Co-Cr-Pt-B ferromagnetic material sputtering target

By uniformly distributing B in the alloy phase in the sputtering target of Co-Cr-Pt-B system ferromagnetic material, the problems of low leakage flux density and unstable discharge are solved, and an efficient sputtering process is achieved.

CN118974307APending Publication Date: 2024-11-15TANAKA KIKINZOKU KOGYO KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380031871.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-14
Filing Date
2023-01-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing magnetron sputtering method, the leakage flux density of the sputtering target of the ferromagnetic material is low and the discharge is unstable, resulting in a decrease in the sputtering yield rate, and the uneven distribution of B leads to arc abnormalities, affecting the sputtering efficiency.

Method used

By distributing B in the Co-Cr-Pt-B-type ferromagnetic material sputtering target, B is distributed in the Co-Cr-Pt alloy phase and the Co or Co-Cr alloy phase to form a uniformly distributed alloy phase to avoid B aggregation. Increase leakage flux density and reduce discharge voltage.

Benefits of technology

High leakage flux density and stable discharge are achieved, which reduces the discharge voltage during sputtering, avoids arc abnormalities, and improves the sputtering yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974307A_ABST
    Figure CN118974307A_ABST
Patent Text Reader

Abstract

A Co-Cr-Pt-B ferromagnetic material sputtering target which is characterized by containing a Co-Cr-Pt-B alloy phase (A) that contains more than 0 at% and 30 at% or less of B and that B is distributed throughout without uneven distribution of B-aggregated phases, and an alloy phase (B) that is any one of a Co-B alloy, a Co-Cr-B alloy, or a Co-Pt-B alloy, the sputtering target contains more than 0 atom% and 20 atom% or less of B, B is distributed throughout the sputtering target without a non-uniform distribution of a B aggregate phase, the alloy phase (A) accounts for 50 vol% or more in the sputtering target, and the alloy phase (B) accounts for less than 50 vol% in the sputtering target.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a sputtering target used for forming a magnetic film of a magnetic recording medium, particularly a magnetic recording layer of a hard disk drive using a perpendicular magnetic recording method, and to a sputtering target capable of obtaining stable discharge at a lower voltage when sputtering is performed using a magnetron sputtering device. Background Art

[0002] In the field of magnetic recording represented by hard disk drives, a material system based on ferromagnetic metals Co, Fe or Ni is used as the material of the magnetic thin film responsible for recording. In particular, the magnetic recording layer of the existing hard disk drive uses a Co-Pt system, a Co-Cr-Pt system or a composition system in which non-magnetic inorganic substances are added.

[0003] In the production of the magnetic recording layer of the hard disk drive, sputtering, especially magnetron sputtering, is mainly used because of its high productivity. As a method for producing a target material that is indispensable when using the sputtering method, a melting method or a powder metallurgy method is generally used. Which method to use depends on the required target and film properties.

[0004] Sputtering is a method of forming a film by applying a negative voltage to a target material in an inert gas atmosphere so that the atoms constituting the target are deposited on a substrate. By applying a negative voltage, the inert gas is ionized, and the inert gas that becomes a cation is attracted to the target, and the atoms constituting the target are knocked out by collision. The atoms are attached to the surface of the substrate, and a film is formed on the substrate. Magnetron sputtering is a method in which a magnet is arranged on the back side of the target in the sputtering method, and the ionization of the plasma gas is promoted by the magnetic field generated on the target surface to improve the sputtering efficiency. In the field of magnetic recording represented by existing hard disk drives, the magnetron sputtering method is mostly used from the viewpoints of its film forming speed, target yield, and sputtering stability.

[0005] However, the target used in the formation of the magnetic recording layer is mainly a ferromagnetic material, which hinders the penetration of the magnetic flux emitted from the magnet disposed on the back. When the penetration of the magnetic flux is excessively hindered, the advantages of using the above-mentioned magnetron sputtering method disappear, resulting in a decrease in the target yield and instability of the sputtering discharge. Therefore, the target used in the magnetron sputtering method requires a leakage flux density as high as possible.

[0006] In order to increase the leakage flux density of the target, various methods have been proposed. For example, Japanese Patent Gazette No. 4673453 (JPB4673453) describes a ferromagnetic material sputtering target, which is characterized by having a metal matrix (A) and a spherical phase (B) with a major axis and minor axis difference of 0 to 50% and a diameter of 30 to 150 μm containing 90 mol% or more of Co in the metal matrix (A), and the ferromagnetic material sputtering target is composed of a metal with a Cr content of less than 20 mol% and a balance of Co, and a metal with a Cr content of less than 20 mol%, a Pt content of more than 5 mol% and less than 30 mol%, and a balance of Co. Specifically, it is described that in a 78Co-12Cr-5TiO 2 -5SiO 2 、65Co-13Cr-15Pt-5TiO 2 -2Cr 2 O 3 In the ferromagnetic material sputtering target with a composition of 85Co-15Cr, 70Co-15Cr-15Pt, the case with a structure including a spherical Co phase (B) has a higher average leakage flux than the case without a spherical Co phase (B).

[0007] Japanese Patent Gazette No. 4758522 (JPB4758522) describes a sputtering target, which is a ferromagnetic material sputtering target characterized by having a metal matrix (A) and a flat phase (B) containing 90% by weight or more of Co in the metal matrix (A), an average grain size of the phase (B) of 10 μm or more and 150 μm or less and an average aspect ratio of 1:2 to 1:10, a target with a composition of Cr of 20 mol% or less and Co as the main component, and a sputtering target with a composition of Cr of 20 mol% or less, Pt of 5 mol% or more and 30 mol% or less, and Co as the main component. Specifically, it is described that in a composition of 78.73Co-13.07Cr-8.2SiO 2 Among the ferromagnetic material sputtering targets having a composition of , the average leakage magnetic flux density of the sputtering target having a structure including a flat Co phase (B) is lower than the average leakage magnetic flux density of the sputtering target made using Co atomized powder (spherical), but higher than the conventional sputtering target (the details are unclear).

[0008] Japanese Patent Gazette No. 5394576 (JPB5394576) describes a sputtering target, which is a ferromagnetic material sputtering target characterized by a structure having a metal matrix (A), a Co-Pt alloy phase (B) containing 40 to 76 mol% of Pt in the metal matrix (A), and a Co alloy phase (C) containing 90 mol% or more of Co different from the Co-Pt alloy phase (B), wherein the sputtering target is composed of a metal having a composition of 20 mol% or less of Cr, 5 mol% or more of Pt, and the remainder being Co. Specifically, a sputtering target having 88(Co-5Cr-15Pt)-5CoO-7SiO 2 、59Co-6Cr-20Pt-5Ru-4TiO 2 -4SiO 2 -2Cr 2 O 3 Among the ferromagnetic material sputtering targets with a composition of , the average leakage magnetic flux density of the sputtering target having a Co-Pt alloy phase (B) with a grain size of 50 to 150 μm and containing 50 mol% of Pt and a structure with a grain size of 70 to 150 μm and containing a pure Co phase (C) is higher than the average leakage magnetic flux density of the sputtering target having a structure without a Co-Pt alloy phase (B) and a Co alloy phase (C) and the sputtering target having a Co-Pt alloy phase (B) with a grain size of 50 to 150 μm and containing 81 mol% of Pt and a structure with a grain size of 70 to 150 μm and containing a pure Co phase (C). It is recorded that in the case of containing 0.5 mol% or more and 10 mol% or less of B as an added element, B is present in the metal matrix (A), and sometimes diffuses slightly into the Co-Pt alloy phase (B) or the Co phase (C) via the interface between the Co-Pt alloy phase (B) and the metal matrix (A) or the interface between the Co phase (C) and the metal matrix (A). That is, B sometimes also exists near the interface between the Co-Pt alloy phase (B) or the Co phase (C) and the metal matrix (A), but is not distributed in the form of the entire Co-Pt alloy phase (B) or the Co phase (C).

[0009] The above-mentioned existing patent documents all disclose that the leakage flux density of the ferromagnetic material sputtering target can be improved by forming a structure of a Co alloy phase containing 90 mol% or more Co in a large spherical shape with a particle size of 10 μm to 150 μm in a metal matrix (A). Although it is recorded that B can be contained as an additive element, there is no embodiment containing B, and it is unclear whether the desired effect can be obtained in a Co-Cr-Pt-B sputtering target. In addition, there is neither disclosure nor suggestion on controlling the distribution state of B. Usually, B is aggregated and unevenly distributed, so those skilled in the art will not understand that the overall distribution of B is disclosed.

[0010] The density of the B aggregate phase in the metal matrix of the Co-Cr-Pt-B sputtering target without oxide increases, and microcracks are generated due to the brittleness of B. The generation of arcs starting from these microcracks becomes a problem. When discharge abnormality caused by arcs occurs, sputtering cannot be performed stably, and the yield rate is significantly reduced.

[0011] As a method for suppressing arcing of a Co-Cr-Pt-B sputtering target, Japanese Patent Publication No. 2015-61946 (JPA 2015-61946) describes adjusting the structure of an ingot made of a Co-Cr-Pt-B alloy by controlling a processing method including precision rolling or forging and heat treatment to form a fine and uniform rolled structure without microcracks. Figure 1 The SEM observation image of the structure of the sputtering target is shown in FIG. 1 , and it can be seen that the target is composed of two phases, the matrix phase and the B-rich phase, and the B-rich phase is in the shape of a cumulus cloud. Compared with the SEM observation image of the embodiment described later, it can be seen that in the sputtering target of the present invention, B is distributed in the entire alloy phase, while in the sputtering target of the present invention, B is distributed in the entire alloy phase. Figure 1 It is shown that B aggregates and is not evenly distributed in the B-rich phase.

[0012] Prior art literature

[0013] Patent Literature

[0014] Patent Document 1: Japanese Patent No. 4673453 (JPB4673453)

[0015] Patent Document 2: Japanese Patent No. 4758522 (JPB4758522)

[0016] Patent Document 3: Japanese Patent No. 5394576 (JPB5394576)

[0017] Patent Document 4: Japanese Patent Application Publication No. 2015-61946 (JPA 2015-61946) Summary of the invention

[0018] Problems to be solved by the invention

[0019] The object of the present invention is to provide a ferromagnetic material sputtering target that can obtain stable discharge without causing discharge abnormality by magnetron sputtering. The object of the present invention is to provide a Co-Cr-Pt-B system ferromagnetic material sputtering target that has a high leakage flux density and can reduce the discharge voltage during sputtering, and a method for producing the same.

[0020] Methods used to solve problems

[0021] The inventors discovered that in a Co-Cr-Pt-B based ferromagnetic sputtering target, by controlling the distribution of B in both the Co-Cr-Pt alloy phase and the Co or Co-Cr alloy phase so that there is no uneven distribution of the B aggregated phase, that is, by forming a structure comprising a Co-Cr-Pt-B alloy phase (A) and an alloy phase (B) of either Co-B alloy or Co-Cr-B alloy, the leakage magnetic flux density can be increased and the discharge voltage can be reduced, thereby completing the present invention.

[0022] According to the present invention, there are provided the following Co—Cr—Pt—B based ferromagnetic material sputtering target and a method for producing the same.

[0023] [1] A Co-Cr-Pt-B based ferromagnetic material sputtering target, comprising:

[0024] A Co-Cr-Pt-B alloy phase (A) containing more than 0 atomic % and less than 30 atomic % of B, B being distributed throughout without an inhomogeneous distribution of a B aggregate phase; and

[0025] The alloy phase (B) is any one of a Co-B alloy, a Co-Cr-B alloy or a Co-Pt-B alloy, containing more than 0 atomic % and less than 20 atomic % of B, and B is distributed throughout without uneven distribution of B aggregate phases,

[0026] The alloy phase (A) accounts for more than 50 volume % in the sputtering target, and the alloy phase (B) accounts for less than 50 volume % in the sputtering target.

[0027] [2] A Co-Cr-Pt-B based ferromagnetic material sputtering target according to the above [1], characterized in that Cr is greater than 0 atomic % and less than 30 atomic %, Pt is greater than 5 atomic % and less than 30 atomic %, B is greater than 0 atomic % and less than 25 atomic %, and the remainder is Co and unavoidable impurities.

[0028] [3] According to the Co-Cr-Pt-B based ferromagnetic material sputtering target described in [1] or [2] above, it is characterized in that the alloy phase (A) also contains more than 0 atomic % and less than 25 atomic % of one or more elements selected from Al, Si, Sc, Ti, V, Mn, Fe, Ni, Cu, Zn, Ge, Y, Zr, Nb, Ta, Mo, W, Ru, Ag, Sn, La, Ce, Pr, Nd, Sm, Gd, Tb, Dy, Ho, and Hf as additive elements.

[0029] [4] A production method, which is the production method of the Co—Cr—Pt—B based ferromagnetic material sputtering target according to any one of [1] to [3] above, characterized by comprising:

[0030] A mixing step, wherein a Co-Cr-Pt-B alloy powder containing more than 0 atomic % and less than 30 atomic % of B is weakly mixed with any one of a Co-B alloy powder containing more than 0 atomic % and less than 20 atomic % of B, a Co-Cr-B alloy powder, and a Co-Pt-B alloy powder to obtain a mixed powder; and

[0031] The sintering step is to sinter the mixed powder to obtain a sintered body.

[0032] [5] The manufacturing method according to the above [4] is characterized in that the Co-Cr-Pt-B alloy powder and the Co-B alloy powder, Co-Cr-B alloy powder or Co-Pt-B alloy powder are atomized alloy powders.

[0033] [6] The manufacturing method according to [4] or [5] above is characterized in that, in the sintering step, the mixed powder is maintained at a pressure of not less than 10 MPa and not more than 100 MPa and a temperature of not less than 700°C and not more than 1300°C for not less than 30 minutes and not more than 3 hours.

[0034] Effects of the Invention

[0035] The Co-Cr-Pt-B based ferromagnetic material sputtering target of the present invention comprises a Co-Cr-Pt-B alloy phase (A) and an alloy phase (B), wherein the Co-Cr-Pt-B alloy phase (A) comprises B greater than 0 atomic % and less than 30 atomic %, and B is distributed throughout the target, and the alloy phase (B) is any one of a Co-B alloy, a Co-Cr-B alloy or a Co-Pt-B alloy, comprises B greater than 0 atomic % and less than 20 atomic %, and B is distributed throughout the target. Since B is distributed throughout the target without uneven distribution of B aggregated phase, the discharge voltage during sputtering can be reduced, discharge anomalies such as arcing caused by excess voltage can be suppressed, and the leakage magnetic flux density is high.

[0036] According to the manufacturing method of the present invention, a Co-Cr-Pt-B based ferromagnetic material sputtering target with high leakage flux density and capable of reducing the discharge voltage during sputtering can be obtained, wherein the sputtering target comprises a Co-Cr-Pt-B alloy phase (A) and an alloy phase (B), wherein the Co-Cr-Pt-B alloy phase (A) contains B greater than 0 atomic % and less than 30 atomic % and B is distributed throughout the target, and the alloy phase (B) is any one of a Co-B alloy, a Co-Cr-B alloy or a Co-Pt-B alloy, contains B greater than 0 atomic % and less than 20 atomic % and B is distributed throughout the target, and B is distributed throughout the target without uneven distribution of B aggregated phases. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1It is a graph showing the relationship between the input power and the voltage value of Examples 1 to 3 and Comparative Examples 1 to 4.

[0038] Figure 2 This is the SEM observation image of Example 1.

[0039] Figure 3 This is the SEM observation image of Example 2.

[0040] Figure 4 This is the SEM observation image of Example 3.

[0041] Figure 5 This is a SEM observation image of Comparative Example 1.

[0042] Figure 6 This is a SEM observation image of Comparative Example 2.

[0043] Figure 7 This is a SEM observation image of Comparative Example 3.

[0044] Figure 8 This is the EPMA-WDX mapping image of Example 1.

[0045] Fig. 9 This is the EPMA-WDX mapping image of Example 2.

[0046] Fig.10 This is the EPMA-WDX mapping image of Example 3.

[0047] Fig.11 This is the EPMA-WDX mapping image of Comparative Example 1.

[0048] Fig.12 This is the EPMA-WDX mapping image of Comparative Example 2.

[0049] Fig.13 This is the EPMA-WDX mapping image of Comparative Example 3. DETAILED DESCRIPTION

[0050] The present invention provides a ferromagnetic material sputtering target which has high leakage magnetic flux density and can reduce the discharge voltage during sputtering.

[0051] The Co-Cr-Pt-B based ferromagnetic material sputtering target of the present invention is characterized in that it comprises a Co-Cr-Pt-B alloy phase (A) and an alloy phase (B), wherein the Co-Cr-Pt-B alloy phase (A) contains more than 0 atomic % and less than 30 atomic % of B, and B is distributed throughout without uneven distribution of B aggregated phases, and the alloy phase (B) is any one of Co-B alloy, Co-Cr-B alloy or Co-Pt-B alloy, contains more than 0 atomic % and less than 20 atomic % of B, and B is distributed throughout without uneven distribution of B aggregated phases, the alloy phase (A) accounts for more than 50 volume % in the sputtering target, and the alloy phase (B) accounts for less than 50 volume % in the sputtering target.

[0052] The alloy phase (A) in the Co-Cr-Pt-B system ferromagnetic material sputtering target of the present invention is more than the alloy phase (B), the alloy phase (A) accounts for 50 volume % or more, preferably 60 volume % or more, more preferably 65 volume % or more, and the alloy phase (B) is less than 50 volume %, preferably less than 40 volume %, more preferably less than 35 volume %. The Co-Cr-Pt-B system ferromagnetic material sputtering target of the present invention is composed of two phases, the alloy phase (A) and the alloy phase (B), and does not contain other phases such as oxide phases.

[0053] The alloy phase (A) contains greater than 0 atomic % and less than 30 atomic %, preferably greater than 3 atomic % and less than 26 atomic %, of B, and the phase (B) contains greater than 0 atomic % and less than 20 atomic %, preferably greater than 3 atomic % and less than 18.5 atomic % of B.

[0054] In the alloy phase (B), “B is distributed throughout” means that under the SEM observation surface at 1000 times magnification and with an acceleration voltage of 20 kV and an irradiation current of 8×10 -5 A. In the EPMA-WDX mapping image with an electron beam diameter of 10 μm and an observation magnification of 200 times, there is no site where B does not exist in any 10 μm×10 μm region.

[0055] In addition, it is preferred that B is distributed throughout the alloy phase (A). Here, “B is distributed throughout the alloy phase (A)” means that B is distributed throughout the alloy phase (A) when observed on a SEM at 1000 times magnification and at an acceleration voltage of 20 kV and an irradiation current of 8×10 -5 A. In the EPMA-WDX mapping image with an electron beam diameter of 10 μm and an observation magnification of 200 times, there is no site where B does not exist in any 10 μm×10 μm region.

[0056] The Co-Cr-Pt-B system ferromagnetic material sputtering target of the present invention preferably has a composition in which Cr is greater than 0 atomic % and less than 30 atomic %, Pt is greater than 5 atomic % and less than 30 atomic %, B is greater than 0 atomic % and less than 25 atomic %, and the balance is Co and inevitable impurities. It is particularly preferred to have a composition in which Cr is greater than 3 atomic % and less than 25 atomic %, Pt is greater than 10 atomic % and less than 25 atomic %, B is greater than 3 atomic % and less than 20 atomic %, and the balance is Co and inevitable impurities.

[0057] The alloy phase (A) may further contain more than 0 atomic % and less than 25 atomic %, preferably more than 1 atomic % and less than 15 atomic %, of one or more elements selected from Al, Si, Sc, Ti, V, Mn, Fe, Ni, Cu, Zn, Ge, Y, Zr, Nb, Te, Mo, W, Ru, Ag, Sn, La, Ce, Pr, Nd, Sm, Gd, Tb, Dy, Ho, and Hf as additional elements.

[0058] In the present invention, the average composition of the alloy phase (A) and the alloy phase (B) is determined by the following method. A cross section perpendicular to the sputtering target is cut out, and the cross section is ground in sequence using abrasive papers with particle sizes of P80 to P1200, and finally polished using diamond abrasives with a particle size of 1 μm, thereby obtaining a ground surface. The ground surface is observed using EPMA. Regarding the observation conditions of EPMA, JXA-8500F manufactured by JEOL is used as the device, the acceleration voltage is 20 kV, the irradiation current is 8×10 -5 A, electron beam diameter is 10μm, observation magnification is 200 times, number of pixels is 128×128, and element mapping images are obtained. During observation, the quantitative analysis mode is used, metal is selected as the measured substance, and the ZAF method is selected as the correction method. In the obtained element mapping image, if a phase in which Co, Cr, Pt, and B as the main components are all detected (corresponding to the alloy phase (A)) and a phase in which Cr or Pt is not detected or the concentration is extremely low compared with the Cr or Pt of the alloy phase (A) (corresponding to the alloy phase (B)) is confirmed, a portion of each phase is selected with a size that a perfect circle with a diameter of 50μm can be placed, and the composition at its center of gravity is measured. The above observations are performed on 3 locations of the alloy phase (A) and 3 locations of the alloy phase (B) in 3 fields of view, and the average values ​​are taken as the average compositions of the alloy phase (A) and the alloy phase (B), respectively.

[0059] In the present invention, the volume ratio of alloy phase (A) and alloy phase (B) is measured by the following method. First, by the above method, the mass concentration diagram of each element is obtained using EPMA. Using the obtained mass concentration diagram, the element (such as Cr or Pt in the case of Co-B, Pt in the case of Co-Cr-B) not detected in alloy phase (B) is analyzed horizontally from the end to the end of the image. During online analysis, in the phase corresponding to the alloy phase (A) and alloy phase (B), the position outside the boundary of alloy phase (A) and alloy phase (B), i.e., the line containing only the region of alloy phase (A) and only the region of alloy phase (B) is selected. The average value of the maximum and minimum values ​​of the contour diagram obtained by line analysis is used as a threshold value, and the image is binarized. Here, the range exceeding the threshold value is defined as alloy phase (A), and the range below the threshold value is defined as alloy phase (B). The obtained binary image is analyzed by the particle analysis of ImageJ to obtain the area ratio of alloy phase (A) and alloy phase (B). The above operation is performed for three viewing fields, and the average value is used as the area ratio of the sample. This area ratio directly corresponds to the volume ratio of each phase. As an element used in the line analysis of the mass concentration diagram, Pt is basically used, but when Pt is contained in all phases, Cr is used.

[0060] The Co-Cr-Pt-B based ferromagnetic material sputtering target of the present invention can be manufactured by powder metallurgy. The manufacturing method of the present invention comprises: a step of weakly mixing a Co-Cr-Pt-B alloy powder containing more than 0 atomic % and less than 30 atomic % of B, a Co-B alloy powder containing more than 0 atomic % and less than 20 atomic % of B, a Co-Cr-B alloy powder or a Co-Pt-B alloy powder to obtain a mixed powder, and a step of sintering the mixed powder to obtain a sintered body.

[0061] The Co—Cr—Pt—B alloy powder and Co—B alloy powder, Co—Cr—B alloy powder or Co—Pt—B alloy powder can use atomized alloy powder, powder produced by chemical method or other production method, and atomized alloy powder is preferred.

[0062] Weak mixing does not mean mixing by applying large mixing and stirring energy to crush each raw material powder, but means that the Co-Cr-Pt-B alloy powder constituting the alloy phase (A) and the Co-B alloy powder, Co-Cr-B alloy powder or Co-Pt-B alloy powder constituting the alloy phase (B) are not crushed, and each alloy powder is slowly mixed while being preserved. In the manufacturing method of the present invention, weak mixing is preferably carried out by mixing at a low rotation speed for a short time when a ball mill is used, for example, at a rotation speed of 30 rpm or more and 100 rpm or less for 10 minutes or more and 1 hour or less, and is particularly preferably carried out by using a vibrator or mixer without a stirring ball and only shaking up and down and left and right.

[0063] Sintering can be carried out in a vacuum atmosphere, at a sintering pressure of 10 MPa or more and 100 MPa or less, a sintering temperature of 700°C or more and 1300°C or less, a holding time of 30 minutes or more and 3 hours or less, preferably a sintering pressure of 20 MPa or more and 80 MPa or less, a sintering temperature of 800°C or more and 1100°C or less, and a holding time of 30 minutes or more and 2 hours or less. When the sintering pressure is too low, the density of the sintered body decreases. When the sintering temperature is too low, the density of the sintered body decreases. On the other hand, when the sintering temperature is too high, B aggregates excessively to form a coarse B aggregate phase as seen in the prior art, and B is not distributed throughout the target and is easily unevenly distributed. When the sintering holding time is too short, the density of the sintered body decreases. On the other hand, when the sintering holding time is too long, B aggregates excessively to form a coarse B aggregate phase as seen in the prior art, and B is not distributed throughout the target and is easily unevenly distributed. The decrease in density can cause particles to be generated from the target during sputtering discharge. On the other hand, the uneven distribution of the coarse B aggregate phase may lead to poor discharge represented by arcing.

[0064] Example

[0065] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited thereto.

[0066] In Examples 1 to 23, the atomized alloy powder of the raw material constituting the alloy phase (A) shown in Table 1 and the atomized alloy powder of the raw material constituting the second phase (representing alloy phase (B) in the embodiment. The same applies below) shown in Table 1 are weighed in such a manner that the second phase content shown in Table 1 and the remainder are the alloy phase (A) content, so as to form the target compositions shown in Table 1, and the mixture is mixed at 15 to 100 rpm for 15 minutes using a vibrator, and the obtained mixed powder is filled into a carbon mold, and sintered by vacuum hot pressing under vacuum atmosphere, pressure of 30 MPa, temperature of 800°C to 1100°C, and holding time of 1 hour. The sintering temperature varies depending on the target composition, but is set to a density of 97% or more for all samples. The obtained sintered body is cut and ground using a surface grinder and a lathe to produce a disk-shaped sputtering target with a diameter of 165 mm and a thickness of 6.4 mm.

[0067] The obtained disk-shaped sputtering target is mounted on a magnetron sputtering device, and while the argon gas is flowed at an argon pressure of 4.0 Pa, sputtering discharge is continuously performed at an arbitrary input power, and the sputtering discharge voltage is measured using a data recorder. The setting conditions of the data recorder are set to repeat the conditions of measuring 15,000 points of data at a sampling period of 2 μ seconds 100 times. The average value of the data measured each time is calculated, and the average value is taken as the average value of 100 times, thereby calculating the sputtering discharge voltage value under the measurement conditions. The results are shown in Table 1.

[0068] [Table 1]

[0069]

[0070] In Comparative Examples 1, 5, 7, 9, 11, and 13, sputtering targets were produced in the same manner as in the examples, except that the alloy atomized powder was not mixed but each metal powder was mixed to prepare a mixed powder.

[0071] Comparative Examples 2 and 3 were prepared in the same manner as in Example, except that atomized alloy powders not containing B were used as raw material powders constituting the second phase.

[0072] Comparative Examples 4, 6, 8, 10, 12, and 14 were prepared in the same manner as in the examples, except that Co metal powder was used as the raw material powder constituting the second phase.

[0073] For the sputtering targets of Examples 1 to 3 and Comparative Examples 1 to 4 having the same composition of Co-15Cr-10Pt-10B, the sputtering discharge voltage was measured while the input power was changed from 100 W to 1000 W by 100 W. The obtained results are shown in Tables 2 and Figure 1 middle.

[0074] [Table 2]

[0075]

[0076] The measured values ​​of PTF (leakage magnetic flux density) are also recorded in Table 2. The measurement of PTF is performed based on ASTM F2086-01. It can be confirmed that the PTF of the sputtering targets of Examples 1 and 2 is higher than the PTF of the sputtering targets of Comparative Examples 1 and 2, and is equivalent to the PTF of the sputtering target of Comparative Example 3. The PTF of the sputtering target of Example 3 is higher than the PTF of any of the sputtering targets of Comparative Examples 1 to 4, and the leakage magnetic flux density can also be improved.

[0077] Depend on Figure 1 It can be seen that when arranged in order from high to low in terms of sputtering discharge voltage, the examples are Comparative Example 4 using Co metal powder as the second phase, Comparative Example 1 using various metal powders instead of alloy atomized powder, and Comparative Examples 3 and 2 using atomized alloy powders without B as the second phase. The sputtering discharge voltages of Examples 1 to 3 in which B is distributed as a whole in the alloy phase (A) and the alloy phase (B) are significantly lower than those of Comparative Examples 1 to 4. In particular, when the input power increases to more than 300 W, the reduction in the sputtering discharge voltage increases. In addition, as can be seen from Table 1, when the sputtering discharge voltage at an input power of 500 W is compared, the embodiment is a low value of less than 330 V, and the comparative example is a high value of more than 330 V.

[0078] The SEM observation images (15.0 V×1,000) of the sputtering targets of Examples 1 to 3 and Comparative Examples 1 to 3 are shown in FIG. Figures 2 to 7 EPMA-WDX mapping images (15.0 V × 2000) of the sputtering targets of Examples 1 to 3 and Comparative Examples 1 to 3 are shown in FIG. Figures 8 to 13 middle.

[0079] Depend on Figure 8 From the EPMA-WDX mapping image, it can be seen that the white area at the bottom of the CP image of the sputtering target of Example 1 is the Co-Cr-Pt-B alloy phase (A) containing Co, Cr, Pt and B, and the gray area at the top of the CP image is the Co-Pt-B alloy phase (B) containing Co, Pt and B. Figure 2 and Figure 8 It can be seen that the sputtering target of Example 1 is composed of a Co-Cr-Pt-B alloy phase (A) and a Co-Pt-B alloy phase (B). In both alloy phases (A) and (B), there is no portion where B does not exist in any 10μm×10μm area, B is distributed in the entire alloy phase (A) and alloy phase (B), and the B in the alloy phase (A) is finely and evenly distributed in the entirety. Although the B in the alloy phase (B) is aggregated compared to the B in the alloy phase (A), it is distributed in the entirety of the alloy phase (B).

[0080] Depend on Fig. 9 From the EPMA-WDX mapping image, it can be seen that the white area on the right side of the CP image of the sputtering target of Example 2 is the Co-Cr-Pt-B alloy phase (A) containing Co, Cr, Pt and B, and the gray area on the left side of the CP image is the Co-Cr-B alloy phase (B) containing Co, Cr and B. Figure 3 and Fig. 9 It can be seen that the sputtering target of Example 2 is composed of a Co-Cr-Pt-B alloy phase (A) and a Co-Cr-B alloy phase (B). In both alloy phases (A) and (B), there is no portion where B does not exist in any 10μm×10μm area, B is distributed in the entire alloy phase (A) and alloy phase (B), and the B in the alloy phase (A) is finely and evenly distributed in the entirety. Although the B in the alloy phase (B) is aggregated compared to the B in the alloy phase (A), it is distributed in the entire alloy phase (B).

[0081] Depend on Fig.10 From the EPMA-WDX mapping image, it can be seen that the white area above the CP image of the sputtering target of Example 3 is the Co-Cr-Pt-B alloy phase (A) containing Co, Cr, Pt and B, and the gray area below the CP image is the Co-B alloy phase (B) containing Co and B. Figure 4 and Fig.10 It can be seen that the sputtering target of Example 3 is composed of a Co-Cr-Pt-B alloy phase (A) and a Co-B alloy phase (B). In both alloy phases (A) and (B), there is no portion where B does not exist in any 10μm×10μm area, B is distributed in the entire alloy phase (A) and alloy phase (B), and the B in the alloy phase (A) is distributed in the entirety. Although the B in the alloy phase (B) is aggregated compared to the B in the alloy phase (A), it is distributed in the entire alloy phase (B).

[0082] Depend on Figure 5 and Fig.11 It is understood that the sputtering target of Comparative Example 1 is a single phase in which Co, Cr, Pt, and B are dispersed throughout the entirety, and does not have an alloy phase (B).

[0083] Depend on Fig.12 From the EPMA-WDX mapping image, it can be seen that the gray area on the right side of the CP image of the sputtering target of Comparative Example 2 is a Co-Pt phase containing Co and Pt but not B, and the area with black spots on the left side of the CP image is a Co-Cr-Pt-B phase (A) containing Co, Cr, Pt, and B. Figure 6 and Fig.12It is found that the sputtering target of Comparative Example 2 is composed of a Co—Cr—Pt—B phase (A) and a Co—Pt phase (second phase), B is not present in the Co—Pt phase, and does not have an alloy phase (B) containing B.

[0084] Depend on Fig.13 From the EPMA-WDX mapping image, it can be seen that the white area in the lower right corner of the CP image of the sputtering target of Comparative Example 3 is the Co-Cr-Pt-B phase (A) containing Co, Cr, Pt and B, and the gray area in the upper left corner of the CP image is the Co-Pt phase containing Co and a trace amount of Pt. The large black area in the gray area is the coarse B aggregate phase unevenly distributed around Co. Figure 7 and Fig.13 It can be seen that the sputtering target of Comparative Example 3 is composed of Co-Cr-Pt-B phase (A) and Co-Pt phase (second phase), B is unevenly distributed around the Co-Pt phase, and there is a 10μm×10μm area in the second phase where B does not exist, and there is no alloy phase (B) in which B is distributed as a whole.

Claims

1. A Co-Cr-Pt-B based ferromagnetic material sputtering target, characterized in that: Include: A Co-Cr-Pt-B alloy phase (A) containing more than 0 atomic % and less than 30 atomic % of B, B being distributed throughout without an inhomogeneous distribution of a B aggregate phase; and The alloy phase (B) is any one of a Co-B alloy, a Co-Cr-B alloy or a Co-Pt-B alloy, containing more than 0 atomic % and less than 20 atomic % of B, and B is distributed throughout without uneven distribution of B aggregate phases, The alloy phase (A) accounts for more than 50 volume % in the sputtering target, and the alloy phase (B) accounts for less than 50 volume % in the sputtering target.

2. The Co-Cr-Pt-B based ferromagnetic material sputtering target according to claim 1, characterized in that: Cr is greater than 0 atomic % and less than 30 atomic %, Pt is greater than 5 atomic % and less than 30 atomic %, B is greater than 0 atomic % and less than 25 atomic %, and the balance is Co and unavoidable impurities.

3. The Co-Cr-Pt-B based ferromagnetic material sputtering target according to claim 1 or 2, characterized in that: The alloy phase (A) also contains more than 0 atomic % and less than 25 atomic % of one or more elements selected from Al, Si, Sc, Ti, V, Mn, Fe, Ni, Cu, Zn, Ge, Y, Zr, Nb, Ta, Mo, W, Ru, Ag, Sn, La, Ce, Pr, Nd, Sm, Gd, Tb, Dy, Ho, and Hf as additional elements.

4. A method for producing a Co-Cr-Pt-B based ferromagnetic material sputtering target according to any one of claims 1 to 3, characterized in that: include: A mixing step, wherein a Co-Cr-Pt-B alloy powder containing more than 0 atomic % and less than 30 atomic % of B is weakly mixed with any one of a Co-B alloy powder containing more than 0 atomic % and less than 20 atomic % of B, a Co-Cr-B alloy powder, and a Co-Pt-B alloy powder to obtain a mixed powder; and The sintering step is to sinter the mixed powder to obtain a sintered body.

5. The manufacturing method according to claim 4, characterized in that: The Co—Cr—Pt—B alloy powder and the Co—B alloy powder, Co—Cr—B alloy powder or Co—Pt—B alloy powder are atomized alloy powders.

6. The manufacturing method according to claim 4 or 5, characterized in that: In the sintering step, the mixed powder is maintained at a pressure of 10 MPa to 100 MPa and a temperature of 700° C. to 1300° C. for 30 minutes to 3 hours.

Citation Information

Patent Citations

  • Production of vinyl chloride tile

    JP1978094576A

  • Co-Cr-Pt-B BASE ALLOY SPUTTERING TARGET AND MANUFACTURING METHOD THEREOF

    JP2015061946A

  • Ferromagnetic material sputtering target

    JP4673453B1

  • Ferromagnetic sputtering target with low particle generation