Polyurethane elastic fiber

By controlling the content of metal soaps, surfactants, antioxidants, tertiary amine compounds, and cross-linking structure modifiers in polyurethane elastic fibers, the problem of property deterioration during recycling is solved, maintaining the excellent performance of the fibers, making them suitable for frequently washed clothing such as underwear.

CN118974333APending Publication Date: 2024-11-15东丽奥培隆特士股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094165.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2022-05-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the recycling process of polyurethane elastic fibers, the properties deteriorate due to the accumulation and decomposition products of substances such as metal soaps, surfactants, antioxidants, tertiary amine compounds and crosslinking structure modifiers, especially during high-frequency recycling.

Method used

By controlling the content of metal soaps, surfactants, antioxidants, tertiary amine compounds, and crosslinking modifiers in polyurethane elastic fibers within specific ranges, and by selecting appropriate recycling methods, the deterioration of properties can be suppressed.

Benefits of technology

It effectively inhibits the deterioration of the properties of polyurethane elastic fibers during the recycling process, maintaining the excellent properties of the fibers, such as unwinding tension, elongation at break, and strength, making it suitable for frequently washed clothing such as underwear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059010430000091
    Figure BDA0005059010430000091
  • Figure BDA0005059010430000161
    Figure BDA0005059010430000161
  • Figure BDA0005059010430000171
    Figure BDA0005059010430000171
Patent Text Reader

Abstract

[Problem] To provide a polyurethane elastic fiber which contains recovered polyurethane and which can suppress deterioration of certain characteristics due to recovery. [Solution] Provided is a polyurethane elastic fiber which uses, as at least one raw material, a recycled polyurethane elastic fiber in which the amount of metallic soap in the polyurethane elastic fiber is 0.003 mass% or more and 3.0 mass% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyurethane elastic fiber, and more particularly, to a polyurethane elastic fiber using recycled polyurethane elastic fibers as at least one raw material. Background Art

[0002] In recent years, contributions to the Sustainable Development Goals (SDGs) have been pursued, and the use of recycled resources is the most significant challenge facing all industrial products. For example, there is a technology for polyurethane elastic fibers in which fiber waste generated in the manufacturing process and necessary fibers from used products are collected and recycled, and there is an older technology of melting and recycling fiber waste dating back several years, as disclosed in Patent Documents 1 and 2. Another technology has been discovered in recent years, as disclosed in Patent Documents 3 and 4, in which cascade-type recycled fibers are produced by decomposing a polyurethane raw material and then dissolving the polyurethane raw material using a solvent.

[0003] However, in horizontally recycling the polyurethane elastic fiber into the polyurethane elastic fiber, problems unique to the polyurethane elastic fiber may occur. Here, the properties of the produced polyurethane elastic fiber may deteriorate due to substances accumulated and reduced during recycling. This problem is particularly significant when the polyurethane elastic fiber is repeatedly recycled and both the amount of recycled polyurethane and the number of recycling times are high.

[0004] [Citation List]

[0005] [Patent Document]

[0006] [Document Name 1] JP S56-122836A

[0007] [Document Name 2] JP S57-042657A

[0008] [File Name 3] CN 101096781 A

[0009] [Document Name 4] JP 2002-538314 A Summary of the invention

[0010] [Technical issues]

[0011] An object of the present invention is to provide a polyurethane elastic fiber containing recycled polyurethane, which can suppress the deterioration of certain characteristics due to recycling.

[0012] [Solution to the problem]

[0013] As mentioned above, the polyurethane elastic fiber containing recycled polyurethane will deteriorate due to the accumulation and reduction of materials during recovery. The main factor for the accumulation of certain materials is the finely divided metal soap present in the polyurethane elastic fiber oil. Typical examples of metal soaps are magnesium stearate and calcium stearate. The oil agent inhibits the adhesion phenomenon that occurs in the wound polyurethane elastic fiber, and can reduce the friction that occurs during the fiber unwinding and the friction that occurs between the fiber and the guide, roller and knitting needle during the weaving process. However, these oil agents also have an adverse effect on the shape of the wound polyurethane elastic fiber. This effect is more significant when the oil agent is added to the fiber than when applied to the outside, and the unwinding tension per unit mass may have a difference of ten times or more. When the oil agent is added to the fiber, the metal soap is dissolved or melted, thereby uniformly coating the fiber surface in the form of a molecular film. This significantly reduces the unwinding tension, but changes the shape of the wound fiber. The so-called bobbin collapse can cause the characteristics to deteriorate, which can reduce the upper limit of the amount that can be wound.

[0014] The second type of adversely affecting deposited materials is decomposition products. Examples of decomposition products include decomposition products of hindered phenols contained in antioxidants and decomposition products of tertiary amine compounds used in dyes. Other examples of adversely affecting deposited materials include cross-linked structure modifiers unique to polyurethane urea. The deterioration of properties caused by these decomposition products includes fading, color changes over time, and deterioration of mechanical properties. The deterioration of properties is particularly significant when the polyurethane elastic fiber is repeatedly recycled and the amount of recycled polyurethane is high.

[0015] The inventors have found that these problems can be solved in polyurethane elastic fibers containing recycled polyurethane that experience deterioration of these properties by keeping the amount of metal soap in the oil agent and the amount of specific substances such as surfactants, amines, acids and catalysts within a specific range (which enables suppression of deterioration of properties) and by selecting raw materials to be recovered with respect to decomposition products using a specific method. The inventors have also found that polyurethane elastic fibers containing recycled polyurethane with improved properties that also enable horizontal recycling of polyurethane elastic fibers can be obtained.

[0016] The present invention has the following configuration.

[0017] (1) A polyurethane elastic fiber using recycled polyurethane elastic fibers as at least one raw material, wherein the amount of metal soap in the polyurethane elastic fiber is 0.003% by mass or more and 3.0% by mass or less.

[0018] (2) The polyurethane elastic fiber according to (1), wherein the polyurethane elastic fiber contains 0.003% by mass or more and 3.0% by mass or less of a surfactant.

[0019] (3) The polyurethane elastic fiber according to (1) or (2), wherein the polyurethane elastic fiber contains 0.002% by mass or more and 5.0% by mass or less of an antioxidant.

[0020] (4) The polyurethane elastic fiber according to any one of (1) to (3), wherein the polyurethane elastic fiber contains 0.2% by mass or more and 5.0% by mass or less of a tertiary amine compound.

[0021] (5) The polyurethane elastic fiber according to any one of (1) to (4), wherein the polyurethane elastic fiber contains 0.002% by mass or more and 2.0% by mass or less of a cross-linking structure modifier.

[0022] (6) The polyurethane elastic fiber according to any one of (1) to (5), wherein the polyurethane elastic fiber contains 0.02% by mass or more and 1.0% by mass or less of a metal soap.

[0023] (7) The polyurethane elastic fiber according to any one of (1) to (6), wherein the number average molecular weight of the recovered polyurethane elastic fiber based on gel permeation chromatography (GPC) is 20,000 or more and 120,000 or less, and there is no peak or shoulder in the detected intensity curve for the region where the molecular weight based on GPC is 30,000 or less.

[0024] (8) The polyurethane elastic fiber according to any one of (1) to (7), wherein the AvC of the recycled polyurethane elastic fiber is 0.1730 cm-1 based on infrared spectroscopy (IR). -1 / AvC=O 1710cm -1 The ratio is 1.05 or more and 1.50 or less.

[0025] (9) The polyurethane elastic fiber according to any one of (1) to (8), wherein the recycled polyurethane elastic fiber is used for clothing that is frequently washed.

[0026] (10) The polyurethane elastic fiber according to (9), wherein the recycled polyurethane elastic fiber is used in underwear.

[0027] [Effects of the invention]

[0028] The present invention can provide a polyurethane elastic fiber whose property degradation is sufficiently suppressed although the polyurethane elastic fiber is a polyurethane elastic fiber containing recycled polyurethane. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] [ Figure 1 ]

[0030] Figure 1 : is a configuration diagram of an unwinding tension measuring device for realizing the unwinding tension measuring method in Examples and Comparative Examples.

[0031] [ Figure 2 ]

[0032] Figure 2 is a graph showing the GPC measurement of Example 21.

[0033] [ Figure 3 ]

[0034] Figure 3 is a graph showing IR spectrum measurement of Example 21. DETAILED DESCRIPTION

[0035] The present invention will now be described in detail with reference to Examples. First, the polyurethane used as the main component of the polyurethane elastic fiber of the present invention will be described. Here, the main component of the polyurethane elastic fiber is a compound used in an amount exceeding 50% by mass.

[0036] Any polyurethane can be used in the present invention, as long as the polyurethane has a structure using a polymer diol and a diisocyanate as starting materials. There is no particular restriction. In addition, there is no particular restriction on the synthesis method used. For example, the polyurethane can be a polyurethane urea composed of a polymer diol, a diisocyanate and a low molecular weight diamine used as a chain extender, or it can be a polyurethane urethane composed of a polymer diol, a diisocyanate and a low molecular weight diol used as a chain extender. Polyurethane urea having a compound having a hydroxyl group and an amino group in the molecule as a chain extender can also be used. Polyfunctional glycols and isocyanates having at least three functional groups can also be used, as long as they do not impair the effects of the present invention. There is no particular restriction on the treatment method for obtaining these compounds. For example, polyurethanes obtained by recycling and re-spinning fibers can also be used.

[0037] The polymer diol is preferably a polyether-based diol, a polyester-based diol or a polycarbonate diol. However, from the viewpoint of imparting flexibility and elasticity to the fiber, the use of a polyether-based diol is preferred.

[0038] Preferred examples of the polyether-based diols that can be used include polyethylene oxide, polyethylene glycol, polyethylene glycol derivatives, polypropylene glycol, polytetramethylene ether glycol (PTMG), modified PTMG as a copolymer of tetrahydrofuran (THF) and 3-methyltetrahydrofuran, modified PTMG as a copolymer of THF and 2-methyltetrahydrofuran, modified PTMG as a copolymer of THF and 2,3-dimethylTHF, polyols having side chains at both ends as disclosed (for example, in JP 2615131 B2), and random copolymers having irregular arrangements of THF and ethylene oxide and / or propylene oxide. These polyether-based diols can be used alone, or can be used as a mixture or copolymer of two or more.

[0039] From the viewpoint of abrasion resistance and light fastness, preferred examples of the polyurethane elastic fiber that can be used include butylene adipate, polycaprolactone diol, polyester-based diols (such as polyester polyols having side chains) as disclosed in JP S61-026612A, and polycarbonate diols as disclosed in JP H02-289516A.

[0040] These polymer diols may be used alone, or may be used as a mixture or a copolymer of two or more.

[0041] From the viewpoint of elasticity, strength and heat resistance of the resulting elastic fiber, the molecular weight of the polymer diol is preferably 1,000 or more and 8,000 or less, and more preferably 1,500 or more and 6,000 or less. By using a polyol having a molecular weight within this range, an elastic fiber having excellent elasticity, strength, elastic recovery and heat resistance can be easily obtained.

[0042] Aromatic diisocyanates such as diphenylmethane diisocyanate (MDI), toluene diisocyanate, 1,4-diisocyanate benzene, xylene diisocyanate or 2,6-naphthalene diisocyanate are particularly suitable for synthesizing polyurethanes with high heat resistance and strength as diisocyanates. Preferred examples of alicyclic diisocyanates include methylene bis (cyclohexyl isocyanate), isophorone diisocyanate, methylcyclohexane 2,4-diisocyanate, methylcyclohexane 2,6-diisocyanate, cyclohexane 1,4-diisocyanate, hexahydroxylene diisocyanate, hexahydrotoluene diisocyanate and octahydro-1,5-naphthalene diisocyanate. Alicyclic diisocyanates are particularly effective in inhibiting yellowing of polyurethane elastic fibers. These diisocyanates can be used alone or in combination of two or more.

[0043] The chain extender used for synthesizing polyurethane is preferably at least one type of low molecular weight diamine and low molecular weight diol. It should be noted that the compound may have both a hydroxyl group and an amino group in one molecule such as ethanolamine.

[0044] Preferred examples of low molecular weight diamines include ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, hexamethylenediamine, p-phenylenediamine, p-phenylenediamine, m-phenylenediamine, p,p'-methylenedianiline, 1,3-cyclohexanediamine, hexahydromethylphenylenediamine, 2-methylpentamethylenediamine and bis(4-aminophenyl)phosphine oxide. These low molecular weight diamines can be used alone or in combination of two or more. Ethylenediamine is particularly preferred. The use of ethylenediamine makes it possible to easily obtain yarns having excellent elasticity, elastic recovery and heat resistance. A triamine compound (such as diethylenetriamine) capable of forming a cross-linked structure can be added to the chain extender as long as it does not impair the effects of the present invention.

[0045] Representative examples of low molecular weight diols include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, bishydroxyethoxybenzene, bishydroxyethylene terephthalate and l-methyl-l,2-ethylene glycol. These low molecular weight diols can be used alone or in combination of two or more. Ethylene glycol, 1,3-propylene glycol and 1,4-butanediol are particularly preferred. When these materials are used, fibers with higher heat resistance and higher strength for diol-extended polyurethanes can be obtained.

[0046] In terms of number average molecular weight, the molecular weight of the polyurethane in the present invention is preferably in the range of 30,000 or more and 150,000 or less from the viewpoint of obtaining a polyurethane elastic fiber having high durability and strength. In terms of polystyrene, the molecular weight is measured by GPC.

[0047] Preferably, one or more blocking agents are used for the polyurethane. Preferred examples of blocking agents include: monoamines such as dimethylamine, diisopropylamine, ethylmethylamine, diethylamine, methylpropylamine, isopropylmethylamine, diisopropylamine, butylmethylamine, isobutylmethylamine, isopentylmethylamine, dibutylamine and dipentylamine; monoalcohols such as ethanol, propanol, butanol, isopropanol, allyl alcohol and cyclopentanol; and monoisocyanates such as phenyl isocyanate.

[0048] In the present invention, the polyurethane elastic fiber made of the polyurethane having the above basic configuration is constituted as a polyurethane elastic fiber using recycled polyurethane elastic fiber as at least one raw material. Here, the recycled polyurethane elastic fiber is a polyurethane elastic fiber that was manufactured as a polyurethane elastic fiber at least once before becoming a product and then recycled. It can be recycled in the form of waste fiber, in the form of fabric, or in the form of a repeatedly recycled product. There is no particular limitation on the recovery method, and the recycled polyurethane elastic fiber can be recycled by any means.

[0049] The first characteristic of the polyurethane elastic fiber using the recycled polyurethane elastic fiber as at least one raw material in the present invention is to maintain the metal soap content in the range of 0.003 mass % or more and 3.0 mass % or less. When the metal soap content is 0.003 mass % or less, the polyurethane elastic fiber will not unwind. When the content is greater than 3.0 mass %, the tension is unstable when the polyurethane elastic fiber is unwound, and the polyurethane elastic fiber will not unwind. By maintaining the metal soap content in the range of 0.003 mass % or more and 3.0 mass % or less, the preferred practical properties of the polyurethane elastic fiber, such as the preferred winding fiber shape, unwinding tension, and elongation and strength at break, are ensured. The metal soap content of the polyurethane elastic fiber of the present invention is preferably 0.03 mass % or more and 2.5 mass % or less, and more preferably 0.3 mass % or more and 2.0 mass % or less.

[0050] In order to maintain the metal soap content within the desired range mentioned above (0.003 mass % or more and 3.0 mass % or less), the metal soap content of the recycled polyurethane elastic fiber used as the raw material can be determined, and the mixing ratio of the recycled polyurethane elastic fiber to the original polyurethane raw material can be adjusted to a ratio that can obtain the desired metal soap content.

[0051] The metal soap content of the recycled polyurethane elastic fiber used as a raw material is preferably in the range of 0.02 mass% or more and 1.0 mass% or less. When the metal soap content of the recycled polyurethane elastic fiber is within this range, the metal soap content in the final polyurethane elastic fiber can be easily maintained within the above-mentioned desired metal soap content range. The metal soap content of the recycled polyurethane elastic fiber is more preferably 0.03 mass% or more and 0.5 mass% or less, and even more preferably 0.05 mass% or more and 0.3 mass% or less.

[0052] Specific examples of the metal soap include magnesium stearate, calcium stearate, and lithium stearate.

[0053] When the polyurethane elastic fiber of the present invention contains a surfactant, the amount is preferably 0.003% by mass or more and 3.0% by mass or less. The surfactant can reduce the influence of the metal soap accumulated during recovery, and when the polyurethane elastic fiber is used, the surfactant has a moderate sustained release characteristic, so the surfactant accumulation is moderate. When the surfactant content is within this range, the preferred practical properties of the polyurethane elastic fiber are ensured, such as the preferred unwinding properties (unwinding tension), the fiber shape of the winding, the elongation and strength at break. The surfactant content is more preferably in the range of 0.03% by mass or more and 2.5% by mass or less, and even more preferably in the range of 0.3% by mass or more and 2.0% by mass or less.

[0054] The amount of the surfactant in the recycled polyurethane elastic fiber recovered and reused as a raw material is preferably in the range of 0.003% by mass or more and 0.5% by mass or less. When the surfactant content of the recycled polyurethane elastic fiber is within this range, the surfactant content in the final polyurethane elastic fiber can be easily maintained within the above-mentioned desired surfactant content range. The surfactant content of the recycled polyurethane elastic fiber is more preferably 0.03% by mass or more and 0.25% by mass or less, and even more preferably 0.05% by mass or more and 0.2% by mass or less.

[0055] The specific example of the surfactant that can be used comprises nonionic surfactant, anionic surfactant and cationic surfactant.The nonionic surfactant that can be used for the present invention comprises polyoxyethylene alkyl ether, alkyl monoglyceryl ether, polyoxyethylene alkylamine, fatty acid sorbitan ester and fatty acid diethanolamide.Among these surfactants, the hydrophilic part (hydrophil) of surfactant is preferably ether type.For example, it is preferred to use at least one of ethylene oxide polymer, propylene oxide polymer and the copolymer of ethylene oxide and propylene oxide.By using the end-modified derivative of at least one ethylene oxide polymer, the end-modified derivative of propylene oxide polymer and the end-modified derivative of the copolymer of ethylene oxide and propylene oxide as nonionic surfactant, it is possible to improve antibacterial properties while improving spinnability.The hydrophobic part (hydrophob) of surfactant has the structure of the above-mentioned end modification, but alkyl, phenyl and styrenated phenyl are preferred. The specific example of nonionic surfactant comprises polyoxyethylene stearyl ether, polyoxyethylene lauryl ether, polyoxyethylene ethylphenol ether, polyoxyethylene propylphenol ether, polyoxyethylene styrenated phenyl ether and polyoxyethylene sorbitol tetraoleate.Even more preferably polyoxyethylene styrenated phenyl ether, such as polyoxyethylene oxypropylene tristyrene phenyl ether, polyoxyethylene oxypropylene distyrene phenyl ether, polyoxyethylene oxypropylene monostyrene phenyl ether, polyoxyethylene oxypropylene-2,4,6-tris (a, a-dimethyl benzyl) phenyl ether, polyoxyethylene oxypropylene-2,4-bis (a, a-dimethyl benzyl) phenyl ether, polyoxyethylene oxypropylene-2-mono (a, a-dimethyl benzyl) phenyl ether and polyoxyethylene oxypropylene-4-mono (a, a-dimethyl benzyl) phenyl ether.Even more preferably the mixture of these substances, in which the number of moles added of these styrene groups is well distributed.

[0056] In the present invention, when used in combination with a quaternary ammonium salt as a cationic surfactant, the antimicrobial activity varies depending on the chain length of the alkyl group in the ammonium ion. A combination with strong antimicrobial activity is desired, but from the perspective of inhibiting thermal decomposition caused by heat in the production of polyurethane elastic fibers, it is preferred to select chain types such as alkyl groups with long chain lengths (such as alkyl groups with a large number of carbon atoms). From a hygienic perspective, it is preferred to use an antimicrobial agent when, for example, recycling used clothes. From this perspective, preferred ammonium ions are didecyl dimethyl ammonium ions and oleyl trimethyl ammonium ions. These ammonium ions are typically provided using inorganic salts (such as chlorides, bromides and iodides) and organic acid salts (such as sulfonates, carboxylates and phosphates). Among these ammonium ions, sulfonates and carboxylates are preferred from the perspective of stability against yellowing and heat resistance.

[0057] Specific examples of the salt having such a structure include didecyldimethylammonium-3-fluoromethylsulfonate, didecyldimethylammonium trifluoromethanesulfonate, didecyldimethylammonium pentafluoroethanesulfonate, n-hexadecyltrimethylammonium trifluoromethanesulfonate, and benzyldimethylpalmitolealkylammonium pentafluoroethanesulfonate.

[0058] From the viewpoint of exhibiting antibacterial properties and maintaining a balance between yellowing and elongation properties, the quaternary ammonium salt-based antibacterial agent is preferably used in a range of 0.1 mass % or more and 5 mass % or less relative to the total mass of the polyurethane elastic fiber.

[0059] When the polyurethane elastic fiber of the present invention contains an antioxidant, the amount is preferably 0.002 mass % or more and 5.0 mass % or less. When the amount of the antioxidant is within this range, the antioxidant with preferred practical properties for the polyurethane elastic fiber includes hindered phenol compounds and phenolic compounds generally referred to as antioxidants. Examples include 3,5-di-tert-butyl-4-hydroxy-toluene, propionic acid n-octadecyl-β-(4'-hydroxy-3',5'-di-tert-butylphenyl) ester, tetrakis[propionic acid methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) ester] methane, l,3,5-trimethyl-2,4,6'-tris(3,5-di-tert-butyl-4)-hydroxybenzyl)benzene, (3,5-di-tert-butyl-4-hydroxy-benzyl-monoethyl-phosphate) calcium, tris( ... Ethylene glycol-bis[propionic acid 3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) ester], 3,9-bis[1,1-dimethyl-2-{β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionyloxy}ethyl]2,4,8,10-tetraoxaspiro[5,5]undecane, tocopherol, 2,2'-ethylenebis(4,6-di-tert-butylphenol), N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl]hydrazine , 2,2'-oxalamide bis[ethyl propionate-3-(3,5-di-tert-butyl-4-hydroxyphenyl) ester], 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, ethylidene-1,2-bis(butyric acid 3-[3-tert-butyl-4-hydroxyphenyl] ester), 1,1-bis(2-methyl-5-tert-butyl-4-hydroxyphenyl)butane, 1,1,3-tris(2-methyl-5-tert-butyl-4-hydroxyphenyl)butane, 1,3, 5-tris(3',5'-di-tert-butyl-4'-hydroxybenzyl)-S-triazine-2,4,6(1H,3H,5H)-trione, 1,3,5-tris(3'-tert-butyl-4'-hydroxy-5-methylbenzyl)-S-triazine-2,4,6(1H,3H,5H)-trione and 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione. Any high molecular weight hindered phenol compound known as an antioxidant for polyurethane elastic fibers is also preferred.

[0060] Preferred examples of high molecular weight hindered phenol compounds that can be used include adducts of divinylbenzene and cresol, adducts of dicyclopentadiene and cresol, isobutylene adducts, and polymers of chloromethylstyrene and compounds such as cresol, ethylphenol, and tert-butylphenol. Here, divinylbenzene and chloromethylstyrene may be para-versions or meta-versions. In addition, cresol, ethylphenol, and tert-butylphenol may be ortho-versions, meta-versions, or para-versions.

[0061] Among these compounds, compounds having a molecular weight of 300 or more are preferred from the viewpoint of stabilizing the viscosity of the raw material spinning solution of the polyurethane fiber, suppressing the volatilization loss during the spinning process, and obtaining good spinnability. In addition, in order to more effectively exhibit high spinning speed, heat resistance during the dyeing process, resistance to unsaturated fatty acids, and resistance to heavy metals, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, triethylene glycol-bis[propionic acid 3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) ester], ethylene-1,2-bis(propionic acid 3,3-bis[3-tert-butyl-4-hydroxyphenyl) ester]]butyrate), an adduct of divinylbenzene with p-cresol, any polymer having 6 to 12 repeating units, or a combination thereof are preferred. Among these compounds, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione is particularly preferred. When a triazine compound is selected for compound (a) and compound (c), a particularly high synergistic effect can be obtained in terms of heat resistance during the dyeing process. Among these compounds, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione is particularly preferred for compound (a), and 2,4-bis(2',4'-dimethylphenyl)-6-(2"-hydroxy-4"-alkoxyphenyl)-1,3,5-triazine is particularly preferred for compound (c).

[0062] In addition, from the viewpoint of suppressing the deterioration of characteristics due to recycling (particularly the elongation and strength at break and yellowing), the polyurethane elastic fiber of the present invention preferably contains a unilaterally hindered phenol compound. The unilaterally hindered phenol compound is preferably a compound containing at least two hydroxyphenyl groups, one of which is hindered and having a skeleton selected from diesters and alkylene groups. Preferably, the alkyl group present at the ring position adjacent to the hydroxyl group in the hydroxyphenyl group is a tert-butyl group, and preferably, the hydroxyl equivalent weight is 600 or less.

[0063] The phenol compound in the present invention is preferably a unilaterally hindered phenol compound. A preferred example of a unilaterally hindered phenol compound is ethylene-1,2-bis(butyric acid 3,3-bis[3-tert-butyl-4-hydroxyphenyl]ester), which has a structure in which a unilaterally hindered hydroxyphenyl group is covalently bonded to a diester backbone (see Chemical Formula 1 below).

[0064] [Formula 1]

[0065]

[0066] When using the above-mentioned unilateral hindered phenol compound, the deterioration of characteristics caused by recycling can be more effectively suppressed. If washing and bleaching are often performed (such as in the case of underwear), this type of hindered phenol compound can effectively suppress the decline in the molecular weight of the polyurethane constituting the polyurethane elastic fiber. From the perspective of satisfactorily achieving this effect without adversely affecting the physical properties of the fiber, the unilateral hindered phenol compound is preferably used in an amount of 0.15 mass % to 4 mass % relative to the mass polyurethane elastic fiber. It is more preferably used in an amount of 0.5 mass % to 3.5 mass % to reliably ensure characteristics such as elongation and strength at break, composite material durability, anti-yellowing property, and light fastness in some cases. The amount of the antioxidant is more preferably in the range of 0.2 mass % or more and 3.0 mass % or less, and even more preferably in the range of 0.5 mass % or more and 2.0 mass % or less.

[0067] The amount of the antioxidant in the recycled polyurethane elastic fiber recovered and used as a raw material is preferably in the range of 0.1 mass % or more and 5.0 mass % or less. When the amount of the antioxidant in the recycled polyurethane elastic fiber is within this range, the antioxidant content in the final polyurethane elastic fiber can be easily maintained within the above-mentioned desired antioxidant range. The amount of the antioxidant of the recycled polyurethane elastic fiber is more preferably 0.2 mass % or more and 3.0 mass % or less, and even more preferably 0.5 mass % or more and 2.0 mass % or less.

[0068] More specifically, the antioxidant is a hindered phenol compound having a molecular weight of 1,000 or more. Preferably, a hindered phenol compound having a molecular weight of 1,000 or more known for use as an antioxidant in polyurethane elastic fibers is preferred. There are no particular restrictions except for a relatively high molecular weight of 1,000 or more. Preferred examples of hindered phenol compounds having such a high molecular weight include adducts of divinylbenzene and cresol, adducts of dicyclopentadiene and cresol, isobutylene adducts, and polymers of chloromethylstyrene with compounds such as cresol, ethylphenol, and tert-butylphenol. Here, divinylbenzene and chloromethylstyrene may be in para-form or meta-form. In addition, cresol, ethylphenol, and tert-butylphenol may be in ortho-form, meta-form, or para-form.

[0069] Among these compounds, hindered phenol compounds derived from polymers of cresol are preferred from the viewpoint of stabilizing the viscosity of the raw material spinning solution of the polyurethane fiber and obtaining good spinnability. In addition, in order to more effectively exhibit high spinning speed, heat resistance during the dyeing process, resistance to unsaturated fatty acids and resistance to heavy metals, etc., it is preferred to use a certain amount of high molecular weight hindered phenol compounds. However, from the viewpoint of obtaining better basic physical properties of the polyurethane fiber, the amount used is preferably not excessive.

[0070] In the polyurethane elastic fiber of the present invention, the amount of the decomposition product derived from the antioxidant is preferably 1.0 mass % or less. When the amount of the decomposition product derived from the antioxidant is within this range, preferred practical properties of the polyurethane elastic fiber, particularly elongation and strength at break, yellowing resistance and durability can be ensured. The amount of the decomposition product derived from the antioxidant is preferably 1.0 mass % or less, and more preferably 0.5 mass % or less.

[0071] When the polyurethane elastic fiber of the present invention contains a tertiary amine compound, the amount thereof is preferably 0.2 mass % or more and 5.0 mass % or less. When the amount of the tertiary amine compound is within this range, the preferred practical properties of the polyurethane elastic fiber, such as spinnability, dyeability, durability and yellowing resistance, can be improved.

[0072] The tertiary amine compound used in the present invention is not particularly limited as long as it has an amino group in structure. Among primary to tertiary amine groups, compounds having only tertiary amino groups in the molecule are preferred from the viewpoint of chlorine and yellowing resistance of polyurethane elastic yarn.

[0073] When the number average molecular weight of the tertiary amine compound is less than 2,000, water repellency deteriorates due to wear with guides and knitting needles during the knitting process of the polyurethane elastic fiber and loss caused by bath liquid outflow during the dyeing process. Therefore, the number average molecular weight must be 2,000 or more. Considering the solubility in the polyurethane spinning stock solution, the number average molecular weight is preferably in the range of 2,000 to 10,000, and more preferably in the range of 2,000 to 4,000.

[0074] When the above-mentioned tertiary amine compound is contained, the recycling performance of the polyurethane elastic fiber, in particular, the anti-yellowing performance can be improved. From the viewpoint of satisfactory effect and no adverse effect on the physical properties of the fiber, the amount of the tertiary amine compound is preferably 0.2 mass% or more and 5.0 mass% or less, and more preferably 0.5 mass% or more and 4.0 mass% or less, relative to the mass of the fiber. The amount of the tertiary amine compound is more preferably in the range of 0.5 mass% or more and 3.0 mass% or less, and even more preferably in the range of 0.5 mass% or more and 2.0 mass% or less.

[0075] The amount of the tertiary amine compound in the recycled polyurethane elastic fiber recovered and used as a raw material is preferably in the range of 0.002 mass % or more and 5.0 mass % or less. When the amount of the tertiary amine compound in the recycled polyurethane elastic fiber is within this range, the tertiary amine compound in the final polyurethane elastic fiber can be easily maintained within the above-mentioned desired tertiary amine compound content range. The amount of the tertiary amine compound of the recycled polyurethane elastic fiber is more preferably 0.002 mass % or more and 3.0 mass % or less, and even more preferably 0.002 mass % or more and 2.0 mass % or less.

[0076] More specifically, the tertiary amine compound is a linear polymer compound having a number average molecular weight of 2,000 or more produced by the reaction of tert-butyl diethanolamine with methylene-bis(4-cyclohexyl isocyanate) and polyethylene imine, or a high molecular weight compound having a branched structure containing primary amino groups, secondary amino groups and tertiary amino groups in the molecular skeleton, etc.

[0077] In the polyurethane elastic fiber of the present invention, the amount of the decomposition product derived from the tertiary amine compound is preferably 1.0% by mass or less. When the amount of the decomposition product derived from the tertiary amine compound is within this range, preferred practical properties of the polyurethane elastic fiber, particularly entangled fiber shape, composite material durability, and yellowing resistance can be ensured. The amount of the decomposition product derived from the antioxidant is preferably 1.0% by mass or less, and more preferably 0.5% by mass or less.

[0078] When the polyurethane elastic fiber of the present invention contains a crosslinking structure modifier, the amount is preferably 0.002% by mass or more and 2.0% by mass or less. When the amount of the crosslinking structure modifier is within this range, preferred practical properties of the polyurethane elastic fiber, particularly elongation and strength at break, permanent deformation and yellowing resistance, can be ensured. The amount of the crosslinking structure modifier is more preferably in the range of 0.02% by mass or more and 1.5% by mass or less, and even more preferably in the range of 0.2% by mass or more and 1.0% by mass or less.

[0079] The amount of the cross-linked structure modifier in the recycled polyurethane elastic fiber recovered and used as a raw material is preferably in the range of 0.002 mass % or more and 2.0 mass % or less. When the amount of the cross-linked structure modifier in the recycled polyurethane elastic fiber is within this range, the cross-linked structure modifier in the final polyurethane elastic fiber can be easily maintained within the above-mentioned desired cross-linked structure modifier content range. The amount of the cross-linked structure modifier of the recycled polyurethane elastic fiber is more preferably 0.02 mass % or more and 1.5 mass % or less, and even more preferably 0.2 mass % or more and 1.0 mass % or less.

[0080] Examples of crosslinking structure modifiers include monoamines and / or diamines. Specific examples include monoamines (such as dimethylamine, diethylamine and cyclohexylamine) and diamines (such as ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, hexamethylenediamine, p-phenylenediamine, p-xylylenediamine, m-xylylenediamine, 1,3-cyclohexanediamine, hexahydromethylphenylenediamine and 2-methylpentamethylenediamine). A mixture of monoamines and diamines is particularly preferred.

[0081] Preferred are low levels of metal soaps, antioxidants, tertiary amine compounds and decomposition products thereof, which accumulate when the recycled polyurethane elastic fiber is repeatedly recycled. When conventional tertiary amine compounds and decomposition products thereof having a number average molecular weight in the range of 2,000 to 10,000 and conventional antioxidants and decomposition products thereof having a molecular weight of 1,000 or more are repeatedly recycled, they accumulate and cause deterioration of properties, particularly deterioration of elongation and strength at break.

[0082] In a recycling process in which waste fibers (such as fibers in industrial products that do not meet standards due to certain defects and are discarded immediately after manufacturing) are used at high concentrations, the elongation and strength at break are generally significantly reduced each time the process is repeated. In order to avoid such deterioration of the characteristics mentioned above, a tertiary amine compound with a high molecular weight or its decomposition product, an antioxidant with a high molecular weight, and a polyurethane source with a low decomposition product content are included to effectively reduce the concentration. Preferably, a polyurethane is added, the number average molecular weight of the polyurethane based on gel permeation chromatography (GPC) is 20,000 or more and 120,000 or less, and in the detected strength curve for a region of 30,000 or less molecular weight based on GPC, there is no peak or shoulder. When considering the elongation and strength at break of the polyurethane elastic fiber, the range of the number average molecular weight is preferably in the range of 30,000 or more and 100,000 or less, and more preferably in the range of 40,000 or more and 80,000 or less. Note that the detected intensity curve refers to a differential molecular weight distribution curve (where the horizontal axis represents the molecular weight, and the vertical axis represents the value obtained by differentiating the concentration fraction by the logarithmic value of the molecular weight), and the shoulder refers to a shoulder peak.

[0083] When a tertiary amine compound having a number average molecular weight in the range of 2,000 to 10,000 and / or a common antioxidant having a molecular weight of 1,000 or more is contained, the molecular weight of the polyurethane elastic fiber using the recycled polyurethane elastic fiber as a raw material according to the present invention is preferably in the range of 10,000 or more and 50,000 or less as a number average molecular weight. The molecular weight is measured by GPC and converted in terms of polystyrene.

[0084] Regarding the two carbonyl expansion and contraction vibrations of the urethane bond of the recycled polyurethane elastic fiber based on infrared spectroscopy (IR), it is preferred that the absorbance AvC=0 1730cm -1 and AvC=O 1710cm -1 Make AvC=O 1730cm -1 With AvC=O 1710cm -1 The ratio (i.e. AvC = O 1730cm -1 / AvC=O 1710cm -1 ) is 1.05 or more and 1.50 or less.

[0085] A preferred source of recycled polyurethane raw materials occurs when the intended use of the clothing product has been achieved and the clothing product is frequently washed. In many cases, this can be achieved by using used clothing (such as underwear) collected from municipalities. This is because repeated washing with anionic surfactants makes the used clothing suitable as a raw material for recycled polyurethane elastic fibers.

[0086] [Example]

[0087] (Examples 1 to 21, Comparative Examples 1 and 3)

[0088] The production and evaluation of recycled polyurethane elastic fibers and elastic fibers to which metal soap has been added will now be described with reference to Examples 1 to 21 and Comparative Examples 1 to 3 in Tables 1 to 4.

[0089] <Production of dry-spun polyurethane elastic fibers>

[0090] In Comparative Example 1, an N,N′-dimethylacetamide (DMAc) solution (35% by mass) of polyurethane having a molecular weight of 2,000 composed of tetramethylene ether glycol, bis-(p-isocyanatephenyl)-methane, and ethylenediamine was polymerized to obtain a polymer solution PUU1.

[0091] Next, a DMAc solution (35% by mass) of a mixture was prepared using a 1:1 (mass ratio) mixture of a polyurethane produced by reacting a condensation polymer of tert-butyldiethanolamine and methylene-bis(4-cyclohexyl isocyanate) (Metachlor (registered trademark) 2462 from DuPont) with p-cresol and divinylbenzene (Metachlor (registered trademark) 2390 from DuPont) as an antioxidant to obtain a cumulative solution (B).

[0092] Solution PUU1, accumulated solution (B), and ethylenediamine (C) were uniformly mixed together at 99 mass%, 1.0 mass%, and 0.1 mass%, respectively, to prepare a spinning solution (D).

[0093] This spinning solution is dry-spun at a dry nitrogen temperature of 300°C or higher with DMAc and a suspended ethylenediamine in the spinning solution that does not exceed 1 / 100 of the spinning solution content. At this time, the speed ratio of the godet roll to the take-up device is 1:1.20, and 22dtex / 3fil multifilament polyurethane elastic fiber is spun. The treatment agent (oil agent) described below is provided by an oiling roller before the fiber is taken up. The fiber is taken up at a winding speed of 600 meters / minute using a surface-driven take-up device, and the fiber is wound around a cylindrical paper tube with a length of 58mm by a transverse guide with a winding width of 38mm. A polyurethane elastic fiber of 500g of the wound fiber is obtained. The polyurethane elastic fiber is a fused yarn of three filaments fused together. The rotation speed of the oiling roller is adjusted so that a predetermined amount of the treatment agent is applied to the fused yarn. Using n-hexane as an extraction solvent, the amount of the applied treatment agent is measured according to JIS-L1073 (test method for synthetic fiber filament yarn). The composition of the treatment agent used here is 80 parts by mass of a 1 x 10 -5 Square meters / second of polydimethylsiloxane, 15 parts by mass, having a viscosity of 1.2 x 10 at 25°C -5 m 2 / s of mineral oil and 5 parts by mass of magnesium distearate having an average particle size of 0.5 μm.

[0094] In Example 1, the fiber obtained in Comparative Example 1 was taken out from the paper tube and dissolved in DMAc to prepare a 35% by mass DMAc solution. This is referred to as the DMAc solution of the polyurethane elastic fiber R1 recycled once. (Here, the number in R1 refers to the number of times the fiber is recycled.) The DMAc solution was used as a spinning solution, and spinning was performed using the same method as in Comparative Example 1.

[0095] In Example 2, the fiber obtained in Example 1 was taken out from the paper tube and dissolved in DMAc to prepare a 35% by mass DMAc solution. This is referred to as the DMAc solution of polyurethane elastic fiber R2. The DMAc solution was used as a spinning solution and spinning was performed using the same method as in Comparative Example 1.

[0096] As shown in Table 1, Examples 3 to 6 were spun after the fibers had been recycled 3 to 9 times.

[0097] In Comparative Example 2, spinning was performed in the same manner as in Example 1, except that the treating agent (oiling agent) used here was 80 parts by mass of a 1×10 -5 m2 / s polydimethylsiloxane, 20 parts by mass, having a viscosity of 1.2 x 10 at 25°C -5m2 / s of mineral oil and 0 parts by mass of magnesium distearate.

[0098] In Tables 1 to 4, the content values ​​refer to the values ​​of the solid polymer content per 100 parts by mass in the spinning solution. In Tables 3 and 4, the recycled polyurethane elastic fiber RA of the previous recycling times refers to a raw material extracted from frequently washed used underwear having a number average molecular weight of 63,000 based on GPC, having no peak or shoulder in the detected intensity curve for a region of 30,000 or less based on GPC, and having an AvC of 0.1730 cm based on IR. -1 / AvC=O 1710cm -1 Recycled polyurethane elastic fiber with a weight of 1.35.

[0099] The resulting dry-spun polyurethane elastic fibers (sample fibers below) were subjected to the following evaluations.

[0100] <Tangled Fiber Shape>

[0101] First, 500g of fiber was wound around a paper tube with a width of 57.5mm, an inner diameter of 73.5mm and a wall thickness of 6.1mm at a winding speed of 500 m / min (circumferential speed of the wound fiber) and a contact pressure of 10kg. The amount of oil applied was 5.0%. When the wound fiber was observed in the width direction, the size of the fiber not wound on both sides was measured at ten points relative to the paper tube width of 57.5mm, and the average value was used as d. Here, d is preferably 0.5mm or more and 6mm or less, more preferably 1.5mm or more and 5mm or less. The value of d is important from the perspective of preventing the packaged cake from contacting and rubbing with the packaging material, which can cause damage such as fiber breakage or cake deformation, and makes it difficult to stably produce a large number of rolls.

[0102] ⊙: d = 1.5 mm or more and 5 mm or less

[0103] ○: d = 1.0 mm or more and less than 1.5 mm

[0104] Δ: d = 0.5 mm or more and less than 1.0 mm

[0105] ×: d = less than 0.5 mm

[0106] <Unwinding Tension>

[0107] use Figure 1 The unwinding tension is measured by the device shown. The wound fiber 1 composed of the sample fiber is wound around the cylindrical paper tube 2 as shown. Figure 1The sample fiber 3 is fixed as shown, and the sample fiber 3 is unwound from one side of the wound fiber 1 at a constant speed of 45.7 meters per minute. The unwound sample fiber 3 is passed through the guide 4 and the ceramic groove guide 5, and pulled along a 90-degree curved track by the tensiometer roller 6. The roller 12 is driven at 45.7 meters per minute, the track is bent 90 degrees, and the fiber is sucked using the wire suction gun 13. The free tensiometer roller 6 is connected to the electric strain gauge 7, the electrical signal is averaged by the integrator 9 through the wire 8, and the data is stored in the recorder 11 through the wire 10. This test is performed for four minutes, and the average unwinding tension is measured for every 183m of fiber length.

[0108] The measurement is performed at a temperature of 25°C and a humidity of 60% RH. The positions on the wound fiber where the measurement is performed are the surface layer, the center layer, and the innermost layer of the wound fiber. Specifically, the surface layer of the wound fiber is a layer in which about 5 g of fiber is removed from the surface of the wound fiber. Since the winding pattern on the surface of the wound fiber is sometimes intentionally changed in this layer, about 5 grams of yarn is removed from the surface of the wound fiber. The innermost layer is a layer in which about 5 g of the wound yarn is retained in the wound fiber, and the center layer is an intermediate layer located between the surface layer and the innermost layer of the wound fiber. The wound fiber used to measure the unwinding tension is first stored at about 20°C for three months or more. The unwinding tension is evaluated according to the following standards.

[0109] ⊙: Less than 0.15cN

[0110] ○: 0.15 cN or more and less than 0.25 cN

[0111] Δ: 0.25 cN or more and less than 0.50 cN

[0112] ×: 0.50cN or more

[0113] <Elongation at break, strength at break, permanent strain rate, stress relaxation rate>

[0114] In the tensile test, the elongation at break, the strength at break, the permanent strain rate and the stress relaxation rate of the polyurethane elastic fiber are measured using the Instron 5564 tensile tester. The sample (L1) with a test length of 5 cm is stretched five times (stretched 300%) at a stretching rate of 50 cm / min. At this time, the stress at 300% elongation is defined as (G1). Then the same length is maintained at 300% elongation and lasts for 30 seconds. The stress after keeping for 30 seconds is defined as (G2). Next, the elongation of the sample is released and the sample length when the stress reaches 0 is defined as (L2). Repeat the stretching 300%, the maintenance and recovery operation, and cut the sample after stretching six times. The stress at break is defined as (G3), and the sample length at break is defined as (L3). These characteristics are calculated using the following equations.

[0115] Strength at break (cN) = (G3)

[0116] ⊙: greater than 20; ○: 17 to 20; Δ: 14 to 17; ×: less than 14

[0117] Strength at break (%) = 100 x ((L3) - (L1)) / (L1)

[0118] ⊙: greater than 480; ○: 460 to 480; Δ: 430 to 460; ×: less than 430

[0119] Permanent strain rate (%) = 100x((L2)-(L1)) / (L1)

[0120] ⊙: less than 20; ○: 20 to 22; Δ: 22 to 24; ×: greater than 24

[0121] Stress relaxation rate (%) = 100 x ((G1) - (G2)) / (G1)

[0122] ⊙: less than 25; ○: 25 to 28; Δ: 28 to 31; ×: greater than 31

[0123] <Composite material durability, light fastness, yellowing>

[0124] For composite durability, the sample fiber was stretched 100% and the retention of breaking strength was determined after the following exposure treatments (A), (B) and (C). For light fastness, the sample fiber was stretched 100% and the retention of breaking strength was determined after the following exposure treatment (A). For yellowing, under minimum load, the sample fiber was tightly wrapped around a 5x 5cm sample plate so that the effect of color on the sample plate did not seem to complete the sample. The front surface and standard white surface (JIS Z87224.3.4) of the sample were evenly flattened and covered with a transparent glass plate with a thickness of about 1mm. The b value was measured using a Hunter colorimeter according to method C (Hunter's method) in JIS L1013 and calculated based on the following equation. Five measurements were made and the average value was used.

[0125] b=7.0(Y-0.847Z) / Y 1 / 2

[0126] (Here, X, Y, and Z are calculated according to JIS Z8701.)

[0127] Yellowing was evaluated based on the extent of yellowing of the samples after exposure treatments (A) and (B). During each exposure treatment, the extent of yellowing (Δb) was calculated as follows.

[0128] Δb = b value after exposure treatment - b value before exposure treatment

[0129] The exposure treatment was performed as follows:

[0130] (A) Ultraviolet (UV) exposure treatment

[0131] The samples were exposed to a temperature and humidity of 63°C and 60% RH for 25 hours using a carbon arc weather meter from Suga Test Instruments.

[0132] (B) Nitrogen oxides (NO x )Exposure treatment

[0133] Using a sealed container with a rotating sample holder (Scott tester), the sample was exposed to 10 ppm of NO2 gas at a temperature and humidity of 40°C and 60% RH for 20 hours.

[0134] (C) Chlorine bleach (Cl2) exposure

[0135] The sample was exposed to a 500 ppm aqueous solution of Kao Haiter from Kao Corporation in a constant temperature bath at 40° C. for 30 minutes, and then washed with water for 10 minutes. These operations were repeated eight times.

[0136] The evaluation criteria are as follows.

[0137] ⊙ ○ Δ × Composite material durability ≥60% 40-60% 20-40% ≤20% Light fastness ≥80% 60-80% 40-60% ≤40% Yellowing ≤3 3 to 6 6-10 ≥10

[0138] GPC molecular weight measurement was performed under the following conditions. Figure 2 is a graph showing the GPC measurement of Example 21.

[0139] Columns: Two SHODEX KF-806M columns from Showa Denko

[0140] Solvent: N,N-dimethylacetamide, 1 ml / min

[0141] Temperature: 40℃

[0142] Detector: Differential refractometer (RI detector)

[0143] IR spectra were measured using a FT / IR7300 infrared spectroscope from JASCO Corporation using the KBr pellet method. Figure 3 is a graph showing IR spectrum measurement of Example 21.

[0144] <Quantitative Analysis of Magnesium Stearate Metal Soap>

[0145] Using the fibers as samples, the Mg concentration was quantified using inductively coupled plasma atomic emission spectrometry (ICP-AES) and multiplied by the molecular weight ratio of magnesium stearate to Mg (24.33).

[0146] [Table 1A]

[0147]

[0148]

[0149] [Table 1B]

[0150]

[0151] [Table 1C]

[0152]

[0153] [Table 1D]

[0154]

[0155]

[0156] [Table 2A]

[0157]

[0158] [Table 2B]

[0159]

[0160] [Table 2C]

[0161]

[0162]

[0163] [Table 2D]

[0164] Yellowing Comprehensive Assessment Example 6 Δ Δ Example 7 Δ Δ Example 8 Δ Δ Example 9 Δ ○ Example 10 Δ ○ Example 11 Δ ○ Comparative Example 3 Δ ×

[0165] [Table 3A]

[0166]

[0167] [Table 3B]

[0168]

[0169]

[0170] [Table 3C]

[0171]

[0172] [Table 3D]

[0173] Light fastness Yellowing Comprehensive Assessment Example 8 Δ Δ Δ Example 12 Δ Δ ○ Example 13 Δ Δ ○

[0174] [Table 4A]

[0175]

[0176] [Table 4B]

[0177]

[0178]

[0179] [Table 4C]

[0180]

[0181] [Table 4D]

[0182] Light fastness Yellowing Comprehensive Assessment Example 12 Δ Δ ○ Example 14 Δ Δ Δ Example 15 Δ Δ Δ Example 16 Δ ○ Δ Example 17 ○ Δ Δ Example 18 ○ ○ ○ Example 19 ○ ○ ○ Example 20 ○ ○ ○ Example 21 ◎ ◎ ◎ Comparative Example 1 ◎ ◎ ◎

[0183] Reference numerals list

[0184] 1: Tangled Fibers

[0185] 2: Cylindrical paper tube

[0186] 3: Unwound traveling elastic fiber (sample fiber)

[0187] 4: Guide

[0188] 5: Ceramic slot guide

[0189] 6: Tension meter roller

[0190] 7: Electrical strain gauge

[0191] 8: Wire

[0192] 9: Integrator

[0193] 10: Wire

[0194] 11: Recorder

[0195] 12: Roller

[0196] 13: Suction fiber.

Claims

1. A polyurethane elastic fiber using recycled polyurethane elastic fibers as at least one raw material, wherein the amount of metal soap in the polyurethane elastic fibers is 0.003% by mass or more and 3.0% by mass or less. 2 . The polyurethane elastic fiber according to claim 1 , wherein the polyurethane elastic fiber contains 0.003% by mass or more and 3.0% by mass or less of a surfactant. 3 . The polyurethane elastic fiber according to claim 1 , wherein the polyurethane elastic fiber contains 0.002% by mass or more and 5.0% by mass or less of an antioxidant. 4 . The polyurethane elastic fiber according to claim 1 , wherein the polyurethane elastic fiber contains 0.2% by mass or more and 5.0% by mass or less of a tertiary amine compound. 5 . The polyurethane elastic fiber according to claim 1 , wherein the polyurethane elastic fiber contains 0.002% by mass or more and 2.0% by mass or less of a cross-linking structure modifier. 6 . The polyurethane elastic fiber according to claim 1 , wherein the polyurethane elastic fiber contains 0.02% by mass or more and 1.0% by mass or less of a metal soap.

7. The polyurethane elastic fiber according to any one of claims 1 to 6, wherein the number average molecular weight of the recycled polyurethane elastic fiber based on gel permeation chromatography (GPC) is 20,000 or more and 120,000 or less, and there is no peak or shoulder in the detected intensity curve for the region where the molecular weight based on GPC is 30,000 or less.

8. The polyurethane elastic fiber according to any one of claims 1 to 7, wherein the AvC of the recycled polyurethane elastic fiber is 0.1730 cm-1 based on infrared spectroscopy (IR). -1 / AvC=O 1710cm -1 The ratio is 1.05 or more and 1.50 or less.

9. The polyurethane elastic fiber according to any one of claims 1 to 8, wherein the recycled polyurethane elastic fiber is used in clothing that is frequently washed.

10. The polyurethane elastic fiber according to claim 9, wherein the recycled polyurethane elastic fiber is used in underwear.