methacrylate, polyethylene terephthalate, glycol-modified polyethylene terephthalate, polyhydroxyalkanoates, polylactic acid, starch, polyvinyl alcohol, natural rubber, ethylene-propylene-diene monomer, polydimethylsiloxane, acrylonitrile butadiene rubber, polyether amide block copolymers, thermoplastic polyolefin elastomers, styrene block copolymers, thermoplastic polyurethane elastomers, thermoplastic vulcanizates, thermoplastic copolyester elastomers, and combinations thereof.
46. The masterbatch composition according to claim 44 or 45, in, The surface tension modifier is polystyrene.
47. The masterbatch composition according to claim 44, in, The rheology modifier is selected from the group consisting of erucamide, oleamide, behenamide, stearamide, ethylene bisoleamide, stearyl erucamide, oleyl palmitamide, and combinations thereof.
48. The masterbatch composition according to claim 44, in, The inorganic compound is selected from the group consisting of talc, calcium carbonate, sodium carbonate, silicate, mica, silicon dioxide, aluminum hydroxide, magnesium hydroxide, montmorillonite, sepiolite, and combinations thereof.
49. A masterbatch composition according to any one of claims 43 to 48, in, The carrier polymer is selected from the group consisting of low density polyethylene, linear low density polyethylene, polypropylene, ethylene vinyl acetate copolymer, ethylene methyl acrylate copolymer, ethylene butyl acrylate copolymer, ethylene-propylene copolymer, ethylene-propylene diene copolymer, thermoplastic elastomer including polyetheramide block copolymer, copolyester, polyolefin elastomer, vulcanized thermoplastic elastomer or styrene block copolymer, metallocene polymer, polyvinylidene fluoride, chlorinated derivatives of the above substances and combinations thereof.
Citation Information
Cited By
Secondary battery cell, battery device, electric device, and separator and preparation method therefor
WO2026175027A1