Flame retardant thermally conductive polycarbonate compositions with high comparative tracking index

By adding talc, phosphorus-containing flame retardant and acid anhydride modified α-olefin polymer to polycarbonate, a high-performance thermoplastic composition is solved, compared with leakage trace index of polycarbonate materials in the electronic/electrical field, the electronic/electrical field is solved. and the lack of flame retardancy achieves the safety and thermal conductivity requirements for high-voltage applications.

CN118974169APending Publication Date: 2024-11-15COVESTRO DEUTSCHLAND AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032891.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-14
Filing Date
2023-04-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing polycarbonate materials lack high leakage trace index and good flame retardancy in the electronics/electrical field, making it difficult to meet the safety requirements of high voltage applications, especially in the electric vehicle field.

Method used

By combining aromatic polycarbonate with a specific range of talc, phosphorus-containing flame retardant, drip-proof agent and anhydride-modified alpha-olefin polymer, a thermally conductive thermoplastic composition is formed, preferably containing more than 50% bis Phenol A homopolycarbonate, 32-37% talc, 4-10% phosphorus flame retardant, 0.3-2% fluorine-containing anti-drip agent and 1-3% acid anhydride modified α-olefin polymer , the composition does not contain other fillers.

Benefits of technology

The composition has achieved a high leakage trace index of above 400V and a UL94V0 grade flame retardancy of below 2mm, and has good heat deformation resistance and thermal conductivity, and is suitable for electronic components such as high voltage switches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005073271350000071
    Figure BDA0005073271350000071
  • Figure BDA0005073271350000081
    Figure BDA0005073271350000081
  • Figure BDA0005073271350000091
    Figure BDA0005073271350000091
Patent Text Reader

Abstract

A thermally conductive flame retardant composition having a high comparative tracking index is described that includes a bisphenol A homo-polycarbonate, talc, a phosphorus-containing flame retardant, a fluorine-containing anti-drip agent, and an anhydride-modified alpha-olefin polymer. The composition has a high comparative tracking index such that a smaller distance between the electrical conductors can be achieved in an EE component compared to the distances that were hitherto possible to achieve.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a thermally conductive flame retardant thermoplastic composition based on polycarbonate having a high relative tracking index.

[0002] Polycarbonate has many advantages over other thermoplastic polymers due to its high impact toughness, high heat deformation resistance and certain inherent flame retardancy. Due to this unique property profile, polycarbonate compositions are in principle suitable for a wide variety of different applications, for example in the field of electrical and electronic components. In particular, good insulation properties and high flame retardancy are essential safety-related basic requirements for materials used in this field.

[0003] In applications where plastics are in direct contact with electrical conductor strips, a high resistance to leakage currents under voltage load is a prerequisite so that there are no short circuits within the component and therefore no fire. The comparative tracking index (CTI), "comparative tracking index", generally describes the resistance of a plastic material to environmental influences. The CTI value is a measure of the tendency of a plastic to form conductive paths on its surface under voltage under environmental influences such as moisture and dirt and to promote the generation of leakage currents thereby. The higher the resistance to leakage currents or the comparative tracking index (CTI value) of a material, the more suitable it is for high-voltage applications, such as modern electric vehicle applications. Another advantage of materials with high CTI values ​​is that the electrical conductor strips in EE components can be arranged closer together without the risk of short circuits, which in turn enables the component size to be reduced, thus achieving a more compact design and weight reduction.

[0004] Compared with other thermoplastic polymers such as polystyrene and polyester, polycarbonate itself has a very low comparative tracking index and moderate flame retardancy. Due to the high proportion of aromatic structures, polycarbonate has a relatively high carbonization tendency. The CTI of pure polycarbonate is about 250V or even lower (F. Acquasanta et al., Polymer Degradation and Stability, 96 (2011), 2098-2103). However, for many applications in the field of electronics / electrical (EE), such as the field of electric vehicles, for safety reasons, the CTI of the materials used is required to be higher. Therefore, to date, polycarbonate has not been considered as a material for many applications that just need a high comparative tracking index of the material.

[0005] For applications requiring a high comparative tracking index of the material, the material must at the same time also have a high flame retardancy, ie a V0 rating according to UL94V, in particular even in the case of thin wall thicknesses.

[0006] Although pure polycarbonate usually has a certain inherent flame retardancy (V2 rating according to UL94V), this is not enough for most applications in the EE field. In order to achieve the required V0 rating according to UL94V, it is necessary to add suitable flame retardants. Polycarbonates usually use halogenated sulfonates (such as Rimar salts (potassium perfluorobutanesulfonate, C4 salts) or KSS salts (potassium diphenyl sulfone 3-sulfonate)) or organic phosphates (such as bisphenol A bis(diphenyl phosphate) (BDP), resorcinol bis(diphenyl phosphate) (RDP)) or phosphazenes. In principle, the flame retardancy of polycarbonate can be well adjusted by adding corresponding flame retardant additives. However, the mechanism of action of these flame retardants is based on the formation of a solid carbonized surface layer, which blocks the oxygen supply and thus inhibits the combustion process.

[0007] For example, WO 2020 / 212245 A1 describes a thermally conductive polycarbonate-based composition containing 50 to 75% by weight of an aromatic polycarbonate, 15 to 35% by weight of talc, 0.5 to 3% by weight of an anhydride-modified α-olefin polymer, 0.4 to 0.6% by weight of a fluorinated anti-drip agent, 3 to 10% by weight of phosphazenes or 3 to 5% by weight of phosphoric acid esters and 3 to 10% by weight of barium sulfate, which is included as a flame retardant synergist.

[0008] However, the basic effect for a good comparative tracking index is in particular the low tendency to form conductive paths on the surface. This is completely opposite to the action mechanism of surface-active flame retardants, "charring", and therefore presents a special challenge to achieve a high comparative tracking index and good flame retardancy in polycarbonate materials.

[0009] Particularly in the field of electronic components or current-carrying components, materials with a high comparative tracking index are required. Any current flow is associated with the generation of heat, which increases with increasing power. In order to prevent technical failures and thus ensure the service life of such components, the generated heat must be adequately dissipated. It would be ideal to be able to provide a polycarbonate material with a high comparative tracking index and flame retardancy, which can also contribute to the dissipation of heat.

[0010] Thermally conductive polycarbonate materials are known in principle from the prior art. For example, WO 2018 / 037037 A1 describes corresponding compositions which have improved thermal conductivity due to the use of talc. By adding maleic anhydride-modified olefin waxes, the alkaline polymer degradation caused by talc is greatly suppressed, resulting in a material with favorable mechanical properties. However, this material is not characterized by good flame retardancy and the comparative tracking index is not significantly increased compared to pure polycarbonate. Until now, experts also believed that there were no polycarbonate materials with a high comparative tracking index to date.

[0011] The object is therefore to provide thermally conductive polycarbonate-based compositions having a high CTI of at least 400 V, preferably at least 450 V, preferably determined according to a rapid test method based on IEC 60112:2009, and preferably also achieving a UL94 V0 rating at 2 mm. The thermal conductivity (in-plane) should preferably be at least 1.0 W / (mK), determined according to ASTM E 1461-13. Due to the application areas and heat generation in EE components, the composition should preferably also have good heat distortion resistance, in particular a Vicat softening temperature of at least 110° C., preferably at least 112° C., particularly preferably at least 115° C., determined according to ISO 306:2014-3, VST method B.

[0012] Surprisingly, it has been shown that an improvement in the comparative tracking index can be achieved by adding talc. The object of providing a composition having the above-mentioned complex property profile is achieved by combining an aromatic polycarbonate with talc and a phosphorus-containing flame retardant, an anti-drip agent and an anhydride-modified α-olefin polymer in each case in a selected amount range.

[0013] The subject of the present invention is therefore a thermoplastic composition comprising

[0014] A) at least 50% by weight of bisphenol A homopolycarbonate,

[0015] B) 32 to 37% by weight of talc,

[0016] C) 4 to 10% by weight of a phosphorus-containing flame retardant,

[0017] D) 0.3 to 2% by weight of a fluorinated anti-drip agent,

[0018] E) 1 to 3% by weight of an anhydride-modified α-olefin polymer,

[0019] The composition does not contain any other fillers.

[0020] In addition to components A, B, C, D and E, the composition according to the present invention may also contain other components, for example other additives in the form of component F. The composition may also contain one or more other thermoplastics that are different from the above-mentioned components and do not belong to any of components A to F as a blending partner (component G). In the context of the present invention - unless otherwise explicitly stated - the weight % shown for components A, B, C, D, E, optional F and optional G are each based on the total weight of the composition. It should be understood that all components included in the composition according to the present invention add up to 100%. When the upper limit of a numerical range is shown with "to X", this includes the numerical value shown and the range rounded up thereof.

[0021] Thermoplastic polymers other than components A, E and F and suitable as blending partners include, for example, other aromatic polycarbonates which are not bisphenol A homopolycarbonate (i.e. different from component A), polystyrene, styrene copolymers, aromatic polyesters such as polyethylene terephthalate (PET) or polybutylene terephthalate (PBT), PET-cyclohexanedimethanol copolymers (PETG), polyethylene naphthalate (PEN), PMMA and PMMA copolymers, PMMI, polyolefins such as polyethylene or polypropylene, and copolymers with styrene such as transparent polystyrene-acrylonitrile (PSAN) or also thermoplastic polyurethanes.

[0022] It is very particularly preferred that the above composition does not contain any further components, but the amounts of components A, B, C, D, E, optionally F, and optionally G, in particular in the preferred embodiment, add up to 100% by weight, i.e. the composition according to the invention consists of components A, B, C, D, E, optionally F, and optionally G, particularly preferably consisting of components A to F.

[0023] It is to be understood that the components used may contain conventional impurities, for example from their production process. It is preferred to use components that are as pure as possible. It is also to be understood that these impurities may also be contained in the closed formulation of the composition.

[0024] The subject of the present invention is also a molding made of a thermoplastic composition according to the invention, i.e. a molding consisting of a thermoplastic composition according to the invention or comprising a region made of a thermoplastic composition according to the invention. Such moldings are especially moldings for which the above-mentioned performance profile is particularly attractive, i.e. moldings as part of components in the EE field, in particular high-voltage switches, inverters, relays, electronic connectors, electrical connectors, circuit breakers, components for photovoltaic applications, motors, radiators, chargers and charging plugs for electric vehicles, electrical junction boxes, housings for smart meters, miniature circuit breakers, busbars. The component is preferably designed for an operating voltage of at least 400 V. For this purpose, the material advantageously used preferably has a comparative tracking index of at least 400 V, in particular at least 450 V, determined as described above according to a rapid test method based on IEC 60112:2009.

[0025] When at least 50 drops of 0.1% strength ammonium chloride solution are applied at 400 V, further preferably at 450 V, the composition of the present invention does not exhibit a significant leakage current (> 0.5 A within 2 seconds), wherein the test is preferably carried out according to the rapid test method based on IEC 60112: 2009 described in the description. The composition of the present invention also has a flame retardancy of V0 according to UL94V at a test specimen thickness of 2 mm. In addition to high CTI and good flame retardancy, the composition preferably also has good heat deformation resistance, which is manifested by a Vicat softening temperature of at least 110°C, preferably at least 112°C, and in particular 115°C, measured according to ISO 306: 2014-3, VST method B.

[0026] The individual components of the composition according to the invention are explained in more detail below:

[0027] Component A

[0028] Component A of the thermoplastic composition according to the invention is a bisphenol A homopolycarbonate, ie an aromatic polycarbonate based on bisphenol A as the sole monomer unit.

[0029] The melt volume flow rate MVR of the aromatic bisphenol A homopolycarbonate used, determined in accordance with ISO 1133:2012-03 at a test temperature of 300° C. and a load of 1.2 kg, is preferably 5 to 35 cm 3 / (10min), more preferably 6 to 21cm 3 / (10min), particularly preferably 10 to 19cm 3 / (10 min), very particularly preferably 11 to 15 cm 3 / (10min).

[0030] Details of the preparation of polycarbonates have been given in numerous patent documents over the past approximately 40 years. Reference may be made here, for example, to Schnell, "Chemistry and Physics of Polycarbonates", Polymer Reviews, Vol. 9, Interscience Publishers, New York, London, Sydney 1964, to D. Freitag, U. Grigo, PR Müller, H Nouvertné, BAYER AG, "Polycarbonates", Encyclopedia of Polymer Science and Engineering, Vol. 11, 2nd edition, 1988, pp. 648-718, and finally to U. Grigo, K. Kirchner and PR Müller "Polycarbonate", Becker / Braun, Kunststoff-Handbuch, Vol. 3 / 1, Polycarbonate, Polyacetale, Polyester, Celluloseester, Carl Hanser Verlag München, Wien 1992, pp. 117-299.

[0031] Aromatic polycarbonates are prepared, for example, by the reaction of dihydroxyaryl compounds with carbonyl halides, preferably phosgene, and / or with aromatic dicarboxylic acid dihalides, preferably phthalic acid dihalides, by the phase interface process, optionally with the use of chain terminators and optionally with trifunctional or more than trifunctional branching agents. They can likewise be prepared by the melt polymerization process by reaction of dihydroxyaryl compounds with, for example, diphenyl carbonate.

[0032] In the case of bisphenol A homopolycarbonate, only bisphenol A is used as the dihydroxyaryl compound.

[0033] In the preparation of bisphenol A homopolycarbonate, the preferred chain terminator is a linear or branched, preferably unsubstituted C1 to C 30 The chain terminators are preferably phenols which are mono- or polysubstituted with tert-butyl groups or tert-alkyl groups. Particularly preferred chain terminators are phenol, cumylphenol and / or p-tert-butylphenol. The amount of chain terminators used is preferably 0.1 to 5 mol %, based on the number of moles of dihydroxyaryl compounds used in each case. The chain terminators can be added before, during or after the reaction with the carbonic acid derivatives.

[0034] In principle, the homopolycarbonates can also be branched.

[0035] Suitable branching agents are the trifunctional or more than trifunctional compounds known from polycarbonate chemistry, in particular those having three or more than three phenolic OH groups.

[0036] Examples of suitable branching agents include 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, tris(4-hydroxyphenyl)phenylmethane, 2,4-bis(4-hydroxyphenylisopropyl)phenol, 2,6-bis(2-hydroxy-5′-methylbenzyl)-4-methylphenol, 2-(4-hydroxyphenyl)-2-(2,4-dihydroxyphenyl)propane, tetrakis(4-hydroxyphenyl)methane, tetrakis(4-(4-hydroxyphenylisopropyl)phenoxy)methane and 1,4-bis((4′,4″-dihydroxytriphenyl)methyl)benzene and 3,3-bis(3-methyl-4-hydroxyphenyl)-2-oxo-2,3-dihydroindole.

[0037] The amount of branching agents optionally used is preferably from 0.05 mol % to 2.00 mol %, based on the moles of bisphenol A used in each case.

[0038] The branching agent can be initially charged together with bisphenol A and the chain terminator in the alkaline aqueous phase or added as a solution in an organic solvent prior to the phosgenation. In the case of the transesterification process, the branching agent is used together with bisphenol A.

[0039] As additional blending partners of component G, in principle, other aromatic polycarbonates can also be included in the composition of the invention, as long as they do not have a negative impact on the performance profile required by the invention (i.e. a high comparative tracking index and good flame retardancy at 2 mm) and do not lower the Vicat temperature too much, i.e. preferably not below 110° C., preferably not below 112° C., in particular not below a Vicat temperature of 115° C.

[0040] The thermoplastic composition according to the invention contains at least 50% by weight, preferably at least 54% by weight, of aromatic bisphenol A homopolycarbonate, ie is based on aromatic polycarbonate.

[0041] Component B

[0042] Talc in the context of the present invention is preferably talc, or a mixture of talcs, having essentially the same chemical composition, particle size, porosity and / or BET surface area.

[0043] Talc is generally a layered silicate. It can be described as a magnesium silicate hydrate, with a general chemical composition of Mg3[Si4O 10 (OH)2]. However, different types of talc contain different impurities and can therefore deviate from this general composition.

[0044] The talc or talc mixture used to prepare the composition of the present invention can be sized or unsized. Talc is preferably unsized. In the context of the present invention, sizing is considered to be the targeted (chemical or physical adsorption) enrichment of molecules on the surface. Therefore, unsized talc is talc without surface treatment, that is, after obtaining talc particles with the desired particle size and optionally compacting, talc is preferably not subjected to any further method steps, which method steps change the surface of talc by chemical adsorption and / or physical adsorption in a targeted manner. However, this does not exclude that impurities, dust or similar particles accidentally arrive at the surface portion in the process of further processing of talc, provided that the surface of talc does not significantly lose its performance, especially the performance relevant to the pH value.

[0045] The pH value of the talc is preferably 8 to 10, particularly preferably 8.5 to 9.8, very particularly preferably 9.0 to 9.7, wherein the pH value is determined in accordance with EN ISO 787-9: 1995. It should be noted that EN ISO 787-9: 1995 also mentions the possibility of adding ethanol or other organic solvents to improve the dispersibility of the solid to be analyzed. According to the invention, it is preferred to use only distilled water for determining the pH value in accordance with EN ISO 787-9: 1995.

[0046] Component B, talc, preferably has an iron (II) oxide and / or iron (III) oxide content of 0.2 to 2.5% by weight, particularly preferably 0.3 to 2.3% by weight, very particularly preferably 0.3 to 2.0% by weight. The content is preferably measured by X-ray fluorescence or atomic absorption spectroscopy. The iron oxide content in the talc has an influence on the degree of degradation of the polycarbonate. It is advantageous to use talc with the indicated iron oxide content.

[0047] Likewise preferably, component B has an aluminum oxide content of 0.01 to 0.5% by weight, particularly preferably 0.05 to 0.48% by weight, very particularly preferably 0.15 to 0.45% by weight.

[0048] The median particle size D50 of component B is preferably 0.01 to 10 μm, particularly preferably 0.25 to 10.00 μm, further preferably 0.5 to 10.00 μm, particularly preferably 1 to 5 μm, wherein the particle size D50 is determined by sedimentation analysis. A person skilled in the art understands that the median D50 refers to the median particle size at which 50% of the particles are smaller than this specific value. The particle size D50 is preferably determined according to ISO 13317-3:2001.

[0049] The BET surface area of ​​component B is preferably from 7.5 to 20.0 m 2 / g, particularly preferably 9.0 to 15.0 m 2 / g, very particularly preferably 9.5 to 14.0 m 2 / g. The determination of the surface area by gas adsorption according to Brunauer, Emmett and Teller is known per se to the person skilled in the art. The BET surface area is preferably determined according to ISO 4652:2012-06. The preferred BET surface area is particularly preferably correlated with the median particle size D50 of the above-mentioned talcs. It has been found that in the case of this combination, the component B used according to the invention is optimally matched to the component C used according to the invention. By means of the specific acid number and molar mass of component E, the degradation of the polycarbonate caused by component B can be minimized.

[0050] Particularly preferably, the talc has a talc content of >96% by weight, particularly preferably >97% by weight, very particularly preferably ≥98% by weight.

[0051] It is likewise preferred if the talc has a loss on ignition of 5.0 to 7.0% by weight, particularly preferably 5.2 to 6.5% by weight, very particularly preferably 5.3 to 6.2% by weight at 1050° C. The loss on ignition is preferably determined in accordance with DIN 51081:2002.

[0052] The talc (also a talc mixture) is preferably present in compacted form according to component B. In the case of a talc mixture, the abovementioned numerical data are each based on the talc mixture, ie component B as a whole.

[0053] The composition according to the invention has a talc content of 32 to 37% by weight, preferably 34 to 36% by weight, particularly preferably 34.5 to 35.5% by weight, based on the entire composition.

[0054] Component C

[0055] Component C of the composition according to the invention is a phosphorus-containing flame retardant. It can be a single phosphorus-containing flame retardant, but it can also be a mixture of different phosphorus-containing flame retardants.

[0056] Preferred phosphorus-containing flame retardants are cyclic phosphazenes, phosphorus compounds of formula (10) and mixtures thereof:

[0057]

[0058] in

[0059] R 1 , R 2 , R 3 and R 4 are independently of one another C1- to C8-alkyl, in each case optionally halogenated and in each case branched or unbranched, and / or C5- to C6-cycloalkyl, C6- to C8 ... 20 -aryl or C7- to C 12 -aralkyl,

[0060] n is independently 0 or 1,

[0061] q is a value from 0 to 30, and

[0062] X is a monocyclic or polycyclic aromatic radical having 6 to 30 carbon atoms or a straight-chain or branched aliphatic radical having 2 to 30 carbon atoms, which in each case may be substituted or unsubstituted, bridged or unbridged.

[0063] Preferably, R 1 , R 2 , R 3 and R 4 are independently branched or unbranched C1- to C4-alkyl, phenyl, naphthyl or phenyl substituted by C1- to C4-alkyl. 1 , R 2 , R 3 and / or R 4 In the case of , these themselves may be substituted by halogen and / or alkyl, preferably chlorine, bromine and / or branched or unbranched C1- to C4-alkyl. Particularly preferred aryl groups are tolyl, phenyl, xylyl, propylphenyl and butylphenyl, and the corresponding brominated and chlorinated derivatives thereof.

[0064] X in formula (10) is preferably derived from a dihydroxyaryl compound.

[0065] X in formula (10) is particularly preferably

[0066]

[0067] or chlorinated and / or brominated derivatives thereof. X (together with the adjacent oxygen atom) is preferably derived from hydroquinone, bisphenol A or diphenylphenol. It is also preferred that X is derived from resorcinol. X is particularly preferably derived from bisphenol A. n in formula (10) is preferably equal to 1. q is preferably 0 to 20, particularly preferably 0 to 10, and in the case of a mixture is an average value of 0.8 to 5.0, preferably 1.0 to 3.0, further preferably 1.05 to 2.00, particularly preferably 1.08 to 1.60.

[0068] The phosphorus compound of general formula (10) is preferably a compound of formula (11):

[0069]

[0070] in

[0071] R 1 , R 2 , R 3 and R 4Each independently of one another is a linear or branched C1- to C8-alkyl group and / or a C5- to C6-cycloalkyl group, a C6- to C8-cycloalkyl group, a C6- to C8-cycloalkyl group, a C5- to C6 ...6- to C8-cycloalkyl group, a C6- to C8- 10 -aryl or C7- to C 12 -aralkyl,

[0072] n is independently 0 or 1,

[0073] q is independently 0, 1, 2, 3 or 4,

[0074] N is a value from 1 to 30,

[0075] R5 and R6 are independently of one another straight-chain or branched C1- to C4-alkyl, preferably methyl, and

[0076] Y is a straight chain or branched C1- to C7-alkylidene group, a straight chain or branched C1- to C7-alkylene group, a C5- to C7- 12 -cycloalkylene, C5- to C 12 -cycloalkylidene, -O-, -S-, -SO-, SO2 or -CO-.

[0077] The phosphorus compounds of the formula (10) are in particular tributyl phosphate, triphenyl phosphate, tricresyl phosphate, diphenylcresyl phosphate, diphenyloctyl phosphate, diphenyl 2-ethylcresyl phosphate, tri(isopropylphenyl) phosphate, resorcinol-bridged oligophosphates and bisphenol A-bridged oligophosphates. If phosphorus compounds of the formula (10) are used, it is particularly preferred to use oligophosphates of the formula (10) derived from bisphenol A.

[0078] Preference is further given to using mixtures of identical structure and different chain lengths, wherein the indicated q values ​​are average q values. The average q value is determined by determining the composition (molecular weight distribution) of the phosphorus compound mixture at 40° C. in a mixture of acetonitrile and water (50:50) by means of high pressure liquid chromatography (HPLC) and calculating the average value of q therefrom.

[0079] Particularly preferably, oligomeric phosphates based on bisphenol A according to formula (12) (bisphenol A bis(diphenyl phosphate)) wherein q=1 to 20, in particular wherein q=1.0 to 1.2, are contained in the composition according to the invention.

[0080]

[0081] Such phosphorus compounds are known (see, for example, EP 0 363 608 A1, EP 0 640 655 A2) or can be prepared in an analogous manner by known methods (see, for example, Ullmanns der technischen Chemie, Vol. 18, p. 301 ff., 1979; Houben-Weyl, Methoden der organischen Chemie, Vol. 12 / 1, p. 43; Beilstein, Vol. 6, p. 177).

[0082] Alternatively, cyclic phosphazenes according to formula (13) are particularly preferably used as component C:

[0083]

[0084] in

[0085] R is the same or different in each case and is

[0086] - amine groups,

[0087] - in each case optionally halogenated, preferably by fluorine, further preferably monohalogenated C1- to C8-alkyl, preferably methyl, ethyl, propyl or butyl,

[0088] - C1- to C8-alkoxy, preferably methoxy, ethoxy, propoxy or butoxy,

[0089] - in each case optionally alkyl-substituted, preferably C1- to C4-alkyl-substituted, and / or halogen-substituted, preferably chlorine- and / or bromine-substituted, C5- to C6-cycloalkyl,

[0090] - in each case optionally alkyl-substituted, preferably C1- to C4-alkyl-substituted, and / or halogen-substituted, preferably chlorine-, bromine- and / or hydroxy-substituted C6- to C4- 20 - aryloxy, preferably phenoxy, naphthoxy,

[0091] - in each case optionally alkyl-substituted, preferably C1- to C4-alkyl-substituted, and / or halogen-substituted, preferably chlorine- and / or bromine-substituted, C7- to C4- 12 - aralkyl, preferably phenyl-C1- to C4-alkyl, or

[0092] - a halogen group, preferably chlorine or fluorine, or

[0093] -OH group,

[0094] k is an integer from 1 to 10, preferably from 1 to 8, particularly preferably from 1 to 5, very particularly preferably 1.

[0095] Commercially available phosphazenes are preferably used here. These are usually mixtures of rings of different ring sizes.

[0096] Further preferred are, individually or as a mixture: propoxyphosphazene, phenoxyphosphazene, methylphenoxyphosphazene, aminophosphazene, fluoroalkylphosphazene, and phosphazene having the following structure:

[0097]

[0098] In compounds 13a-f shown above, k=1, 2 or 3.

[0099] Preferably, the proportion of phosphazenes substituted on phosphorus by halogen (eg from incompletely reacted starting materials) is less than 1000 ppm, further preferably less than 500 ppm.

[0100] The phosphazenes can be used alone or as a mixture. The radical R can always be identical, or two or more radicals in these formulae can be different. The radicals R of the phosphazenes are preferably identical.

[0101] In one embodiment, only phosphazenes having the same R are used.

[0102] Preferably, the proportion of tetramers (k=2), based on component B, is 2 to 50 mol %, further preferably 5 to 40 mol %, even more preferably 10 to 30 mol %, particularly preferably 10 to 22 mol %.

[0103] Preferably, the proportion of higher oligophosphazenes (k=3, 4, 5, 6 and 7), based on component B, is 0 to 30 mol %, further preferably 2.5 to 25 mol %, even more preferably 5 to 20 mol % and particularly preferably 6-15 mol %.

[0104] Preferably, the proportion of oligomers with k≧8, based on component B, is from 0 to 2.0 mol %, preferably from 0.10 to 1.00 mol %.

[0105] It is further preferred that the phosphazene of component C meets all three of the abovementioned conditions regarding the oligomer ratio.

[0106] Particularly preferably, phenoxyphosphazenes (all R=phenoxy, formula 13g) are included as component C, either alone or together with other phosphazenes according to formula (13), wherein the proportion of oligomers with k=1 (hexaphenoxyphosphazenes) is 50 to 98 mol %, particularly preferably 60 to 72 wt %, based on the amount of phenoxyphosphazenes. If phenoxyphosphazenes are used, the proportion of oligomers with k=2 is very particularly preferably 15 to 22 wt %, and the proportion of oligomers with k≥3 is 10 to 13 wt %.

[0107]

[0108] Alternatively, component C very particularly preferably comprises, and very particularly preferably is, a phenoxyphosphazene having a trimer (k=1) proportion of 70 to 85 mol %, a tetramer (k=2) proportion of 10 to 20 mol %, a higher oligomeric phosphazene proportion (k=3, 4, 5, 6 and 7) of 3 to 8 mol % and a phosphazene oligomer with k≥8 of 0.1 to 1 mol %.

[0109] In an alternative preferred embodiment, n, defined as the arithmetic mean of k, is from 1.10 to 1.75, preferably from 1.15 to 1.50, further preferably from 1.20 to 1.45, particularly preferably from 1.20 to 1.40 (range limits inclusive).

[0110]

[0111] Phosphazenes and their preparation are described, for example, in EP 728 811 A2, DE 1961668 A and WO 97 / 40092 A1.

[0112] After compounding, 31 P NMR detected and quantified the oligomer composition in the respective blend samples (chemical shifts; delta trimer: 6.5 to 10.0 ppm; delta tetramer: -10 to -13.5 ppm; delta higher oligomers: -16.5 to -25.0 ppm).

[0113] Particularly preferably, component C comprises an oligomeric phosphate based on bisphenol A according to formula (12) and / or a cyclic phosphazene according to formula (13); very particularly preferably, component C is an oligomeric phosphate based on bisphenol A according to formula (12) and / or a cyclic phosphazene according to formula (13); particularly preferably, component C is a cyclic phosphazene according to formula (13).

[0114] The proportion of phosphorus-containing flame retardants in the composition of the invention is 4% to 10% by weight, preferably 5% to 8% by weight, particularly preferably 5.0% to 8.0% by weight, based on the entire composition.

[0115] The higher the amount of phosphorus-containing flame retardant used, the more the Vicat temperature decreases. When the amount used exceeds 10% by weight, the Vicat temperature decreases to such an extent that applications for which polycarbonate can be used due to its inherent high heat resistance can no longer be performed by this material.

[0116] Component D

[0117] The composition of the invention contains a fluorinated anti-drip agent as component D, which may be a mixture of a plurality of anti-drip agents. The total amount of the anti-drip agent (anti-drip agent) is 0.3% to 2% by weight, preferably 0.3% to 1.0% by weight, particularly preferably 0.4% to 0.7% by weight of at least one anti-drip agent, based on the entire composition.

[0118] The anti-drip agent used is preferably a fluorinated polymer, in particular a polyolefin.

[0119] Fluorinated polyolefins preferably used as anti-drip agents have a high molecular weight, a glass transition temperature above -30°C, typically above 100°C, and a fluorine content of preferably 65 to 76% by weight, in particular 70 to 76% by weight. Preferred fluorinated polyolefins are polytetrafluoroethylene, polyvinylidene fluoride, tetrafluoroethylene / hexafluoropropylene copolymers and ethylene / tetrafluoroethylene copolymers. Fluorinated polyolefins are known (see Schildknecht, "Vinyl and Related Polymers", John Wiley & Sons, Inc., New York, 1962, pp. 484-494; Wall, "Fluoropolymers", Wiley-Interscience, John Wiley & Sons, Inc., New York, Vol. 13, 1970, pp. 623-654; "Modern Plastics Encyclopedia", 1970-1971, Vol. 47, No. 10A, October 1970, McGraw-Hill, Inc., New York, pp. 134 and 774; "Modern Plastics Encyclopedia", 1975-1976, October 1975, Vol. 52, No. 10A, McGraw-Hill, Inc., New York, pp. 27, 28 and 472 and U.S. Pat. No. 3,837,891). 671 487 A, 3 723 373 A and 3 838 092 A). They can be prepared by known methods, for example by reacting tetrafluoroethylene in an aqueous medium containing a free radical forming catalyst, for example sodium peroxodisulfate, potassium peroxodisulfate or ammonium peroxodisulfate at 7 to 71 kg / cm 2 The polymerization is carried out under a pressure of 100° C. and at a temperature of 0 to 200° C., preferably at a temperature of 20 to 100° C. More details are given, for example, in US Pat. No. 2,393,967 A.

[0120] Depending on the form of use, the density of the fluorinated polyolefin can be between 1.2 and 2.3 g / cm 3 , preferably 2.0g / cm 3 Up to 2.3g / cm 3, determined according to ISO 1183-1 (2019-09), and the average particle size is 0.05 to 1000 μm, determined by optical microscopy or white light interferometry.

[0121] Suitable tetrafluoroethylene polymer powders are commercial products and are available, for example, under the trade name Obtained from DuPont.

[0122] Particularly preferably, polytetrafluoroethylene (PTFE) itself and in the form of a PTFE-containing composition are used as fluorinated anti-drip agents. If a PTFE-containing composition is used as a fluorinated anti-drip agent, the minimum amount used is sufficient to contain at least 0.2% by weight, preferably at least 0.21% by weight, and particularly preferably at least 0.25% by weight of PTFE in the entire composition. PTFE-containing compositions include those of Chemtura TF2021 or PTFE blends, e.g. B449 (approximately 50% by weight PTFE and approximately 50% by weight SAN [composed of 80% by weight styrene and 20% by weight acrylonitrile]). Particularly preferably, PTFE or a PTFE / SAN blend is used as the fluorinated anti-drip agent; particularly preferably, the fluorinated anti-drip agent is PTFE or PTFE / SAN.

[0123] Component E

[0124] Component E of the composition according to the present invention is an anhydride-modified α-olefin polymer.

[0125] The α-olefin polymer is preferably based on at least one monomer selected from ethylene, 1-propylene, 1-butene, 1-isobutylene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-octadecene, 1-nondecene, but may also be based on a mixture of these monomers. Further preferably, the α-olefin polymer is based on at least one monomer selected from ethylene, propylene, 1-hexene, 1-octene. Particularly preferably, the α-olefin polymer is based on ethylene, propylene and / or 1-octene.

[0126] In this context, "based on" means based on the total weight of the respective α-olefin polymers not modified with anhydride in the polycarbonate-containing composition, preferably at least 90% by weight, further preferably at least 95% by weight, and particularly preferably at least 98% by weight of the α-olefin polymers are formed from the respective monomer or monomers.

[0127] The α-olefin polymer is modified with anhydride, wherein the modified polymer is a saturated carboxylic anhydride. The carboxylic anhydride is preferably selected from maleic anhydride, phthalic anhydride, fumaric anhydride, itaconic anhydride and mixtures thereof. Maleic anhydride is particularly preferred.

[0128] The anhydride-modified α-olefin polymer is preferably free of styrene-butadiene rubber and very particularly preferably free of rubber.

[0129] Preferred anhydride-modified α-olefin polymers include

[0130] E1) 90.0-99.5 wt %, preferably 92.0-97.5 wt %, more preferably 94.0-97.0 wt % of an α-olefin polymer, and

[0131] E2) 0.5-10.0 wt %, further preferably 2.5-8.0 wt %, more preferably 3.0-6.0 wt % of anhydride.

[0132] The olefin part E1) of the α-olefin polymers here particularly preferably has the following characteristics:

[0133] The proportion of ethylene is 65.0 to 96.0% by weight, further preferably 80.0 to 96.0% by weight, very particularly preferably 84.0 to 92.0% by weight,

[0134] The proportion of propene is 2.0 to 10.0% by weight, very particularly preferably 4.0 to 8.0% by weight, and

[0135] The proportion of 1-octene is from 2.0 to 25.0% by weight, further preferably from 2.0 to 10.0% by weight and very particularly preferably from 4.0 to 8.0% by weight.

[0136] Very particularly preferably, the α-olefin polymer is not based on any other monomers.

[0137] Alternatively, the olefin portion C1) of the α-olefin polymer is particularly preferably based on propylene and / or ethylene, very particularly preferably to an extent of at least 98% by weight. Particularly preferably, the only monomer unit of the α-olefin polymer is propylene.

[0138] The average molecular weight M of the anhydride-modified α-olefin polymer W The molecular weight M is preferably 300 to 40,000 g / mol, more preferably 800 to 32,000 g / mol, further preferably 1,000 to 22,000 g / mol, and particularly preferably 3,000 to 21,000 g / mol. W It is determined by gel permeation chromatography in o-dichlorobenzene with polystyrene calibration at 150° C. The values ​​indicated here are preferably the average of duplicate determinations.

[0139] The acid value of the anhydride-modified α-olefin polymer is preferably at least 30 mg KOH / g, more preferably 45 to 170 mg KOH / g, particularly preferably up to 100 mg KOH / g, as determined by potentiometric titration with potassium hydroxide alcohol solution according to DIN ISO 17025:2005-08.

[0140] Very particularly preferably, the anhydride-modified α-olefin polymer according to component C is based on propylene, is maleic anhydride-modified, and further preferably has an average molecular weight M of 1000 to 22000 g / mol, further preferably 3000 to 21000 g / mol, determined by gel permeation chromatography in o-dichlorobenzene at 150° C. with polystyrene calibration. w , and an acid number of 45 to 170 mg KOH / g, further preferably 50 to 100 mg KOH / g, determined by potentiometric titration in accordance with DIN ISO 17025:2005-08.

[0141] The content of the anhydride-modified α-olefin polymer in the entire composition is 1 to 3 wt %, preferably 1.2 to 2.5 wt %, further preferably 1.3 to 2.3 wt %, particularly preferably 1.4 to 2 wt %, and especially to 1.6 wt %.

[0142] Other additives (component F)

[0143] The polycarbonate composition according to the invention may contain one or more further additives different from components B, C, D and E, which are grouped herein under "component F".

[0144] Optionally, other conventional additives ("other additives") are included (0 wt. %), preferably up to 10 wt. %, further preferably 0.1 wt. % to 5 wt. %, particularly preferably 0.1 wt. % to 3 wt. %, very particularly preferably 0.2 wt. % to 1.0 wt. %, wherein these weight percentages are based on the total weight of the composition. The other additive group does not include any talc (component B) and does not include any phosphorus-containing flame retardant according to component C. The other additive group also does not include any fluorine-containing anti-drip agent, as this has been described as component D, nor any anhydride-modified α-olefin polymer according to component E.

[0145] Such other additives which are usually added to polycarbonates are in particular heat stabilizers, antioxidants, mold release agents, UV absorbers, infrared absorbers, impact modifiers, antistatic agents, flame retardants other than component C, fluorescent whitening agents, light scattering agents, hydrolysis stabilizers, transesterification stabilizers, (organic) dyes, (organic / inorganic) pigments, compatibilizers and / or laser marking additives, in particular in amounts typical for compositions based on polycarbonate. Such additives are described, for example, in EP 0 839 623 A1, WO 96 / 15102 A1, EP 0 500 496 A1 or in "Plastics Additives Handbook", Hans Zweifel, 5th edition, 2000, Hanser Verlag, München. These additives can be added individually or in mixtures and are preferred additives according to the invention.

[0146] If other additives are present, it is further preferred to contain one or more other additives as other additives, which are selected from heat stabilizers, antioxidants, mold release agents, organic dyes, organic pigments, inorganic pigments. In particular, the proportion of the other additives is preferably 0% by weight to 3% by weight. It is very particularly preferred to contain at least one heat stabilizer, antioxidant, dye, pigment and / or mold release agent as other additives, particularly preferably a heat stabilizer and / or pigment.

[0147] It should be understood that such additives can only be added and can only be added in such amounts, provided that they do not significantly negatively affect the high CTI and good flame retardancy effect according to the present invention, and preferably do not reduce the Vicat temperature determined according to ISO 306:2014-3, VST method B to below 110° C., preferably below 115° C. Therefore, in addition to the phosphorus-containing flame retardant in component C, it is particularly preferred to include no more than 0.05% by weight of other flame retardants.

[0148] Although the composition according to the invention may contain further flame retardants in addition to component C, it preferably does not contain those selected from the group consisting of alkali metal, alkaline earth metal or ammonium salts of aliphatic or aromatic sulfonic acids, sulfonamides or sulfonimide derivatives and combinations thereof, wherein "derivatives" are understood to mean compounds whose molecular structure has different atoms or different atomic groups instead of hydrogen atoms or functional groups or in which one or more atoms / atomic groups have been removed. The parent compound is thus still identifiable.

[0149] Such flame retardants, which are preferably not contained in the composition according to the invention, are in particular one or more compounds selected from the group consisting of sodium or potassium perfluorobutane sulfate, sodium or potassium perfluoromethanesulfonate, sodium or potassium perfluorooctane sulfate, sodium or potassium 2,5-dichlorobenzene sulfate, sodium or potassium 2,4,5-trichlorobenzene sulfate, sodium or potassium diphenyl sulfone sulfonate, sodium or potassium 2-formylbenzenesulfonate, sodium or potassium (N-phenylsulfonyl)benzenesulfonamide or mixtures thereof, of which sodium or potassium perfluorobutane sulfate, sodium or potassium perfluorooctane sulfate, sodium or potassium diphenyl sulfone sulfonate or mixtures thereof, in particular potassium perfluoro-1-butanesulfonate, which can be used as C4 is available from Lanxess, Leverkusen, Germany. Very particularly preferably no further flame retardants are present at all.

[0150] Particularly preferably included additives are mold release agents, further preferably based on fatty acid esters, further preferably on stearates, particularly preferably on pentaerythritol. Particular preference is given to using pentaerythritol tetrastearate (PETS) and / or glycerol monostearate (GMS). If one or more mold release agents are used, their amount is preferably up to 1.0% by weight (inclusive), further preferably 0.01% to 0.7% by weight, particularly preferably 0.02% to 0.60% by weight, in each case based on the entire composition.

[0151] Particularly preferably, the additive also contains a heat stabilizer. The amount of the heat stabilizer is preferably up to 0.20% by weight, more preferably 0.01% by weight to 0.10% by weight, even more preferably 0.01% by weight to 0.05% by weight, particularly preferably 0.015% by weight to 0.040% by weight, based on the entire composition.

[0152] Suitable heat stabilizers are in particular phosphorus-based stabilizers selected from phosphates, phosphites, phosphonites, phosphines and mixtures thereof. Examples include triphenyl phosphite, diphenyl alkyl phosphites, phenyl dialkyl phosphites, tris(nonylphenyl) phosphite, trilauryl phosphite, tri(octadecyl) phosphite, pentaerythritol distearyl diphosphite, tris(2,4-di-tert-butylphenyl) phosphite ( 168), pentaerythritol diphosphite diisodecyl ester, pentaerythritol diphosphite bis(2,4-di-tert-butylphenyl) ester, pentaerythritol diphosphite bis(2,4-dicumylphenyl) ester ( S-9228), pentaerythritol diphosphite bis(2,6-di-tert-butyl-4-methylphenyl) ester, pentaerythritol diphosphite diisodecyl ester, pentaerythritol diphosphite bis(2,4-di-tert-butyl-6-methylphenyl) ester, pentaerythritol diphosphite bis(2,4,6-tri(tert-butylphenyl) ester, sorbitol triphosphite tristearyl ester, 4,4'-biphenylene diphosphite tetra(2,4-di-tert-butylphenyl) ester, 6-isooctyloxy-2,4,8,10-tetra-tert-butyl-12H-dibenzo[d,g]-1,3,2-dioxaphosphooctate, phosphite bis(2,4-di-tert-butyl-6-methylphenyl) methyl ester, phosphite bis(2,4-di-tert-butyl-6-methylphenyl) ethyl ester, 6-fluoro-2 ,4,8,10-tetra-tert-butyl-12-methyldibenzo[d,g]-1,3,2-dioxaphosphinic acid octane, 2,2′,2″-nitrilo[triethyltris(3,3′,5,5′-tetra-tert-butyl-1,1′-biphenyl-2,2′-diyl)phosphite], 2-ethylhexyl(3,3′,5,5′-tetra-tert-butyl-1,1′-biphenyl-2,2′-diyl)phosphite, 5-butyl-5-ethyl-2-(2,4,6-tri-tert-butylphenoxy)-1,3,2-dioxaphosphinic acid propane, pentaerythritol diphosphite bis(2,6-di-tert-butyl-4-methylphenyl) ester, triphenylphosphine (TPP), trialkylphenylphosphine, bisdiphenylphosphinoethane or trinaphthylphosphine. They are used alone or in combination, for example B900( 168 and Antioxidants 1076 in a 4:1 ratio) or S-9228 and B900 or 1076. It is particularly preferred to use triphenylphosphine (TPP), 168 or tris(nonylphenyl) phosphite or a mixture thereof.

[0153] Phenolic antioxidants such as alkylated monophenols, alkylated sulfanylphenols, hydroquinones and alkylated hydroquinones may also be used. 1010 (pentaerythritol 3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate; CAS: 6683-19-8) and Irganox (octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate), preferably in an amount of 0.05 wt% to 0.5 wt%.

[0154] Sulfonates or alkyl phosphates, such as monohexyl phosphate, dihexyl phosphate and / or trihexyl phosphate, triisooctyl phosphate and / or trinonyl phosphate, can also be added as transesterification inhibitors. The alkyl phosphate used is preferably triisooctyl phosphate (tri-2-ethylhexyl phosphate). Mixtures of different monoalkyl phosphates, dialkyl phosphates and trialkyl phosphates can also be used. Triisooctyl phosphate is preferably used in an amount of 0.003% to 0.05% by weight, more preferably 0.005% to 0.04% by weight, and particularly preferably 0.01% to 0.03% by weight based on the entire composition.

[0155] Examples of impact modifiers are: core-shell polymers such as ABS or MBS; olefin-acrylate copolymers such as ABRADE from DuPont; Type or from Dow Type: Silicone acrylate rubber, such as from Mitsubishi Rayon Co., Ltd. The composition according to the invention already has an outstanding performance profile without further impact modifiers. The composition according to the invention is therefore preferably free of impact modifiers.

[0156] The composition of the invention does not contain any further fillers, such as barium sulfate, besides talc. Titanium dioxide is not considered a "filler" here, but an inorganic pigment according to component F.

[0157] If titanium dioxide is included, the composition of the invention preferably contains from 0.1 to 2 wt. %, preferably from 0.5 to 1.2 wt. % titanium dioxide.

[0158] The titanium dioxide in the composition of the present invention preferably has a median particle size D of 0.1 to 5 μm, preferably 0.2 μm to 0.5 μm, as determined by scanning electron microscopy (STEM). 50 However, the titanium dioxide may also have a different particle size, for example an average particle size D of ≥ 0.5 μm, for example 0.65 to 1.15 μm, as determined by scanning electron microscopy (STEM). 50 .

[0159] Titanium dioxide preferably has a rutile structure.

[0160] The titanium dioxide used according to the invention is a white pigment Ti(IV)O2. In addition to titanium, colored titanium dioxide also contains a large amount of elements such as Sb, Ni, Cr, etc., which produces a color impression other than "white". It is understood that titanium dioxide white pigments may also contain traces of other elements as impurities. However, these amounts are very small, so that the titanium dioxide does not exhibit any color tone.

[0161] Suitable titanium dioxide is preferably titanium dioxide produced by the chloride process, hydrophobized, particularly post-treated and suitable for polycarbonate. In principle, in the composition according to the invention, instead of sized titanium dioxide, unsized titanium dioxide or a mixture of the two can also be used. However, preference is given to using sized titanium dioxide.

[0162] Possible surface modifications of titanium dioxide include inorganic modifications and organic modifications. These include, for example, surface modifications based on aluminum or polysiloxanes. The inorganic coating may contain 0.0% to 5.0% by weight of silicon dioxide and / or aluminum oxide. Organic-based modifications may contain 0.0% to 3.0% by weight of hydrophobic wetting agents. Titanium dioxide preferably has an oil absorption value of 12 to 18 g / 100 g titanium dioxide, further preferably 13 to 17 g / 100 g titanium dioxide, particularly preferably 13.5 to 15.5 g / 100 g titanium dioxide, determined according to DIN EN ISO 787-5: 1995-10.

[0163] Particularly preferred is titanium dioxide having the standard designation R2 according to DIN EN ISO 591-1:2001-08, which is stabilized with aluminum compounds and / or silicon compounds and has a titanium dioxide content of at least 96.0% by weight. Such titanium dioxide is commercially available under the trade names Kronos 2233 and Kronos 2230.

[0164] The polymer composition of the present invention comprising mixed components A, B, C, D, E, optional F and optional other ingredients can be prepared using a powder premix. It is also possible to use a premix of a granular material or a granular material and a powder with an additive according to the present invention. It is also possible to use a premix made from a solution of the mixture components in a suitable solvent, wherein optionally homogenization is carried out in solution and then the solvent is removed. In particular, the additive called component F and other ingredients of the composition according to the present invention can be introduced by known methods or in the form of a masterbatch. The use of a masterbatch is particularly preferred for introducing additives and other ingredients, wherein a masterbatch based on a respective polymer matrix is ​​particularly used.

[0165] For example, the composition according to the invention can be extruded. After extrusion, the extrudate can be cooled and crushed. The combination and mixing of the premix in the melt can also be carried out in the plasticizing unit of an injection molding machine. In this case, the melt is directly converted into a molded article in a subsequent step.

[0166] The composition of the present invention is preferably used for the production of molded articles for EE field components, in particular high-voltage switches, inverters, relays, electronic connectors, electrical connectors, circuit breakers, photovoltaic application components, motors, radiators, electric vehicle chargers or charging plugs, electrical junction boxes, smart meter housings, miniature circuit breakers, busbars (busbars). Therefore, the subject of the present invention is also a molded article consisting of the composition of the present invention or containing a region made of the composition of the present invention, and a corresponding component comprising an element, i.e., a molded article consisting of the composition of the present invention or containing a region made of the composition of the present invention (which is referred to as "an element made of the thermoplastic composition of the present invention").

[0167] The molding consisting of the thermoplastic composition according to the invention or comprising a region made of the thermoplastic composition according to the invention or a layer made of the thermoplastic composition according to the invention is preferably used in those EE components which are designed for an operating voltage of at least 400 V, further preferably at least 450 V. However, it can also be designed for a typical European household operating voltage of 230 V ± 23 V, although smaller distances between the electrical conductors can now be achieved.

[0168] The high relative tracking index of the polycarbonate composition according to the invention makes it possible to achieve smaller distances between two electrical conductors of a component using polycarbonate materials than has been possible hitherto using polycarbonate.

[0169] The subject of the invention is therefore also an EE component comprising a first electrical conductor and a second electrical conductor having a first distance d1 and a second distance d2 from one another,

[0170] They are connected via an element made of the thermoplastic composition according to the invention which is in direct contact with the first and second electrical conductors,

[0171] wherein the distance d1 is the shortest distance between the first electrical conductor and the second electrical conductor along the surface of the element made of the thermoplastic composition, and

[0172] Wherein the distance d2 is the shortest distance through air between the first electrical conductor and the second electrical conductor,

[0173] where d2 is selected in such a way as to prevent arcing through air at the respective operating voltages, and

[0174] Wherein, at the operating voltage U listed below, d1 is:

[0175] d1i(0V≤U≤250V):1.8mm to <2.5mm

[0176] dlii(250V<U≤500V)=3.6mm to <5.0mm

[0177] dliii(500V<U≤1000V)=7.1mm to<10.0mm.

[0178] Such small distances can only be achieved using materials with a CTI of at least 400 V.

[0179] The subject matter of the invention is therefore also a corresponding EE component, in which a corresponding distance is achieved and preferably with an applied operating voltage of at least 400 V, preferably at least 450 V.

[0180] It is known that the degree of dirtiness affects the conductivity. The above distances d1 and d2 can be used in practice for components where, for example, due to structural shielding, IP6K9K protection class according to ISO 20653:2013-02 is met.

[0181] The selection of d2 is within the capabilities of those skilled in the art. Preferably, d2 is at least 1.2 mm.

[0182] The present invention also relates to the use of talc for increasing the comparative tracking index of bisphenol A homopolycarbonate. This targeted use also exists, for example, when the corresponding composition is used for insulating layers which require a CTI of 400 V due to the application. For example, the composition according to the invention can be used as an insulating layer for other electrical components, such as transistors. The electrical components of the transistors are protected by overmolding with a plastic having a high CTI. The plastic protects the electrical components from contact with adjacent metal components, such as metal heat sinks, or electrical components and avoids undesired electrical interactions therewith.

[0183] Transistors are also often mounted directly on heat sinks due to the large amount of heat generated during operation. Here, the thermoplastic composition of the present invention introduced between the heat sink and the transistor ensures safe operation.

[0184] Another area of ​​application is the mounting brackets for busbars, where materials with a high CTI must also be used. The mounting brackets essentially have two functions: to fix the busbars in the component group to prevent position changes during operation, and to act as a spacer to enable the parallel operation of multiple busbars, wherein here too a sufficiently large distance must be selected between two busbars to prevent air arcs. In addition, however, tracking on the surface of the mounting bracket must be prevented between the busbars and between the busbars and other metal components, such as screws for fixing the mounting bracket to the underlying structure. Mounting brackets with a high CTI can increase the component density and the energy density.

[0185] In the case of plugs, plug devices and sockets, there is a high risk of leakage currents forming, which can lead to electrical faults and possible fires. A housing that seals the current-carrying conductors can improve this situation because the level of dirt is low. Plugs for charging devices or USB-C plugs are at a higher risk because the current-carrying conductor strips cannot be covered or sealed and are additionally exposed to dirt such as sweat, moisture, fabric particles, dust and other materials. Materials with high CTI values ​​are needed to provide adequate protection against tracking, but also to enable miniaturization or increased power density.

[0186] A subject of the present invention is likewise the use of the composition according to the invention, also in the preferred, particularly preferred etc. described embodiments, for achieving the aforementioned small distances between electrical conductors in EE components.

[0187] Of course, features mentioned as preferred, particularly preferred etc. for the composition also apply to the use according to the invention.

[0188] According to the classification according to DIN EN 60664-1:2008, the thermoplastic compositions preferred according to the invention belong to the insulating material group II (400 V ≤ CTI < 600 V).

[0189] They have a thermal conductivity (in-plane), determined in accordance with ASTM E 1461-13, of preferably at least 1.0 W / (mK), preferably at least 1.1 W / (mK), and thus additionally allow good heat dissipation.

[0190] Various embodiments of the present invention are described as follows:

[0191] 1. A thermoplastic composition comprising

[0192] A) at least 50% by weight of bisphenol A homopolycarbonate,

[0193] B) 32 to 37% by weight of talc,

[0194] C) 4 to 10% by weight of a phosphorus-containing flame retardant,

[0195] D) 0.3 to 2% by weight of a fluorinated anti-drip agent,

[0196] E) 1 to 3% by weight of an anhydride-modified α-olefin polymer,

[0197] The composition does not contain any other fillers.

[0198] 2. The thermoplastic composition according to embodiment 1, wherein the talc content of the thermoplastic composition is 34 to 36% by weight.

[0199] 3. The thermoplastic composition according to embodiment 1 or 2, wherein the talc content of the thermoplastic composition is 34.5 to 35.5% by weight.

[0200] 4. The thermoplastic composition according to any of the preceding embodiments, wherein the amount of fluorine-containing anti-drip agent is 0.4 to 1.0 wt%.

[0201] 5. The thermoplastic composition according to any of the preceding embodiments, wherein the content of aromatic polycarbonate is at least 54 wt%.

[0202] 6. The thermoplastic composition according to any of the preceding embodiments, which does not comprise any other polycarbonate.

[0203] 7. The thermoplastic composition according to any of the preceding embodiments, wherein the phosphorus-containing flame retardant is a phosphazene or a mixture of different phosphazenes.

[0204] 8. The thermoplastic composition according to any one of the preceding embodiments, wherein the anhydride-modified α The α-olefin polymer includes a maleic anhydride-modified propylene polymer, and such a polymer is preferred.

[0205] 9. The thermoplastic composition according to any of the preceding embodiments, wherein the composition contains 0.1 to 2 wt. % titanium dioxide.

[0206] 10. The thermoplastic composition according to any of the preceding embodiments, comprising 5 to 8 wt% of a phosphorus-containing flame retardant.

[0207] 11. The thermoplastic composition according to any one of the preceding embodiments, comprising as a further component

[0208] F) one or more additives selected from heat stabilizers, antioxidants, mold release agents, ultraviolet absorbers, infrared absorbers, impact modifiers, antistatic agents, fluorescent brighteners, light scattering agents, hydrolysis stabilizers, transesterification stabilizers, organic dyes, organic or inorganic pigments, compatibilizers, laser marking additives.

[0209] 12. The thermoplastic composition according to any one of the preceding embodiments, wherein the composition is free of impact modifiers and blending partners.

[0210] 13. The thermoplastic composition according to any one of the preceding embodiments, comprising

[0211] A) at least 50% by weight of bisphenol A homopolycarbonate,

[0212] B) 34 to 36% by weight of talc,

[0213] C) 5 to 8% by weight of a phosphorus-containing flame retardant,

[0214] D) 0.3 to 1% by weight of a fluorinated anti-drip agent,

[0215] E) 1 to 2% by weight of an anhydride-modified α-olefin polymer.

[0216] 14. The thermoplastic composition according to any one of the preceding embodiments, further comprising

[0217] F) one or more additives selected from heat stabilizers, antioxidants, mold release agents, ultraviolet absorbers, infrared absorbers, antistatic agents, fluorescent brighteners, light scattering agents, hydrolysis stabilizers, transesterification stabilizers, organic dyes, organic or inorganic pigments, compatibilizers, laser marking additives.

[0218] 15. The thermoplastic composition according to any one of the preceding embodiments, which does not contain any other components besides the above components.

[0219] 16. A thermoplastic composition consisting of

[0220] A) at least 50% by weight of bisphenol A homopolycarbonate,

[0221] B) 34 to 36% by weight of talc,

[0222] C) 5 to 8% by weight of a phosphorus-containing flame retardant,

[0223] D) 0.3 to 1% by weight of a fluorinated anti-drip agent,

[0224] E) 1 to 2% by weight of an anhydride-modified α-olefin polymer,

[0225] F) 0.1 to 2% by weight of titanium dioxide,

[0226] G) one or more additives selected from heat stabilizers, antioxidants, mold release agents, ultraviolet absorbers, infrared absorbers, antistatic agents, fluorescent brighteners, light scattering agents, hydrolysis stabilizers, transesterification stabilizers, organic dyes, organic or inorganic pigments, compatibilizers, laser marking additives.

[0227] 17. The thermoplastic composition according to any one of the preceding embodiments, wherein the phosphorus-containing flame retardant comprises a cyclic phosphazene and / or a phosphorus compound of formula (10).

[0228] 18. The thermoplastic composition according to any one of the preceding embodiments, wherein the phosphorus-containing flame retardant is a cyclic phosphazene and / or a phosphorus compound of formula (10):

[0229]

[0230] in

[0231] R 1 , R 2 , R 3 and R 4 independently of one another are C1- to C8-alkyl, in each case optionally halogenated and in each case branched or unbranched, and / or C5- to C6-cycloalkyl, C6- to C8 ... 20 -aryl or C7- to C 12 -aralkyl,

[0232] n is independently 0 or 1,

[0233] q is a value from 0 to 30, and

[0234] X is a monocyclic or polycyclic aromatic radical having 6 to 30 carbon atoms or a straight-chain or branched aliphatic radical having 2 to 30 carbon atoms, which in each case may be substituted or unsubstituted, bridged or unbridged.

[0235] 19. The thermoplastic composition according to embodiment 17 or 18, wherein the cyclic phosphazene is a phosphazene of formula (13)

[0236]

[0237] in

[0238] R is the same or different in each case and is

[0239] - amine groups,

[0240] - in each case optionally halogenated, preferably by fluorine, further preferably monohalogenated C1- to C8-alkyl, preferably methyl, ethyl, propyl or butyl,

[0241] - C1- to C8-alkoxy, preferably methoxy, ethoxy, propoxy or butoxy,

[0242] - in each case optionally alkyl-substituted, preferably C1- to C4-alkyl-substituted, and / or halogen-substituted, preferably chlorine- and / or bromine-substituted, C5- to C6-cycloalkyl,

[0243] - in each case optionally alkyl-substituted, preferably C1- to C4-alkyl-substituted, and / or halogen-substituted, preferably chlorine-, bromine- and / or hydroxy-substituted C6- to C4- 20 - aryloxy, preferably phenoxy, naphthoxy,

[0244] - in each case optionally alkyl-substituted, preferably C1- to C4-alkyl-substituted, and / or halogen-substituted, preferably chlorine- and / or bromine-substituted, C7- to C4-12 - aralkyl, preferably phenyl-C1- to C4-alkyl, or

[0245] - a halogen group, preferably chlorine or fluorine, or

[0246] -OH group,

[0247] k is an integer from 1 to 10, preferably from 1 to 8, particularly preferably from 1 to 5, very particularly preferably 1.

[0248] 20. The thermoplastic composition according to embodiment 17, 18 or 19, wherein the phosphorus compound of formula (10) is a bisphenol A-based oligomeric phosphate of formula (12)

[0249]

[0250] Therein, q=1 to 20, in particular q=1.0 to 1.2.

[0251] 21. Thermoplastic composition according to any of the preceding embodiments, wherein the anhydride-modified α-olefin polymer according to component C is based on propylene, is maleic anhydride-modified, and preferably has an average molecular weight Mw determined by gel permeation chromatography in o-dichlorobenzene at 150° C. with polystyrene calibration of 1000 to 22000 g / mol, preferably 3000 to 21000 g / mol, and an acid number determined by potentiometric titration according to DIN ISO 17025:2005-08 of 45 to 170 mg KOH / g, preferably 50 to 100 mg KOH / g.

[0252] 22. The thermoplastic composition according to embodiment 21, wherein the aromatic bisphenol A homopolycarbonate used has an MVR of 11 to 15 cm2, measured according to ISO 1133:2012-03 at a test temperature of 300° C. and a load of 1.2 kg. 3 / (10min).

[0253] 23. A molded article consisting of or comprising a region made of the thermoplastic composition according to any one of the preceding embodiments.

[0254] 24. The molded article according to embodiment 23, wherein the molded article is part of a high voltage switch, an inverter, a relay, an electronic connector, an electrical connector, a circuit breaker, a photovoltaic device, a motor, a radiator, an electric vehicle charger or charging plug, an electrical junction box, a smart meter housing, a miniature circuit breaker, or a busbar.

[0255] 25. EE component designed for an operating voltage of at least 375 V, comprising a molding according to embodiment 23 or 24 or a layer made of a thermoplastic composition according to any one of embodiments 1 to 22.

[0256] 26. EE component designed for an operating voltage of 400 V, comprising the molding according to embodiment 23 or 24 or a layer made of the thermoplastic composition according to any one of embodiments 1 to 22.

[0257] 27.EE components, including

[0258] a first electrical conductor and a second electrical conductor having a first distance d1 and a second distance d2 from each other,

[0259] They are connected via an element made of the thermoplastic composition according to any one of embodiments 1 to 22, which is in direct contact with the first electrical conductor and the second electrical conductor,

[0260] wherein the distance d1 is the shortest distance between the first electrical conductor and the second electrical conductor along the surface of the element made of the thermoplastic composition, and

[0261] Wherein the distance d2 is the shortest distance through air between the first electrical conductor and the second electrical conductor,

[0262] where d2 is selected in such a way as to prevent arcing through air at the respective operating voltages, and

[0263] Wherein, at the operating voltage U listed below, d1 is:

[0264] d1i(0V≤U≤250V):1.8mm to <2.5mm

[0265] d1ii(250V<U≤500V)=3.6mm to <5.0mm

[0266] d1iii(500V<U≤1000V)=7.1mm to <10.0mm.

[0267] 28. The EE component according to any one of embodiments 25 to 27, wherein d2 ≥ 1.2 mm.

[0268] 29. The EE component according to any one of embodiments 25 to 28, wherein the EE component is a high voltage switch, an inverter, a relay, an electronic connector, an electrical connector, a circuit breaker, a part of a photovoltaic device, a part of an electric motor, a part of an electric vehicle charger or a charging plug, a part of an electrical junction box, a part of a smart meter housing, a part of a miniature circuit breaker, or a part of a busbar.

[0269] 30. The EE assembly of any one of embodiments 25 to 30, wherein the EE assembly has an IP6K9K protection rating according to ISO 20653:2013-02. Example:

[0270] 1. Raw material description and test methods

[0271] a) Raw materials

[0272] Component A-1: ​​Linear polycarbonate based on bisphenol A, melt volume flow rate of 12 cm 3 / (10 min) (according to ISO 1133: 2012-03, at a test temperature of 300° C. and a load of 1.2 kg), containing 250 ppm (=0.025% by weight, based on the total weight of component A) of triphenylphosphine heat stabilizer as component F-2.

[0273] Component B-1: compacted talc, talc content 98% by weight, iron oxide content 1.9% by weight, aluminum oxide content 0.2% by weight, loss on ignition (DIN 51081: 2002 / 1000° C.) 5.4% by weight, pH value (according to EN ISO 787-9: 1995) 9.15, D(0.5) (sedimentation analysis) 2.2 μm; BET surface area according to ISO 4652: 2012-06 10 m 2 / g, Model: Finntalc M05SLC, Manufacturer: Elementis Minerals BV

[0274] Component B*-2: Glass fiber from Nittobo Corporation (2-4-1, Kojimachi, Chiyoda-ku, Tokyo 102-8489, Japan) with the trade name CSG 3PA-830. This is a flat glass fiber with a cut length of 3 mm and a cross-sectional ratio of 1.4.

[0275] Component B*-3: fumed silica Amosil FW 600 from Quarzwerke GmbH, Frechen, unsized, average particle size D(0.5) of about 4 μm, D(0.98) of about 13 μm, D(0.1) / D(0.9) ratio of about 1.5 / 10, specific surface area of ​​about 6 m 2 / g, measured according to DIN-ISO 9277:2014-01.

[0276] Component C-1: Phenoxy cyclophosphazene Rabitle FP 110 from Fushimi Pharmaceutical Co., Ltd. of Japan, formula (13g), trimer ratio (k=1) is about 68 mol%.

[0277] Component D-1: SAN-encapsulated polytetrafluoroethylene ADS5000 (about 50 wt % PTFE (fluorinated anti-drip agent) and about 50 wt % SAN) from Chemical Innovation Co., Ltd. of Thailand.

[0278] Component E-1: Propylene-maleic anhydride polymer, average molecular weight (gel permeation chromatography in o-dichlorobenzene at 150°C, calibrated with polystyrene) M w =20700g / mil, M n =1460 g / mol, acid number 78 mg KOH / g, determined by potentiometric titration according to DIN ISO 17025:2005-08.

[0279] Component F-1: Titanium dioxide from Kronos, D 50 =210nm (scanning electron microscope, ECD method; 2230).

[0280] b) Test methods

[0281] Comparative tracking index (CTI):

[0282] To determine the comparative tracking index, the compositions described herein were tested according to the rapid test method based on IEC 60112: 2009. For this purpose, a 0.1% strength ammonium chloride test solution (395 ohm*cm resistance) was applied dropwise to the surface of a specimen measuring 60 mm x 40 mm x 4 mm at intervals of 30 seconds between two adjacent electrodes spaced 4 mm apart. A test voltage was applied between the electrodes, which was varied during the test. The first specimen was tested at a starting voltage of 300 V or 350 V. As long as no leakage current > 0.5 A occurred within 2 seconds or the sample did not burn, a total of up to 50 drops per voltage were applied (one drop every 30 seconds). After 50 drops, the voltage was increased by 50 V and a new specimen was tested at this higher voltage according to the above procedure. This process was continued until 600 V was reached or a leakage current or burning occurred. If one of the above effects had occurred before 50 drops, the voltage was reduced by 25 V and a new specimen was tested at this lower voltage. The voltage is reduced until the test is passed at 50 drops without leakage current or burning. Thus, this procedure is used to determine the maximum possible voltage until the composition can withstand 50 drops of the test solution without leakage current. Finally, four more samples, each with 50 drops, are tested at the maximum voltage determined for confirmation. This confirmed value is shown as the CTI in the examples. The value of 100 drops was not determined, so it is a "quick test method based on the standard".

[0283] PTI ("proof tracking index"):

[0284] The PTI test is based on IEC 60112:2009 with the following modifications. For this purpose, a 0.1% ammonium chloride test solution (395 ohm*cm resistance) is applied dropwise on the surface of a sample measuring 60mm x 40mm x 4mm between two adjacent electrodes 4mm apart, with a time interval of 30 seconds. Unlike the CTI test, in the PTI test a fixed test voltage is applied between the electrodes and a total of 5 samples are tested at each voltage. A maximum of 50 drops (one drop every 30 seconds) are applied to each sample, as long as no leakage current > 0.5A or sample burning occurs within 2 seconds.

[0285] Flame retardant:

[0286] The flame retardancy of the polycarbonate compositions was tested according to Underwriters Laboratory method UL 94V at a thickness of 2 mm.

[0287] Different fire protection classes are assigned depending on the behavior of the test specimens. This includes the time until the flame goes out, the resistance to dripping, or whether the material produces burning drippings. The classes determined hereafter are designated V0, V1 and V2 and are determined based on a total of five tested specimens.

[0288] V0: The specimen placed with its longitudinal axis at 180° (vertical) to the flame has an average afterflame time of not more than 10 seconds after the flame is removed, and does not produce any dripping plastic particles that could ignite the cotton wool located below the specimen. The total afterflame time of the five specimens is a maximum of 50 seconds, with two flame applications in each case.

[0289] V1: In contrast to V0, the average maximum afterflame time here was <30 s, with dripping particles and ignition of cotton wool also not permitted. The total afterflame time of the five specimens was <250 s, with two flame applications in each case.

[0290] V2: Unlike V0 and V1, dripping plastic particles that ignite cotton wool are formed in this level. The single afterflame time is <30s, the total afterflame time of 5 specimens is <250s, and the flame is applied twice in each case.

[0291] nb: If the afterflame time is exceeded, this test does not provide a flame retardancy classification.

[0292] FOT: Flame out time (afterburn time), expressed in seconds.

[0293] Heat deformation resistance:

[0294] The heat deformation resistance of the compositions was determined by means of the Vicat softening temperature (method B, test force 50 N, heating rate 50 K / h) on test specimens with dimensions of 80 mm×10 mm×4 mm in accordance with ISO 306:2014-3.

[0295] Thermal Conductivity:

[0296] According to ASTM E 1461 (Nano-flash method) for the size of 60x60x2mm 3 Thermal conductivity of injection molded specimens was measured. "In-plane" means measurement in the x and y directions, and "through-plane" means measurement in the z direction.

[0297] 2. Sample production

[0298] The compositions were prepared on a BUSS kneader. Material temperature, speed, throughput and torque must be adjusted according to procedures known to the person skilled in the art and adapted to the respective composition. The filler was metered in as a "split feed", where 10% of the total amount of filler was added via the main feed port and the remainder via a side extruder. Test specimens with dimensions of 60 mm x 40 mm x 4 mm were produced from the molding compound using a standard injection molding process at a material temperature of 280°C and a mold temperature of 80°C.

[0299] 3. Results

[0300] In the following table, "ng" means "not tested" and "nb" means "failed".

[0301]

[0302] Table 1 shows the trend of how the CTI improves with increasing amounts of talc (V-1-V-3). However, without the addition of flame retardant, the flammability increases with increasing amounts of talc (see afterflame time). Comparing Examples V-4, E-7 and V-11, each containing 5% by weight of flame retardant, here one can also see the trend of increasing CTI (325V-450V-500V) with increasing amounts of talc. Not more than 10% of flame retardant, preferably not more than 8% of flame retardant, should be used, so that the heat deformation resistance is not reduced too much, which would normally call into question the use of polycarbonate. When other reinforcing fillers are used, such as glass fibers or quartz, it is not possible to achieve a high comparative tracking index as with talc when combined with a flame retardant (FR) package (see V2 with V-9 and V-10).

Claims

1. A thermoplastic composition comprising A) at least 50% by weight of bisphenol A homopolycarbonate, B) 32 to 37% by weight of talc, C) 4 to 10% by weight of a phosphorus-containing flame retardant, D) 0.3 to 2% by weight of a fluorinated anti-drip agent, E) 1 to 3% by weight of an anhydride-modified α-olefin polymer, The composition does not contain any other fillers.

2. Thermoplastic composition according to claim 1, which does not contain any other polycarbonate.

3. The thermoplastic composition according to claim 1 or 2, comprising 5 to 8% by weight of a phosphorus-containing flame retardant.

4. The thermoplastic composition of any one of the preceding claims, wherein the anhydride-modified α-olefin polymer comprises a maleic anhydride-modified propylene polymer.

5. Thermoplastic composition according to any one of the preceding claims, comprising 34 to 36% by weight of talc.

6. Thermoplastic composition according to any of the preceding claims, which contains as further components F) one or more additives selected from heat stabilizers, antioxidants, mold release agents, UV absorbers, infrared absorbers, impact modifiers, antistatic agents, fluorescent brighteners, light scattering agents, hydrolysis stabilizers, transesterification stabilizers, organic dyes, organic or inorganic pigments, compatibilizers, laser marking additives.

7. Thermoplastic composition according to any one of the preceding claims, containing 0.1 to 2% by weight of titanium dioxide.

8. Thermoplastic composition according to any one of the preceding claims, comprising A) at least 50% by weight of bisphenol A homopolycarbonate, B) 34 to 36% by weight of talc, C) 5 to 8% by weight of a phosphorus-containing flame retardant, D) 0.3 to 1% by weight of a fluorinated anti-drip agent, E) 1 to 2% by weight of an anhydride-modified α-olefin polymer.

9. The thermoplastic composition according to claim 8, further comprising F) one or more additives selected from heat stabilizers, antioxidants, mold release agents, ultraviolet absorbers, infrared absorbers, antistatic agents, fluorescent brighteners, light scattering agents, hydrolysis stabilizers, transesterification stabilizers, organic dyes, organic or inorganic pigments, compatibilizers, laser marking additives, It contains 0.1 to 2% by weight of titanium dioxide.

10. Thermoplastic composition according to any one of the preceding claims, which does not contain any other components than those mentioned above.

11. A moulding consisting of a thermoplastic composition as claimed in any one of the preceding claims or comprising a region made of a thermoplastic composition as claimed in any one of the preceding claims.

12. The molded article according to claim 11, wherein the molded article is a part of a high voltage switch, an inverter, a relay, an electronic connector, an electrical connector, a circuit breaker, a photovoltaic device, a motor, a radiator, a charger or a charging plug for an electric vehicle, an electrical junction box, a housing of a smart meter, a miniature circuit breaker, a busbar, wherein the EE component preferably has an IP6K9K protection grade according to ISO20653:2013-02.

13. EE component comprising a molding according to claim 11 or 12 or a layer made from a thermoplastic composition according to any one of claims 1 to 10.

14. The EE assembly according to claim 13, comprising a first electrical conductor and a second electrical conductor having a first distance d1 and a second distance d2 between each other, They are connected via a thermoplastic composition according to any one of claims 1 to 10 which is in direct contact with the first electrical conductor and the second electrical conductor, wherein the distance d1 is the shortest distance between the first electrical conductor and the second electrical conductor along the surface of the thermoplastic composition, and Wherein the distance d2 is the shortest distance through air between the first electrical conductor and the second electrical conductor, where d2 is selected in such a way as to prevent arcing through air at the respective operating voltages, and in, At the operating voltage U listed below, d1 is: d1i (0V ≤ U ≤ 250V): 1.8 mm to < 2.5 mm d1i (250V < U ≤ 500V) = 3.6 mm to < 5.0 mm d1iii (500V < U ≤ 1000V) = 7.1 mm to < 10.0 mm.