Method for producing sulfide solid electrolyte
By heating the electrolyte precursor in a high boiling point solvent, the problems of low ion conductivity of sulfide solid electrolyte in the liquid phase method are solved, and efficient and stable sulfide solid electrolyte manufacturing is achieved.
Patent Information
- Application Number
- CN202380031544.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-15
AI Technical Summary
The existing liquid phase method produces sulfide solid electrolytes with low ionic conductivity and difficulty in mass production, especially in the process of removing complexing agents, which can easily lead to deterioration of solid electrolytes and difficulty in large-scale equipment.
The electrolyte precursor is heated in a solvent with a boiling point higher than the complexing agent to remove the complexing agent, thereby improving the ionic conductivity and facilitating the device to scale up.
The efficient manufacturing and mass production of sulfide solid electrolytes with high ionic conductivity is achieved, and the problems of deterioration of solid electrolytes and low device contact efficiency are avoided.
Smart Images

Figure BDA0005064859510000221 
Figure HDA0005064859530000011 
Figure HDA0005064859530000021
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a sulfide solid electrolyte. Background Art
[0002] In recent years, with the rapid popularization of information-related devices or communication devices such as personal computers, cameras and mobile phones, the development of batteries used as their power sources has also received attention. In the past, in batteries used for such purposes, electrolytes containing flammable organic solvents were used, but by making the battery fully solid, the safety device is simplified because no flammable organic solvent is used in the battery, and the manufacturing cost and productivity are excellent. Therefore, the development of batteries in which the electrolyte is replaced by a solid electrolyte layer is carried out.
[0003] The manufacturing method of the solid electrolyte used for the solid electrolyte layer is roughly divided into a solid phase method and a liquid phase method, and the liquid phase method includes a uniform method in which the solid electrolyte material is completely dissolved in a solvent, and an inhomogeneous method in which the solid electrolyte material is not completely dissolved but a suspension is coexistent with solid and liquid. For example, as a uniform method in the liquid phase method, a method of dissolving a solid electrolyte in a solvent and reprecipitating it is known (for example, see Patent Document 1), and as an inhomogeneous method, a method of reacting a solid electrolyte raw material such as lithium sulfide in a solvent containing a polar aprotic solvent is known (for example, see Patent Documents 2 and 3, Non-Patent Document 1).
[0004] Furthermore, there are also known methods for producing a solid electrolyte comprising using a specific compound having an amino group as a complexing agent and mixing the complexing agent with a solid electrolyte raw material to prepare an electrolyte precursor (for example, see Patent Document 4), and methods for producing a solid electrolyte comprising drying a slurry containing a complexing agent and an electrolyte precursor by fluidized drying using dielectric particles (for example, see Patent Document 5).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-191899
[0008] Patent Document 2: International Publication No. 2014 / 192309
[0009] Patent Document 3: International Publication No. 2018 / 054709
[0010] Patent Document 4: International Publication No. 2020 / 105737
[0011] Patent Document 5: International Publication No. 2021 / 230189
[0012] Non-patent literature
[0013] Non-patent document 1: Chemistry of Materials, 2017, No. 29, pp. 1830-1835 Summary of the invention
[0014] Technical problem to be solved by the invention
[0015] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a sulfide solid electrolyte having high ion conductivity easily and efficiently by a liquid phase method or by mass production.
[0016] Solutions for solving the above technical problems
[0017] The method for producing the sulfide solid electrolyte of the present invention is:
[0018] A method for manufacturing a sulfide solid electrolyte, comprising:
[0019] Mixing a raw material containing lithium atoms, phosphorus atoms, sulfur atoms and halogen atoms with a complexing agent to obtain an electrolyte precursor containing material;
[0020] Next, heating is performed in a solvent having a boiling point higher than that of the complexing agent.
[0021] Effects of the Invention
[0022] According to the present invention, it is possible to provide a method for producing or mass-producing a sulfide solid electrolyte having high ion conductivity by a liquid phase method and easily and efficiently. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the X-ray diffraction spectrum of the powder obtained in Example 1.
[0024] Figure 2 This is a SEM (scanning electron microscope) photograph of the crystalline sulfide solid electrolyte obtained in Example 1.
[0025] Figure 3 These are the X-ray diffraction spectra of the powders obtained in Example 1 and Comparative Examples 1 and 2.
[0026] Figure 4 This is the X-ray diffraction spectrum of the powders obtained in Examples 1 and 2.
[0027] Figure 5 These are the X-ray diffraction spectra of the powders obtained in Examples 1, 3 and 4.
[0028] Figure 6This is a SEM (scanning electron microscope) photograph of the crystalline sulfide solid electrolyte obtained in Comparative Example 3.
[0029] Figure 7 This is the particle size distribution of the powders obtained in Examples 1 and 2 and Comparative Examples 3 and 4.
[0030] Figure 8 This is the X-ray diffraction spectrum of the powder obtained in Example 5. DETAILED DESCRIPTION
[0031] Hereinafter, an embodiment of the present invention (hereinafter sometimes referred to as "the present embodiment") is described. In addition, in this specification, the upper and lower limit values involved in the numerical ranges of "above", "below", and "to" are values that can be arbitrarily combined, and the values of the embodiments can also be used as the upper and lower limit values. In addition, preferred regulations can be adopted arbitrarily. That is, a preferred regulation can be combined with another preferred regulation or multiple regulations and adopted. It can be said that the combination of preferred substances is more preferred.
[0032] (Discovery made by the present inventors to complete the present invention)
[0033] The present inventors have conducted intensive studies to solve the above-mentioned technical problems and, as a result, have found the following matters and completed the present invention.
[0034] However, in recent years, with the goal of practical application of all-solid-state batteries, the liquid phase method has attracted attention as a method that can be synthesized easily and in large quantities in addition to its versatility and applicability.
[0035] The liquid phase method has the advantages as described above, but on the other hand, in order to dissolve the solid electrolyte, due to the decomposition and defects of a part of the solid electrolyte components during precipitation, there is a problem of difficulty in achieving high ionic conductivity compared with the solid phase method. For example, in the uniform method, since the raw materials and the solid electrolyte are temporarily completely dissolved, the components can be uniformly dispersed in the liquid. However, in the subsequent precipitation process, precipitation is carried out according to the solubility inherent to each component, so it is extremely difficult to precipitate it under the state of maintaining the dispersed state of the components. As a result, each component is separated and precipitated. In addition, in the uniform method, the affinity of the solvent and lithium becomes too strong, so even if it is dried after precipitation, it is not easy to separate the solvent. Thus, in the uniform method, there is a problem of greatly reduced ionic conductivity of the solid electrolyte. In addition, in the inhomogeneous method where solid and liquid coexist, since a part of the solid electrolyte is dissolved, there is also a problem of separation due to the elution of a specific component, and it is difficult to obtain the desired solid electrolyte.
[0036] In addition, regarding the liquid phase method (heterogeneous method), for example, in the method of producing a sulfide solid electrolyte using a complexing agent via an electrolyte precursor described in Patent Document 4, a step of removing the complexing agent is required. The present inventors have focused on a method of removing the complexing agent in the method of producing a sulfide solid electrolyte using a complexing agent via an electrolyte precursor.
[0037] In the manufacturing method described in patent document 4, the removal of the complexing agent is carried out in the following manner: after the electrolyte precursor containing material in the form of a slurry is dried under vacuum and at room temperature to form a powdered electrolyte precursor, the electrolyte precursor is heated at 120°C under vacuum (Example 1, etc.), specifically, a jacketed heater (vibration dryer, etc.) is used under vacuum to remove the complexing agent. In this way, when a complexing agent is used, the complexing agent cannot be removed from the electrolyte precursor only by drying, but a jacketed heater (vibration dryer, etc.) is used for heating. However, in such a heater, even if the complexing agent can be removed, the wall surface inside the heater locally becomes a high temperature, and sometimes the condensation of the halogen compound contained in the solid electrolyte is generated, resulting in the degradation of the solid electrolyte. Therefore, the temperature conditions when removing the complexing agent are limited, and there is room for improvement in efficiently manufacturing solid electrolytes. Furthermore, when heating is performed for removal of the complexing agent and crystallization, secondary particles formed by aggregation of primary particles having an average particle size of about 0.1 μm are generated, which increases the oil absorption of the solid electrolyte. It may be necessary to pulverize (micro-particleize) the crystallized solid electrolyte.
[0038] Furthermore, as the demand for sulfide solid electrolytes increases, there is a demand for mass production. However, in the conventional method, since heating is performed under vacuum, the complexing agent is removed in an environment where heat is transferred only by contact between the powder and the inner wall surface (heat transfer surface) of the jacket-type heater, which has a great impact on the large-scale equipment and may not be able to fully cope with it.
[0039] Regarding the removal of the complexing agent, no complexing agent is used in Patent Documents 1 to 3. Furthermore, although it is assumed that a solvent is used during the reaction of the solid electrolyte raw material, there is no research on a method for removing the solvent.
[0040] In the manufacturing method described in Patent Document 5, the slurry containing the complexing agent and the electrolyte precursor is dried by using fluidized drying of the medium particles. However, in the manufacturing method described in Patent Document 5, the operation of removing the complexing agent from the electrolyte precursor is not performed during the drying of the slurry, so the complexing agent is removed from the electrolyte precursor obtained by the drying by heating at 110° C. under vacuum in the same manner as the manufacturing method described in Patent Document 4 (Example 1, etc.), specifically, a jacketed heater (vibration dryer, etc.) is used under vacuum. Therefore, the same problem as the manufacturing method described in Patent Document 4 is generated.
[0041] Therefore, the present inventors, in particular, studied a method for removing a complexing agent from an electrolyte precursor formed by a complexing agent and a solid electrolyte raw material, and found that by heating the electrolyte precursor containing material in a solvent having a boiling point higher than that of the complexing agent, the complexing agent can be removed from the electrolyte precursor contained in the electrolyte precursor containing material. If the complexing agent is removed from the electrolyte precursor by heating in a solvent, the deterioration of the solid electrolyte caused by the contact of the powder of the solid electrolyte with the wall surface of a jacketed heater (vibration dryer, etc.) which becomes a high temperature locally can be suppressed.
[0042] Furthermore, it can be seen that since part of the solid electrolyte is dissolved, the effect of suppressing separation due to the elution of specific components can be obtained. This is a surprising effect that was not expected in an environment where the elution of specific components is easy to occur in the liquid phase. In addition, since heating can be performed in the liquid phase, it also has the advantage of being easy to cope with the large-scale device.
[0043] Based on the above findings, it was discovered that in a method for producing a sulfide solid electrolyte based on a liquid phase method (inhomogeneous method) in which a complexing agent is reacted with a solid electrolyte raw material, the complexing agent is removed from a powder of an electrolyte precursor by heating in a solvent having a boiling point higher than that of the complexing agent, thereby efficiently obtaining a sulfide solid electrolyte having high ion conductivity while adopting a liquid phase method, and mass production becomes easy.
[0044] (Various Aspects of the Present Embodiment)
[0045] The method for producing a sulfide solid electrolyte according to the first aspect of the present embodiment is as follows:
[0046] A method for manufacturing a sulfide solid electrolyte, comprising:
[0047] Mixing a raw material containing lithium atoms, phosphorus atoms, sulfur atoms and halogen atoms with a complexing agent to obtain an electrolyte precursor containing material;
[0048] Next, heating is performed in a solvent having a boiling point higher than that of the complexing agent.
[0049] In the method for producing a sulfide solid electrolyte of the present embodiment, in the electrolyte precursor containing material obtained by mixing a solid electrolyte raw material with a complexing agent, a complexing agent and a solid electrolyte raw material that do not contribute to the formation of the electrolyte precursor, and a solvent may be included together with the electrolyte precursor. In the method for producing a sulfide solid electrolyte of the present embodiment, the complexing agent can be removed from the electrolyte precursor by heating in a solvent having a boiling point higher than the boiling point of the complexing agent contained in the electrolyte precursor in the electrolyte precursor containing material (hereinafter, sometimes referred to as a "high boiling point solvent"). It is considered that if heating is performed in a solvent having a boiling point higher than the boiling point of the complexing agent, the complexing agent becomes easy to flow, and is separated from the electrolyte precursor and removed.
[0050] The electrolyte precursor is a precursor of the sulfide solid electrolyte obtained by the manufacturing method of the present embodiment, and is a substance that can become a sulfide solid electrolyte by removing the complexing agent. Here, the complexing agent refers to a reagent for complexing, that is, a reagent that can form a complex, and refers to a compound that easily forms a complex with the solid electrolyte raw material contained in the raw material content. Therefore, the electrolyte precursor is obtained by mixing the raw material content with the complexing agent, so more specifically, it can be said that it is a complex formed by the solid electrolyte raw material via the complexing agent.
[0051] The manufacturing method of this embodiment includes: heating in a high boiling point solvent after obtaining the electrolyte precursor-containing material. The heating can be performed after obtaining the electrolyte precursor-containing material, and the heating object during heating is the electrolyte precursor-containing material, and in the case of drying described later, the electrolyte precursor.
[0052] When heating the electrolyte precursor content and removing the complexing agent from the electrolyte precursor, the key point is to heat the electrolyte precursor content, especially the electrolyte precursor contained in the electrolyte precursor content, in a high boiling point solvent. Through the direct contact between the electrolyte precursor in the electrolyte precursor content and the high boiling point solvent, the complexing agent contained in the electrolyte precursor is efficiently heated and quickly removed. Therefore, the regeneration of the complex between the substance obtained by removing the complexing agent from the electrolyte precursor and the complexing agent, and the generation of impurities caused by the electrolyte precursor and the complexing agent are suppressed, so that a sulfide solid electrolyte with less impurities, high quality and high ion conductivity can be obtained.
[0053] A method for producing a sulfide solid electrolyte according to a second aspect of the present embodiment is, in the above-mentioned first aspect,
[0054] The heating temperature of the solvent is set to be higher than the boiling point of the complexing agent.
[0055] As mentioned above, the complexing agent contained in the electrolyte precursor becomes easy to flow by being heated, and is removed from the electrolyte precursor. Here, by heating the high boiling point solvent to a boiling point exceeding the complexing agent, the complexing agent volatilizes, and is therefore easily separated from the electrolyte precursor. And then, the gaseous complexing agent separated is easily separated from the high boiling point solvent and discharged outside the system, so the complexing agent separated is not easy to be retained in the high boiling point solvent. And, in addition to the complexing agent remaining in the electrolyte precursor, there is also the complexing agent retained in the high boiling point solvent, etc., which causes the regeneration of the complex obtained from the electrolyte precursor by removing the complexing agent, and the generation of impurities are suppressed, and it is easy to obtain a sulfide solid electrolyte with few impurities, high quality, and high ionic conductivity.
[0056] A method for producing a sulfide solid electrolyte according to a third aspect of the present embodiment is, in the first or second aspect,
[0057] When heating is performed in the solvent, the solvent is boiled.
[0058] By boiling the high boiling point solvent, not only is the complexing agent easily separated from the electrolyte precursor, but it is also discharged to the outside of the system together with the gas of the high boiling point solvent generated by boiling the high boiling point solvent, thereby promoting rapid separation. As a result, the regeneration of the complex with the powder obtained by removing the complexing agent from the electrolyte precursor and the generation of impurities are suppressed, and it is easy to more efficiently obtain a sulfide solid electrolyte with less impurities, high quality and high ion conductivity.
[0059] A fourth aspect of the present embodiment provides a method for producing a sulfide solid electrolyte, in the third aspect,
[0060] A solvent having a boiling point higher than that of the complexing agent is separately prepared, and a mixture of the electrolyte precursor-containing material and the separately prepared solvent is prepared and added to the solvent used for the heating.
[0061] As a method for supplying electrolyte precursors, the following method is adopted: a high boiling point solvent prepared separately from the high boiling point solvent heated in the above-mentioned heating is mixed with the electrolyte precursor containing material, and the obtained mixture is added to the high boiling point solvent used for heating in the above-mentioned heating. The details are described later, and the mixture is preferably added to the solvent after the high boiling point solvent for heating is heated, and preferably added to the solvent after the high boiling point solvent is boiled. By adopting such a method, unlike the method of pre-adding an electrolyte precursor to the heated high boiling point solvent for heating, the amount of electrolyte precursor added is slowly controlled while the electrolyte precursor is instantly heated to the target temperature. Therefore, the regeneration of the complex between the powders obtained by removing the complexing agent from the electrolyte precursor and the generation of impurities are suppressed, and it is easy to more efficiently obtain a sulfide solid electrolyte with few impurities, high quality and high ionic conductivity.
[0062] Here, the separately prepared high boiling point solvent may be the same type of solvent as the high boiling point solvent heated and boiled in the above-mentioned heating, or a different type of solvent may be used. From the viewpoint of more efficiently obtaining a sulfide solid electrolyte with less impurities, high quality, and high ion conductivity, it is preferred to use the same type of solvent.
[0063] A fifth method for producing a sulfide solid electrolyte according to the present embodiment is, in the first to fourth methods described above,
[0064] The amount of the solvent used is 20 mL or more and 2000 mL or less relative to 1 g of the supplied electrolyte precursor contained in the electrolyte precursor-containing material.
[0065] By using a high boiling point solvent in an amount within the above range, the complexing agent can be separated and removed more efficiently. Therefore, the regeneration of the complex with the powder obtained by removing the complexing agent from the electrolyte precursor and the generation of impurities can be suppressed, and it is easy to more efficiently obtain a sulfide solid electrolyte with less impurities, high quality and high ion conductivity.
[0066] Furthermore, by suppressing the amount of the high-boiling-point solvent used within a certain range, it is also possible to more easily cope with mass production.
[0067] A sixth method for producing a sulfide solid electrolyte according to the present embodiment is, in the first to fifth methods described above,
[0068] The method comprises drying the electrolyte precursor-containing material.
[0069] As described above, in the manufacturing method of the present embodiment, the key point is to heat the electrolyte precursor in a high boiling point solvent. As a previous stage, the electrolyte precursor containing the electrolyte precursor and the solvent is dried, the solvent is removed, the electrolyte precursor is separated as a powder, and the separated substance is heated in a high boiling point solvent, thereby being able to heat the electrolyte precursor more directly. Thus, by more directly heating the complexing agent contained in the electrolyte precursor, the complexing agent can be separated and removed more efficiently.
[0070] As a result, regeneration of the complex with a substance obtained by removing the complexing agent from the electrolyte precursor and generation of impurities are suppressed, and a sulfide solid electrolyte with less impurities, high quality and high ion conductivity can be easily obtained more efficiently.
[0071] On the other hand, it is obvious that in the heating under vacuum using a jacket-type heater in the conventional method, heat is transferred only by contact between the electrolyte precursor and the wall surface inside the heater, so the contact efficiency is poor and the heat conduction efficiency is low. Therefore, it can be said that according to the production method of this embodiment, it is easy to obtain a sulfide solid electrolyte more efficiently than the conventional method.
[0072] Like this, the main purpose of drying in the manufacture method of the present embodiment is to remove solvent from the electrolyte precursor containing thing, and can also remove the complexing agent that does not contribute to the formation of electrolyte precursor and remains.Therefore, in the manufacture method of the present embodiment, removing complexing agent from electrolyte precursor is not carried out by drying, but by heating in high boiling point solvent.In addition, removing complexing agent from electrolyte precursor certainly can also heat electrolyte precursor containing thing in high boiling point solvent so as to carry out.
[0073] A seventh aspect of the present embodiment provides a method for producing a sulfide solid electrolyte, in the sixth aspect,
[0074] The drying is performed under normal pressure or reduced pressure at 5° C. to 110° C.
[0075] The electrolyte precursor-containing material can be dried more efficiently to obtain a powder of the electrolyte precursor by setting the pressure condition from normal pressure to reduced pressure and the temperature condition to 5° C. to 110° C. when drying the electrolyte precursor-containing material.
[0076] An eighth aspect of the present embodiment is a method for producing a sulfide solid electrolyte, in the first to seventh aspects,
[0077] The method comprises: after heating in the solvent, further heating at a temperature higher than the heating temperature in the solvent.
[0078] By heating the electrolyte precursor in the above solvent, the complexing agent is removed from the electrolyte precursor to obtain an amorphous sulfide solid electrolyte. By further heating the electrolyte precursor at a temperature higher than the heating temperature in the solvent, a crystalline sulfide solid electrolyte can be obtained.
[0079] In the production method of the present embodiment, an amorphous sulfide solid electrolyte or a crystalline sulfide solid electrolyte can be produced as needed.
[0080] A ninth aspect of the present embodiment is a method for producing a sulfide solid electrolyte, in the first to eighth aspects,
[0081] The complexing agent is a compound having an amino group,
[0082] A tenth aspect of the present embodiment is a method for producing a sulfide solid electrolyte, wherein in the first to ninth aspects,
[0083] The complexing agent is a compound having at least two tertiary amino groups in the molecule.
[0084] In the sulfide solid electrolyte of the present embodiment, as described above, the complexing agent is a solvent having the property of forming a complex with the solid electrolyte raw material contained in the raw material content. Regarding the complexing agent, as described later, a compound having a heteroatom easily has the property of forming a complex with the solid electrolyte raw material, and is a preferred compound as a complexing agent. Among them, if it is a compound having a nitrogen atom as a heteroatom and further having a nitrogen atom in the form of an amino group, it is not only easier to form a complex, but also it is easy to introduce halogen atoms that are difficult to introduce in the formation of the complex, and it is easy to uniformly maintain the dispersed state of the solid electrolyte raw material. Therefore, it is easy to obtain a higher ionic conductivity.
[0085] In addition, if a compound having an amino group is used as a complexing agent, in addition to the above properties, it also has the property of being easily separated from the electrolyte precursor and easily removed. Therefore, the regeneration of the complex between the powder obtained by removing the complexing agent from the powder of the electrolyte precursor and the generation of impurities are suppressed, and it is easy to obtain a sulfide solid electrolyte with less impurities, high quality and high ion conductivity very efficiently.
[0086] The eleventh method of producing a sulfide solid electrolyte according to the present embodiment is, in the first to tenth methods described above,
[0087] The solvent is a hydrocarbon solvent containing no heteroatoms,
[0088] A twelfth aspect of the present embodiment is a method for producing a sulfide solid electrolyte, in the above-mentioned first to eleventh aspects,
[0089] The solvent is at least one organic solvent selected from aliphatic hydrocarbon solvents and alicyclic hydrocarbon solvents,
[0090] A thirteenth aspect of the present embodiment is a method for producing a sulfide solid electrolyte, in the twelfth aspect,
[0091] The organic solvent has 8 or more carbon atoms.
[0092] As described above, compounds having heteroatoms have the property of easily forming complexes with solid electrolyte raw materials. By using a hydrocarbon solvent that does not contain heteroatoms as a high boiling point solvent, the formation of complexes between the high boiling point solvent and the electrolyte precursor is suppressed, thereby suppressing the generation of impurities, and easily and efficiently obtaining a sulfide solid electrolyte with few impurities, high quality, and high ion conductivity.
[0093] In addition, as a high boiling point solvent, considering the suppression of the formation of impurities and the ease of selecting a solvent with a higher boiling point than the complexing agent, it is preferably at least one organic solvent selected from aliphatic hydrocarbon solvents and alicyclic hydrocarbon solvents, and the carbon number is preferably 8 or more.
[0094] A method for producing a sulfide solid electrolyte according to a fourteenth aspect of the present embodiment is, in the first to thirteenth aspects,
[0095] After heating in the solvent, no pulverization treatment is performed.
[0096] The electrolyte precursor obtained by using a complexing agent originally has a small average particle size, but as mentioned above, a jacketed heater (vibration dryer, etc.) is used for heating to remove the complexing agent and crystallize, so secondary particles are generated, and the oil absorption increases, so sometimes pulverization (micronization) is performed. However, according to the manufacturing method of this embodiment, secondary particles are not generated by using a jacketed heater (vibration dryer, etc.), so there is no need to perform pulverization (micronization) treatment.
[0097] This greatly contributes to energy saving in the production of the sulfide solid electrolyte, and enables more efficient production of the sulfide solid electrolyte.
[0098] A fifteenth aspect of the present embodiment is a method for producing a sulfide solid electrolyte, in the first to fourteenth aspects,
[0099] When heating is performed in the solvent, the complexing agent is removed from the electrolyte precursor contained in the electrolyte precursor content.
[0100] By heating in the solvent, the complexing agent can be removed from the electrolyte precursor contained in the electrolyte precursor-containing material, and the electrolyte precursor can be made into a sulfide solid electrolyte.
[0101] A sixteenth method for producing a sulfide solid electrolyte according to the present embodiment is, in the first to fifteenth methods described above,
[0102] The sulfide solid electrolyte has a sulfide crystalline lithium superion conductor region type II crystal structure.
[0103] In the manufacturing method of this embodiment, by changing the type and blending ratio of the solid electrolyte raw material contained in the raw material content, a desired sulfide solid electrolyte can be manufactured. Sulfide solid electrolytes having a sulfide crystalline lithium superion conductor region II type crystal structure are known to be sulfide solid electrolytes with extremely high ion conductivity, and are preferably used as the sulfide solid electrolytes intended to be obtained by the manufacturing method of this embodiment.
[0104] (Solid Electrolyte)
[0105] In this specification, a "solid electrolyte" refers to an electrolyte that remains solid at 25° C. in a nitrogen atmosphere. The solid electrolyte in this embodiment contains lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms, and has ion conductivity due to lithium atoms.
[0106] The “solid electrolyte” includes both amorphous solid electrolytes and crystalline solid electrolytes.
[0107] In this specification, a crystalline solid electrolyte refers to a solid electrolyte in which a peak originating from a solid electrolyte is observed in an X-ray diffraction pattern in an X-ray diffraction measurement, and is a solid electrolyte that is independent of whether or not there is a peak originating from a raw material of the solid electrolyte. That is, the crystalline solid electrolyte includes a crystal structure originating from a solid electrolyte, and may be a part of it that is a crystal structure originating from the solid electrolyte, or may be a crystal structure originating from the solid electrolyte in its entirety. Furthermore, as long as the crystalline solid electrolyte has such an X-ray diffraction pattern as described above, an amorphous solid electrolyte may also be included in a part thereof. Therefore, the crystalline solid electrolyte includes a so-called glass ceramic obtained by heating an amorphous solid electrolyte to a temperature above the crystallization temperature.
[0108] In this specification, an amorphous solid electrolyte refers to an X-ray diffraction pattern having a halo pattern in which substantially no peaks other than peaks derived from the material are observed in X-ray diffraction measurement, regardless of the presence or absence of peaks derived from the raw materials of the solid electrolyte.
[0109] [Method for producing sulfide solid electrolyte]
[0110] The method for producing the sulfide solid electrolyte of the present embodiment is as follows:
[0111] A method for manufacturing a sulfide solid electrolyte, comprising:
[0112] Mixing a raw material containing lithium atoms, phosphorus atoms, sulfur atoms and halogen atoms with a complexing agent to obtain an electrolyte precursor containing material;
[0113] Next, heating is performed in a solvent having a boiling point higher than that of the complexing agent.
[0114] [Obtaining electrolyte precursor containing material]
[0115] The manufacturing method of this embodiment includes:
[0116] A raw material-containing material including lithium atoms, phosphorus atoms, sulfur atoms, and halogen atoms is mixed with a complexing agent to obtain an electrolyte precursor-containing material.
[0117] First, the production method of this embodiment will be described starting from the raw material contents.
[0118] (Ingredients contained in raw materials)
[0119] The raw material content used in this embodiment includes lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms, and more specifically, includes the following compounds (hereinafter also referred to as "solid electrolyte raw materials"): compounds containing one or more atoms selected from the group consisting of these atoms. The raw material content used in this embodiment preferably contains two or more solid electrolyte raw materials.
[0120] Representative examples of the solid electrolyte raw material included in the raw material content include: lithium sulfide; lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide; phosphorus trisulfide (P 2 S 3 ), phosphorus pentasulfide (P 2 S 5 ) and other phosphorus sulfides; various phosphorus fluorides (PF 3 PF 5 ), various phosphorus chlorides (PC l 3 、PC l 5 , P 2 C l 4 ), various phosphorus bromides (PBr 3 , PBr 5 ), various phosphorus iodides (PI 3 , P 2 I 4 ) and other phosphorus halides; thiophosphoryl fluoride (PSF 3 ), phosphorus oxychloride (PSC l 3 ), thiophosphoryl bromide (PSBr 3 ), phosphoryl iodide (PS I 3 ), phosphoryl thiofluoride dichloride (PSC l 2 F), thiophosphoryl fluoride dibromide (PSBr 2 F) and other thiophosphoryl halides; raw materials consisting of at least two atoms selected from the above four atoms; fluorine (F 2 ), chlorine (Cl 2 ), bromine (Br 2 ), iodine (I 2 ) and other halogen monomers, preferably bromine (Br 2 ), iodine (I 2 ).
[0121] As a substance other than the above that can be used as a solid electrolyte raw material, for example, a solid electrolyte raw material containing at least one atom selected from the above four atoms and atoms other than the four atoms, more specifically, lithium compounds such as lithium oxide, lithium hydroxide, and lithium carbonate; alkali metal sulfides such as sodium sulfide, potassium sulfide, rubidium sulfide, and cesium sulfide; silicon sulfide, germanium sulfide, boron sulfide, gallium sulfide, tin sulfide (SnS, SnS 2 ), metal sulfides such as aluminum sulfide and zinc sulfide; phosphoric acid compounds such as sodium phosphate and lithium phosphate; alkali metal halides other than lithium such as sodium iodide, sodium fluoride, sodium chloride, sodium bromide and other sodium halides; metal halides such as aluminum halides, silicon halides, germanium halides, arsenic halides, selenium halides, tin halides, antimony halides, tellurium halides, bismuth halides; phosphorus oxychloride (POC l 3 ), phosphorus oxybromide (POBr 3 ) and other halogen phosphorus oxides; etc.
[0122] Among the above, preferred are: lithium sulfide; phosphorus trisulfide (P 2 S 3 ), phosphorus pentasulfide (P 2 S 2 ) and other phosphorus sulfides; fluorine (F 2 ), chlorine (Cl 2 ), bromine (Br 2 ), iodine (I 2 ) and other halogen monomers; lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide. In addition, when oxygen atoms are introduced into the solid electrolyte, phosphate compounds such as lithium oxide, lithium hydroxide, and lithium phosphate are preferred. As a combination of solid electrolyte raw materials, for example, a combination of lithium sulfide, phosphorus pentasulfide, and lithium halides, and a combination of lithium sulfide, phosphorus pentasulfide, and halogen monomers can be preferably exemplified, preferably lithium bromide and lithium iodide as lithium halides, and preferably bromine and iodine as halogen monomers.
[0123] In this embodiment, it is possible to use a PS 4 Structure of Li 3 PS 4 As part of the raw materials. Specifically, first make Li 3 PS 4 etc. and use them as raw materials.
[0124] L i 3 PS 4 The content relative to the total of the raw materials is preferably 60 to 100 mol%, more preferably 65 to 90 mol%, and further preferably 70 to 80 mol%.
[0125] In addition, when using Li 3 PS 4In the case of halogen monomers, the halogen monomers are relative to Li 3 PS 4 The content is preferably 1 to 50 mol%, more preferably 10 to 40 mol%, further preferably 20 to 30 mol%, and further preferably 22 to 28 mol%.
[0126] The lithium sulfide used in the embodiment is preferably in the form of particles.
[0127] The average particle size of lithium sulfide particles (D 50 ) is preferably 0.1 μm to 1000 μm, more preferably 0.5 μm to 100 μm, and even more preferably 1 μm to 20 μm. In this specification, the average particle size (D 50 ) is the particle size when the particle size distribution cumulative curve is drawn from the smallest particle size to 50% (volume basis) of the whole, and the volume distribution is, for example, the average particle size that can be measured using a laser diffraction / scattering particle size distribution measuring device. In addition, among the substances exemplified as the above-mentioned raw materials, it is preferred that the solid raw material has an average particle size of the same degree as the above-mentioned lithium sulfide particles, that is, the average particle size is preferably within the same range as the average particle size of the above-mentioned lithium sulfide particles.
[0128] When lithium sulfide, phosphorus pentasulfide and lithium halide are used as solid electrolyte raw materials, from the viewpoint of obtaining higher chemical stability and higher ion conductivity, the ratio of lithium sulfide to the total of lithium sulfide and phosphorus pentasulfide is preferably 70 to 80 mol%, more preferably 72 to 78 mol%, and further preferably 74 to 78 mol%.
[0129] When using lithium sulfide, phosphorus pentasulfide, lithium halide and other solid electrolyte raw materials used as needed, the content of lithium sulfide and phosphorus pentasulfide relative to the total of these raw materials is preferably 50 to 100 mol%, more preferably 55 to 85 mol%, and further preferably 60 to 75 mol%.
[0130] In addition, when lithium bromide and lithium iodide are used in combination as lithium halides, from the viewpoint of improving ionic conductivity, the ratio of lithium bromide to the total of lithium bromide and lithium iodide is preferably 1 to 99 mol%, more preferably 20 to 80 mol%, further preferably 30 to 70 mol%, and particularly preferably 40 to 60 mol%.
[0131] When a halogen monomer is used as a solid electrolyte raw material and lithium sulfide and phosphorus pentasulfide are used, the ratio of the mole number of lithium sulfide obtained by removing the same mole number of lithium sulfide as the mole number of the halogen monomer to the total mole number of lithium sulfide and phosphorus pentasulfide obtained by removing the same mole number of lithium sulfide as the mole number of the halogen monomer is preferably in the range of 60 to 90%, more preferably in the range of 65 to 85%, further preferably in the range of 68 to 82%, further preferably in the range of 72 to 78%, and particularly preferably in the range of 73 to 77%. This is because if these ratios are used, higher ion conductivity can be obtained.
[0132] Furthermore, from the same viewpoint, when lithium sulfide, phosphorus pentasulfide and a halogen monomer are used, the content of the halogen monomer relative to the total amount of lithium sulfide, phosphorus pentasulfide and the halogen monomer is preferably 1 to 50 mol%, more preferably 2 to 40 mol%, further preferably 3 to 25 mol%, and further preferably 3 to 15 mol%.
[0133] When lithium sulfide, phosphorus pentasulfide, halogen monomer and lithium halide are used, the content of the halogen monomer relative to the total amount of these (α mol %) and the content of the lithium halide relative to the total amount of these (β mol %) preferably satisfy the following formula (2), more preferably satisfy the following formula (3), further preferably satisfy the following formula (4), and further preferably satisfy the following formula (5).
[0134] 2≤2α+β≤100…(2)
[0135] 4≤2α+β≤80…(3)
[0136] 6≤2α+β≤50…(4)
[0137] 6≤2α+β≤30…(5)
[0138] When two halogens are used as monomers, if the number of moles of one halogen atom in the substance is set to A1, and the number of moles of the other halogen atom in the substance is set to A2, then A1:A2 is preferably 1:99 to 99:1, more preferably 10:90 to 90:10, further preferably 20:80 to 80:20, and further preferably 30:70 to 70:30.
[0139] In addition, when the two halogen monomers are bromine and iodine, if the number of moles of bromine is set to B1 and the number of moles of iodine is set to B2, then B1:B2 is preferably 1:99 to 99:1, more preferably 15:85 to 90:10, further preferably 20:80 to 80:20, further preferably 30:70 to 75:25, and particularly preferably 35:65 to 75:25.
[0140] (Complexing agent)
[0141] As described above, the complexing agent is a compound that easily forms a complex with the solid electrolyte raw material contained in the raw material content, for example, lithium sulfide, phosphorus pentasulfide, or Li obtained when using these, which are preferably used as solid electrolyte raw materials. 3 PS 4 , and a compound that forms a complex with a solid electrolyte raw material containing a halogen atom (hereinafter these are collectively referred to as "solid electrolyte raw material, etc.").
[0142] As the complexing agent, any complexing agent having the above-mentioned properties can be used without particular limitation, and in particular, preferably, compounds containing atoms having high affinity with lithium atoms, such as nitrogen atoms, oxygen atoms, chlorine atoms and other heteroatoms can be exemplified, and more preferably, compounds containing groups containing these heteroatoms can be exemplified. This is because these heteroatoms and groups containing the heteroatoms can coordinate (bond) with lithium.
[0143] It is believed that the heteroatoms present in the molecules of the complexing agent have a high affinity for lithium atoms and have the property of easily bonding with the solid electrolyte raw material and the like to form a complex (hereinafter also referred to as a "complex"). Therefore, it is believed that by mixing the above-mentioned solid electrolyte raw material with the complexing agent to form a complex, it is easy to uniformly maintain the dispersion state of the solid electrolyte raw material, especially the dispersion state of the halogen atoms, so that a sulfide solid electrolyte with high ion conductivity can be obtained.
[0144] Whether the complexing agent can form a complex with the solid electrolyte raw material or the like can be directly confirmed by, for example, infrared absorption spectrum measured by FT-IR analysis (diffuse reflectance method).
[0145] When tetramethylethylenediamine (hereinafter, also referred to as "TMEDA"), one of the preferred complexing agents, and lithium iodide (LiI) were stirred to obtain a powder and the complexing agent itself, the FT-IR analysis (diffuse reflectance method) showed that the FT-IR analysis ... -1 The peaks derived from CN stretching vibrations at 100 nm are different from the spectrum of TMEDA itself. In addition, it is known that the Li-TMEDA complex is formed by stirring and mixing TMEDA and lithium iodide (e.g., Aust. J. Chem., 1988, 41, especially 1925-34). Figure 2 etc.), it is not wrong to think that a LiI-TMEDA complex is formed.
[0146] In addition, for example, for the complexing agent (TMEDA) and Li 3 PS 4The powder obtained by stirring was also analyzed by FT-IR analysis (diffuse reflectance method) in the same manner as above, and it was confirmed that the -1 The peaks derived from CN stretching vibration at 100 nm are different from those of TMEDA itself, but on the other hand, they are similar to those of LiI-TMEDA complex. 3 PS 4 -TMEDA complex.
[0147] In the production method of the present embodiment, the complex obtained by mixing the raw material-containing substance and the complexing agent is used as an electrolyte precursor, and the complexing agent is removed from the powder of the electrolyte precursor using a high boiling point solvent to produce a sulfide solid electrolyte.
[0148] Preferably, the complexing agent has at least two heteroatoms capable of coordination (bonding) in the molecule, and more preferably has at least two groups containing heteroatoms in the molecule. By having at least two groups containing heteroatoms in the molecule, the solid electrolyte raw material can be bonded via at least two heteroatoms in the molecule. In addition, among the heteroatoms, nitrogen atoms are preferred, and as the group containing nitrogen atoms, amino groups are preferred. That is, amine compounds are preferred as complexing agents.
[0149] As an amine compound, as long as it has an amino group in the molecule, it can promote the formation of the complex, so there is no particular limitation, but a compound having at least two amino groups in the molecule is preferred. By having such a structure, solid electrolyte raw materials can be bonded via at least two nitrogen atoms in the molecule to form a complex.
[0150] Examples of such amine compounds include amine compounds such as aliphatic amines, alicyclic amines, heterocyclic amines and aromatic amines, and these amine compounds may be used alone or in combination of two or more.
[0151] More specifically, the aliphatic amines may be preferably and representatively exemplified: aliphatic primary diamines such as ethylenediamine, diaminopropane, and diaminobutane; aliphatic secondary diamines such as N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N'-dimethyldiaminopropane, and N,N'-diethyldiaminopropane; aliphatic tertiary diamines such as N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetraethylethylenediamine, N,N,N',N'-tetramethyldiaminopropane, N,N,N',N'-tetraethyldiaminopropane, N,N,N',N'-tetramethyldiaminobutane, N,N,N',N'-tetramethyldiaminopentane, and N,N,N',N'-tetramethyldiaminohexane; and the like. Here, in the examples in this specification, for example, if it is diaminobutane, unless otherwise specified, in addition to isomers related to the position of the amino group such as 1,2-diaminobutane, 1,3-diaminobutane, 1,4-diaminobutane, all isomers such as linear isomers and branched isomers are included in butane.
[0152] The carbon number of the aliphatic amine is preferably 2 or more, more preferably 4 or more, and further preferably 6 or more, and the upper limit is preferably 10 or less, more preferably 8 or less, and further preferably 7 or less. In addition, the carbon number of the aliphatic hydrocarbon group in the aliphatic amine is preferably 2 or more, and the upper limit is preferably 6 or less, more preferably 4 or less, and further preferably 3 or less.
[0153] The alicyclic amines may be preferably and representatively exemplified as primary alicyclic diamines such as cyclopropylene diamine and cyclohexyl diamine; secondary alicyclic diamines such as bisaminomethyl cyclohexane; tertiary alicyclic diamines such as N,N,N',N'-tetramethyl-cyclohexyl diamine and bis(ethylmethylamino)cyclohexane; and the like. Furthermore, the heterocyclic amines may be preferably and representatively exemplified as primary heterocyclic diamines such as isophorone diamine; secondary heterocyclic diamines such as piperazine and dipiperidyl propane; tertiary heterocyclic diamines such as N,N-dimethylpiperazine and bismethylpiperidyl propane; and the like.
[0154] The carbon number of the alicyclic amine or heterocyclic amine is preferably 3 or more, more preferably 4 or more, and the upper limit is preferably 16 or less, more preferably 14 or less.
[0155] In addition, as the aromatic amine, representative and preferred examples include: aromatic primary diamines such as phenylenediamine, toluene diamine, and naphthalene diamine; aromatic secondary diamines such as N-methylphenylenediamine, N,N'-dimethylphenylenediamine, N,N'-dimethylphenylphenylenediamine, N,N'-dimethylnaphthalene diamine, and N-naphthylethylenediamine; aromatic tertiary diamines such as N,N-dimethylphenylenediamine, N,N,N',N'-tetramethylphenylenediamine, N,N,N',N'-tetramethyldiaminodiphenylmethane, and N,N,N',N'-tetramethylnaphthalene diamine; and other aromatic diamines.
[0156] The number of carbon atoms in the aromatic amine is preferably 6 or more, more preferably 7 or more, and even more preferably 8 or more, and the upper limit is preferably 16 or less, more preferably 14 or less, and even more preferably 12 or less.
[0157] The amine compound used in the present embodiment may be substituted with a substituent such as an alkyl group, an alkenyl group, an alkoxy group, a hydroxyl group, a cyano group, or a halogen atom.
[0158] In addition, although diamines are exemplified as specific examples, the amine compounds that can be used in the present embodiment are obviously not limited to diamines. For example, trimethylamine, triethylamine, ethyldimethylamine, aliphatic monoamines corresponding to various diamines such as the above-mentioned aliphatic diamines, piperidine compounds such as piperidine, methylpiperidine, and tetramethylpiperidine, pyridine compounds such as pyridine, methylpyridine, morpholine compounds such as morpholine, methylmorpholine, and thiomorpholine, imidazole compounds such as imidazole, and methylimidazole, and cyclohexane compounds corresponding to the above-mentioned alicyclic diamines can also be used. In addition to alicyclic monoamines such as monoamines corresponding to the above-mentioned heterocyclic diamines, heterocyclic monoamines corresponding to the above-mentioned aromatic diamines, and aromatic monoamines corresponding to the above-mentioned aromatic diamines, for example, polyamines having three or more amino groups such as diethylenetriamine, N,N',N"-trimethyldiethylenetriamine, N,N,N',N",N"-pentamethyldiethylenetriamine, triethylenetetramine, N,N'-bis[(dimethylamino)ethyl]-N,N'-dimethylethylenediamine, hexamethylenetetramine, and tetraethylenepentamine can also be used.
[0159] Among the above, from the viewpoint of obtaining higher ion conductivity, a tertiary amine having a tertiary amino group as an amino group is preferred, a tertiary diamine having two tertiary amino groups is more preferred, a tertiary diamine having two tertiary amino groups at both terminals is further preferred, and an aliphatic tertiary diamine having tertiary amino groups at both terminals is further preferred. Among the above amine compounds, as the aliphatic tertiary diamine having tertiary amino groups at both terminals, tetramethylethylenediamine, tetraethylethylenediamine, tetramethyldiaminopropane, and tetraethyldiaminopropane are preferred. In consideration of availability, tetramethylethylenediamine and tetramethyldiaminopropane are preferred.
[0160] In addition, the same effects can be obtained by using a compound containing a nitrogen atom as a heteroatom and having a group other than an amino group, such as a nitro group, an amide group, or the like.
[0161] In the production method of the present embodiment, as the complexing agent, in addition to the compound containing the above-mentioned nitrogen atom as a heteroatom, a compound containing an oxygen atom is also preferred.
[0162] As the compound containing an oxygen atom, a compound having one or more functional groups selected from an ether group and an ester group as a group containing an oxygen atom is preferred, and a compound having an ether group is particularly preferred. That is, as the complexing agent containing an oxygen atom, an ether compound is particularly preferred.
[0163] Examples of the ether compound include ether compounds such as aliphatic ether, alicyclic ether, heterocyclic ether and aromatic ether, and these ether compounds may be used alone or in combination of two or more.
[0164] More specifically, the aliphatic ethers include monoethers such as dimethyl ether, diethyl ether, diisopropyl ether, dibutyl ether, and tert-butyl methyl ether; diethers such as dimethoxymethane, dimethoxyethane, diethoxymethane, and diethoxyethane; polyethers having three or more ether groups such as diethylene glycol dimethyl ether (diglyme) and triethylene glycol dimethyl ether (triglyme); and ethers containing hydroxyl groups such as diethylene glycol and triethylene glycol.
[0165] The carbon number of the aliphatic ether is preferably 2 or more, more preferably 3 or more, and even more preferably 4 or more, and the upper limit is preferably 10 or less, more preferably 8 or less, and even more preferably 6 or less.
[0166] The carbon number of the aliphatic hydrocarbon group in the aliphatic ether is preferably 1 or more, and the upper limit is preferably 6 or less, more preferably 4 or less, and further preferably 3 or less.
[0167] Examples of the alicyclic ether include ethylene oxide, propylene oxide, tetrahydrofuran, tetrahydropyran, dimethoxytetrahydrofuran, cyclopentyl methyl ether, dioxane, dioxolane, and the like. Examples of the heterocyclic ether include furan, benzofuran, benzopyran, dioxene, dioxin, morpholine, methoxyindole, and hydroxymethyldimethoxypyridine.
[0168] The carbon number of the alicyclic ether or heterocyclic ether is preferably 3 or more, more preferably 4 or more, and the upper limit is preferably 16 or less, more preferably 14 or less.
[0169] Examples of the aromatic ether include methyl phenyl ether (anisole), ethyl phenyl ether, dibenzyl ether, diphenyl ether, benzyl phenyl ether and naphthyl ether.
[0170] The number of carbon atoms in the aromatic ether is preferably 7 or more, more preferably 8 or more, and the upper limit is preferably 16 or less, more preferably 14 or less, and further preferably 12 or less.
[0171] The ether compound used in the present embodiment may be substituted with a substituent such as an alkyl group, an alkenyl group, an alkoxy group, a hydroxyl group, a cyano group, or a halogen atom.
[0172] From the viewpoint of obtaining higher ion conductivity, among the above ether compounds, aliphatic ethers are preferred, and dimethoxyethane and tetrahydrofuran are more preferred.
[0173] Examples of the ester compound include ester compounds such as aliphatic esters, alicyclic esters, heterocyclic esters and aromatic esters, and these ester compounds may be used alone or in combination of two or more.
[0174] More specifically, the aliphatic esters include formic acid esters such as methyl formate, ethyl formate and triethyl formate; acetates such as methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate and isobutyl acetate; propionic acid esters such as methyl propionate, ethyl propionate, propyl propionate and butyl propionate; oxalic acid esters such as dimethyl oxalate and diethyl oxalate; malonic acid esters such as dimethyl malonate and diethyl malonate; and succinic acid esters such as dimethyl succinate and diethyl succinate.
[0175] The carbon number of the aliphatic ester is preferably 2 or more, more preferably 3 or more, and further preferably 4 or more, and the upper limit is preferably 10 or less, more preferably 8 or less, and further preferably 7 or less. In addition, the carbon number of the aliphatic hydrocarbon group in the aliphatic ester is preferably 1 or more, more preferably 2 or more, and the upper limit is preferably 6 or less, more preferably 4 or less, and further preferably 3 or less.
[0176] Examples of the alicyclic esters include methyl cyclohexanecarboxylate, ethyl cyclohexanecarboxylate, dimethyl cyclohexanedicarboxylate, dibutyl cyclohexenedicarboxylate, and dibutyl cyclohexenedicarboxylate. Examples of the heterocyclic esters include methyl pyridinecarboxylate, ethyl pyridinecarboxylate, propyl pyridinecarboxylate, methyl pyrimidinecarboxylate, ethyl pyrimidinecarboxylate, and lactones such as acetyl lactone, propiolactone, butyrolactone, and valerolactone.
[0177] The carbon number of the alicyclic ester or heterocyclic ester is preferably 3 or more, more preferably 4 or more, and the upper limit is preferably 16 or less, more preferably 14 or less.
[0178] Examples of the aromatic ester include benzoic acid esters such as methyl benzoate, ethyl benzoate, propyl benzoate, and butyl benzoate; phthalic acid esters such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, benzyl butyl phthalate, and dicyclohexyl phthalate; and trimellitic acid esters such as trimethyl trimellitate, triethyl trimellitate, tripropyl trimellitate, tributyl trimellitate, and trioctyl trimellitate.
[0179] The number of carbon atoms in the aromatic ester is preferably 8 or more, more preferably 9 or more, and the upper limit is preferably 16 or less, more preferably 14 or less, and further preferably 12 or less.
[0180] The ester compound used in the present embodiment may be substituted with a substituent such as an alkyl group, an alkenyl group, an alkoxy group, a hydroxyl group, a cyano group, or a halogen atom.
[0181] From the viewpoint of obtaining higher ion conductivity, among the above ester compounds, aliphatic esters are preferred, acetates are more preferred, and ethyl acetate is particularly preferred.
[0182] Regarding the amount of complexing agent added, from the viewpoint of efficiently forming a complex, the molar ratio of the amount of complexing agent added to the total molar amount of lithium atoms contained in the raw material content is preferably 0.1 to 2.0, more preferably 0.5 to 1.5, further preferably 0.8 to 1.2, and most preferably 1.0.
[0183] (mix)
[0184] In the production method of the present embodiment, the above-mentioned solid electrolyte raw material and the complexing agent are mixed.
[0185] In the present embodiment, the form of the mixed solid electrolyte raw material and the complexing agent can be any one of solid and liquid, but usually the solid electrolyte raw material comprises a solid and the complexing agent is a liquid, therefore usually the solid electrolyte raw material is present in the form of the liquid complexing agent and mixed. In addition, when mixing raw materials and complexing agents, solvents can be further mixed as needed. Below, in the description about the mixing of raw materials and complexing agents, in the absence of special instructions, the complexing agent also includes a solvent added as needed.
[0186] The method of mixing the solid electrolyte raw material and the complexing agent is not particularly limited, as long as the solid electrolyte raw material and the complexing agent are put into a device capable of mixing the solid electrolyte raw material and the complexing agent and mixed. For example, if the solid electrolyte raw material is gradually added after the complexing agent is supplied to the tank and the stirring blade is operated, a good mixing state of the solid electrolyte raw material can be obtained, and the dispersibility of the raw material is improved, so it is preferred.
[0187] However, when a halogen monomer is used as a solid electrolyte raw material, the solid electrolyte raw material is sometimes not solid. Specifically, at normal temperature and pressure, fluorine and chlorine become gases, and bromine becomes liquid. In such a case, for example, when the solid electrolyte raw material is liquid, it can be supplied to the tank together with the complexing agent separately from other solid solid electrolyte raw materials. In addition, when the solid electrolyte raw material is gas, it can be supplied in a manner of blowing into a substance obtained by adding a solid solid electrolyte raw material to a complexing agent.
[0188] The manufacturing method of the present embodiment is characterized in that it includes mixing solid electrolyte raw materials and complexing agents. That is, the solid electrolyte raw materials are mixed with the complexing agent, and there is no need to crush them. Therefore, it is also possible to manufacture by not using a method in which a medium-type pulverizer such as a ball mill, a bead mill, etc. is usually referred to as a pulverizer for the purpose of crushing the solid electrolyte raw materials. In the manufacturing method of the present embodiment, it is only necessary to simply mix the solid electrolyte raw materials with the complexing agent, and the solid electrolyte raw materials and the complexing agent contained in the raw material content are mixed to form a complex, i.e., an electrolyte precursor. In addition, in order to shorten the mixing time for obtaining the complex or to perform micronization, the mixture of the raw material and the complexing agent can also be crushed by a pulverizer, but as described above, it is preferred not to use a pulverizer.
[0189] On the other hand, the electrolyte precursor may be pulverized by a pulverizer.
[0190] As a device for mixing the solid electrolyte raw material with the complexing agent, for example, a mechanical stirring mixer with stirring blades in a tank can be exemplified. The mechanical stirring mixer can exemplify a high-speed stirring type mixer, a double-arm type mixer, etc., and from the viewpoint of improving the uniformity of the solid electrolyte raw material in the mixture of the solid electrolyte raw material and the complexing agent and obtaining higher ionic conductivity, it is preferred to use a high-speed stirring type mixer. In addition, as a high-speed stirring type mixer, a vertical axis rotating type mixer, a horizontal axis rotating type mixer, etc. can be exemplified, and any type of mixer can also be used.
[0191] As the shape of the stirring blade used in the mechanical stirring mixer, anchor type, blade type, arm type, belt type, multi-stage blade type, two-arm type, bucket type, biaxial blade type, flat blade type, C-type blade type etc. can be exemplified, from the viewpoint of improving the uniformity of solid electrolyte raw materials, obtaining higher ionic conductivity, preferably use bucket type, flat blade type, C-type blade type. In addition, in the mechanical stirring mixer, preferably set the circulation line that returns to the inside of the mixer again after the stirring object is discharged to the outside of the mixer. Thus, the raw materials with heavier specific gravity such as lithium halides will not precipitate and will not be stirred by retention, and more uniform mixing can be carried out.
[0192] Although the location of the circulation line is not particularly limited, it is preferably located at a location where the liquid is discharged from the bottom of the mixer and returned to the upper part of the mixer. Thus, the solid electrolyte raw material that is easy to precipitate is easily stirred evenly with the convection of the circulation. Furthermore, the return port is preferably located below the liquid surface of the stirring object. Thus, it is possible to suppress liquid splashing and cause the stirring object to adhere to the wall surface inside the mixer.
[0193] The temperature conditions for mixing the solid electrolyte raw material and the complexing agent are not particularly limited, and are, for example, -30 to 100°C, preferably -10 to 50°C, and more preferably about room temperature (23°C) (for example, about room temperature ±5°C). In addition, the mixing time is about 0.1 to 150 hours, and from the viewpoint of more uniform mixing and obtaining higher ion conductivity, it is preferably 1 to 120 hours, more preferably 4 to 100 hours, and even more preferably 8 to 80 hours.
[0194] By mixing the solid electrolyte raw material with the complexing agent, a complex is formed by the above-mentioned solid electrolyte raw material and the complexing agent. More specifically, it can be considered that the complex is obtained by the action of the lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms contained in the solid electrolyte raw material and the complexing agent, and these atoms are bonded via the complexing agent and / or directly bonded to each other without the complexing agent. That is, in the manufacturing method of this embodiment, the complex obtained by mixing the solid electrolyte raw material with the complexing agent can also be said to be composed of the complexing agent, lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms.
[0195] The complex obtained in this embodiment is not a complex completely dissolved in the complexing agent as a liquid, but is generally solid, so a suspension in which the complex is suspended in the complex and a solvent added as needed can be obtained. Therefore, the method for manufacturing a solid electrolyte in this embodiment is equivalent to a so-called inhomogeneous system in a liquid phase method.
[0196] (Solvent)
[0197] In the present embodiment, a solvent may be further added when the solid electrolyte raw material and the complexing agent are mixed.
[0198] When a complex as a solid is formed in a complexing agent as a liquid, if the complex is easily dissolved in the complexing agent, separation of components may sometimes occur. Therefore, by using a solvent that does not dissolve the complex, the elution of the components in the electrolyte precursor can be suppressed. In addition, by using a solvent to mix the solid electrolyte raw material and the complexing agent, the complex formation can be promoted, and each main component is more widely present, and the dispersed state of the solid electrolyte raw material, especially the dispersed state of the halogen atoms, can be obtained. The electrolyte precursor remains uniform, so the result is easy to play the effect of obtaining high ionic conductivity.
[0199] The method for manufacturing the solid electrolyte of the present embodiment is a so-called inhomogeneous method, and it is preferred that the complex is not completely dissolved and precipitated relative to the complexing agent as a liquid. By adding a solvent, the solubility of the complex can be adjusted. In particular, halogen atoms are easily eluted from the complex, so by adding a solvent to suppress the elution of halogen atoms, a desired complex can be obtained. As a result, it is easy to obtain a sulfide solid electrolyte with high ionic conductivity through an electrolyte precursor in which components such as a solid electrolyte raw material, especially a solid electrolyte raw material containing halogen atoms, are uniformly dispersed.
[0200] As a solvent having such properties, a solvent having a solubility parameter of 10 or less can be preferably mentioned. In the present specification, the solubility parameter is described in various documents, such as "Chemical Handbook" (published in 2004, 5th revised edition, Maruzen Co., Ltd.), and is a value δ ((ca l / cm 3 ) 1 / 2 ), also known as Hildebrand parameter, SP value.
[0201] [Number 1]
[0202]
[0203] (In mathematical formula (1), ΔH is the molar heat of vaporization, R is the gas constant, T is the temperature, and V is the molar volume.)
[0204] By using a solvent with a solubility parameter of less than 10, it can be set to be relatively difficult to dissolve compared with the above-mentioned complexing agent, such as raw materials containing halogen atoms such as halogen atoms, lithium halides, and components containing halogen atoms (for example, aggregates obtained by bonding lithium halides with complexing agents) of solid electrolyte raw materials, particularly halogen atoms, and the like. Therefore, it is particularly easy to fix halogen atoms in the complex, and halogen atoms are present in the obtained electrolyte precursor and then in the solid electrolyte in a good dispersed state, and it is easy to obtain a solid electrolyte with high ionic conductivity. That is, the solvent used in the present embodiment preferably has the property of insoluble complexes. From the same viewpoint as it, the solubility parameter of the solvent is preferably less than 9.5, more preferably less than 9.0, and further preferably less than 8.5.
[0205] As the solvent used in the present embodiment, more specifically, a wide range of solvents that have been used in the manufacture of solid electrolytes can be used, for example, hydrocarbon solvents such as aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, and aromatic hydrocarbon solvents; alcohol solvents, ester solvents, aldehyde solvents, ketone solvents, ether solvents with a carbon number of 4 or more on one side, solvents containing carbon atoms and heteroatoms, etc.; and among these, it is preferred to appropriately select and use solvents having a solubility parameter in the above range.
[0206] More specifically, examples include aliphatic hydrocarbon solvents such as hexane (7.3), pentane (7.0), 2-ethylhexane, heptane (7.4), octane (7.5), decane, undecane, dodecane, and tridecane; alicyclic hydrocarbon solvents such as cyclohexane (8.2) and methylcyclohexane; benzene, toluene (8.8), xylene (8.8), mesitylene, ethylbenzene (8.8), tert-butylbenzene, trifluoromethylbenzene, nitrobenzene, chlorobenzene (9.5), chlorotoluene ( 8.8), aromatic hydrocarbon solvents such as bromobenzene; alcohol solvents such as ethanol (12.7), butanol (11.4); aldehyde solvents such as formaldehyde, acetaldehyde (10.3), dimethylformamide (12.1); ketone solvents such as acetone (9.9), methyl ethyl ketone; ether solvents such as dibutyl ether, cyclopentyl methyl ether (8.4), tert-butyl methyl ether, anisole; solvents containing carbon atoms and heteroatoms such as acetonitrile (11.9), dimethyl sulfoxide, carbon disulfide, etc. In addition, the values in parentheses in the above examples are SP values.
[0207] In addition, the above examples are only examples, and solvents having isomers may also include all isomers. In addition, if it is a solvent substituted by a halogen atom, an alicyclic hydrocarbon solvent, or an aromatic hydrocarbon solvent, it may also include a solvent substituted by an aliphatic group such as an alkyl group.
[0208] Among these solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, and ether solvents are preferred. From the viewpoint of obtaining high ion conductivity more stably, heptane, cyclohexane, toluene, ethylbenzene, diethyl ether, diisopropyl ether, dibutyl ether, dimethoxyethane, cyclopentyl methyl ether, tert-butyl methyl ether, and anisole are more preferred. Diethyl ether, diisopropyl ether, and dibutyl ether are further preferred. Diisopropyl ether and dibutyl ether are further preferred, and cyclohexane is particularly preferred. As the solvent used in this embodiment, the organic solvents exemplified above and organic solvents different from the above-mentioned complexing agents are preferred. In this embodiment, these solvents can be used alone or in combination.
[0209] 〔dry〕
[0210] The production method of this embodiment may include drying the electrolyte precursor-containing material after obtaining the electrolyte precursor-containing material.
[0211] When removing the complexing agent, the electrolyte precursor obtained by drying the electrolyte precursor-containing material is heated in a high-boiling-point solvent. This allows the electrolyte precursor to be heated more directly, and thus the complexing agent can be separated and removed more efficiently.
[0212] As a drying method, there can be mentioned filtration using a glass filter, etc., solid-liquid separation by decantation, solid-liquid separation using a centrifuge, etc. As solid-liquid separation, specifically, the suspension is transferred to a container, and after solid precipitation, the complexing agent and the solvent added as needed are removed by decantation to become the supernatant, or filtration using a glass filter having a pore size of about 10 to 200 μm, preferably 20 to 150 μm, is easier.
[0213] In addition, it is also possible to use a dryer etc. to dry by heating. The drying of the electrolyte precursor containing material can be carried out under any pressure conditions under pressure, normal pressure and reduced pressure, preferably under normal pressure or under reduced pressure. In particular, if it is considered to dry at a lower temperature, it is preferably dried under reduced pressure, further under vacuum, using a vacuum pump etc.
[0214] As the temperature condition for drying, it can be carried out at a temperature above the boiling point of the solvent. Since the specific temperature condition can be changed according to the type of complexing agent and solvent used, it is impossible to generalize, but it is preferably above 5°C, more preferably above 10°C, and further preferably above 15°C, and the upper limit is preferably below 110°C, more preferably below 85°C, and further preferably below 70°C.
[0215] In addition, as described above, the pressure condition is preferably set at normal pressure or reduced pressure. When set at reduced pressure, specifically, it is preferably below 85 kPa, more preferably below 80 kPa, and further preferably below 70 kPa. The lower limit may be vacuum (0 kPa). Considering the ease of adjusting the pressure, it is preferably above 1 kPa, more preferably above 2 kPa, and further preferably above 3 kPa.
[0216] In the production method of the present embodiment, when drying is performed, the drying may be performed while heating after the above-mentioned solid-liquid separation.
[0217] In addition, in the manufacturing method of the present embodiment, drying may be performed or not. That is, in the manufacturing method of the present embodiment, the heating object heated in the high boiling point solvent may be an electrolyte precursor containing material or an electrolyte precursor obtained by drying. Moreover, as described above, since the electrolyte precursor can be heated more directly, the electrolyte precursor is preferably used as the heating object.
[0218] 〔Heating in solvent〕
[0219] The manufacturing method of this embodiment includes:
[0220] After the electrolyte precursor-containing material is obtained, it is heated in a solvent having a boiling point higher than that of the complexing agent.
[0221] The electrolyte precursor-containing material obtained in the step of obtaining the electrolyte precursor-containing material is further heated in a high boiling point solvent after the above-mentioned drying, thereby removing the complexing agent from the electrolyte precursor, that is, removing the complexing agent from the complex formed by the solid electrolyte raw material and the complexing agent, thereby obtaining a sulfide solid electrolyte. This phenomenon can also be called "complex decomposition" because the complex (electrolyte precursor) is decomposed, and can also be called "decomplexation" because the complexing agent is separated from the complex (electrolyte precursor).
[0222] (Solvent having a boiling point higher than that of the complexing agent)
[0223] As the solvent (high boiling point solvent) having a boiling point higher than that of the complexing agent used in the manufacturing method of the present embodiment, there is no particular limitation as long as it is a solvent having a boiling point higher than that of the complexing agent contained in the electrolyte precursor. However, as described above, considering that the solvent having a heteroatom has the property of easily forming a complex with the solid electrolyte raw material, the high boiling point solvent is preferably a hydrocarbon solvent that does not contain a heteroatom.
[0224] As the hydrocarbon solvent, any solvent having a boiling point higher than that of the complexing agent can be selected from the organic solvents exemplified as solvents that can be used in the step of obtaining the above-mentioned electrolyte precursor-containing material. Preferably, it is an aliphatic hydrocarbon solvent, an alicyclic hydrocarbon solvent, or an aromatic hydrocarbon solvent, and more preferably an aliphatic hydrocarbon solvent or an alicyclic hydrocarbon solvent.
[0225] As for the carbon number of the high boiling point solvent, if it is considered that it is easy to have a boiling point higher than the boiling point of the complexing agent, preferably an aliphatic hydrocarbon solvent with a carbon number of 8 or more, more preferably 9 or more, and the upper limit is preferably 24 or less, more preferably 20 or less, and further preferably 16 or less.
[0226] As the aliphatic hydrocarbon solvent preferably used as the high boiling point solvent, for example, octane, 2-ethylhexane, decane, undecane, dodecane, tridecane and the like aliphatic hydrocarbon solvents can be mentioned. In addition, these examples are only examples, 2-ethylhexane is an isomer of octane, but for such a solvent having isomers, all isomers can also be included. In addition, solvents obtained by substitution with halogen atoms such as perfluorooctane can also be included.
[0227] In addition, as alicyclic hydrocarbon solvents preferably used as high boiling point solvents, for example, representative and preferred examples include cyclopentane hydrocarbon solvents such as trimethylcyclopentane (C8, 105°C), methylethylcyclopentane (C8, 149°C), propylcyclopentane (C8, unknown), and butylcyclopentane (C9, 157°C); dimethylcyclohexane (C8, 118-120°C), ethylcyclohexane (C8, 130-132°C), propylcyclopentane (C8, unknown), and butylcyclopentane (C9, 157°C); Cyclohexane hydrocarbon solvents such as cyclohexane (C9, 155°C), isopropylcyclohexane (C9, 155°C), and butylcyclohexane (C10, 178-180°C); cycloheptane hydrocarbon solvents such as methylcycloheptane (C8, 145°C) and ethylcycloheptane (C9, 145°C); cyclooctane hydrocarbon solvents such as cyclooctane (C8, 151°C) and dimethylcyclooctane (C10, 158-159°C); cyclononane, cyclodecane, etc. In addition, these examples are only examples, and solvents having isomers such as isopropylcyclohexane relative to propylcyclohexane may also include all isomers. In addition, if it is a solvent substituted with a halogen atom or an alicyclic hydrocarbon solvent, it may also include a solvent substituted with an aliphatic group such as an alkyl group.
[0228] As the high boiling point solvent, among the solvents exemplified above, one kind may be used alone or two or more kinds may be used in combination.
[0229] (heating)
[0230] In the production method of this embodiment, the electrolyte precursor-containing material is heated in a high boiling point solvent, or the electrolyte precursor is heated when the above drying is performed (hereinafter, these are also collectively referred to as "electrolyte precursor-containing material, etc."), thereby removing the complexing agent from the electrolyte precursor.
[0231] The heating conditions for the high boiling point solvent are not particularly limited as long as the complexing agent is heated to such an extent that the complexing agent can be easily fluidized and separated from the electrolyte precursor and removed.
[0232] The heating temperature of the high boiling point solvent can be changed according to the pressure conditions, so it cannot be generalized. If the boiling point of the complexing agent is used as a reference, it is preferably -50°C or higher relative to the boiling point of the complexing agent. From the viewpoint of more efficient removal of the complexing agent, it is preferably 0°C (i.e., the boiling point of the complexing agent) or higher, and more preferably higher than 0°C (i.e., the boiling point of the complexing agent). From the viewpoint of more stable removal of the complexing agent, it is preferably 1°C or higher relative to the boiling point of the complexing agent, more preferably 3°C or higher, further preferably 5°C or higher, and further preferably 10°C or higher.
[0233] Under the heating condition of the above-mentioned high boiling point solvent, from the viewpoint of more efficiently removing the complexing agent, it is effective to exceed the boiling point of the complexing agent. This is because, by being heated to the boiling point exceeding the complexing agent, the high boiling point solvent is heated to the boiling point exceeding the complexing agent as mentioned above, the complexing agent volatilizes, and is therefore easily separated from the electrolyte precursor.
[0234] In addition, as the heating condition of the high boiling point solvent, the high boiling point solvent is preferably boiled. That is, it is preferred to make the high boiling point solvent become more than the boiling point of the high boiling point solvent. By boiling the high boiling point solvent, as mentioned above, not only the complexing agent is easily separated from the electrolyte precursor, but also the gas of the high boiling point solvent generated by boiling the high boiling point solvent is discharged outside the system, so rapid separation is promoted.
[0235] The heating conditions for the high boiling point solvent can be changed according to the pressure conditions as described above, and therefore cannot be generalized, but are preferably 60° C. or higher, more preferably 65° C. or higher, further preferably 70° C. or higher, and further preferably 75° C. or higher, and the upper limit is preferably 130° C. or lower, more preferably 120° C. or lower, and further preferably 115° C. or lower. If heated within the above temperature range, the complexing agent can be removed efficiently.
[0236] About the heating conditions of high boiling point solvent, as pressure condition, preferably below 100kPa, more preferably below 85kPa, further preferably below 70kPa, as lower limit can be vacuum (0KPa), if considering the ease of adjusting pressure, then preferably above 1kPa, more preferably above 2kPa, further preferably above 3kPa. If pressure condition is within the above range, then heating condition can be made gentle, can suppress the enlargement of device.
[0237] (Heating method)
[0238] The method of heating the electrolyte precursor-containing material etc. in a high boiling point solvent is not particularly limited as long as the heating can be performed in the high boiling point solvent. For example, the electrolyte precursor-containing material etc. may be supplied to the heated high boiling point solvent, or the electrolyte precursor-containing material etc. may be supplied to the high boiling point solvent and then heated.
[0239] Alternatively, for example, a high boiling point solvent may be prepared separately from the high boiling point solvent for heating, the electrolyte precursor-containing material and the separately prepared high boiling point solvent may be mixed to prepare a mixture, and the mixture may be added to the high boiling point solvent used for heating the electrolyte precursor-containing material.
[0240] In this case, the mixture can be added to the solvent after the high boiling point solvent for the heating of the electrolyte precursor containing the thing etc. is heated, or the mixture can be added to the boiling solvent. In addition, the mixture can be added to the high boiling point solvent for the heating of the electrolyte precursor containing the thing etc. and then heated, or it can be heated to make it boil. In either case, from the viewpoint of more efficiently removing the complexing agent, it is preferred that the high boiling point solvent for heating is boiled.
[0241] As the content of the electrolyte precursor in the mixture of the electrolyte precursor containing material and the high boiling point solvent prepared separately, it is preferably 1% by mass or more, more preferably 5% by mass or more, more preferably 10% by mass or more, and more preferably 20% by mass or more, and the upper limit is preferably 50% by mass or less, and more preferably 40% by mass or less. If the content is within the above range, the mixture is easy to handle and can be easily added to the high boiling point solvent for heating.
[0242] As a high boiling point solvent prepared separately from the high boiling point solvent for heating (a high boiling point solvent for forming a mixture containing an electrolyte precursor), it is sufficient to appropriately select and use the solvents exemplified as the high boiling point solvent for heating. The same type of solvent as the high boiling point solvent for heating can be used, or a different type of solvent can be used. From the perspective of more efficiently obtaining a sulfide solid electrolyte with less impurities, high quality, and high ion conductivity, it is preferred to use the same type of solvent. If the same type of solvent is used, recycling based on the separation and purification treatment of the solvent also becomes easy.
[0243] In the manufacturing method of this embodiment, the amount of the high boiling point solvent used for heating is preferably 20 mL or more, more preferably 100 mL or more, and further preferably 150 mL or more, relative to the supply amount of 1 g of the electrolyte precursor contained in the electrolyte precursor-containing material, and the upper limit is preferably 2000 mL or less, more preferably 1500 mL or less, and further preferably 1000 mL or less. If the amount of the high boiling point solvent used for heating is within the above range, a sulfide solid electrolyte with less impurities, high quality, and high ion conductivity can be obtained more efficiently, and the waste treatment of the solvent also becomes easy.
[0244] Since the high boiling point solvent for heating is also heated, a part of it sometimes evaporates and decreases. On the other hand, it can also be said that the amount of the high boiling point solvent for heating is preferably an amount greater than a certain amount relative to the supply amount of the electrolyte precursor. In the manufacturing method of the present embodiment, when the high boiling point solvent is reduced during heating, it is preferred to add a high boiling point solvent. By adding a high boiling point solvent, the reduced high boiling point solvent can be supplemented, and a sulfide solid electrolyte with less impurities, high quality and high ion conductivity can be obtained more efficiently.
[0245] The method of adding the high boiling point solvent is not particularly limited, and as described above, for example, the high boiling point solvent may be added alone or as a mixture of the high boiling point solvent and the electrolyte precursor-containing material.
[0246] (Content of complexing agent)
[0247] By heating in the above solvent, the complexing agent can be removed from the electrolyte precursor, and the electrolyte precursor becomes an amorphous sulfide solid electrolyte, but the complexing agent cannot be completely removed from the electrolyte precursor, and as a result, the complexing agent may remain in the amorphous sulfide solid electrolyte. In this case, the content of the complexing agent contained in the sulfide solid electrolyte is preferably 0% by mass, that is, the complexing agent is not contained at all, but from the viewpoint of efficiently obtaining a sulfide solid electrolyte with high ion conductivity, it is usually 20% by mass or less, and further 17.5% by mass or less, 15% by mass or less, 10% by mass or less, and the lower limit is about 0.1% by mass or more.
[0248] In addition, similarly to the complexing agent, a high boiling point solvent may remain. In this case, the content of the high boiling point solvent is also in the same numerical range as the content of the complexing agent.
[0249] (Constant speed drying period and deceleration drying period)
[0250] When heating is performed in a solvent in the production method of the present embodiment, it can be divided into two periods according to the temperature of the electrolyte precursor and the removal status of the complexing agent.
[0251] The first period is the constant rate drying period, during which the entire surface of the electrolyte precursor powder is covered with the complexing agent, the surface and center temperatures of the electrolyte precursor remain the same, and the amount of the complexing agent contained in the electrolyte precursor decreases linearly over time. During the constant rate drying period, the complexing agent contained in the electrolyte precursor reaches the limit content, and the content of the complexing agent is generally reduced to about 25% by mass.
[0252] The second period is the deceleration drying period. After the constant rate drying period, the surface temperature of the electrolyte precursor rises to the temperature of the high boiling point solvent, and the center temperature of the powder gradually rises, eventually approaching the temperature of the high boiling point solvent. During the deceleration drying period, the complexing agent contained in the electrolyte precursor reaches an equilibrium content rate, and the content of the complexing agent does not further decrease at this temperature. The content of the complexing agent contained in the electrolyte precursor after the deceleration drying period is reduced to the numerical range described as the content of the complexing agent contained in the above-mentioned sulfide solid electrolyte.
[0253] In the manufacturing method of the present embodiment, when heating is performed in a solvent, it is preferably performed by heating in a high boiling point solvent, but a part of the step of heating in a solvent may also be performed by heating in a high boiling point solvent. When a part of the step of heating in a solvent is performed by heating in a high boiling point solvent, it is preferably performed by heating in a high boiling point solvent at least during the constant rate drying.
[0254] The time during constant rate drying can vary depending on the type and content of the complexing agent contained in the electrolyte precursor and cannot be generalized. After starting heating in the solvent, it is usually more than 10 minutes, preferably more than 45 minutes, and the upper limit is usually less than 1 hour and 30 minutes, more preferably 1 hour and 15 minutes.
[0255] The time of the deceleration drying period is usually 10 minutes or more, preferably 45 minutes or more, and the upper limit is usually 6 hours or less, preferably 5 hours or less, and more preferably 4 hours or less.
[0256] 〔heating〕
[0257] The manufacturing method of this embodiment may include: after heating in the above-mentioned solvent, further heating at a temperature higher than the heating temperature when heating in the solvent. By heating in the above-mentioned solvent, an amorphous sulfide solid electrolyte is obtained from the electrolyte precursor. In the case of obtaining a crystalline sulfide solid electrolyte, the amorphous sulfide solid electrolyte can be converted into a crystalline sulfide solid electrolyte by further heating at a temperature higher than the heating temperature when heating in the solvent (hereinafter also referred to as "post-heating").
[0258] In addition, in the amorphous sulfide solid electrolyte obtained by heating in the above-mentioned solvent, a complexing agent and a high boiling point solvent may remain. By further post-heating, the content of the complexing agent and the high boiling point solvent remaining in the amorphous sulfide solid electrolyte is reduced, so the quality of the sulfide solid electrolyte is improved, and high ion conductivity is easily obtained. In addition, by heating in the above-mentioned solvent, sometimes it does not become an amorphous sulfide solid electrolyte, but remains in the state of an electrolyte precursor. In this case, by post-heating, the complexing agent can be removed from the electrolyte precursor, and a crystalline sulfide solid electrolyte can be obtained via an amorphous sulfide solid electrolyte.
[0259] The heating temperature is not particularly limited as long as it is set to a temperature higher than the heating temperature when heating in a solvent. For example, the heating temperature can be determined according to the structure of the crystalline solid electrolyte obtained by heating the amorphous sulfide solid electrolyte obtained by removing the complexing agent from the electrolyte precursor. Specifically, the amorphous solid electrolyte is subjected to differential thermal analysis (DTA) under the condition of a temperature increase of 10°C / min using a differential thermal analyzer (DTA device). The temperature of the peak top of the exothermic peak observed on the lowest temperature side is preferably set to a range of 5°C or more, more preferably 10°C or more, and further preferably 20°C or more. The upper limit is not particularly limited, but it can be set to about 40°C or less. By setting it to such a temperature range, not only can a crystalline solid electrolyte be obtained more efficiently and reliably, but also the content of the complexing agent and the high boiling point solvent remaining in the sulfide solid electrolyte can be reduced, and by reducing the content of the electrolyte precursor, the purity of the sulfide solid electrolyte can be improved.
[0260] The heating temperature cannot be generally specified because it varies depending on the structure of the crystalline solid electrolyte, but is generally preferably above 130°C, more preferably above 140°C, and further preferably above 150°C. There is no particular upper limit, but it is preferably below 300°C, more preferably below 280°C, and further preferably below 250°C.
[0261] The heating time is not particularly limited as long as it is the time for obtaining the desired crystalline solid electrolyte, for example, preferably more than 1 minute, more preferably more than 10 minutes, more preferably more than 30 minutes, and more preferably more than 1 hour. In addition, the upper limit of the heating time is not particularly limited, but is preferably less than 24 hours, more preferably less than 10 hours, more preferably less than 5 hours, and more preferably less than 3 hours.
[0262] The heating can be performed under normal pressure, but in order to lower the heating temperature, it can also be performed under a reduced pressure atmosphere or further under a vacuum atmosphere.
[0263] As a pressure condition, when heating is performed under a reduced pressure atmosphere, it is preferably 85 kPa or less, more preferably 80 kPa or less, and further preferably 70 kPa or less. The lower limit may be vacuum (0 kPa). If the ease of adjusting the pressure is considered, it is preferably 1 kPa or more, more preferably 2 kPa or more, and further preferably 3 kPa or more. If the pressure condition is within the above range, the heating condition can be mild, and the enlargement of the device can be suppressed.
[0264] Furthermore, heating is preferably performed in an inert gas atmosphere (eg, a nitrogen atmosphere or an argon atmosphere) because this can prevent the crystalline solid electrolyte from being degraded (eg, oxidized).
[0265] The heating method is not particularly limited, but examples thereof include methods using a hot plate, a vacuum heating device, an argon atmosphere furnace, a firing furnace, etc. In addition, in industry, a horizontal dryer or a horizontal vibrating fluidized dryer having a heating unit and a feeding mechanism can also be used, and the method can be selected according to the amount of heating treatment.
[0266] Post-heating can also be implemented in a high boiling point solvent. Compared with the heating temperature when heating in the above-mentioned solvent, the heating temperature during post-heating (crystallization) is higher. Therefore, after removing the complexing agent by heating in the solvent, the pressure is restored with an inert gas, etc., and heating under a boiling state can be performed at a specified temperature. Thus, heating in a solvent and crystallization based on post-heating can be continuously implemented in the same device, thus becoming a very efficient heating method.
[0267] (Amorphous sulfide solid electrolyte)
[0268] The sulfide solid electrolyte obtained by the production method of the present embodiment can be either an amorphous sulfide solid electrolyte or a crystalline sulfide solid electrolyte as desired as described above.
[0269] The amorphous sulfide solid electrolyte obtained by the production method of this embodiment contains lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms. As a representative amorphous sulfide solid electrolyte, for example, Li 2 SP 2 S 5 -L i I, L i 2 SP 2 S 5 -L i C l、L i 2 SP 2 S 5 -L i Br, L i 2 SP 2 S 5 -Li-I-L-I-Br, etc., a solid electrolyte composed of lithium sulfide, phosphorus sulfide and lithium halide; and other solid electrolytes such as Li-I-Br, which also contain oxygen atoms, silicon atoms and other atoms. 2 SP 2 S 5 -Li 2 OL i I、L i 2 SS i S 2 -P 2 S 5 -Li I and other solid electrolytes. From the viewpoint of obtaining higher ion conductivity, Li I is preferred. 2 SP 2 S5 -L i I, L i 2 SP 2 S 5 -L i C l、L i 2 SP 2 S 5 -L i Br, L i 2 SP 2 S 5 -LiI-LiBr, etc. are solid electrolytes composed of lithium sulfide, phosphorus sulfide and lithium halide.
[0270] The types of atoms constituting the amorphous sulfide solid electrolyte can be confirmed by, for example, an ICP emission spectrometer.
[0271] The amorphous sulfide solid electrolyte obtained by the production method of this embodiment has at least Li 2 SP 2 S 5 In the case of 2 S and P 2 S 5 The molar ratio of is preferably 65-85:15-35, more preferably 70-80:20-30, further preferably 72-78:22-28.
[0272] In the amorphous sulfide solid electrolyte obtained by the production method of this embodiment, for example, Li 2 SP 2 S 5 In the case of -L i IL i Br, the total content of lithium sulfide and phosphorus pentasulfide is preferably 60 to 95 mol%, more preferably 65 to 90 mol%, and further preferably 70 to 85 mol%. In addition, the ratio of lithium bromide to the total of lithium bromide and lithium iodide is preferably 1 to 99 mol%, more preferably 20 to 90 mol%, further preferably 40 to 80 mol%, and particularly preferably 50 to 70 mol%.
[0273] In the amorphous sulfide solid electrolyte obtained by the production method of the present embodiment, the blending ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms is preferably 1.0 to 1.8: 1.0 to 2.0: 0.1 to 0.8: 0.01 to 0.6, more preferably 1.1 to 1.7: 1.2 to 1.8: 0.2 to 0.6: 0.05 to 0.5, and further preferably 1.2 to 1.6: 1.3 to 1.7: 0.25 to 0.5: 0.08 to 0.4. In addition, when bromine and iodine are used in combination as halogen atoms, the blending ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, bromine and iodine is preferably 1.0-1.8: 1.0-2.0: 0.1-0.8: 0.01-0.3: 0.01-0.3, more preferably 1.1-1.7: 1.2-1.8: 0.2-0.6: 0.02-0.25: 0.02-0.25, more preferably 1.2-1.6: 1.3-1.7: 0.25-0.5: 0.03-0.2: 0.03-0.2, and further preferably 1.35-1.45: 1.4-1.7: 0.3-0.45: 0.04-0.18: 0.04-0.18. By setting the mixing ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms within the above range, a solid electrolyte having a sulfide crystalline lithium superion conductor region type II crystal structure described later and having higher ion conductivity can be easily obtained.
[0274] The shape of the amorphous sulfide solid electrolyte is not particularly limited, and may be, for example, a particle shape.
[0275] The average particle size (D 50 ), for example, 0.01 μm or more, further 0.03 μm or more, 0.05 μm or more, 0.1 μm or more, and the upper limit is 5 μm or less, further 3.0 μm or less, 1.5 μm or less, 1.0 μm or less, 0.5 μm or less. In this way, the sulfide solid electrolyte obtained by the manufacturing method of this embodiment does not use a jacketed heater (vibration dryer, etc.) used in the conventional heating for removing the complexing agent and crystallization, so the generation of secondary particles caused by the aggregation of primary particles is suppressed, and the average particle size becomes a smaller particle size in the above range.
[0276] Therefore, in the production method of the present embodiment, the pulverization (microparticulation) process does not need to be performed.
[0277] (Crystalline sulfide solid electrolyte)
[0278] The crystalline sulfide solid electrolyte obtained by the production method of this embodiment may be a so-called glass ceramic obtained by heating an amorphous sulfide solid electrolyte to a crystallization temperature or higher. As its crystal structure, Li 3 PS 4 Crystal structure, Li 4 P 2 S 6 Crystal structure, Li 7 PS 6 Crystal structure, Li 7 P 3 S 11 A crystal structure, a crystal structure having peaks near 2θ=20.2° and 23.6° (for example, Japanese Patent Application Laid-Open No. 2013-16423), and the like.
[0279] Another example is Li 4-x Ge 1-x P x S 4 The sulfide-like crystalline lithium superion conductor region II (thioLISI CONRegion II) type crystal structure (see Kanno et al., Journal of The Electrochemical Society, 148 (7) A742-746 (2001)) and Li 4-x Ge 1-x P x S 4 The crystalline sulfide solid electrolyte obtained by the manufacturing method of this embodiment is preferably a crystalline sulfide lithium superion conductor region II type crystal structure from the aspect of obtaining higher ion conductivity. Here, the “crystalline sulfide lithium superion conductor region II type crystal structure” means that the crystalline sulfide solid electrolyte has a crystalline sulfide lithium superion conductor region II type crystal structure. 4-x Ge 1-x P x S 4 Sulfide-like crystalline lithium superion conductor region II (th i oLI S I CON Region II) type crystal structure, and Li 4-x Ge 1-x P x S 4Any crystal structure similar to the sulfide crystalline lithium superion conductor region II (thioLI SICON Region II) type.
[0280] The crystalline sulfide solid electrolyte obtained by the manufacturing method of this embodiment may be a crystalline sulfide solid electrolyte containing the above-mentioned crystalline lithium sulfide superion conductor region type II crystal structure, or may contain the crystalline lithium sulfide superion conductor region type II crystal structure as a main crystal. From the viewpoint of obtaining higher ion conductivity, it is preferred that the crystalline lithium sulfide superion conductor region type II crystal structure be contained as a main crystal. In this specification, "containing as a main crystal" means that the proportion of the target crystal structure in the crystal structure is 80% or more, preferably 90% or more, and more preferably 95% or more. In addition, from the viewpoint of obtaining higher ion conductivity, the crystalline sulfide solid electrolyte obtained by the manufacturing method of this embodiment preferably does not contain crystalline Li 3 PS 4 (β-L i 3 PS 4 ).
[0281] In X-ray diffraction measurements using CuKα radiation, Li 3 PS 4 The diffraction peaks of the crystal structure appear near 2θ=17.5°, 18.3°, 26.1°, 27.3°, and 30.0°, for example. 4 P 2 S 6 The diffraction peaks of the crystal structure appear near 2θ=16.9°, 27.1°, and 32.5°, for example. 7 PS 6 The diffraction peaks of the crystal structure appear at around 2θ=15.3°, 25.2°, 29.6°, and 31.0°, for example. 7 P 3 S 11 The diffraction peaks of the crystal structure appear near 2θ=17.8°, 18.5°, 19.7°, 21.8°, 23.7°, 25.9°, 29.6°, and 30.0°, for example. 4-x Ge 1-x P x S 4 The diffraction peaks of the sulfide-like lithium superion conductor region II (thioLISICONRegionII) type crystal structure appear at 2θ=20.1°, 23.9°, and 29.5°, which are similar to the Li 4-x Ge 1-x P x S4 The diffraction peaks of the sulfide crystal lithium superion conductor region II type-like crystal structure appear, for example, near 2θ=20.2 and 23.6°. The peak positions may fluctuate within a range of ±0.5°.
[0282] A crystalline sulfide solid electrolyte having the following crystal structure can also be preferably exemplified: having the above-mentioned Li 7 PS 6 The structural skeleton is a argyrodite-type crystal structure formed by replacing part of P with Si.
[0283] As the composition formula of the argyrodite type crystal structure, for example, the composition formula Li 7-x P 1-y S i y S 6 and Li 7+x P 1-y S i y S 6 (x is -0.6 to 0.6, y is 0.1 to 0.6). The argyrodite-type crystal structure represented by the composition formula is cubic or orthorhombic, preferably cubic, and has peaks mainly appearing at 2θ=15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0° and 52.0° in X-ray diffraction measurement using CuKα rays.
[0284] As the composition formula of the argyrodite type crystal structure, the composition formula Li 7-x-2y PS 6-x-y C l x (0.8≤x≤1.7, 0<y≤-0.25x+0.5). The argyrodite-type crystal structure represented by the composition formula is preferably cubic, and in X-ray diffraction measurement using CuKα rays, it mainly has peaks appearing at positions of 2θ=15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0° and 52.0°.
[0285] In addition, as the composition formula of the argyrodite type crystal structure, the composition formula Li 7-x PS 6-x Ha x(Ha is Cl or Br, and x is preferably 0.2 to 1.8). The argyrodite-type crystal structure represented by the composition formula is preferably cubic, and in X-ray diffraction measurement using CuKα rays, it mainly has peaks appearing at positions of 2θ=15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°.
[0286] In addition, these peak positions can fluctuate within a range of ±0.5°.
[0287] After the removal, further heating is performed, so that the content of the complexing agent contained in the crystalline sulfide solid electrolyte is reduced more than the content of the complexing agent contained in the amorphous sulfide solid electrolyte.
[0288] The content of the complexing agent contained in the crystalline sulfide solid electrolyte is preferably 0 mass%, that is, no complexing agent is contained at all, but from the viewpoint of efficiently obtaining a sulfide solid electrolyte with high ion conductivity, it is usually 10 mass% or less, further 8 mass% or less, 5 mass% or less, 3 mass% or less, 1 mass% or less, and the lower limit is about 0.01 mass% or more.
[0289] In addition, similarly to the complexing agent, a high boiling point solvent may remain. In this case, the content of the high boiling point solvent is also in the same numerical range as the content of the complexing agent.
[0290] In this specification, the contents of the complexing agent and the high-boiling-point solvent contained in the sulfide solid electrolyte are measured using a gas chromatograph (GC) on a solution obtained by dissolving the powder obtained in the examples, etc. in a mixed solution of water and pentanol, and the complexing agent and the high-boiling-point solvent are quantified using an absolute standard curve (GC standard curve method).
[0291] The shape of the crystalline sulfide solid electrolyte is not particularly limited, but for example, a particle shape may be mentioned.
[0292] The average particle size (D 50 ), for example, 0.01 μm or more, further 0.03 μm or more, 0.05 μm or more, 0.1 μm or more, and the upper limit is 5 μm or less, further 3.0 μm or less, 1.5 μm or less, 1.0 μm or less, 0.5 μm or less. In this way, the sulfide solid electrolyte obtained by the manufacturing method of this embodiment does not use a jacketed heater (vibration dryer, etc.) used in the past for removing the complexing agent, so the generation of secondary particles caused by the aggregation of primary particles is suppressed, so that the average particle size becomes a smaller particle size in the above range.
[0293] Therefore, in the production method of the present embodiment, the pulverization (microparticulation) process does not need to be performed.
[0294] The specific surface area of the sulfide solid electrolyte obtained by the production method of this embodiment is usually 10 m 2 / g or more, and further 15m 2 / g or more, 20m 2 / g or more, 25m 2 There is no particular upper limit, for example, 50 m 2 In this specification, the specific surface area is a value measured by the BET method (gas adsorption method), and the gas used may be nitrogen (nitrogen method) or krypton (krypton method), and is appropriately selected according to the size of the specific surface area.
[0295] [Sulfide solid electrolyte]
[0296] The sulfide solid electrolyte of the present embodiment includes lithium atoms, phosphorus atoms, sulfur atoms, halogen atoms, a complexing agent, and a solvent having a boiling point higher than that of the complexing agent.
[0297] The particle size distribution obtained by laser diffraction scattering particle size distribution measurement has peaks at a peak position of less than 0.5 μm and a peak position of more than 0.5 μm.
[0298] The volume ratio of the peak at the peak position of 0.5 μm or less is smaller than the volume ratio of the peak at the peak position of more than 0.5 μm.
[0299] The sulfide solid electrolyte of the present embodiment can be produced by the method for producing a sulfide solid electrolyte of the present embodiment described above, and is preferably produced by the method for producing a sulfide solid electrolyte of the present embodiment described above from the viewpoint of more efficient production. That is, the sulfide solid electrolyte of the present embodiment becomes a sulfide solid electrolyte having improved ion conductivity.
[0300] The sulfide solid electrolyte of the present embodiment contains lithium atoms, phosphorus atoms, sulfur atoms, and halogen atoms, which are derived from the solid electrolyte raw material contained in the raw material content used in the production method of the present embodiment.
[0301] In addition, the sulfide solid electrolyte of the present embodiment includes a complexing agent and a solvent having a boiling point higher than that of the complexing agent (high boiling point solvent). The complexing agent and the high boiling point solvent are complexing agents and high boiling point solvents used in the manufacturing process, and can also be said to be the characteristics of the sulfide solid electrolyte obtained by the manufacturing method of the present embodiment.
[0302] The complexing agent and the solvent having a boiling point higher than that of the complexing agent are the same as those described in the production method of the present embodiment. The contents of the complexing agent and the high-boiling-point solvent contained in the sulfide solid electrolyte of the present embodiment are also as described above.
[0303] (Peak of particle size distribution)
[0304] The sulfide solid electrolyte of this embodiment has the following characteristics regarding particle size distribution:
[0305] The particle size distribution obtained by laser diffraction scattering particle size distribution measurement has peaks at a peak position of less than 0.5 μm and a peak position of more than 0.5 μm.
[0306] The volume ratio of the peak at the peak position of 0.5 μm or less is smaller than the volume ratio of the peak at the peak position of more than 0.5 μm.
[0307] In this specification, the particle size distribution obtained by laser diffraction scattering particle size distribution measurement is a particle size distribution measured on a volume basis.
[0308] As described above, such a characteristic of the particle size distribution, that is, the particle size distribution has two peaks and the volume ratio of the peak with a smaller particle size is larger. This characteristic cannot be confirmed in the sulfide solid electrolyte obtained by the conventional liquid phase method (inhomogeneous method) and can be said to be a characteristic unique to the sulfide solid electrolyte obtained by heating in a high boiling point solvent to remove the complexing agent.
[0309] The sulfide solid electrolyte of the present embodiment may be any of an amorphous sulfide solid electrolyte and a crystalline sulfide solid electrolyte. As the amorphous sulfide solid electrolyte and the crystalline sulfide solid electrolyte that can be the sulfide solid electrolyte of the present embodiment, the amorphous sulfide solid electrolyte and the crystalline sulfide solid electrolyte described as the amorphous sulfide solid electrolyte and the crystalline sulfide solid electrolyte obtained by the production method of the present embodiment described above can be preferably exemplified.
[0310] As the crystalline sulfide solid electrolyte, if it is a crystalline sulfide solid electrolyte having a sulfide crystalline lithium superion conductor region type II crystal structure or an argyrodite type crystal structure, high ion conductivity can be obtained.
[0311] The average particle size (D 50) As described as the properties of the sulfide solid electrolyte obtained by the manufacturing method of the present embodiment, for example, it is 0.01 μm or more, further 0.03 μm or more, 0.05 μm or more, 0.1 μm or more, and the upper limit is 5 μm or less, further 3.0 μm or less, 1.5 μm or less, 1.0 μm or less, 0.5 μm or less. Considering the use for the positive electrode, the negative electrode and the electrolyte layer, it is preferably 0.03 μm or more, more preferably 0.05 μm or more, and more preferably 0.1 μm or more, and the upper limit is preferably 5.0 μm or less, more preferably 1.0 μm or less, and more preferably 0.5 μm or less.
[0312] Furthermore, the specific surface area of the sulfide solid electrolyte of the present embodiment is consistent with the content described as the property of the sulfide solid electrolyte obtained by the production method of the present embodiment described above.
[0313] (use)
[0314] The sulfide solid electrolyte of the present embodiment has high ion conductivity and excellent battery performance, and therefore is suitable for use in batteries.
[0315] The sulfide solid electrolyte of this embodiment can be used for the positive electrode layer, the negative electrode layer, or the electrolyte layer. In addition, each layer can be produced by a known method.
[0316] In addition, the battery preferably uses a current collector in addition to the positive electrode layer, the electrolyte layer and the negative electrode layer, and the current collector can use a known current collector. For example, a layer obtained by coating a substance that reacts with the solid electrolyte with Au, Pt, Al, Ti or Cu, etc., can be used.
[0317] 〔Electrode composite materials〕
[0318] The electrode composite material using the sulfide solid electrolyte of the present embodiment is an electrode composite material including the sulfide solid electrolyte of the present embodiment described above and an electrode active material.
[0319] (Electrode Active Material)
[0320] As the electrode active material, a positive electrode active material or a negative electrode active material is used, depending on whether the electrode composite material is used for a positive electrode or a negative electrode.
[0321] As the positive electrode active material, any positive electrode active material can be used without particular limitation as long as it can promote the battery chemical reaction through the relationship with the negative electrode active material, and the battery chemical reaction is accompanied by the movement of lithium ions caused by the atom adopted as the atom reflecting ionic conductivity, preferably the lithium atom. As the positive electrode active material that can carry out such insertion and extraction of lithium ions, oxide-based positive electrode active materials, sulfide-based positive electrode active materials, etc. can be cited.
[0322] As the oxide-based positive electrode active material, preferably, LMO (lithium manganese oxide), LCO (lithium cobalt oxide), NMC (lithium nickel manganese cobalt oxide), NCA (lithium nickel cobalt aluminum oxide), LNCO (lithium nickel cobalt oxide), olivine-type compounds (LiMeNPO 4 , Me=Fe, Co, Ni, Mn) and other lithium-containing transition metal composite oxides.
[0323] Examples of sulfide-based positive electrode active materials include titanium sulfide (TiS 2 ), molybdenum sulfide (MoS 2 ), iron sulfide (FeS, FeS 2 ), copper sulfide (CuS), nickel sulfide (Ni 3 S 2 )wait.
[0324] In addition to the above-mentioned positive electrode active materials, niobium selenide (NbSe 3 )wait.
[0325] The positive electrode active material can be used alone or in combination of two or more.
[0326] As the negative electrode active material, any negative electrode active material that can promote the battery chemical reaction accompanied by the movement of lithium ions caused by atoms used as atoms that embody ionic conductivity, preferably metals that can form alloys with lithium atoms, their oxides, alloys of the metals and lithium atoms, etc., preferably lithium atoms, can be used without particular limitation. As such a negative electrode active material that can allow lithium ions to be inserted and removed, a substance that is known as a negative electrode active material in the battery field can be used without limitation.
[0327] Examples of such negative electrode active materials include metallic lithium such as metallic lithium, metallic indium, metallic aluminum, metallic silicon, and metallic tin, or metals capable of forming alloys with metallic lithium, oxides of these metals, and alloys of these metals with metallic lithium.
[0328] The electrode active material may be one having a coating layer coated on its surface.
[0329] As a material for forming the coating layer, an atom that exhibits ionic conductivity in the sulfide solid electrolyte, preferably a nitride, an oxide, or an ion conductor such as a complex of lithium atoms, can be cited. Specifically, lithium nitride (Li 3 N), with Li 4 GeO 4 For example, Li 4-2x Zn x GeO 4 Conductors with LI SI CON crystal structure, Li 3 PO 4 The framework structure of the type, such as Li 4-x Ge 1-x P x S 4 Conductors with thio-LISICON crystal structures, La 2 / 3-x Li 3x T i 3 Conductors with perovskite crystal structures, such as LiTi 2 (PO 4 ) 3 Conductors with NASI CON type crystal structures, etc.
[0330] In addition, Li y T i 3-y O 4 (0<y<3), Li 4 T i 5 O 12 (LTO) and other lithium titanate, Li NbO 3 、LiTaO 3 Metallic acid lithium of metals belonging to Group 5 of the periodic table, and Li 2 OB 2 O 3 -P 2 O 5 Class, Li 2 OB 2 O 3 -ZnO, Li 2 O-Al 2 O 3 -SiO 2 -P 2 O 5 -T iO 2 Oxide-type conductors, etc.
[0331] The electrode active material having a coating layer is obtained by, for example, attaching a solution containing various atoms constituting a material forming the coating layer to the surface of the electrode active material and calcining the attached electrode active material preferably at 200° C. to 400° C.
[0332] Here, as the solution containing various atoms, for example, a solution containing alkoxides of various metals such as lithium ethoxide, titanium isopropoxide, niobium isopropoxide, tantalum isopropoxide, etc. can be used. At this time, as the solvent, an alcohol solvent such as ethanol and butanol; an aliphatic hydrocarbon solvent such as hexane, heptane, octane; an aromatic hydrocarbon solvent such as benzene, toluene, xylene, etc. can be used.
[0333] In addition, the above-mentioned attachment may be performed by dipping, spraying, or the like.
[0334] From the viewpoint of improving manufacturing efficiency and battery performance, the firing temperature is preferably 200° C. to 400° C., more preferably 250° C. to 390° C., and the firing time is usually about 1 minute to 10 hours, preferably 10 minutes to 4 hours.
[0335] As the coating rate of the coating layer, based on the surface area of the electrode active material, it is preferably more than 90%, more preferably more than 95%, and further preferably 100%, that is, preferably the entire surface is coated. In addition, as the thickness of the coating layer, it is preferably more than 1nm, more preferably more than 2nm, and as the upper limit, it is preferably below 30nm, more preferably below 25nm.
[0336] The thickness of the coating layer can be measured by cross-sectional observation using a transmission electron microscope (TEM), and the coverage can be calculated from the thickness of the coating layer, elemental analysis values, and BET specific surface area.
[0337] (Other ingredients)
[0338] The electrode composite material using the sulfide solid electrolyte of the present embodiment may contain other components such as a conductive material and a binder in addition to the above-mentioned sulfide solid electrolyte and electrode active material. That is, the method for manufacturing the electrode composite material of the present embodiment may use other components such as a conductive material and a binder in addition to the above-mentioned sulfide solid electrolyte and electrode active material. Other components such as a conductive material and a binder may be further added to the sulfide solid electrolyte and the electrode active material in the mixing of the above-mentioned sulfide solid electrolyte and the electrode active material and mixed for use.
[0339] As conductive materials, from the viewpoint of improving battery performance by improving electron conductivity, examples include artificial graphite, graphite carbon fiber, resin-fired carbon, pyrolysis vapor-grown carbon, coke, mesophase carbon microbeads, furfuryl alcohol resin-fired carbon, polyphenylene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and carbon materials that are difficult to graphitize.
[0340] By using a binder, the strength of the positive electrode and the negative electrode can be improved.
[0341] There are no particular restrictions on the binder as long as it can impart functions such as adhesion and flexibility. Examples include fluorine-based polymers such as polytetrafluoroethylene and polyvinylidene fluoride, thermoplastic elastomers such as butene rubber and styrene-butadiene rubber, acrylic resins, acrylic polyol resins, polyvinyl acetal resins, polyvinyl butyral resins, silicone resins and other resins.
[0342] The blending ratio (mass ratio) of the electrode active material and the sulfide solid electrolyte in the electrode composite material is preferably 99.5:0.5 to 40:60, more preferably 99:1 to 50:50, and even more preferably 98:2 to 60:40 in consideration of improvement in battery performance and manufacturing efficiency.
[0343] When containing a conductive material, the content of the conductive material in the electrode composite material is not particularly limited. If the battery performance is improved and the manufacturing efficiency is taken into consideration, it is preferably 0.5 mass % or more, more preferably 1 mass % or more, and further preferably 1.5 mass % or more. As an upper limit, it is preferably 10 mass % or less, preferably 8 mass % or less, and further preferably 5 mass % or less.
[0344] In addition, when containing a binder, the content of the binder in the electrode composite material is not particularly limited. If the battery performance is improved and the manufacturing efficiency is taken into consideration, it is preferably 1% by mass or more, more preferably 3% by mass or more, and further preferably 5% by mass or more. As an upper limit, it is preferably 20% by mass or less, preferably 15% by mass or less, and further preferably 10% by mass or less.
[0345] 〔Lithium-ion battery〕
[0346] The lithium ion battery using the sulfide solid electrolyte of the present embodiment is a lithium ion battery including at least one selected from the above-mentioned sulfide solid electrolyte of the present embodiment and the above-mentioned electrode composite material.
[0347] The lithium ion battery using the sulfide solid electrolyte of the present embodiment has no particular limitation on its structure as long as it includes the sulfide solid electrolyte of the present embodiment and an electrode composite material including the sulfide solid electrolyte, and may have the structure of a general lithium ion battery.
[0348] As a lithium ion battery using the sulfide solid electrolyte of the present embodiment, for example, a lithium ion battery including a positive electrode layer, a negative electrode layer, an electrolyte layer and a current collector is preferred. As the positive electrode layer and the negative electrode layer, it is preferred that the positive electrode layer and the negative electrode layer use an electrode composite material using the sulfide solid electrolyte of the present embodiment, and as the electrolyte layer, it is preferred that the electrolyte layer use the sulfide solid electrolyte of the present embodiment.
[0349] As the current collector, any known current collector may be used. For example, a layer obtained by coating a substance that reacts with the above-mentioned solid electrolyte, such as Au, Pt, Al, Ti, or Cu, with Au or the like can be used.
[0350] Example
[0351] Next, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples at all.
[0352] (Measurement of powder XRD diffraction)
[0353] Powder X-ray diffraction (XRD) measurements were performed as follows.
[0354] The powder of the sulfide solid electrolyte obtained in the examples and comparative examples was filled into a groove with a diameter of 20 mm and a depth of 0.2 mm and flattened with glass to prepare a sample. The sample was sealed with a kapton film for XRD and measured under the following conditions in a manner that it was not in contact with air.
[0355] Measuring device: D2 PHASER, manufactured by Bruker Corporation
[0356] Tube voltage: 30kV
[0357] Tube current: 10mA
[0358] X-ray wavelength: Cu-Kα ray
[0359] Optical system: Concentration method
[0360] Slit configuration: Sola slit 4°, divergence slit 1mm, Kβ filter (N i plate)
[0361] Detector: Semiconductor detector
[0362] Measuring range: 2θ = 10-60 degrees
[0363] Step width, scanning speed: 0.05deg, 0.05deg / sec
[0364] (Measurement of ionic conductivity)
[0365] In this example, the measurement of ion conductivity was performed as follows.
[0366] The crystalline solid electrolytes obtained in the examples and comparative examples were formed into a 10 mm diameter (cross-sectional area S: 0.785 cm 2 ), round particles with a height (L) of 0.1 to 0.3 cm are made into a sample. The upper and lower parts of the sample are taken as electrode terminals, and the AC impedance method is used for measurement at 25°C (frequency range: 5MHz to 0.5Hz, amplitude: 10mV) to obtain a Cole-Cole plot. Near the right end of the arc observed in the high-frequency side area, the real part Z'(Ω) at the point where -Z"(Ω) is the smallest is taken as the bulk resistance R(Ω) of the electrolyte, and the ionic conductivity σ(S / cm) is calculated according to the following formula.
[0367] R=ρ(L / S)
[0368] σ=1 / ρ
[0369] (Measurement of specific surface area)
[0370] The specific surface area was measured by the BET method based on nitrogen adsorption using a gas adsorption amount measuring device.
[0371] (Measurement of Contents of Complexing Agent and Solvent Contained in Sulfide Solid Electrolyte)
[0372] The content of the complexing agent and the solvent contained in the sulfide solid electrolyte is measured using a gas chromatograph (GC). The measurement outline is as follows: The powder of the sulfide solid electrolyte etc. decomposed by a mixture of water and pentanol (content of pentanol in the mixture: 90 volume %) is measured by GC, and the complexing agent and the solvent are quantified using an absolute calibration curve.
[0373] First, accurately weigh 0.1g of sample and put it into a vial. Add a mixture of 10ml water and amyl alcohol to the vial to completely decompose and dissolve the sample. Add about 1.5ml of the dissolved sample to a GC vial, cover it with a lid and fix it with a crimper. Set the automatic sampler to GC for measurement. As a standard curve, weigh 0.5g of the solvent used and make it constant to volume with a mixture of 50ml water and amyl alcohol (equivalent to 10000μg / ml). Dilute it and adjust it to 2500, 1000, 250, 25, 2.5μg / ml (standard solution) for GC measurement. According to the peak area and the concentration of the standard solution, a standard curve is prepared by the least squares method. Substitute the GC peak area value of the sample solution into the standard curve and calculate the concentration in the sample solution according to the following formula.
[0374] Content of complexing agent and solvent in powder of sulfide solid electrolyte etc. (mass %) = [concentration obtained from standard curve (μg / ml) × amount of mixture of water and pentanol used for sample dissolution (10 ml)] ÷ sample amount (g)
[0375] (Measurement of particle size distribution)
[0376] The measurement was performed using a laser diffraction / scattering particle size distribution measuring device ("Parti ca LA-950 (model)", manufactured by Horiba, Ltd.). Specifically, a mixture of dehydrated toluene (special grade, manufactured by Wako Pure Chemical Industries, Ltd.) and tert-butyl alcohol (special grade, manufactured by Wako Pure Chemical Industries, Ltd.) at a mass ratio of 93.8:6.2 was used as a dispersion medium. 50 mL of the dispersion medium was injected into the flow cell of the device and circulated, and then the powder to be measured was added and ultrasonicated, and then the particle size distribution was measured.
[0377] In addition, the average particle size (D 50 ) is the particle size when the cumulative curve of the above-mentioned particle size distribution is drawn, starting from the particle with the smallest particle size and reaching 50% (volume basis) of the total.
[0378] (Measurement of complex weight ratio)
[0379] The complex mass ratio was measured by weight reduction ratio using a thermogravimetric measuring device (TG device). The powder (sample) used as the measurement object in each implementation and comparative example was vacuum dried at 80°C for 1 hour as a pretreatment for removing the solvent. After the pretreatment, 20 mg of the sample was heated from room temperature (23°C) to 600°C at 10°C / min under a nitrogen stream. The value calculated by the following mathematical formula based on the weight change before and after the treatment was used as the weight ratio of the complex in the powder.
[0380] Complex weight ratio (weight %) = (weight before heating - weight after heating) / weight before heating × 100
[0381] (Example 1)
[0382] In a 1-liter reaction tank with a stirring blade, 13.19 g of lithium sulfide, 21.26 g of phosphorus pentasulfide, 4.15 g of lithium bromide and 6.40 g of lithium iodide were introduced under a nitrogen atmosphere. 100 mL of tetramethylethylenediamine (TMEDA, boiling point: 120° C.) as a complexing agent and 800 mL of cyclohexane as a solvent were added thereto, and the stirring blade was operated to perform mixing under stirring at 30° C. for 72 hours. 456 g of zirconia balls (diameter: 0.5 mm φ) were placed in a bead mill capable of circulating operation ("LABSTAR Mini LMZ015 (trade name)", manufactured by Ashizawa Fintech Co., Ltd.) (bead filling rate relative to the grinding chamber: 80%), and the mixture was circulated between the above-mentioned reaction tank and the grinding chamber under the conditions of pump flow rate: 550 mL / min, peripheral speed: 8 m / s, and mill jacket temperature: 20°C, and ground for 60 minutes to obtain a slurry of an electrolyte precursor (complex). Then, the obtained slurry was immediately dried at room temperature (23°C) under vacuum to obtain a powder of an electrolyte precursor (complex). The weight ratio of the complex was measured for the obtained powder by the above-mentioned method, and the result was 53% by weight.
[0383] The obtained powder of the electrolyte precursor was subjected to vacuum drying treatment at 70°C for 5 hours using a vibration dryer (manufactured by Chuo Kakoki Co., Ltd.) and dried at a constant rate. The weight ratio of the complex was measured by the above method for the obtained powder, and the result was 22% by weight. 3.5 g of the powder was mixed with 225 mL of n-decane (boiling point: 174°C) to prepare a n-decane slurry of the electrolyte precursor.
[0384] Next, add 200 mL of n-decane (boiling point: 174°C) as a high boiling point solvent into a 500 mL flask equipped with a thermometer and a stirrer, control the flask to be decompressed with a vacuum pump and a decompression controller, immerse it in an oil bath for heating, and thus become a state of boiling at 100°C under 8 kPa. Next, slowly add the n-decane slurry of the above-mentioned electrolyte precursor into the flask to make the liquid level in the flask constant. Furthermore, slowly add n-decane, keep this state for 1 hour, heat to 110°C (the pressure in the flask is 13 kPa, and the n-decane becomes a boiling state), keep this state for 1 hour, and perform deceleration drying to remove the complexing agent. At this time, use a circulating cooler to cool and recover the high boiling point solvent and complexing agent volatilized in the flask.
[0385] After the removal of the complexing agent, the temperature in the flask was raised from 110°C to 160°C at a rate of 20°C / hour (the pressure in the flask was slowly restored to 68 kPa with nitrogen) to perform crystallization. In addition, in order to keep the liquid level in the flask constant, n-decane was supplied to the flask as needed, similarly to the deceleration drying.
[0386] Then, the weight ratio of the complex was measured by the above-mentioned method for the powder obtained by drying n-decane at 90° C. for 1 hour, and the result was 4% by weight.
[0387] The powder obtained after crystallization was subjected to XRD measurement. The results showed that crystallization peaks were mainly detected at 2θ=20.2° and 23.6° in the X-ray diffraction spectrum, confirming that it was a crystalline sulfide solid electrolyte having a type II crystal structure in the sulfide crystallized lithium superion conductor region. The results are shown in Figure 1 The ionic conductivity was measured and the result was 2.4 (mS / cm) and the specific surface area was 31 (m 2 / g). In addition, the contents of the complexing agent and decane contained in the crystalline sulfide solid electrolyte were 0.8 mass % and 0.03 mass %, respectively.
[0388] In addition, the crystallized sulfide solid electrolyte was observed using a scanning electron microscope (SEM). The scanning electron microscope (SEM) photograph is shown in Figure 2 .
[0389] In addition, XRD measurements were also performed on the powder before the removal of the complexing agent (powder of the electrolyte precursor) and the powder after constant-speed drying when the complexing agent was removed. In the X-ray diffraction spectrum of the powder obtained after constant-speed drying when the complexing agent was removed, there was no peak derived from the powder of the electrolyte precursor and the raw material, but a halo pattern was shown, confirming that it was an amorphous sulfide solid electrolyte. The results of the XRD measurements of the powder of the electrolyte precursor and the powder after constant-speed drying are shown in Figure 1 In addition, the results of XRD measurement of the powder before removal of the complexing agent (powder of the electrolyte precursor) are also shown in Figure 3 The results of XRD measurements of crystalline sulfide solid electrolytes are also shown in Figure 4 and 5 .
[0390] (Example 2)
[0391] As in Example 1, n-decane is heated to 90°C (pressure is 5kPa, n-decane is in a boiling state) in a flask, then n-decane slurry is slowly added, this state is maintained for 1 hour, then heated to 110°C (pressure in the flask is restored to 13kPa, n-decane is in a boiling state), this state is maintained for 1 hour, and deceleration drying is performed to remove the complexing agent. At this time, the high boiling point solvent and complexing agent volatilized in the flask are cooled and recovered with a circulating cooler. In addition, in order to keep the liquid level in the flask constant, n-decane is supplied to the flask as required.
[0392] After the complexing agent was removed, the powder was dried in n-decane at 90° C. under vacuum conditions for 1 hour. The weight ratio of the complex was measured by the above method and found to be 12% by weight.
[0393] Furthermore, the powder after the removal of the complexing agent was transferred to a LAB Schlenk flask and heated at 160° C. for 2 hours for crystallization while being evacuated with a vacuum pump (under a vacuum atmosphere), thereby obtaining a powder of a crystalline sulfide solid electrolyte.
[0394] The obtained crystalline sulfide solid electrolyte powder was subjected to XRD measurement. As a result, crystallization peaks were detected mainly at 2θ=20.2° and 23.6° in the X-ray diffraction spectrum, confirming that it was a crystalline sulfide solid electrolyte having a sulfide crystalline lithium superion conductor region type II crystal structure. The results are shown in Figure 4 In addition, XRD measurements of the powder after deceleration drying were also performed. The results are shown in Figure 4 .
[0395] (Example 3)
[0396] In Example 2, an electrolyte precursor (complex) powder (complex weight ratio: 53 wt%) was used, heated to 80°C (pressure was 4 kPa, and n-decane was in a boiling state), and this state was maintained for 1 hour for constant-speed drying. Then, the same method as in Example 2 was used until the drying was slowed down. Then, the weight ratio of the complex was measured by the above method for the powder obtained by drying n-decane at 90°C under vacuum conditions for 1 hour, and the result was 8.5 wt%.
[0397] The obtained powder was transferred to a LAB Schlenk bottle and heated at 110° C. for 2 hours while being evacuated with a vacuum pump (in a vacuum atmosphere) to obtain a powder. The weight ratio of the complex was measured by the above method and found to be 6.4% by weight.
[0398] In addition, the powder obtained by heating was subjected to XRD measurement. The results showed that although a slight crystallization peak due to the type II crystal structure of the sulfide crystal lithium superion conductor region was detected mainly at 2θ=20.2° and 23.6° in the X-ray diffraction spectrum, it was confirmed to be an amorphous sulfide solid electrolyte with a halo pattern. These results are shown in Figure 5 In addition, XRD measurements of the powder after deceleration drying were also performed. The results are shown in Figure 5 .
[0399] (Example 4)
[0400] The powder obtained by removing the complexing agent in Example 3 was transferred to a LAB Schlenk bottle and heated at 160° C. for 2 hours for crystallization while evacuating with a vacuum pump (in a vacuum atmosphere) to obtain a powder. The weight ratio of the complex in the obtained powder was measured by the above method and found to be 2.3% by weight.
[0401] Furthermore, XRD measurement was performed, and the results showed that crystallization peaks were mainly detected at 2θ=20.2° and 23.6° in the X-ray diffraction spectrum, confirming that it was a crystalline sulfide solid electrolyte having a sulfide crystal lithium superion conductor region type II crystal structure. The results are shown in Figure 5 .
[0402] The ionic conductivity of the obtained crystalline sulfide solid electrolyte was measured and found to be 1.5 (mS / cm). The contents of the complexing agent and decane contained in the crystalline sulfide solid electrolyte were 0.8% by mass and 0.03% by mass, respectively.
[0403] (Comparative Example 1)
[0404] The powder of the electrolyte precursor (complex weight ratio: 53 wt %) is obtained in the same manner as in Example 1. The obtained powder is mixed with 225 mL of heptane (boiling point: 98° C.) to prepare a heptane slurry of the electrolyte precursor. Next, 200 mL of heptane (boiling point: 98° C.) is added as a solvent to a 500 mL flask equipped with a thermometer and a stirrer, and the mixture is boiled at 80° C. at 57 kPa. While further heating, the heptane slurry of the electrolyte precursor is slowly added to the flask, the pressure is restored to normal pressure, the temperature is raised to 100° C. (heptane becomes boiling), and the state is maintained for 2 hours to remove the complexing agent. At this time, the solvent and complexing agent volatilized in the flask are cooled and recovered with a circulating cooler. In addition, in order to keep the liquid level in the flask constant, heptane is supplied to the flask as needed, and constant-rate drying is performed to remove the complexing agent. Then, the weight ratio of the complex was measured by the above-mentioned method for the powder obtained by drying heptane at 80° C. for 1 hour, and the result was 22% by weight.
[0405] The obtained powder was transferred to a LAB Schlenk bottle, and heated at 110° C. for 2 hours while exhausting the air with a vacuum pump (under a vacuum atmosphere) to perform accelerated drying to obtain a powder.
[0406] XRD measurements were performed on the powder dried at a constant speed and the powder dried at a reduced speed, and peaks due to various impurities were confirmed. These results are shown in Figure 3 .
[0407] (Comparative Example 2)
[0408] The powder obtained in Comparative Example 1 was further crystallized by heating at 160° C. for 2 hours in a LAB Schlenk bottle while being evacuated with a vacuum pump (under a vacuum atmosphere) to obtain a powder.
[0409] The crystallized powder was subjected to XRD measurement. As a result, crystallization peaks were slightly detected at 2θ=20.2° and 23.6° in the X-ray diffraction spectrum. Although it is suspected to have a type II crystal structure in the sulfide crystallized lithium superion conductor region, peaks due to various impurities were also confirmed. The results are shown in Figure 3 .
[0410] (Comparative Example 3)
[0411] A powder of an electrolyte precursor (complex) was obtained in the same manner as in Example 1. The weight ratio of the complex in the obtained powder was measured by the above-mentioned method and found to be 53% by weight.
[0412] The obtained powder was further dried at 110° C. under reduced pressure for 6 hours, and then heated at 160° C. under reduced pressure for 2 hours to crystallize, thereby obtaining a crystalline powder.
[0413] The obtained crystalline powder was observed using a scanning electron microscope (SEM). The scanning electron microscope (SEM) photograph is shown in Figure 6 .
[0414] (Comparative Example 4)
[0415] 100 g of the crystalline powder obtained in Comparative Example 3 was introduced into a 3-liter reaction tank with a stirring blade, and 2144 mL of heptane and 138 mL of diisopropyl ether (D i PE) were added and stirred for 10 minutes to obtain a slurry. The obtained slurry was crushed for 3 minutes by operating a micro bead mill capable of circulating operation ("MAX nanogetter (trade name)", manufactured by Ashizawa Finetech Co., Ltd.) under specified conditions (bead diameter: 0.05 mmφ, bead usage: 1573 g (bead filling amount relative to the grinding chamber: 65%), pump flow rate: 1000 mL / min, peripheral speed 6 m / s).
[0416] Furthermore, the slurry pulverized by the micro bead mill was dried at room temperature (23° C.) under vacuum to obtain pulverized powder.
[0417] The particle size distribution of the crystalline sulfide solid electrolyte powders obtained in Examples 1 and 2, the crystallized powder obtained in Comparative Example 3, and the powder obtained in Comparative Example 4 was measured by the above method. The measurement results are shown in Figure 7 .
[0418] according to Figure 7 As a result, it was confirmed that the powders of Examples 1 and 2 had peaks at peak positions below 0.5 μm and peak positions above 0.5 μm, and the volume ratio of the peak at the peak position below 0.5 μm was smaller than the volume ratio of the peak at the peak position above 0.5 μm. On the other hand, it was confirmed that the crystallized powder of Comparative Example 3 had two peaks like the powder of Example 1, but the volume ratio of the peak at the peak position below 0.5 μm was larger than the volume ratio of the peak at the peak position above 0.5 μm.
[0419] In addition, according to Figure 7 The results also confirmed that the shape of the peak at the peak position below 0.5 μm of the powders of Examples 1 and 2 is sharper than the shape of the peak at the peak position above 0.5 μm, and the half-width value of the peak at the peak position below 0.5 μm is smaller than the half-width value of the peak at the peak position above 0.5 μm.
[0420] And according to Figure 7 It was confirmed that the powder of Comparative Example 4 obtained by pulverizing (micronizing) the powder of Comparative Example 3 had the same particle size distribution as the powders of Examples 1 and 2. It can be seen from this that the powder of Example 1 has a particle size distribution that cannot be obtained without pulverizing (micronizing) in the conventional liquid phase method (inhomogeneous method) even if it is not pulverized (micronized).
[0421] In addition, according to the above-mentioned particle size distribution measurement, the average particle size (D 50 ) are 0.15 μm and 0.12 μm respectively, and the average particle size (D 50 ) is 3.0 μm, and the average particle size (D 50 ) is 0.15μm.
[0422] The average particle size (D 50 ) and the average particle size (D 50 ) is much larger than that of Example 1, which indicates that the crystalline sulfide solid electrolyte obtained in Example 1 hardly undergoes agglomeration ( Figure 2 ), and the crystallized powder of Comparative Example 3 agglomerated in large quantities to form secondary particles ( Figure 6 ) This situation has also been confirmed.
[0423] (Example 5)
[0424] In the same manner as in Example 1, a powder of an electrolyte precursor (complex) was obtained (complex weight ratio: 53 wt %).
[0425] 3.5 g of the obtained electrolyte precursor (powder) was mixed with 225 mL of n-decane (boiling point: 174° C.) to prepare a n-decane slurry of the electrolyte precursor. The n-decane was heated to 80° C. in a flask (the pressure was 4 kPa, and the n-decane was in a boiling state), and then the n-decane slurry was slowly added, and this state was maintained for 1 hour, and then dried at a constant rate. At this time, the high boiling point solvent and complexing agent volatilized in the flask were cooled and recovered with a circulating cooler. In addition, in order to keep the liquid level in the flask constant, n-decane was supplied to the flask as needed, and this state was maintained to obtain a slurry.
[0426] Next, the obtained slurry was recovered, n-decane was heated to 110° C. in a flask (pressure was 13 kPa, n-decane was in a boiling state), and then the slurry was slowly added and maintained for 1 hour, thereby performing deceleration drying. In addition, the liquid level in the flask was also set to be constant.
[0427] The slurry was recovered, n-decane was heated to 160° C. (pressure was 68 kPa, n-decane was in a boiling state) in a flask, and the slurry was then slowly added and maintained for 1 hour to perform crystallization. The liquid level in the flask was also kept constant.
[0428] Then, the weight ratio of the complex was measured by the above-mentioned method for the powder obtained by drying n-decane at 90° C. for 1 hour, and the result was 2.7% by weight.
[0429] The powder obtained after crystallization was subjected to XRD measurement. The results showed that crystallization peaks were mainly detected at 2θ=20.2° and 23.6° in the X-ray diffraction spectrum, confirming that it was a crystalline sulfide solid electrolyte having a type II crystal structure in the sulfide crystallized lithium superion conductor region. The results are shown in Figure 8 The ionic conductivity was measured and the result was 1.3 (mS / cm).
[0430] Industrial Applicability
[0431] According to the method for producing a sulfide solid electrolyte of this embodiment, a sulfide solid electrolyte with high ion conductivity can be produced efficiently. In addition, the amount of complexing agent that can be removed can be increased simply by increasing the amount of high boiling point solvent used, so mass production can be easily achieved.
[0432] The sulfide solid electrolyte of the present embodiment obtained by the production method of the present embodiment is suitable for use in batteries, particularly batteries used in information-related equipment or communication equipment such as personal computers, video cameras, and mobile phones.
Claims
1. A method for producing a sulfide solid electrolyte, characterized in that: include: Mixing a raw material containing lithium atoms, phosphorus atoms, sulfur atoms and halogen atoms with a complexing agent to obtain an electrolyte precursor containing material; Next, heating is performed in a solvent having a boiling point higher than that of the complexing agent.
2. The method for producing a sulfide solid electrolyte according to claim 1, wherein: The heating temperature of the solvent is set to be higher than the boiling point of the complexing agent.
3. The method for producing a sulfide solid electrolyte according to claim 1 or 2, wherein: When heating is performed in the solvent, the solvent is boiled.
4. The method for producing a sulfide solid electrolyte according to claim 3, wherein: A solvent having a boiling point higher than that of the complexing agent is separately prepared, and a mixture of the electrolyte precursor-containing material and the separately prepared solvent is prepared and added to the solvent used for the heating.
5. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 4, characterized in that: The amount of the solvent used is 20 mL or more and 2000 mL or less relative to 1 g of the supplied electrolyte precursor contained in the electrolyte precursor-containing material.
6. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 5, wherein: include: The electrolyte precursor content is dried.
7. The method for producing a sulfide solid electrolyte according to claim 6, wherein: The drying is performed under normal pressure or reduced pressure at 5° C. to 110° C.
8. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 7, wherein: include: After heating in the solvent, further heating is performed at a temperature higher than the heating temperature during heating in the solvent.
9. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 8, wherein: The complexing agent is a compound having an amino group.
10. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 9, wherein: The complexing agent is a compound having at least two tertiary amino groups in the molecule.
11. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 10, wherein: The solvent is a hydrocarbon solvent containing no heteroatoms.
12. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 11, wherein: The solvent is at least one organic solvent selected from aliphatic hydrocarbon solvents and alicyclic hydrocarbon solvents.
13. The method for producing a sulfide solid electrolyte according to claim 12, wherein: The organic solvent has 8 or more carbon atoms.
14. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 13, wherein: After heating in the solvent, no pulverization treatment is performed.
15. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 14, wherein: When heating is performed in the solvent, the complexing agent is removed from the electrolyte precursor contained in the electrolyte precursor content.
16. The method for producing a sulfide solid electrolyte according to any one of claims 1 to 15, wherein: The sulfide solid electrolyte has a sulfide crystalline lithium superion conductor region type II crystal structure.