Plastic optical fiber

By optimizing the material and structure of the core and cladding in plastic optical fibers, controlling the transmission loss and frequency band, the problem of high bit error rate in short-distance signal transmission in the prior art is solved, and low bit error rate and high transmission quality are achieved Effect.

CN118974610AInactive Publication Date: 2024-11-15NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029628.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-29
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing plastic optical fibers cannot effectively reduce the bit error rate (BER) in short-range signal transmission. Even if the noise is reduced by increasing the M2 value, there is still room for improvement in the transmission quality.

Method used

Design a plastic optical fiber with a core diameter of more than 30μm and less than 100μm and a length of less than 30m and less than 30m and a transmission loss at a wavelength of 850nm is 70dB/km and less than 500dB/km and less than 30MHz·km and less than 600MHz·km. , perfluoro-based resin or partial fluoro-based resin is used as the core material, and a refractive index adjuster and a reinforcement layer are added to the cladding to control transmission loss and frequency band.

Benefits of technology

It realizes a low bit error rate in short-distance signal transmission, improves transmission quality, and BER can reach below 1×10-7, optimizing the quality of signal transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974610A_ABST
    Figure CN118974610A_ABST
Patent Text Reader

Abstract

This plastic optical fiber (10) is provided with a core (11) and a cladding (12) disposed on the outer periphery of the core (11). The length of the plastic optical fiber (10) is 30 m or less. The core (11) has a diameter of 30 [mu] m or more and 100 [mu] m or less. The plastic optical fiber (10) has a transmission loss of 70 dB / km or more and 500 dB / km or less at a wavelength of 850 nm, and a transmission band of 30 MHz km or more and 600 MHz km or less at a wavelength of 850 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to plastic optical fibers. Background Art

[0002] Plastic optical fiber has a core as the central part of the part that transmits light, and a cladding covering the outer periphery of the core. The core is formed of a resin material with a high refractive index. In order to keep the light in the core, the cladding is formed of a resin material with a lower refractive index than the resin material of the core.

[0003] In recent years, cables capable of transmitting large amounts of data have been required even in short-distance communications within homes, etc. Therefore, studies have been underway to use plastic optical fibers capable of transmitting large amounts of communication signals for short-distance transmission.

[0004] However, when plastic optical fibers are used for short-distance signal transmission, new issues regarding signal quality that were not considered in the case of long-distance transmission arise. 2 Optical fibers with a value of 1.7 or more are considered to be optical fibers that can reduce noise in short-distance transmission and transmit high-quality signals. 2 The value is a parameter conventionally used as a parameter indicating the quality of a light beam.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2019-49658 Summary of the invention

[0008] Problems to be solved by the invention

[0009] As an indicator of the quality of signal transmission (hereinafter referred to as "transmission quality"), there is BER (Bit Error Rate). BER indicates how many 0 and 1 signals are received incorrectly during transmission, and is calculated from the ratio of the number of error bits to the number of transmitted bits (number of error bits / number of transmitted bits). Optical fibers with low BER can have excellent transmission quality.

[0010] As described above, in the optical fiber disclosed in Patent Document 1, by 2 The value is set to 1.7 or more to reduce noise. 2 In other words, in order to reduce BER, it is not necessary to increase M only. 2 The value is not sufficient, and there is room for improvement in conventional optical fibers to enhance transmission quality.

[0011] Therefore, an object of the present invention is to provide a plastic optical fiber having improved transmission quality in short-distance signal transmission.

[0012] Means for solving problems

[0013] The present invention provides a plastic optical fiber comprising a core and a cladding arranged on the outer periphery of the core.

[0014] The length of the plastic optical fiber is less than 30m.

[0015] The core has a diameter of 30 μm or more and 100 μm or less,

[0016] The transmission loss at a wavelength of 850nm is 70dB / km or more and 500dB / km or less.

[0017] The transmission band at a wavelength of 850 nm is greater than or equal to 30 MHz·km and less than or equal to 600 MHz·km.

[0018] Effects of the Invention

[0019] According to the present invention, it is possible to provide a plastic optical fiber having improved transmission quality in short-distance signal transmission. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram showing an example of a cross-sectional structure of a plastic optical fiber according to an embodiment of the present invention.

[0021] Figure 2 It is a schematic diagram showing another example (first modified example) of the cross-sectional structure of the plastic optical fiber according to the embodiment of the present invention.

[0022] Figure 3 It is a schematic diagram showing still another example (second modified example) of the cross-sectional structure of the plastic optical fiber according to the embodiment of the present invention.

[0023] Figure 4 This is a schematic cross-sectional view showing an example of a manufacturing apparatus that can be used to manufacture the plastic optical fiber according to the embodiment of the present invention. DETAILED DESCRIPTION

[0024] A first aspect of the present invention is a plastic optical fiber comprising a core and a cladding arranged on the outer periphery of the core.

[0025] The length of the plastic optical fiber is less than 30m.

[0026] The core has a diameter of 30 μm or more and 100 μm or less,

[0027] The transmission loss at a wavelength of 850nm is 70dB / km or more and 500dB / km or less.

[0028] The transmission band at a wavelength of 850 nm is greater than or equal to 30 MHz·km and less than or equal to 600 MHz·km.

[0029] In the second aspect of the present invention, for example, the plastic optical fiber of the first aspect is a profiled refractive index type.

[0030] In the third aspect of the present invention, for example, in the plastic optical fiber of the first or second aspect, the core includes a first resin, and the first resin is at least one selected from perfluorinated resins, partially fluorinated resins, partially chlorinated resins, and partially deuterated resins.

[0031] In a fourth aspect of the present invention, for example, in the plastic optical fiber of the third aspect, the first resin is at least one selected from a perfluorinated resin and a partially fluorinated resin.

[0032] In a fifth aspect of the present invention, for example, in the plastic optical fiber of the fourth aspect, the first resin includes a fluorine-containing polymer including a structural unit (A) represented by the following formula (1).

[0033] [Chemical formula 1]

[0034]

[0035] (In formula (1), R ff 1 ~R ff 4 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 7 carbon atoms, or a perfluoroalkyl ether group having 1 to 7 carbon atoms. ff 1 and R ff 2 Can be connected to form a ring.)

[0036] In a sixth aspect of the present invention, for example, in the plastic optical fiber of the fifth aspect, the fluorinated polymer further contains a structural unit (B) represented by the following formula (2).

[0037] [Chemical formula 2]

[0038]

[0039] (In formula (2), R 1 ~R 3 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. 4 It represents a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A part of the fluorine atoms may be replaced by a halogen atom other than a fluorine atom. A part of the fluorine atoms in the perfluoroalkyl group may be replaced by a halogen atom other than a fluorine atom.

[0040] In a seventh aspect of the present invention, for example, in the plastic optical fiber of the fifth or sixth aspect, the fluorinated polymer further contains a structural unit (C) represented by the following formula (3).

[0041] [Chemical formula 3]

[0042]

[0043] (In formula (3), R 5 ~R 8 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A portion of the fluorine atoms may be replaced by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be replaced by a halogen atom other than a fluorine atom.

[0044] In an eighth aspect of the present invention, for example, in the plastic optical fiber according to any one of the fifth to seventh aspects, the fluorinated polymer further contains a structural unit (D) represented by the following formula (4).

[0045] [Chemical formula 4]

[0046]

[0047] (In formula (4), Z represents an oxygen atom, a single bond, or -OC(R 19 R 20 )O-,R 9 ~R 20 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. A portion of the fluorine atoms may be replaced by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be replaced by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkoxy group may be replaced by a halogen atom other than a fluorine atom. s and t are each independently 0 to 5, and s+t represents an integer of 1 to 6 (wherein, when Z is -OC(R 19 R 20 )O-, s+t can be 0).

[0048] In a ninth aspect of the present invention, for example, in the plastic optical fiber according to any one of the third to eighth aspects, the core further includes a refractive index adjusting agent.

[0049] In a tenth aspect of the present invention, for example, the plastic optical fiber according to any one of the first to ninth aspects further includes a reinforcement layer disposed on the outer periphery of the cladding.

[0050] Hereinafter, an embodiment of the plastic optical fiber (hereinafter referred to as "POF") of the present invention is described. The POF of this embodiment includes a core and a cladding arranged on the outer periphery of the core. The POF of this embodiment is, for example, a distributed refractive index (GI) type POF.

[0051] Figure 1 An example of the cross-sectional structure of the POF according to the present embodiment is shown.

[0052] Figure 1 The POF 10 shown includes a core 11 and a cladding 12 arranged on the outer periphery of the core 11 .

[0053] The length of the POF 10 of the present embodiment is less than 30m. It should be noted that the "length of the POF 10" here refers to the axial length of the POF 10. That is, the POF 10 of the present embodiment is used for short-distance signal transmission, for example, it can also be used at home. In addition, in the POF 10 of the present embodiment, the diameter of the core 11 is greater than 30μm and less than 100μm. In the POF 10 of the present embodiment having such a length and core diameter, the transmission loss at a wavelength of 850nm is greater than 70dB / km and less than 500dB / km, and the transmission band at a wavelength of 850nm is greater than 30MHz·km and less than 600MHz·km.

[0054] Here, in this specification, the diameter of the core 11 (hereinafter referred to as "core diameter") is a diameter at which the light intensity is 5% measured by the NFP (Near Field Pattern) method using light of a wavelength of 850 nm in the method according to IEC60793-1-20 and IEC60793-2-40 subcategory A4h. In addition, the transmission loss of the POF 10 at a wavelength of 850 nm is a value measured by the cut-back method in the method according to IEC60793-1-40. In addition, the conduction band of the POF 10 is a value measured by the pulse method in the method according to IEC60793-1-41.

[0055] Although the POF 10 of this embodiment has a short length range and a small core diameter range that are more likely to generate noise as described above, a low BER can be achieved by making the conduction loss and the transmission band meet the above range. As mentioned above, BER is the ratio of the number of error bits to the number of transmitted bits (number of error bits / number of transmitted bits), and is an indicator of transmission quality. A low BER means good transmission quality. Therefore, the POF 10 of this embodiment can achieve improved transmission quality in short-distance signal transmission. Here, the BER is preferably 1×10 -7 Below, more preferably 1×10-8 the following.

[0056] As described above, the length of the POF 10 of the present embodiment is 30 m or less. The length of the POF 10 of the present embodiment can be, for example, 20 m or less, 15 m or less, or 10 m or less. The POF 10 of the present embodiment can achieve excellent transmission quality even if it is a POF of a shorter distance as described above. The length of the POF 10 of the present embodiment can be more than 0 m, for example, it can be more than 0.1 m.

[0057] As described above, in the POF 10 of this embodiment, the core diameter is 30 μm or more and 100 μm or less. The core diameter may be 80 μm or less, 60 μm or less, or 55 μm or less. The core diameter may be 40 μm or more, or 45 μm or more.

[0058] As described above, in the POF 10 of the present embodiment, the transmission loss at a wavelength of 850nm is greater than 70dB / km and less than 500dB / km, and the transmission band at a wavelength of 850nm is greater than 30MHz·km and less than 600MHz·km. The transmission loss and the transmission band are factors that affect the BER. In addition, the transmission loss is also related to the noise. Therefore, by controlling the transmission loss within the above range, the noise can be indirectly controlled within an appropriate range. The POF 10 of the present embodiment can reduce the BER by controlling the transmission loss and the transmission band to be a combination within the above range. The preferred combination of the range of the transmission loss and the transmission band can be appropriately determined, for example, by considering the material used for the core 11 (such as the type of resin, etc.).

[0059] The transmission loss at a wavelength of 850 nm is preferably 70 dB / km to 400 dB / km, more preferably 70 dB / km to 350 dB / km, and even more preferably 80 dB / km to 300 dB / km.

[0060] The transmission band at a wavelength of 850 nm is preferably 50 MHz·km to 580 MHz·km, more preferably 60 MHz·km to 560 MHz·km, and still more preferably 70 MHz·km to 540 MHz·km.

[0061] The transmission loss of the POF 10 of the present embodiment can be controlled within the above range by, for example, the manufacturing conditions of the POF 10, specifically, the filtering conditions for removing foreign matter such as minute dirt from the material of the POF 10 (for example, the material of the core 11 and the material of the cladding 12). Regarding the filtering conditions, for example, the type of resin used as the material and additives such as refractive index adjustment can be considered to determine appropriate conditions so that the transmission loss at a wavelength of 850 nm is within the range of 70 dB / km or more and 500 dB / km or less.

[0062] In addition, in order to set the transmission loss of the POF 10 of the present embodiment within the above range, for example, it is preferred to heat-treat the material of the POF 10 (e.g., the material of the core 11, the material of the cladding 12) at a high temperature. By such a heat treatment, organic impurities such as by-products during resin synthesis can be removed. Such organic impurities cause scattering. Therefore, by performing such a heat treatment at a high temperature, a POF 10 with low transmission loss in which organic scatterers are reduced can be obtained. The temperature of such a heat treatment varies depending on the type of resin used for the material of the core 11 and the resin used for the material of the cladding 12. For example, when the glass transition temperature of the resin used is recorded as Tg, the temperature of the heat treatment is preferably above Tg+70°C, more preferably above Tg+90°C, and further preferably above Tg+110°C. For example, when a perfluoro-4-methyl-2-methylene-1,3-dioxolane polymer used in Examples described below is used, the temperature of the heat treatment is preferably 220° C. or higher, more preferably 240° C. or higher, and even more preferably 250° C. or higher.

[0063] The transmission band of the POF 10 of the present embodiment can be controlled within the above range by, for example, controlling the refractive index distribution of the core 11. Specifically, regarding the conditions for diffusing the refractive index modifier contained in the material of the core 11, for example, appropriate conditions can be determined by considering the type of resin used as the material and the refractive index adjustment so that the transmission band is within the range of 30 MHz·km or more and 600 MHz·km or less. The so-called conditions for diffusing the refractive index modifier include, for example, the time for the fiber structure as the precursor of the POF 10 to pass through the diffusion tube, the length of the diffusion tube, the set temperature of the diffusion tube, and the spinning speed.

[0064] The POF 10 of this embodiment preferably has a first end where light is incident and a second end where light is emitted, and the M of the light emitted from the second end is preferably 2 As described in Japanese Patent Application Publication No. 2019-49658 (Patent Document 1), which is a prior application of the present applicant, M, which has been used as a parameter to indicate the quality of a laser beam, is 2The value is used as the design value of the optical fiber for short-distance communication, that is, M 2 By controlling the M value to be greater than 1.7, the return light from the second end as the emission end to the first end as the incident end is greatly expanded in space, and the amount of light returning to the light source such as the VCSEL is reduced, thereby reducing the return light noise. 2 The POF 10 of this embodiment can further improve the transmission quality. 2 The upper limit of the value is not particularly limited, and may be, for example, 6 or less, or 5 or less. 2 The value can be controlled to a desired value according to, for example, the type of material of the core 11 and the manufacturing conditions of the POF 10 .

[0065] Hereinafter, each structure of the POF 10 of this embodiment will be described in more detail.

[0066] (Core 11)

[0067] The core 11 is a region where light propagates. The core 11 has a higher refractive index than the cladding 12. With this configuration, light incident on the core 11 is confined inside the core 11 by the cladding 12 and propagates through the POF 10.

[0068] The core 11 contains the first resin. The core 11 may contain the first resin as a main component. Here, the core 11 contains the first resin as a main component means that the first resin is the largest component in the core 11 in terms of mass ratio. The core 11 may contain 75% by mass or more of the first resin, or 80% by mass or more, or 85% by mass or more.

[0069] The core 11 may further include an additive in addition to the first resin. The additive is, for example, a refractive index adjuster. That is, the core 11 may be formed from a resin composition including the first resin and an additive such as a refractive index adjuster. As the refractive index adjuster, for example, a known refractive index adjuster used in the material of the core 11 of the POF 10 may be used. The material of the core 11 may also include other additives in addition to the refractive index adjuster.

[0070] When the POF 10 of this embodiment is a GI type, for example, the core 11 has a refractive index distribution in which the refractive index varies in the radial direction. Such a refractive index distribution can be formed by adding a refractive index adjuster to the first resin and diffusing the refractive index adjuster in the first resin (for example, by thermal diffusion).

[0071] The first resin contained in the core 11 is not particularly limited as long as it has high transparency. Examples of the first resin include fluorine-containing resins, acrylic resins such as methyl methacrylate, styrene resins, and carbonate resins.

[0072] The first resin contained in the core 11 can be at least one selected from perfluoro resin, partial fluoro resin, partial chlorine resin and partially deuterated resin. Here, partial fluoro resin, partial chlorine resin and partially deuterated resin refer to resins in which a part of the hydrogen atoms of CH bonds in a resin known in the technical field as a core material of POF is replaced by fluorine, chlorine and deuterium, respectively. Here, perfluoro resin refers to a resin in which all the hydrogen atoms of CH bonds in a resin known in the technical field as a core material of POF are replaced by fluorine. Examples of resins known in the technical field as core materials include acrylic resins such as methyl methacrylate, styrene resins and carbonate resins as mentioned above. Polymers with an aliphatic ring structure such as a polymer with a dioxolane structure can also be used.

[0073] The first resin is preferably at least one selected from a perfluorinated resin and a partially fluorinated resin. That is, the first resin is preferably a fluorinated resin.

[0074] The first resin of the core 11 is preferably a fluorine-containing resin containing a fluorine-containing polymer. Hereinafter, the fluorine-containing resin contained in the core 11 is referred to as a first fluorine-containing resin, and the fluorine-containing polymer contained in the first fluorine-containing resin is referred to as a first fluorine-containing polymer.

[0075] From the viewpoint of suppressing light absorption caused by the stretching energy of the CH bond, the first fluoropolymer contained in the first fluororesin preferably does not substantially contain hydrogen atoms, and it is particularly preferred that all hydrogen atoms bonded to carbon atoms are substituted by fluorine atoms. That is, the first fluoropolymer preferably does not substantially contain hydrogen atoms and is perfluorinated. In this specification, the fluoropolymer does not substantially contain hydrogen atoms means that the content of hydrogen atoms in the fluoropolymer is less than 1 mol%.

[0076] The first fluorinated polymer preferably has a fluorinated aliphatic ring structure. The fluorinated aliphatic ring structure may be contained in the main chain of the fluorinated polymer or in the side chain of the first fluorinated polymer. The first fluorinated polymer has, for example, a structural unit (A) represented by the following structural formula (1).

[0077] [Chemical formula 1]

[0078]

[0079] In formula (1), R ff 1 ~R ff 4 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 7 carbon atoms, or a perfluoroalkyl ether group having 1 to 7 carbon atoms. ff 1 and R ff2 Can be connected to form a ring. "Perfluoro" means that all hydrogen atoms bonded to carbon atoms are replaced by fluorine atoms. In formula (1), the number of carbon atoms in the perfluoroalkyl group is preferably 1 to 5, more preferably 1 to 3, and further preferably 1. The perfluoroalkyl group may be linear or branched. Examples of the perfluoroalkyl group include trifluoromethyl, pentafluoroethyl, heptafluoropropyl, and the like.

[0080] In formula (1), the number of carbon atoms in the perfluoroalkyl ether group is preferably 1 to 5, more preferably 1 to 3. The perfluoroalkyl ether group may be linear or branched. Examples of the perfluoroalkyl ether group include perfluoromethoxymethyl and the like.

[0081] In R ff 1 and R ff 2 When the rings are connected to form a ring, the ring may be a 5-membered ring or a 6-membered ring. Examples of the ring include a perfluorotetrahydrofuran ring, a perfluorocyclopentane ring, and a perfluorocyclohexane ring.

[0082] Specific examples of the structural unit (A) include structural units represented by the following formulae (A1) to (A8).

[0083] [Chemical formula 5]

[0084]

[0085] The structural unit (A) is preferably the structural unit (A2) among the structural units represented by the above formulae (A1) to (A8), that is, the structural unit represented by the following formula (5).

[0086] [Chemical formula 6]

[0087]

[0088] The first fluoropolymer can include one or more structural units (A). In the first fluoropolymer, the content of the structural unit (A) is preferably 20 mol% or more relative to the total of all structural units, and more preferably 40 mol% or more. By comprising more than 20 mol% of the structural unit (A), the first fluoropolymer has a tendency to have higher heat resistance. In the case of comprising more than 40 mol% of the structural unit (A), the first fluoropolymer has a tendency to have higher transparency and high mechanical strength in addition to high heat resistance. In the first fluoropolymer, the content of the structural unit (A) is preferably less than 95 mol% relative to the total of all structural units, and more preferably less than 70 mol%.

[0089] The structural unit (A) is derived from, for example, a compound represented by the following formula (6). In formula (6), R ff1 ~R ff 4 The same as formula (1). The compound represented by formula (6) can be obtained by a known production method such as the production method disclosed in JP-A-2007-504125.

[0090] [Chemical formula 7]

[0091]

[0092] Specific examples of the compound represented by the above formula (6) include compounds represented by the following formulas (M1) to (M8).

[0093] [Chemical formula 8]

[0094]

[0095] The fluorinated polymer may further contain other structural units in addition to the structural unit (A). Examples of the other structural units include the following structural units (B) to (D).

[0096] The structural unit (B) is represented by the following formula (2).

[0097] [Chemical formula 2]

[0098]

[0099] In formula (2), R 1 ~R 3 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. 4 It represents a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A part of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A part of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom.

[0100] The fluorinated polymer may contain one or more structural units (B). In the fluorinated polymer, the content of the structural unit (B) is preferably 5 to 10 mol% relative to the total of all structural units. The content of the structural unit (B) may be 9 mol% or less, or 8 mol% or less.

[0101] The structural unit (B) is derived from, for example, a compound represented by the following formula (7). 1 ~R 4 The same as formula (2). The compound represented by formula (7) is a fluorine-containing vinyl ether such as perfluorovinyl ether.

[0102] [Chemical formula 9]

[0103]

[0104] The structural unit (C) is represented by the following formula (3).

[0105] [Chemical formula 3]

[0106]

[0107] In formula (3), R 5 ~R 8 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A portion of the fluorine atoms may be replaced by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be replaced by a halogen atom other than a fluorine atom.

[0108] The fluorinated polymer may contain one or more structural units (C). In the fluorinated polymer, the content of the structural unit (C) is preferably 5 to 10 mol% relative to the total of all structural units. The content of the structural unit (C) may be 9 mol% or less, or 8 mol% or less.

[0109] The structural unit (C) is derived from, for example, a compound represented by the following formula (8). 5 ~R 8 The same as formula (3). The compound represented by formula (8) is a fluorine-containing olefin such as tetrafluoroethylene and chlorotrifluoroethylene.

[0110] [Chemical formula 10]

[0111]

[0112] The structural unit (D) is represented by the following formula (4).

[0113] [Chemical formula 4]

[0114]

[0115] In formula (4), Z represents an oxygen atom, a single bond, or -OC(R 19 R 20 )O-,R 9 ~R 20 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. A portion of the fluorine atoms may be replaced by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be replaced by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkoxy group may be replaced by a halogen atom other than a fluorine atom. s and t are each independently 0 to 5, and s+t represents an integer of 1 to 6 (wherein, when Z is -OC(R 19 R20 )O-, s+t can be 0).

[0116] The structural unit (D) is preferably represented by the following formula (9). The structural unit represented by the following formula (9) is the case where Z is an oxygen atom, s is 0, and t is 2 in the above formula (4).

[0117] [Chemical formula 11]

[0118]

[0119] In formula (9), R 141 , R 142 , R 151 and R 152 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. A portion of the fluorine atoms may be substituted with a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted with a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkoxy group may be substituted with a halogen atom other than a fluorine atom.

[0120] The fluorinated polymer may contain one or more structural units (D). In the fluorinated polymer, the content of the structural unit (D) is preferably 30 to 67 mol% relative to the total of all structural units. The content of the structural unit (D) is, for example, 35 mol% or more, 60 mol% or less, or 55 mol% or less.

[0121] The structural unit (D) is derived from, for example, a compound represented by the following formula (10). 9 ~R 18 , s and t are the same as those in formula (4). The compound represented by formula (10) is a fluorine-containing compound having two or more polymerizable double bonds and capable of cyclopolymerization.

[0122] [Chemical formula 12]

[0123]

[0124] The structural unit (D) is preferably derived from a compound represented by the following formula (11). In formula (11), R 141 , R 142 , R 151 and R 152 Same as formula (9).

[0125] [Chemical formula 13]

[0126]

[0127] Specific examples of the compound represented by formula (10) or formula (11) include the following compounds.

[0128] CF2=CFOCF2CF=CF2

[0129] CF2=CFOCF(CF3)CF=CF2

[0130] CF2=CFOCF2CF2CF=CF2

[0131] CF2=CFOCF2CF(CF3)CF=CF2

[0132] CF2=CFOCF(CF3)CF2CF=CF2

[0133] CF2=CFOCFClCF2CF=CF2

[0134] CF2=CFOCCl2CF2CF=CF2

[0135] CF2=CFOCF2OCF=CF2

[0136] CF2=CFOC(CF3)2OCF=CF2

[0137] CF2=CFOCF2CF(OCF3)CF=CF2

[0138] CF2=CFCF2CF=CF2

[0139] CF2=CFCF2CF2CF=CF2

[0140] CF2=CFCF2OCF2CF=CF2

[0141] CF2=CFOCF2CFClCF=CF2

[0142] CF2=CFOCF2CF2CCl=CF2

[0143] CF2=CFOCF2CF2CF=CFCl

[0144] CF2=CFOCF2CF(CF3)CCl=CF2

[0145] CF2=CFOCF2OCF=CF2

[0146] CF2=CFOCCl2OCF=CF2

[0147] CF2=CClOCF2OCCl=CF2

[0148] The first fluorinated polymer may further contain other structural units other than the structural units (A) to (D), but preferably does not substantially contain other structural units other than the structural units (A) to (D). It should be noted that the fluorinated polymer does not substantially contain other structural units other than the structural units (A) to (D) means that the total amount of the structural units (A) to (D) is 95 mol% or more, preferably 98 mol% or more, relative to the total amount of all structural units in the fluorinated polymer.

[0149] The polymerization method of the first fluorinated polymer is not particularly limited, and for example, a common polymerization method such as radical polymerization may be used. The polymerization initiator used for polymerizing the fluorinated polymer may be a perfluorinated compound.

[0150] The first fluorinated polymer constitutes the first fluorinated resin used as the first resin. The first glass transition temperature Tg1 of the first resin is not particularly limited, and is, for example, 100°C to 140°C, may be 105°C or higher, or may be 120°C or higher. In this specification, the glass transition temperature refers to the midpoint glass transition temperature (Tg1) determined in accordance with the provisions of JIS K7121:1987. mg ).

[0151] The refractive index of the core 11 is not particularly limited as long as it is higher than the refractive index of the cladding 12. In order to achieve a high numerical aperture in the POF 10, it is preferred that the difference between the refractive index of the core 11 and the refractive index of the cladding 12 is greater for the wavelength of the light used. For example, for the wavelength of the light used (e.g., a wavelength of 850 nm), the refractive index of the core 11 can be set to be greater than 1.320, or can be set to be greater than 1.330. The upper limit of the refractive index of the core 11 is not particularly limited, and is, for example, less than 1.4000.

[0152] (Clad 12)

[0153] In the POF 10 of the present embodiment, the cladding 12 contains, for example, the second resin. The cladding 12 may contain the second resin as a main component. Here, the cladding 12 containing the second resin as a main component means that the second resin is the largest component in the cladding 12 in terms of mass ratio. The cladding 12 may contain 80% or more of the second resin, or may contain 90% or more of the second resin, or may contain 95% or more of the second resin. The cladding 12 may consist only of the second resin. The cladding 12 may further contain additives in addition to the second resin.

[0154] The second resin contained in the cladding layer 12 is not particularly limited as long as it has high transparency. Examples of the second resin are the same as those exemplified as the resin that can be used as the first resin. As the second resin, a fluorine-containing resin is preferably used.

[0155] The second resin of the cladding 12 is preferably a fluorine-containing resin containing a fluorine-containing polymer. Hereinafter, the fluorine-containing resin contained in the cladding 12 is referred to as a second fluorine-containing resin, and the fluorine-containing polymer contained in the second fluorine-containing resin is referred to as a second fluorine-containing polymer.

[0156] Examples of fluorinated resins that can be used as the second fluorinated resin are the same as those exemplified as the fluorinated resins that can be used as the first fluorinated resin. That is, examples of fluorinated polymers that can be used as the second fluorinated polymer are the same as those exemplified as the fluorinated polymers that can be used as the first fluorinated polymer.

[0157] The second fluorine-containing polymer constitutes the second fluorine-containing resin used as the second resin. As described above, the second glass transition temperature Tg2 of the second resin is not particularly limited, and is, for example, 100°C to 150°C, may be 105°C or higher, or may be 125°C or higher.

[0158] The second resin may be a resin different from the first resin, but preferably has affinity with the first resin. For example, the second resin may contain the same polymerized units as those contained in the first resin, or may be the same as the first resin. Thus, peeling is less likely to occur at the interface between the core 11 and the cladding 12, and, for example, transmission loss can be suppressed to a low level.

[0159] The refractive index of the cladding 12 is not particularly limited as long as it is designed according to the refractive index of the core 11. The cladding 12 may have a refractive index of, for example, 1.340 or less, 1.330 or less, or 1.320 or less at the wavelength of light used (e.g., 850 nm).

[0160] Figure 2 A first modified example of the POF according to the present embodiment is shown. Figure 2 The POF 20 shown has a structure in which a reinforcement layer 21 arranged on the periphery of the cladding 12 is further provided relative to the POF 10. The reinforcement layer 21 is provided to improve the mechanical strength of the POF 10. For the reinforcement layer 21, for example, materials and structures used as reinforcement layers in known POFs can be applied. As materials for the reinforcement layer 21, for example, various engineering plastics such as polycarbonate, polyester, cycloolefin polymer, cycloolefin copolymer, polytetrafluoroethylene (PTFE), modified PTFE and tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA), or copolymers and mixtures thereof can be cited.

[0161] In the POF of this embodiment, for example, the cladding layer may be composed of a plurality of layers. For example, the POF of this embodiment may be as follows: Figure 3The POF 30 shown in the second modified example includes a core 11, a cladding 32 disposed on the periphery of the core, and a coating layer 21 disposed on the periphery of the cladding. In the POF 30, the cladding 32 has a two-layer structure formed by a first cladding layer 321 disposed in contact with the core 11 and a second cladding layer 322 disposed on the outer peripheral side of the first cladding layer 321, that is, a double cladding structure. In the POF 30, the coating layer 21 is in contact with the second cladding layer 322. It should be noted that in Figure 3 In the figure, an example in which the cladding 32 has a two-layer structure is shown, but the number of layers included in the cladding 32 is not limited thereto, and may include three or more layers.

[0162] (Manufacturing method of POF)

[0163] The POF of the present embodiment is manufactured, for example, using a melt spinning method. That is, an example of a method for manufacturing the POF of the present embodiment includes:

[0164] Melting the core material and extruding it into a fiber shape to produce a fibrous molded body including the core material; and

[0165] The cladding material is melted and extruded so as to cover the surface of the molded body, thereby producing a laminated body in which the core material and the cladding material are concentrically laminated.

[0166] The core material includes, for example, a first resin. The cladding material includes, for example, a second resin.

[0167] In manufacturing Figure 2 In the case of the POF 20 shown, the production method may further include: stretching the laminate while heating it to a predetermined temperature, and spinning the laminate.

[0168] In manufacturing Figure 3 In the case of the POF 30 shown, for example, as cladding materials, a material for forming the first cladding layer 321 (first cladding material) and a material for forming the second cladding layer 322 (second cladding material) are prepared. In the above-mentioned manufacturing method, when manufacturing a laminated body in which the core material and the cladding material are stacked in a concentric manner, the first cladding material can be melted and extruded so as to cover the surface of a fibrous molded body including the core material, and the melted second cladding material can be extruded so as to cover the surface thereof, thereby manufacturing a laminated body in which the core material, the first cladding material and the second cladding material are stacked in a concentric manner.

[0169] Figure 4 It means that it can be used to manufacture Figure 2 Schematic cross-sectional view of an example of a manufacturing apparatus for POF 20 shown.

[0170] Figure 4 The device 100 shown includes a first extrusion device 101a for forming a core, a second extrusion device 101b for forming a cladding layer, and a third extrusion device 101c for forming a reinforcing layer. The device 100 further includes a first chamber 110 and a second chamber 120. The first chamber 110 and the second chamber 120 are arranged in sequence below in the vertical direction.

[0171] The first extrusion device 101a has a first receiving portion 102a for receiving a core material 1a, and a first extrusion portion 103a for extruding the core material 1a received in the first receiving portion 102a from the first receiving portion 102a. In the first extrusion device 101a, a heating portion such as a heater (not shown) may be further provided so that the core material 1a can be melted in the first receiving portion 102a, and the melted core material 1a can be kept in a molten state until it is formed. In this case, for example, a rod-shaped core material (preform) 1a is inserted into the first receiving portion 102a through an opening at the top of the first receiving portion 102a, and is heated and melted in the first receiving portion 102a.

[0172] In the first extrusion device 101a, the core material 1a is extruded outward from the first housing portion 102a through the first extrusion portion 103a, for example, by gas extrusion, so as to form the core 2. The core material 1a extruded through the first extrusion portion 103a so as to form the core 2 is then moved downward in the vertical direction and is sequentially supplied to the first chamber 110 and the second chamber 120, respectively.

[0173] The second extrusion device 101b has a second housing portion 102b for housing the cladding material 1b, and a second extrusion portion 103b for extruding the cladding material 1b housed in the second housing portion 102b from the second housing portion 102b. The second extrusion device 101b extrude the melted cladding material 1b in a manner that covers the outer periphery of the core 2 formed by the core material 1a extruded from the first extrusion device 102a. Specifically, the cladding material 1b extruded from the second extrusion device 101b is supplied to the first chamber 110. In the first chamber 110, the core 2 formed by the core material 1a is covered with the cladding material 1b, thereby forming a cladding 3 covering the outer periphery of the core 2. The laminate formed by the core 2 and the cladding 3 covering the outer periphery of the core 2 moves from the first chamber 110 to the second chamber 120.

[0174] The third extrusion device 101c includes, for example, a third storage portion 102c for storing the reinforcing layer material 1c, a screw 104 disposed in the third storage portion 102c, and a hopper 105 connected to the third storage portion 102c. In the third extrusion device 101c, for example, a granular reinforcing layer material 1c is supplied to the third storage portion 102c through the hopper 105. The reinforcing layer material 1c supplied to the third storage portion 102c is kneaded by the screw 104 while being heated, for example, so that it is softened and can flow. The softened reinforcing layer material 1c is extruded from the third storage portion 102c by the screw 104.

[0175] The reinforcing layer material 1c extruded from the third extruder 101c is supplied to the second chamber 120. In the second chamber 120, the surface of the laminate formed of the core 2 and the cladding 3 is coated with the reinforcing layer material 1c, thereby forming the reinforcing layer 4 covering the outer periphery of the cladding 3.

[0176] The laminate 5 formed by stacking the core 2, the cladding 3 and the reinforcement layer 4 in a concentric circle shape moves from the second chamber 120 to the diffusion tube 130 arranged vertically below the second chamber 120. A heater (not shown) for heating the laminate may be arranged in the diffusion tube 130, for example. The diffusion tube 130 can diffuse dopants such as a refractive index adjuster contained in the laminate 5 passing through the inside of the diffusion tube 130 in the laminate 5. In order to make the transmission band of the POF 20 finally obtained to be within the range of 30 MHz·km or more and 600 MHz·km or less, for example, the diffusion tube 130 is appropriately adjusted for the time when the laminate 5 passes through the inside, the length of the diffusion tube 130, the spinning speed and the temperature, etc.

[0177] The diffuser 130 is connected to the internal flow path of the nozzle 140. That is, the lower opening of the diffuser 130 is connected to the inlet of the nozzle 140, and the laminate 5 that has passed through the diffuser 130 flows into the internal flow path through the inlet of the nozzle 140. The laminate 5 is reduced in diameter through the internal flow path and is ejected from the ejection port of the nozzle 140 in a fibrous form.

[0178] The positional relationship between the second chamber 120 and the diffuser 130 may be reversed. That is, the diffuser 130 may be disposed below the first chamber 110, the second chamber 120 may be disposed below the diffuser 130, and the nozzle 140 may be provided further below the second chamber.

[0179] The laminate 5 ejected in a fiber form from the ejection outlet of the nozzle 140 flows into, for example, the internal space 151 of the cooling pipe 150, is cooled while passing through the internal space 151, and is ejected from the opening to the outside of the cooling pipe 150. The laminate 5 ejected from the cooling pipe 150 passes between, for example, two rollers 161 and 162 of the nip roller 160, and further passes through guide rollers 163 to 165, and is wound on the winding roller 166 as the POF 20. A displacement meter 170 for measuring the outer diameter of the POF 20 may be further provided near the winding roller 166, for example, between the guide roller 165 and the winding roller 166.

[0180] Here, the manufacturing apparatus 100 having a configuration suitable for manufacturing the POF 20 is exemplified and described in detail, but the manufacturing apparatus 100 can also be used when manufacturing the POF 10 .

[0181] When the POF 10 is produced, the third extrusion device 101 c for forming the reinforcing layer in the production device 100 may not be used.

[0182] In addition, when manufacturing POF 30, a further extrusion device may be added between the second extrusion device 101b and the third extrusion device 101c relative to the manufacturing device 100. The additional extrusion device may have the same structure as the second extrusion device 101b, for example. In this case, the second extrusion device 101b is used to form the first cladding layer 321, and the newly added extrusion device is used to form the second cladding layer 322. In addition, in this case, a third chamber for forming the second cladding layer 322 is provided between the first chamber 110 and the second chamber 120. That is, in the first chamber 110, the core 2 formed by the core material 1a is coated with the cladding material 1b (the first cladding material), thereby forming the cladding 3 (equivalent to the first cladding layer) covering the outer periphery of the core 2. The laminated body formed by the core 2 and the cladding 3 (equivalent to the first cladding layer) covering the outer periphery of the core 2 moves from the first chamber 110 to the third chamber, and in the third chamber, the outer periphery of the laminated body is coated with the second cladding material extruded from the extrusion device for forming the second cladding layer 322. The laminated body formed by the core 2, the cladding 3 (equivalent to the first cladding layer) covering the outer periphery of the core 2, and the second cladding layer further covering the outer periphery moves from the third chamber to the second chamber 120, and forms a coating layer in the second chamber 120.

[0183] Example

[0184] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited thereto.

[0185] (Example 1)

[0186] [Preparation of the First Fluorine-Containing Resin and the Second Fluorine-Containing Resin]

[0187] As the first fluorine-containing resin and the second fluorine-containing resin, a polymer of perfluoro-4-methyl-2-methylene-1,3-dioxolane (the compound of the above formula (M2), "PFMMD") is prepared. Perfluoro-4-methyl-2-methylene-1,3-dioxolane is synthesized by first synthesizing 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane, fluorinating it, and separating the resulting carboxylate by decarboxylation. In the polymerization of perfluoro-4-methyl-2-methylene-1,3-dioxolane, perfluorobenzoyl peroxide is used as a polymerization initiator.

[0188] The synthesis of 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane, the fluorination of 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane, the synthesis of perfluoro-4-methyl-2-methylene-1,3-dioxolane, and the polymerization of perfluoro-4-methyl-2-methylene-1,3-dioxolane are described in detail below.

[0189] <Synthesis of 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane>

[0190] Prepare a 3L three-necked flask, a thermometer, a magnetic stirrer and an isobaric dropping funnel with a water-cooled condenser, and put 139.4g (a total of 1.4 moles) of a mixture of 2-chloro-1-propanol and 1-chloro-2-propanol into a flask. The flask is cooled to 0 ° C, methyl trifluoropyruvate is slowly added thereto, and stirred for another 2 hours. After spending 1 hour to add 100mL of dimethyl sulfoxide (DMSO) and 194g of potassium carbonate thereto, stirring was continued for further 8 hours to obtain a reaction mixture. The generated reaction mixture was mixed with 1L of water, an aqueous phase was separated, and after further extraction with dichloromethane, the dichloromethane solution was mixed with an organic reaction mixture, and the solution was dried over magnesium sulfate. After the solvent was removed, 245.5g of crude product was obtained. The crude product was fractionated under reduced pressure (12 Torr) to obtain 230.9 g of purified 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane. The boiling point of the purified product was 77 to 78°C, and the yield was 77%. 19 FNMR confirmed that the obtained purified product was 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane.

[0191] HNMR (ppm): 4.2-4.6, 3.8-3.6 (CHCH2, multiplet (multiplet), 3H), 3.85-3.88 (COOCH3, multiplet, 3H), 1.36-1.43 (CCH3, multiplet, 3H)

[0192] 19 FNMR (ppm): -81.3 (CF3, s, 3F)

[0193] <Fluorination of 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane>

[0194] Inject 4L of 1,1,2-trichlorotrifluoroethane into a 10L stirred reaction tank. In the stirred reaction tank, nitrogen is flowed at a flow rate of 1340cc / min, and fluorine is flowed at a flow rate of 580cc / min, and the atmosphere is set to nitrogen / fluorine. After 5 minutes, 290g of the previously prepared 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane is dissolved in 750mL of 1,1,2-trichlorotrifluoroethane solution, and the solution is added to the reaction tank at a rate of 0.5ml / min. The reaction tank is cooled to 0°C. After taking 24 hours to add all the dioxolanes, the fluorine gas flow is stopped. After purging nitrogen, potassium hydroxide aqueous solution is added until it becomes weakly alkaline.

[0195] After removing the volatile substances under reduced pressure, the surrounding of the reaction tank was cooled, and then dried under reduced pressure at 70°C for 48 hours to obtain a solid reaction product. The solid reaction product was dissolved in 500 mL of water, and excess hydrochloric acid was added to separate it into an organic phase and an aqueous phase. The organic phase was separated and distilled under reduced pressure to obtain perfluoro-2,4-dimethyl-1,3-dioxolane-2-carboxylic acid. The boiling point of the main distillate was 103°C-106°C / 100mmHg. The fluorination yield was 85%.

[0196] <Synthesis of perfluoro-4-methyl-2-methylene-1,3-dioxolane>

[0197] The above distillate was neutralized with an aqueous potassium hydroxide solution to obtain perfluoro-2,4-dimethyl-2-carboxylic acid potassium-1,3-dioxolane. The potassium salt was vacuum dried at 70°C for 1 day. The salt was decomposed at 250°C to 280°C in a nitrogen or argon atmosphere. Condensation was performed using a cold trap cooled to -78°C to obtain perfluoro-4-methyl-2-methylene-1,3-dioxolane with a yield of 82%. The boiling point of the product is 45°C / 760 mmHg. Use 19 The product was identified by FNMR and GC-MS.

[0198] 19 FNMR: -84ppm (3F, CF3), -129ppm (2F, =CF2)

[0199] GC-MS: m / e244 (Molecular ion) 225, 197, 169, 150, 131, 100, 75, 50.

[0200] <Polymerization of perfluoro-4-methyl-2-methylene-1,3-dioxolane>

[0201] 100 g of perfluoro-4-methyl-2-methylene-1,3-dioxolane and 1 g of perfluorobenzoyl peroxide obtained by the above method were sealed in a glass tube. The glass tube was deoxygenated by freeze degassing, then filled with argon and heated at 50°C for several hours. The contents became solid, and after further heating at 70°C overnight, 100 g of a transparent rod was obtained.

[0202] The obtained transparent rod-like substance was dissolved in Fluorinert FC-75 (manufactured by Sumitomo 3M Co.), and the obtained solution was injected into a glass plate to obtain a thin film of the polymer. The obtained polymer had a glass transition temperature of 117°C and was completely amorphous. The transparent rod-like substance was dissolved in hexafluorobenzene, and chloroform was added thereto to precipitate it, thereby purifying the product. The glass transition temperature of the purified polymer was about 131°C. The polymers were used as the first fluorine-containing resin and the second fluorine-containing resin.

[0203] [Refractive index adjuster]

[0204] Chlorotrifluoroethylene oligomer (molecular weight 585) was used as the refractive index adjuster. Specifically, "DAIFLOIL #10" manufactured by DAIKIN INDUSTRIES was distilled, and only a component having a molecular weight of 585 was separated and used.

[0205] [Core material]

[0206] The first fluororesin prepared by the above method is dissolved in Vertrel XF-UP (manufactured by Chemours-Mitsui Fluoroproducts) as a solvent. The solution is filtered with a filter "LPJ-CTA-001-N3" (manufactured by ROKI TECHNO) with a pore size of 100 nm, and the filtrate is dripped into a Hastelloy container heated to 260°C to evaporate the solvent and dry and solidify it. The first fluororesin after the filtration treatment obtained by drying and solidification and the above refractive index modifier are melt-mixed at 260°C to prepare a resin composition. The concentration of the refractive index modifier in the obtained resin composition is 12% by mass. The resin composition is used as a core material.

[0207] [First cladding material]

[0208] The second fluororesin prepared by the above method is filtered in the same way as the first fluororesin in the preparation of the core material to obtain a filtered second fluororesin. The filtered second fluororesin is used as a first cladding material for forming a first cladding layer.

[0209] [Second cladding material]

[0210] "Teflon AF1600" (manufactured by Chemours-Mitsui Fluoroproducts) as a fluororesin and "Fomblin YR" (manufactured by Solvay) as a viscosity modifier are dissolved in Vertrel XF-UP (manufactured by Chemours-Mitsui Fluoroproducts) as a solvent. It should be noted that the mixing ratio of "Teflon AF1600" and "Fomblin YR" is set to "Teflon AF1600": "Fomblin YR" = 7:3 in terms of mass ratio. The obtained solution is filtered using a filter "LPA-SLF-003-N2" (manufactured by ROKI TECHNO) with a pore size of 300nm, and the filtrate is added dropwise to a Hastelloy container heated to 260°C to evaporate the solvent and dry and solidify it. The resin composition obtained by drying and solidification is used as the second cladding material.

[0211] [Reinforcement layer material]

[0212] Xylex (manufactured by SABIC, glass transition temperature: 113° C.) was used as the reinforcing layer material.

[0213] [POF]

[0214] Using the core material, the first cladding material, the second cladding material and the reinforcement layer prepared by the above method, a fiber-reinforced fiber having the same structure as that of the fiber-reinforced fiber is produced by melt spinning. Figure 3 POF 30 shown in FIG. 1 is a POF having the same structure as the POF 30 shown in FIG. Figure 4 The manufacturing device 100 shown in the figure is a device obtained by further adding an extrusion device for forming a second coating layer between the second extrusion device 101b and the third extrusion device 101c. The added extrusion device has the same structure as the second extrusion device 101b. That is, in this embodiment, the second extrusion device 101b is used to form the first coating layer 321, and the added extrusion device is used to form the second coating layer 322. The third chamber for forming the second coating layer 322 is provided between the first chamber 110 and the second chamber 120.

[0215] The melting temperature of the core material is 250° C., the melting temperature of the first cladding material is 255° C., the melting temperature of the second cladding material is 260° C., and the melting temperature of the reinforcing layer material is 240° C. In addition, the temperature of the diffuser 130 is set to 260° C. The stretching temperature of the laminate including the core, cladding (first cladding layer and second cladding layer) and reinforcing layer is 240° C.

[0216] The melt extrusion was performed at a volume ratio of 1.5 for the first cladding material, 1.5 for the second cladding material, and 50 for the reinforcing layer material relative to 1 for the core material. The diffusion time, i.e., the time it takes for the laminate to pass through the diffusion tube 130, was 960 seconds.

[0217] In the obtained POF, the core diameter was 49 μm, and the outer diameter of the reinforcing layer (that is, the outer diameter of the POF) was 235 μm. The core diameter was measured by the method described below.

[0218] [Evaluation of core diameter]

[0219] The core diameter is measured by the NFP method using light with a wavelength of 850nm in accordance with IEC60793-1-20 and IEC60793-2-40 sub-category A4h. A 6m long POF is prepared, and 850nm LED light is incident from one end. The light intensity distribution of the emitted light at a distance of 6m is measured, and the diameter at which the light intensity is 5% is calculated.

[0220] [Evaluation of Numerical Aperture (NA)]

[0221] NA is measured by the FFP method (Far Field Pattern) using light with a wavelength of 850nm in accordance with the methods of IEC60793-1-43 and IEC60793-2-40 sub-category A4h. A 6m long POF is prepared, and 850nm LED light is incident from one end. The light intensity distribution relative to the angular position of the emitted light at a distance of 6m is measured, and the NA is calculated.

[0222] [Evaluation of propagation loss]

[0223] The transmission loss is measured by the back-cut method in accordance with IEC60793-1-40. A 40m long POF is prepared and 850nm LED light is incident from one end. The light intensity of the emitted light is measured using a power meter. The POF is cut off in sequence, and the light intensity at each m is measured. The propagation loss is calculated based on the change in light intensity.

[0224] [Evaluation of frequency band]

[0225] The measurement is performed using the pulse method in accordance with IEC60793-1-41. A POF of 20 m in length is prepared, and an optical pulse is injected from one end, and the optical pulse of the emitted light at a distance of 20 m is measured. Then, the POF is cut to a length of 2 m, and an optical pulse is injected in the same manner, and the emitted pulse is measured. The transfer function is obtained by performing Fourier transformation specified in IEC60793-1-41 on the two emitted pulses, and the -3 dB frequency is obtained using the optical power.

[0226] [M 2 Evaluation of value]

[0227] M 2 The value was evaluated using the same method as that described in Japanese Patent Publication No. 2019-49658. Figure 3 The same measurement system as the measurement system for NFP and FFP shown in the figure is used to determine the beam radius W (Dσ4) defined by the second moment and the beam expansion angle θ (half angle) by the same method as the method described in paragraph 0088 of Japanese Patent Publication No. 2019-49658. Using the determined results, M is calculated using the following mathematical formula (1): 2 value.

[0228] Mathematical formula (1): M 2 =πWθ / λ

[0229] [BER's evaluation]

[0230] The BER value was evaluated using the same method as that described in Japanese Patent Application Publication No. 2019-49658. Figure 4 The BER measurement system shown is the same as the measurement system, and the BER value is calculated by the same method as the method described in paragraph 0089 of Japanese Patent Application Laid-Open No. 2019-49658.

[0231] (Example 2)

[0232] A POF was produced by the same method as in Example 1 except for the following points.

[0233] In the production of POF, the ejection amount of each material was set to a volume ratio of 1.5 for the first cladding material, 1.5 for the second cladding material, and 90 for the reinforcement material relative to 1 for the core material, and melt extrusion was performed at this volume ratio.

[0234] The diffusion tube length and the spinning speed were adjusted so that the time for the laminate to pass through the diffusion tube 130 was set to 1000 seconds.

[0235] The core diameter of the obtained POF measured by the same method as in Example 1 was 79 μm, and the outer diameter of the reinforcing layer (ie, the outer diameter of the POF) was 490 μm.

[0236] (Example 3)

[0237] Production with Figure 2 A POF having the same structure as the POF 20 shown in the figure. That is, in Example 3, a POF having a cladding layer of one layer was produced. As the cladding material, the first cladding material of Example 1 was prepared, and the second cladding material was not used. The differences between Example 3 and Example 1 are as follows. The POF of Example 3 was produced by the same method as Example 1 except for the following aspects. In the obtained POF, the core diameter measured by the same method as Example 1 was 44 μm, and the outer diameter of the reinforcement layer (i.e., the outer diameter of the POF) was 235 μm. In addition, for the obtained POF, the various characteristics were evaluated by the same method as Example 1.

[0238] The difference from Example 1 is:

[0239] In the preparation of the core material, the first fluororesin was filtered by filtering the first fluororesin solution twice with a filter "LPJ-CTA-001-N3" (manufactured by ROKI TECHNO) with a pore size of 100 nm, and then with a filter "DFA1ANDESW44" (manufactured by PALL) with a pore size of 40 nm.

[0240] The refractive index adjusting agent was filtered using a filter "DFA1ANDESW44" (manufactured by PALL) having a pore size of 40 nm.

[0241] In the production of POF, no second cladding material is used and no second cladding layer is formed.

[0242] The volume ratio of each material ejected was set to 1.5 for the first cladding material and 53 for the reinforcement layer material relative to 1 for the core material.

[0243] (Example 4)

[0244] A POF was produced by the same method as in Example 1 except for the following points.

[0245] In the preparation of the core material, the added refractive index adjusting agent was filtered using a filter "DFA1ANDESW44" (manufactured by PALL) having a pore size of 40 nm.

[0246] The length of the diffusion tube and the spinning speed were adjusted so that the time for the laminate to pass through the diffusion tube 130 was set to 480 seconds.

[0247] The core diameter of the obtained POF measured by the same method as in Example 1 was 50 μm, and the outer diameter of the reinforcing layer (ie, the outer diameter of the POF) was 235 μm.

[0248] (Example 5)

[0249] A POF was produced by the same method as in Example 1 except for the following points.

[0250] In the preparation of the core material, the synthesized first fluorine-containing resin was heated at 260° C. without being dissolved in a solvent or filtered, and melt-mixed with a refractive index adjuster to prepare a resin composition.

[0251] In the preparation of the first cladding material, the synthesized second fluorine-containing resin is used as the first cladding material as it is without being dissolved in a solvent or filtered.

[0252] The temperature of the diffusion pipe 130 was set to 265°C.

[0253] The core diameter of the obtained POF measured by the same method as in Example 1 was 50 μm, and the outer diameter of the reinforcing layer (ie, the outer diameter of the POF) was 235 μm.

[0254] (Example 6)

[0255] A POF was produced by the same method as in Example 1 except for the following points.

[0256] In the preparation of the core material and the first cladding material, the first fluororesin solution and the second fluororesin solution were filtered twice using a filter "LPJ-CTA-001-N3" (manufactured by ROKI TECHNO) with a pore size of 100 nm, and then filtered using a filter "DFA1ANDESW44" (manufactured by PALL) with a pore size of 40 nm.

[0257] The refractive index adjusting agent was filtered using a filter "DFA1ANDESW44" (manufactured by PALL) having a pore size of 40 nm.

[0258] The temperature of the diffusion pipe 130 was set to 265°C.

[0259] The length of the diffusion tube and the spinning speed were adjusted so that the time for the laminate to pass through the diffusion tube 130 was set to 1440 seconds.

[0260] In the obtained POF, the outer diameter of the core measured by the same method as in Example 1 was 48 μm, and the outer diameter of the reinforcing layer (ie, the outer diameter of the POF) was 235 μm.

[0261] (Comparative Example 1)

[0262] As the POF of Comparative Example 1, "FONTEX50" manufactured by AGC Corporation was used. By the same method as in Example 1, the evaluation of each characteristic was performed.

[0263] (Comparative Example 2)

[0264] A POF was produced by the same method as in Example 1 except for the following points.

[0265] In the production of POF, the temperature of the diffusion tube was set to 250°C.

[0266] The length of the diffusion tube and the spinning speed were adjusted so that the time for the laminate to pass through the diffusion tube 130 was set to 480 seconds.

[0267] In the obtained POF, the outer diameter of the core measured by the same method as in Example 1 was 50 μm, and the outer diameter of the reinforcing layer (ie, the outer diameter of the POF) was 235 μm.

[0268] Table 1 shows the evaluation results of POF of each example and comparative example.

[0269] [Table 1]

[0270]

[0271] The POFs of Examples 1 to 6, which have a transmission loss of 70 dB / km or more and 500 dB / km or less at a wavelength of 850 nm and a transmission band of 30 MHz·km or more and 600 MHz·km or less, can all achieve 1×10 -7 The BER of the POF of Comparative Example 1, which has a transmission loss of less than 70 dB / km, is 3.11×10 -6 , which is higher than that of the POFs of Examples 1 to 6. Although the POF of Comparative Example 2, whose transmission band is less than 30 MHz·km, has an M of more than 1.7 2 value, but the BER is 1.12×10 -5, which is higher than the POF of Examples 1 to 6. Based on these results, it was confirmed that for a POF having a length of 30 m or less and a core diameter of 30 μm or more and 100 μm or less, by satisfying a transmission loss of 70 dB / km or more and 500 dB / km or less and a transmission band of 30 MHz·km or more and 600 MHz·km or less, a POF having improved transmission quality in short-distance signal transmission can be realized.

[0272] It should be noted that, for comparison, the BER of the POF produced by the same method as in Example 2 was evaluated at a length of 40 m. The result showed that the BER was poor, 2.20×10 -2 As can be seen from the above, the present invention is a technology for effectively solving the problems arising from POF signal transmission over a short distance of 30 m or less.

[0273] Industrial Applicability

[0274] The POF of the present invention is suitable for short-distance signal transmission in a home or the like.

Claims

1. A plastic optical fiber comprising a core and a cladding arranged on the outer periphery of the core, The length of the plastic optical fiber is less than 30 m, The core has a diameter of 30 μm or more and 100 μm or less, The transmission loss of the plastic optical fiber at a wavelength of 850 nm is greater than 70 dB / km and less than 500 dB / km, The transmission band of the plastic optical fiber at a wavelength of 850 nm is greater than or equal to 30 MHz·km and less than or equal to 600 MHz·km.

2. The plastic optical fiber according to claim 1, wherein: The plastic optical fiber is of a refractive index distribution type.

3. The plastic optical fiber according to claim 1, wherein: The core comprises a first resin, The first resin is at least one selected from the group consisting of a perfluorinated resin, a partially fluorinated resin, a partially chlorinated resin, and a partially deuterated resin.

4. The plastic optical fiber according to claim 3, wherein: The first resin is at least one selected from perfluorinated resins and partially fluorinated resins.

5. The plastic optical fiber according to claim 4, wherein: The first resin comprises a fluorine-containing polymer containing a structural unit (A) represented by the following formula (1), In formula (1), R ff 1 ~R ff 4 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 7 carbon atoms, or a perfluoroalkyl ether group having 1 to 7 carbon atoms, and R ff 1 and R ff 2 Optionally linked to form a ring.

6. The plastic optical fiber according to claim 5, wherein: The fluorine-containing polymer further contains a structural unit (B) represented by the following formula (2): In formula (2), R 1 ~R 3 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms, and R 4 It represents a perfluoroalkyl group having 1 to 7 carbon atoms, the perfluoroalkyl group may have a ring structure, a part of the fluorine atoms may be substituted with a halogen atom other than a fluorine atom, and a part of the fluorine atoms in the perfluoroalkyl group may be substituted with a halogen atom other than a fluorine atom.

7. The plastic optical fiber according to claim 5, wherein: The fluorine-containing polymer further contains a structural unit (C) represented by the following formula (3): In formula (3), R 5 ~R 8 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms, the perfluoroalkyl group may have a ring structure, a part of the fluorine atoms may be substituted with a halogen atom other than a fluorine atom, and a part of the fluorine atoms in the perfluoroalkyl group may be substituted with a halogen atom other than a fluorine atom.

8. The plastic optical fiber according to claim 5, wherein: The fluorine-containing polymer further contains a structural unit (D) represented by the following formula (4), In formula (4), Z represents an oxygen atom, a single bond, or -OC(R 19 R 20 )O-,R 9 ~R 20 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms, a portion of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom, a portion of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom, a portion of the fluorine atoms in the perfluoroalkoxy group may be substituted by a halogen atom other than a fluorine atom, s and t are each independently 0 to 5, and s+t represents an integer of 1 to 6, wherein Z is -OC(R 19 R 20 )O-, s+t can be 0.

9. The plastic optical fiber according to claim 3, wherein: The core further comprises a refractive index adjuster. 10 . The plastic optical fiber according to claim 1 , further comprising a reinforcement layer disposed on an outer periphery of the cladding.