Substrate for electronic device

By forming a porous treatment on the SiC substrate to reduce Young's modulus, the problem of mechanical stress in the SiC substrate during the brazing process is solved, extending the service life of the electronic device and simplifying the manufacturing process.

CN118974881APending Publication Date: 2024-11-15SOITEC SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031213.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-04
Filing Date
2023-04-04
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the brazing process, the existing SiC substrates do not match the thermal expansion coefficient and Young's modulus of the copper stack, resulting in uneven mechanical stress, causing cracks, layering and peeling, shortening the service life of electronic devices, and thinning the substrate. The process is complex and costly.

Method used

Using a self-supporting substrate made of polycrystalline silicon carbide, the porous portion extending on the back of the substrate has a porosity of more than 5%, and at least one radio frequency or power electronic component is formed on the surface layer of single-crystalline silicon carbide, thereby reducing Yang by porous treatment. modulus, reduce deformation and mechanical stress caused by temperature changes.

Benefits of technology

It effectively reduces the mechanical stress at the brazing interface, extends the service life of electronic devices, and simplifies the substrate manufacturing process and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974881A_ABST
    Figure CN118974881A_ABST
Patent Text Reader

Abstract

The invention relates to a substrate for a power or radio frequency electronic device, said substrate comprising: a support substrate (30) made of polycrystalline silicon carbide, said support substrate (30) having a front side (10) and a rear side (20), said support substrate (30) being self-supporting, and a single crystal silicon carbide surface layer (1) extending on the front side (10) of said support substrate (30), said substrate being characterized in that said support substrate (30) comprises a single crystal silicon carbide surface layer (1) extending on the rear side (20) of said support substrate (30). The support substrate (30) has at least one porous portion (3) extending from the back side (20), the porous portion (3) having a porosity greater than 5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a substrate for electronic devices, in particular a substrate for radio frequency or power electronic devices. The present invention also relates to an electronic device comprising such a substrate and a method for manufacturing such a substrate. Background Art

[0002] Silicon carbide (SiC) is widely used in the manufacture of radio frequency or power electronic components.

[0003] The substrate used to manufacture such components generally comprises a support substrate which may be made of polycrystalline SiC (p-SiC) and a surface layer of single crystal SiC (m-SiC) extending on the support substrate. The electronic components are manufactured in or on the single crystal SiC layer. The structure is cut into the form of chips, each chip comprising one or more electronic components. Each chip is brazed to a directly bonded copper stack comprising a metal layer, a thermally conductive ceramic and a heat sink.

[0004] Heat is therefore mainly released through the directly bonded copper laminate, causing significant thermal stresses on the filler material connecting the electronic component to the upper metal layer of the directly bonded copper laminate by soldering.

[0005] However, the coefficient of thermal expansion (CTE) and Young's modulus of SiC and the directly bonded copper laminate (especially copper) are very different. Therefore, temperature changes cause non-uniform deformation in the layers below and above the braze joint.

[0006] As a result, the filler is subjected to high loads, causing cracks, delamination, or spalling at the solder interface, resulting in a shortened device life.

[0007] In order to reduce these mechanical stresses, it is known practice to thin the layers of the composite structure, in particular the layers of the base substrate made of polycrystalline SiC. However, grinding such a base substrate requires a lot of time and effort, resulting in an increase in the cost of the electronic component. In addition, thinning involves the risk of fractures that would render the composite structure unusable.

[0008] Another solution is to change the material used to produce the braze, which is difficult to implement, especially while maintaining the mechanical stability of the braze as well as the electrical and thermal conductivity. Summary of the invention

[0009] The object of the present invention is to propose a composite structure for producing electronic devices which has a better resistance to temperature cycles while avoiding cracks, delamination and spalling at the soldering interface.

[0010] To this end, the present invention proposes a substrate for a radio frequency or power electronic device, the substrate comprising:

[0011] a support substrate made of polycrystalline silicon carbide, the support substrate having a front side and a back side, the support substrate being self-supporting, and

[0012] a single-crystal silicon carbide surface layer extending on the front side of the support substrate,

[0013] The substrate is characterized in that the support substrate has at least one porous portion extending from the back surface, the porous portion having a porosity greater than 5%.

[0014] The support substrate has a thickness greater than 50 μm, advantageously greater than 80 μm, more advantageously greater than 100 μm and even more advantageously greater than 150 μm.

[0015] The porous portion preferably includes a porosified SiC layer.

[0016] In some embodiments, the support substrate includes: a non-porous portion between the single crystal silicon carbide surface layer and the porous portion.

[0017] In some embodiments, the porous portion has a rear portion having a first porosity and a front portion having a second porosity less than the first porosity.

[0018] The porous portion may have a porosity gradient that decreases from the back side to the front side.

[0019] The porous portion may have pores filled with a material having a Young's modulus lower than that of the silicon carbide.

[0020] Advantageously, the average distance between the pores is greater than 10 nm, preferably greater than 50 nm.

[0021] The present invention also relates to an electronic device comprising the substrate as described above and at least one radio frequency or power electronic component formed in or on the single crystal silicon carbide surface layer.

[0022] The electronic device preferably further includes a heat release means, the substrate being brazed to the heat release means via a filler so that the filler is in integral contact with at least a portion of the porous portion on the back surface of the support substrate.

[0023] Another subject of the present invention relates to a method for manufacturing a radio frequency or power electronic device, the radio frequency or power electronic device comprising:

[0024] a self-supporting support substrate made of polycrystalline silicon carbide having a front side and a back side, and

[0025] a single-crystal silicon carbide surface layer extending on the front side of the support substrate,

[0026] The method is characterized in that it includes: a step of forming at least one porous portion extending from the back side in the support substrate, the porous portion having a porosity greater than 5% and a thickness greater than 100nm, advantageously greater than 1μm, and more advantageously greater than 3μm.

[0027] The method may further include the step of assembling the surface layer and the support substrate.

[0028] The support substrate preferably has a thickness greater than 50 μm, advantageously greater than 80 μm, more advantageously greater than 100 μm and even more advantageously greater than 150 μm.

[0029] Advantageously, the forming of the support substrate comprises the step of making at least a portion of a non-porous silicon carbide base substrate porous to form the porous portion.

[0030] In some embodiments, the porosification is performed on all of the base substrate to form a fully porous support substrate.

[0031] The porosification may be performed to form a porosity gradient that decreases from the back side to the front side in the porous portion.

[0032] The porosification may be performed to form a bonding area having a porosity of less than 40% on the front side of the support substrate.

[0033] In some embodiments, the method includes the step of filling at least some of the pores of the porous portion with a material having a Young's modulus lower than that of silicon carbide.

[0034] The method may further include the step of thinning the support substrate via the back surface so that the thickness of the porous portion (3) remains greater than or equal to 100 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Other features and advantages of the present invention will become apparent from the following detailed description made with reference to the accompanying drawings, in which:

[0036] Figure 1 A device comprising two electronic components manufactured from a substrate according to the invention and a directly bonded copper stack is illustrated.

[0037] Figure 2 A substrate according to the present invention is exemplified, which includes a surface layer made of single-crystal silicon carbide and a supporting substrate including a porous portion.

[0038] Figure 3A substrate according to the present invention is exemplified, which includes a surface layer made of single-crystal silicon carbide and a supporting substrate including a porous portion and a non-porous portion made of porosified polycrystalline SiC.

[0039] Figure 4 A substrate according to one embodiment is illustrated, which includes a surface layer made of single-crystal silicon carbide and a support substrate including a porous portion and a non-porous portion made of sintered SiC.

[0040] Figure 5 A substrate according to another embodiment is illustrated, which includes a surface layer made of single-crystal silicon carbide and a supporting substrate including a non-porous portion and a porous portion including two regions of different porosities.

[0041] Figure 6 is a graph measuring the fracture resistance of a substrate made of porous silicon carbide as a function of the porosity of the substrate.

[0042] FIG. 7A to FIG. 7D The steps of one embodiment of a process for manufacturing a substrate according to the present invention are illustrated.

[0043] FIG. 8A to FIG. 8C Steps of another embodiment of the method for manufacturing a substrate according to the present invention are illustrated.

[0044] FIG. 8D to FIG. 8I Illustrated FIG. 8A to FIG. 8C Steps of variations of the embodiments of the illustrated methods.

[0045] Fig. 9A and Fig. 9B The steps of the third embodiment of the method for manufacturing a substrate according to the present invention are illustrated.

[0046] FIG. 10A to FIG. 10F The steps of a fourth embodiment of a process for manufacturing a substrate according to the present invention are illustrated.

[0047] FIG. 11A to FIG. 11E The steps of the fifth embodiment of the method for manufacturing a substrate according to the present invention are illustrated.

[0048] Fig.12 is a graph of the Young's modulus of various samples made of porous silicon carbide as a function of the porosity of the samples.

[0049] Fig.13 is a graph of Young's modulus for various samples made of silicon carbide.

[0050] To make the drawings easier to read, the structures shown are not necessarily shown to scale. DETAILED DESCRIPTION

[0051] Figure 1A radio frequency or power electronic device comprising one or more electronic chips 11, 12 manufactured from a substrate according to the invention is illustrated. The chips may be connected by mutual connections. In the case of a radio frequency device, the electronic chip may carry a lateral device made of gallium nitride.

[0052] The electronic chips 11, 12 are mounted on a direct bonded copper structure by means of soldering 21, 22. The direct bonded copper (DBC) structure comprises two copper metallizations 17, 19 and a substrate 18 made of a thermally conductive and electrically insulating ceramic, for example of aluminum nitride. Electrical connections 27, 28 are fixed to the copper metallization 17 by means of soldering 25, 26.

[0053] The solder joints 29 secure the device to the heat sink 34 and the base plate 32. A layer of thermal grease 31 ensures thermal contact between the heat sink 34 and the base plate 32. The radio frequency or power electronic device is enclosed in a housing 39, typically made of plastic.

[0054] Each chip is formed by a substrate comprising a support substrate made of silicon carbide and a single-crystalline silicon carbide surface layer in or on which at least one power electronic component or radio-frequency electronic component is formed.

[0055] The thickness of the surface layer made of monocrystalline silicon carbide is typically between 100 nm and 1500 nm. On this surface layer, a monocrystalline layer made of silicon carbide with a thickness between 1 μm and 150 μm can be epitaxially deposited in which at least a part of the electronic component is formed.

[0056] The support substrate has a front side and a back side opposite to the front side, and the surface layer extends on the front side.

[0057] According to an embodiment to be described later, the surface layer may already be assembled on a supporting substrate, which may then be polycrystalline.

[0058] The support substrate itself may be a single piece or consist of a stack of at least two layers. Preferably, the thickness of the support substrate is selected so that the support substrate is self-supporting without the surface layer, that is, it is mechanically stable enough to be handled by itself without adding an additional handling substrate or support. For this purpose, the support substrate typically has a thickness of more than 150 μm, advantageously more than 100 μm, more advantageously more than 80 μm and even more advantageously more than 50 μm. Using a self-supporting support substrate advantageously makes the step of manufacturing the substrate easier.

[0059] In some cases, electronic devices can be manufactured from a support substrate that is not necessarily self-supporting without thickness restrictions. In this case, the heat release device can mechanically stabilize the electronic components. The manufacture of such a substrate may require processing support. However, the support substrate can be manufactured according to the same embodiment as the self-supporting support substrate.

[0060] In the case of power electronic devices, good electrical conductivity between the thin layer and the supporting substrate is essential. For such devices, the supporting substrate has a resistivity of, for example, 50 mΩ.cm or less, in particular 20 mΩ.cm or less.

[0061] In the case of radio frequency devices, the support substrate advantageously has a high resistivity, for example a resistivity greater than 500 Ω·cm.

[0062] The support substrate has at least one porous portion extending from the back side. In contrast, the surface layer is non-porous, that is to say it has a porosity of less than 5% or zero.

[0063] The porosity of silicon carbide is defined as the fraction of the volume within the silicon carbide that is unoccupied that can be filled with air or other gases or solid inclusions of other materials. For example, the pores of a porous silicon carbide layer may be filled with carbon inclusions.

[0064] The pores may be interconnected or separated from each other, depending on the method of forming the porous layer. Typically, the pores obtained by electrochemical porosification of silicon carbide are at least partially interconnected and are generally filled with air. In the case of porous silicon carbide obtained by sintering, the pores are generally separated from each other and may be at least partially filled with carbon inclusions.

[0065] In the case of air-filled and interconnected pores, the porosity can be measured gravimetrically. In other cases, the porosity can be measured by the reflectivity of the porous surface of the silicon carbide. The porosity can also be measured by observing a cross section of the porous silicon carbide using an optical microscope or electron beam scanning and by estimating the quotient between the surface area occupied by pores and / or inclusions and the surface area occupied by the silicon carbide.

[0066] The porosity of the porous portion of the support substrate is advantageously between 5% and 30%, and in the case of a substrate made of porous silicon carbide, more advantageously between 5% and 20%. According to an embodiment described later, the porosity can be constant over the entire thickness of the porous portion, or vary gradually or continuously along a gradient.

[0067] The presence of this porosity makes it possible to reduce the Young's modulus of silicon carbide. Fig.12The Young's modulus (elastic modulus, E) of silicon carbide as a function of porosity Φ according to LL Snead et al. is illustrated. Despite the broad scatter, it is noted that the decrease in Young's modulus is visible even for low porosities and is particularly pronounced from about 5% porosity.

[0068] If the pores are filled with inclusions of a solid material, the solid material advantageously has a Young's modulus less than that of silicon carbide so as not to offset the reduction in Young's modulus provided by the porosity of the silicon carbide. Furthermore, in order not to adversely affect the electrical conductivity of the support substrate, the solid material advantageously is an electrical conductor. For example, the inclusions may include carbon, silicon, a metal or a metal alloy.

[0069] A porosity of less than or equal to 30% makes it possible to preserve an acceptable fracture strength in the face of mechanical stresses that may be applied to the chip, in particular when all the supporting substrates are porous. Figure 6 The porosity of porous silicon carbide samples is shown in MPa·m 1 / 2 A measure of the breaking strength in units of Å. For porosity up to about 25%, the change in breaking strength is negligible for the behavior of electronic chips.

[0070] In some embodiments, the porous portion extends throughout the thickness of the support substrate.

[0071] In other embodiments, the porous portion extends over only part of the thickness of the supporting substrate. In this case, the non-porous intermediate portion extends between the porous portion and the surface layer. Such a structure generally has better resistance to substrate fracture.

[0072] In all cases, the porous portion has a total thickness greater than 100 nm, preferably greater than 1 μm, or even greater than 3 μm.

[0073] Due to this thickness, combined with the aforementioned porosity, the porous portion of the support substrate has a much lower Young's modulus than non-porous silicon carbide and therefore behaves more favourably to reduce the mechanical stresses exerted on the brazing filler when the device is subjected to temperature changes.

[0074] Fig.13It is a graph (obtained by computer simulation) of the relative stress at the fatigue point in the brazed portion as a function of the Young's modulus E of various substrates made of silicon carbide with porous portions of various thicknesses. The total thickness of each substrate is 350 μm. Curve 1 corresponds to a substrate without a porous portion, curve 2 corresponds to a porous portion thickness of 1 μm, curve 3 corresponds to 5 μm, curve 4 corresponds to 10 μm, curve 5 corresponds to 25 μm, curve 6 corresponds to 50 μm, and curve 7 corresponds to a porous portion thickness of 100 μm. Each curve represents the stress in the brazed portion at the outermost contact point between the brazed portion and the porous SiC divided by the stress in the absence of a porous layer.

[0075] When the thickness of the porous part increases, the stress at the fatigue point of the brazed part decreases. In the simulation, it is assumed that the Young's modulus of the porous SiC depends on the porosity, as Fig.12 As shown. For example, in the case of a porosity of 5%, the Young's modulus is 400 GPa. In the case of a 10 μm thick layer (curve 4), a relative stress at the fatigue point of 0.93 is obtained, that is to say a stress reduction of 7% compared to a substrate without porous parts. For a porosity of 15%, corresponding to a Young's modulus of 300 GPa and a porous layer of 20 μm thickness, the relative stress at the fatigue point is 0.8 and is therefore reduced by 20% compared to a substrate without porous parts.

[0076] The Young's modulus of the porous portion of the support substrate at the soldering interface is closer to that of the DBC structure than the Young's modulus of the surface layer. This means that the deformations caused by temperature changes are less significant and closer to the deformations of the DBC structure and soldering. Therefore, the mechanical stresses imposed on the soldering due to these deformations are not as significant as in known chips. The reduction of these stresses prolongs the service life of the soldering and the RF or power electronic devices.

[0077] Finally, the presence of such a porous portion on the back side of the substrate does not adversely affect the conductivity of the substrate in power applications.

[0078] Exemplary Embodiments

[0079] Figure 2 The first substrate according to the present invention is illustrated, and the first substrate includes a support substrate 30 and a surface layer 1. The support substrate 30 is composed of a single porous portion 3 made of porous silicon carbide with uniform porosity. The porous portion is made of sintered silicon carbide, porous polycrystalline silicon carbide or porous single-crystalline silicon carbide. The porous portion extends from the back 20 of the support substrate 30 to the front 10. The surface layer 1 is made of non-porous single-crystalline silicon carbide. The layer is arranged on the front side of the support substrate 30. In some embodiments, the porous portion and the surface layer are formed as a single piece by a single substrate of single-crystalline silicon carbide.

[0080] Figure 3 A second embodiment is illustrated, wherein a support substrate 30 includes a portion 3A made of porous silicon carbide extending from the back side 20 of the substrate. The porosity of the portion 3A is uniform. The holes are interconnected and filled with air. The support substrate 30 additionally includes a non-porous portion 2A made of polycrystalline silicon carbide disposed between the porous portion and the front side 10 of the support substrate 30. A surface layer 1 made of non-porous single-crystal silicon carbide is disposed on the front side 10 of the support substrate 30.

[0081] Figure 4 A third embodiment is illustrated, in which a support substrate 30 includes a portion 3B made of sintered silicon carbide extending from the back side 20 of the substrate. The sintered silicon carbide includes carbon inclusions that can be separated from each other. Therefore, the pores are filled with carbon and are generally not connected to each other. The porosity of this portion is uniform. The support substrate 30 also includes a non-porous portion 2B made of polycrystalline silicon carbide disposed between the porous portion 3B and the front side 10 of the support substrate 30. A surface layer 1 made of non-porous single-crystal silicon carbide is disposed on the front side 10 of the support substrate 30.

[0082] Figure 5 A fourth embodiment is illustrated, in which a support substrate 30 includes the following in order from its back side 20 to its front side: a first porous portion 3C made of porous silicon carbide, a second porous portion 2D made of sintered silicon carbide, and a non-porous portion 2C. The pores of the first porous portion 3C are interconnected and filled with air. The pores of the second porous portion 2D are filled with carbon inclusions and separated from each other. The porosity of the layer 3C made of porous silicon carbide is greater than the porosity of the portion 2D made of sintered silicon carbide. A surface layer 1 made of non-porous single-crystal silicon carbide is provided on the front side 10 of the support substrate 30.

[0083] In other embodiments not illustrated, the porous portion made of porosified silicon carbide has a porosity gradient such that the porosity decreases in a direction from the back surface toward the front surface of the support substrate.

[0084] In other embodiments not illustrated, multiple parts made of sintered silicon carbide or porous silicon carbide can overlap to form the support substrate 30 or parts of the support substrate 30. In the various porous parts, the size and shape of the holes can be similar or different. Advantageously, in each porous part present in the substrate, the average distance between the holes is greater than 10nm, preferably greater than 50nm, to avoid the formation of possible depletion zones in the SiC.

[0085] In some embodiments, a support substrate that may be non-self-supporting is used to form a radio frequency or power electronic device. The substrate includes a support substrate made of polycrystalline silicon carbide having a front side and a back side, and a single crystal silicon carbide surface layer extending on the front side of the support substrate, the substrate being characterized in that the support substrate has at least one porous portion extending from the back side, the porous portion having a porosity greater than 5%. At least one radio frequency or power electronic component is formed in or on the single crystal silicon carbide layer.

[0086] The device may further include a heat release device, the substrate being brazed to the heat release device via a filler material so that the filler material is in integral contact with at least a portion of the porous portion on the back side of the supporting substrate.

[0087] Substrate manufacturing

[0088] Various embodiments of steps for manufacturing a substrate will now be described.

[0089] The formation of the substrate according to the present invention includes the formation of at least one porous portion.

[0090] The porous portion can be formed by making the silicon carbide substrate porous. Known methods for making silicon carbide porous can be applied to form the porous portion, and some methods are described or cited in publications by Y. Shishkin et al. and Gautier et al. Porosification can be performed from the front or back of the substrate.

[0091] The porosification step can be carried out, for example, by immersion in an acid bath or electrochemically or photoelectrochemically. The electrochemical porosification can be an electrochemical anodization, in which the part to be porosified is placed in an electrolyte, for example, a solution containing hydrofluoric acid and / or ethanol. The anode and cathode immersed in the electrolyte are connected to a power supply to apply an electric current between the electrodes. Anodization causes, to a certain extent, electrochemical decomposition of the silicon carbide crystals in the region of the silicon carbide porous layer. Instead of uniformly decomposing the silicon crystals, the electrochemical decomposition can locally remove silicon atoms from the crystal lattice of the silicon carbide, thereby forming small holes or pores in the silicon carbide crystals. At the end of the treatment, the porosified part is rinsed to remove the residues of the electrolyte.

[0092] During the porosification step, the non-porous structure of parts of the substrate can be retained. In this case, the parts concerned remain outside the electrolyte bath.

[0093] In some cases, the porosity thus formed is uniform across the entire support substrate except for the surface layer. In other embodiments, a porosity gradient is created that decreases from the back to the front, so that the porosity near the surface layer is lower and the porosity near the back is greater. The porosity can also be gradually increased by first setting the porosification parameters for a certain thickness of the substrate and continuing the porosification in multiple sections of decreasing thickness extending from the back of the substrate. For each successive section, the porosification parameters can be modified to create a porosity greater than the previous step.

[0094] The porosity can be modified and the gradient created by varying different parameters of the substrate (e.g., doping) and different parameters of the porosification process (e.g., applied current and voltage, temperature, composition of the electrolyte, and in some cases, intensity and wavelength of the applied light).

[0095] As an alternative, the porous portion can be formed by sintering the silicon carbide before assembling the substrate. Sintering is a heat treatment of a structure made of silicon carbide at a temperature between 1600° C. and 2400° C. in an atmosphere that can be, for example, argon, nitrogen or an inert gas. This heat treatment can change the distribution of carbon and silicon present in the substrate, forming inclusions composed of carbon in the silicon carbide.

[0096] In some embodiments, the porous region can be formed directly in the single-crystal silicon carbide substrate including the surface layer by making the substrate porous over part of its thickness. In this case, the porous region is made from the back side.

[0097] In other embodiments, the formation of the substrate may include assembling a support substrate and a surface layer. The porous region of the support substrate may be formed before or after said assembling.

[0098] In some embodiments, the formation of the support substrate may include one or more steps of assembling two or more porous portions and / or a porous portion and a non-porous portion.

[0099] The layers or parts of the substrate can be assembled by bonding, for example from a donor substrate in which weakened areas are created to define the layers to be assembled. In this case, Smart Cut is often used. TM Type treatment. A weakened region is formed in a donor substrate made of single-crystalline silicon carbide, the weakened region being used to delimit the layer to be assembled on the support substrate. The weakened region is typically created by irradiation with ions, such as hydrogen and / or helium ions. The donor substrate is then bonded to the front side of the support substrate, the layer delimited by the weakened region being arranged in direct contact with the front side of the support substrate. The donor substrate is then separated along the weakened region in order to transfer the single-crystalline silicon carbide layer to the support substrate, for example by using a heat treatment.

[0100] Another technique for weakening the donor substrate is to create a weakened region with a higher porosity than the porosity of the material near this region. In this case, after bonding to the support substrate, the donor substrate can be separated by applying a mechanical stress. Such a mechanical stress is, for example, the insertion of a blade or another beveling tool, or the application of an air jet or a water jet. This technique can be used to transfer a porous layer or for a thinning operation as described below.

[0101] Another embodiment of the assembly is deposition on the provided portion of the substrate, such as chemical vapor deposition (CVD) or physical vapor deposition (PVD). For example, a polycrystalline silicon carbide layer can be deposited by CVD or PVD on a single-crystal silicon carbide surface layer or on another layer of (porous or non-porous) polycrystalline silicon carbide, and all or part of the deposited layer can be made porous.

[0102] The step of assembling the support substrate and the single-crystal silicon carbide surface layer may be performed on a base substrate for forming the support substrate, on a finished support substrate, or at the end of one or more steps of forming the support substrate.

[0103] In case of bonding two porous parts or a porous part and a non-porous part, the porosity of the bonding interface is preferably less than 40%, preferably less than 15%, more preferably less than 5% to ensure good bonding between the two parts.

[0104] One or more optional thinning steps may be performed to set the thickness of the support substrate or a portion of the support substrate and the porosity on its back side. To perform this thinning step, a weakened area with a porosity greater than 10%, advantageously greater than 15%, particularly advantageously greater than 30% may be created from the back side of the porous area to be formed at a determined depth corresponding to the thickness of the porous portion to be formed relative to the porous area to be formed. Then, or after a step of assembling one or more layers on the front side of the substrate, the substrate may be cut along the weakened area created. The cutting may be performed by applying a mechanical stress, for example by inserting a blade or by applying an air jet or a water jet. The stress must be suitable for propagating a fracture wave along a weakened area, the mechanical strength of which is less than the mechanical strength of the area surrounding it. Advantageously, such a weakened area is surrounded by a portion made of polycrystalline silicon carbide having a lower porosity than the weakened area (a porosity lower by, for example, 1% or 5%, advantageously a porosity lower by 10%).

[0105] In some embodiments, the substrate is thinned by breaking the porous portion of the surface away from the porous region that will be secured to the soldering of the electronic component. This thinning avoids a polishing step that can be lengthy and expensive.

[0106] The thinning step can also be performed by chemical etching or mechanical abrasion techniques.

[0107] Preferably, a porous portion having a thickness greater than 100 nm, advantageously greater than 1 μm and particularly advantageously greater than 3 μm is retained. The thickness of the layer has an influence on the deformation caused by temperature changes. Thus, as the thickness of the porous portion increases, the mechanical stress applied to the soldering portion of the electronic chip is further reduced.

[0108] One or more thinning steps may also be applied at the end of creating a porous part to set the thickness of the porous part before assembly with another porous or non-porous part.

[0109] An optional step of passivation, or another treatment of the back side, may be performed, for example by depositing a dielectric layer, such as silicon oxide, which forms a barrier to avoid direct contact between silicon carbide and the surrounding air and thus to avoid creating a depletion zone involving a drop in the conductivity of the back side.

[0110] Exemplary Embodiments

[0111] FIG. 7A to FIG. 7D A method of manufacturing a substrate according to the present invention is illustrated in which the surface layer and the support substrate are manufactured from a single starting substrate 40 made of single-crystal silicon carbide.

[0112] Reference Fig. 7A , a front surface 410 is selected, preferably a silicon surface. The front surface 410 may be processed, for example, polished. The portion extending from the front surface 410 is used to form the surface layer 41.

[0113] Then, refer to Figure 7B , porosity is formed from the back surface 420 of the portion for forming the support substrate 43 so that porosity is not formed in the portion for forming the surface layer 41.

[0114] Optionally, one or more additional layers 43B, 43C may then be assembled on the back side of the support substrate 43. The assembly of the first layer 43B is as follows: Figure 7C As illustrated. The first layer 43B has a higher porosity than the portion 43 extending from the back side 420 of the porous single substrate. Such a layer is, for example, a layer made of sintered silicon carbide or a layer made of porous silicon carbide, or a combination of two or more porous layers. The layer made of sintered silicon carbide can be obtained, for example, by reaction sintering at a temperature of about 2000° C. This forms a new back side 421 of the support substrate 430 to be formed.

[0115] The optional assembly of the second layer 43C is Fig.7D 422 of the substrate to be formed. The second layer 43C has a higher porosity than the back of the first layer 43B. This forms a new support substrate 431, the porosity of which increases continuously from the front side 410 to the back side 422 of the support substrate 431 formed.

[0116] One or more layers 43B, 43C may also be assembled on the back side of the substrate 420 and / or additional porosification may be performed after the assembly (not illustrated). For example, a layer made of sintered silicon carbide may first be bonded to the back side of the starting substrate, then a polycrystalline silicon carbide layer may be deposited on the back side of the layer made of sintered silicon carbide, and a step of porosifying the layer made of polycrystalline silicon deposited on the layer made of sintered silicon carbide may be performed.

[0117] exist FIG. 8A to FIG. 8C A preferred embodiment is illustrated in . First, a support substrate 530 is formed and then assembled with a surface layer 51 made of single-crystal silicon carbide.

[0118] Reference Fig. 8A , a substrate 50 made of polycrystalline silicon carbide forms a support substrate. Figure 8B , the portion 53 for forming the porous portion extending from the back surface 520 of the substrate to be formed is made porous. Figure 8C The support substrate is assembled with the single crystal silicon carbide surface layer 51 on its front side 510, usually using the Smart Cut TM Type processing.

[0119] To illustrate this variation of embodiment, FIG. 8D to FIG. 8I A more complex process is illustrated in . In this embodiment, a support substrate is first formed and then assembled with a surface layer 51 made of single-crystal silicon carbide.

[0120] To form a support substrate, refer to Fig.8D , a polycrystalline silicon carbide substrate 50 may be used as a basis. The substrate may then be made porous as described above to form a porous region 53 extending from the back side 520 of the substrate 50. Fig. 8E , porosification may be performed by maintaining the portion 52 extending from the front side 510 in its non-porous initial state so that only the portion 53 extending from the back side 520 of the substrate has porosity. Alternatively, a porosity gradient may be created so that the porosity increases continuously or gradually from the front side 510 to the back side 520 of the substrate 50. In other cases, reference is made to Fig.8F ,like Figure 8B As shown in the example, the substrate is made porous uniformly throughout the entire thickness.

[0121] Then, refer to Figure 8G, an optional step of bonding a layer 53B having a greater porosity to the back side 520 of the substrate and thereby creating a new support substrate 531 having a new back side 521 can be performed. The layer 53B has a higher porosity than the portion 53 extending from the back side 520 of the porous single substrate. Such a layer is, for example, a layer made of sintered silicon carbide or a layer made of porous silicon carbide having a porosity greater than the porosity of the previously porous portion 53, or a combination of two or more porous layers. This forms a new back side 521 of the support substrate 531 to be formed. Referring to Figure 8H , optionally, an additional porosification step can be performed in the portion 53C extending from the new back side 521 of the substrate to be formed. For this additional porosification step, the parameters will be selected so that the portion 53C has a higher porosity than the porous layer 53B in its initial state. As a result, the porosity of the supporting substrate 532 gradually increases from its front side 510 to its back side 522.

[0122] Optionally, one or more bonding operations (not illustrated) to the back side of the substrate may be performed for other layers with greater porosity.

[0123] Optionally, one or more layers with lower porosity may be assembled on the front side of the substrate (not illustrated).

[0124] Reference Figure 8I The support substrate is provided with a single-crystal silicon carbide surface layer 51 on its front side 510 .

[0125] If no layer is assembled on the front surface of the substrate 532 , the surface layer 51 made of single-crystal silicon carbide may be assembled with the support substrate 532 between any two steps of the process for forming the support substrate 532 .

[0126] In some embodiments not illustrated, before all steps of forming the support substrate are completed, a portion of the support substrate and the surface layer made of single-crystal silicon carbide are assembled while the support substrate is being formed.

[0127] Other implementations are FIG. 9A to FIG. 9B Example in. Reference Fig. 9A , the support substrate may be formed of a substrate made of sintered silicon carbide 60. Sintered silicon carbide generally contains carbon inclusions and is therefore a porous material whose pores are filled with these inclusions.

[0128] Reference Fig. 9B , a support substrate 60 of sintered silicon carbide can be assembled with a single-crystal silicon carbide surface layer 61 on its front side 610. As a result, the substrate made of sintered silicon carbide forms a single porous region 60 extending from its back side 620.

[0129] As an alternative, refer to Fig. 10A, based on the same starting substrate 60 made of sintered silicon carbide. Fig. 10B , a polycrystalline silicon carbide layer 62 can be deposited on the front side 610 of a substrate 60 made of sintered silicon carbide. This deposition can be performed, for example, by physical vapor deposition (PVD). Thus, the substrate 60 made of sintered silicon carbide serves as a support and seed for the polycrystalline silicon carbide. Optionally, holes can be created in the silicon carbide layer 62 thus deposited, such as Fig. 10C In this case, the porosity created in the portion 62 deposited on the front side 610 is less than the porosity in the initial substrate 60 made of sintered silicon carbide. In some cases, the layer 62 remains in its non-porous initial state.

[0130] Optionally, refer to Fig. 10D , a second polycrystalline silicon carbide layer 63 may be deposited on the back side 620 of the substrate made of sintered silicon carbide to form a new support substrate 630 having a new back side 621. Then, referring to Fig.10E , a step of making the layer 63 made of polycrystalline silicon carbide on the back side 620 porous is performed so that the layer 63 on the back side has a greater porosity than the substrate 60 made of sintered silicon carbide.

[0131] An optional step (not illustrated) may then be performed of bonding and / or assembling one or more layers with greater porosity onto the back side of the substrate, or bonding and / or assembling one or more layers with lesser porosity onto the front side of the substrate.

[0132] Reference Fig.10F The support substrate thus created is assembled with the surface layer 61 made of single-crystal silicon carbide on the front side 611 of the support substrate.

[0133] In another embodiment, reference Fig.11A , based on a donor substrate 70 made of single-crystal silicon carbide, a portion 71 on the front side 710 of the donor substrate 70 is used to form a surface layer. Fig. 11B , a weakened area 77 is formed to delimit a portion 71 for forming the front side of the substrate to be formed. The weakened area is preferably created by implanting hydrogen and / or helium atoms in the donor substrate.

[0134] Reference Fig. 11C , a portion 73 made of polycrystalline silicon carbide is assembled on the front side 710. The porosity of the portion 73 can be formed before or after the portion 73 is assembled on the front side 71 of the donor substrate 70. For example, the portion 73 can be made of silicon carbide that is porosified or sintered before the bonding operation. Alternatively, the portion 73 made of polycrystalline silicon carbide can be deposited on a donor substrate 70 made of single-crystalline silicon carbide, for example by CVD or PVD, and a porosification step is performed on the portion 73 after the deposition step.

[0135] The porosity of portion 73 may be uniform, have a gradient or multiple levels, or affect only a certain thickness of the substrate.

[0136] Reference Fig.11D , for example, by heat treatment to separate the donor substrate 70 from the portion 71. Fig.11E , portion 73 forms a supporting substrate made of porous silicon carbide, and portion 71 forms a surface layer of a finished substrate made of single-crystal silicon carbide.

[0137] In some embodiments, a substrate made of single crystal silicon carbide for forming a surface layer is used as a basis. Then, a support substrate is formed on the substrate made of single crystal silicon carbide so that the front of the substrate contacts the substrate made of single crystal silicon carbide. The formation of the support substrate may include one or more steps of deposition, porosification, sintering and assembling multiple parts of the support substrate. Then, the substrate made of single crystal silicon carbide as described above can be thinned.

[0138] Chips for radio frequency and / or power electronic applications can then be formed from this substrate. When the device is designed for radio frequency applications, the electronic chip can be formed in a layer of silicon carbide or nitride from the III-N group, for example a stack of layers GaN / AlGaN / AlGaNInN defining a two-dimensional electron gas. This layer or this stack is carried by a surface layer made of single-crystalline silicon carbide.

[0139] References

[0140] Y.Shishkin et al.:Photoelectrochemical etching of n-type 4H siliconcarbide,Journal of Applied Physics 96,2311,2004

[0141] Gautier et al.:Electrochemical formation of porous silicon carbide for micro-device applications,Materials science forum,ISSN:1662-9752,vol.924,pages 943-946,2018

[0142] LLSnead et al.,Journal of Nuclear Materials 371(2007)329-377

Claims

1. A substrate for a radio frequency or power electronic device, the substrate include: o a support substrate (30) made of polycrystalline silicon carbide, the support substrate having a front side (10) and a back side (20), the support substrate (30) being self-supporting, and o a single-crystal silicon carbide surface layer (1) extending on the front side (10) of the support substrate (30), The substrate is characterized in that the support substrate (30) has at least one porous portion (3) extending from the back side (20), and the porous portion (3) has a porosity greater than 5%.

2. The substrate according to claim 1, in, The support substrate (30) has a thickness greater than 50 μm, advantageously greater than 80 μm, more advantageously greater than 100 μm and even more advantageously greater than 150 μm.

3. The substrate according to any one of claims 1 and 2, in, The porous portion (3) includes a porous SiC layer (3, 3A, 3C).

4. The substrate according to any one of claims 1 to 3, in, The support substrate (30) includes: a non-porous portion (2A, 2B, 2C) between the single-crystal SiC surface layer (1) and the porous portion (3).

5. The substrate according to any one of the preceding claims, in, The porous portion (3) has a rear portion (3A, 3B, 3C) having a first porosity and a front portion (2A, 2B, 2C) having a second porosity smaller than the first porosity.

6. The substrate according to any one of the preceding claims, in, The porous portion (3) has a porosity gradient that decreases from the back side (20) to the front side (10).

7. The substrate according to any one of the preceding claims, in, The porous portion (3) has pores filled with a material having a Young's modulus lower than that of the silicon carbide.

8. The substrate according to any one of the preceding claims, in, The porous part (3) has pores, the average distance between the pores being greater than 10 nm, preferably greater than 50 nm.

9. An electronic device comprising a substrate according to any one of the preceding claims and at least one radio frequency or power electronic component formed in or on the single crystal silicon carbide surface layer (1).

10. The electronic device according to claim 9 further comprises a heat release device, wherein the substrate is brazed to the heat release device via a filler so that the filler is in integral contact with at least a portion of the porous portion (3) on the back side (20) of the supporting substrate (30).

11. A method for manufacturing a radio frequency or power electronic device, the radio frequency or power electronic device include: o a self-supporting support substrate (30) made of polycrystalline silicon carbide having a front side (10) and a back side (20), and o a single-crystal silicon carbide surface layer (1) extending on the front side (10) of the support substrate (30), The method is characterized in that it comprises the step of forming at least one porous portion (3) extending from the back surface (20) in the support substrate (30), the porous portion (3) having a porosity greater than 5%.

12. The method according to claim 11, further comprising: include: The step of assembling the surface layer (1) and the supporting substrate (30).

13. The method according to claim 11 or 12, in, The support substrate (30) has a thickness greater than 50 μm, advantageously greater than 80 μm, more advantageously greater than 100 μm and even more advantageously greater than 150 μm.

14. The method according to any one of claims 11 to 13, in, The formation of the support substrate (30) includes the step of making at least a portion of a non-porous silicon carbide base substrate porous to form the porous portion (3).

15. The method according to claim 14, in, Porosification is performed on all of the base substrates to form a fully porous support substrate (30).

16. The method according to any one of claims 14 and 15, in, The porosification is performed so as to form a porosity gradient which decreases from the back side (20) to the front side (10) in the porous portion (3).

17. The method according to any one of claims 14 to 16, in, The porosification is performed so as to form a bonding area having a porosity of less than 40% on the front side (10) of the support substrate (30).

18. A method according to any one of claims 11 to 17, comprising the step of filling at least some of the pores of the porous portion (3) with a material having a Young's modulus lower than that of silicon carbide.

19. The method according to any one of claims 11 to 18, further comprising the step of thinning the support substrate (30) via the back surface (20) so that the thickness of the porous portion (3) remains greater than or equal to 100 nm.