Preparation method of silicon block thermoelectric conversion material, silicon block thermoelectric conversion material and thermoelectric conversion element
By combining nanoporous structures and nanocrystal structures in silicon bulk thermoelectric conversion materials, the bonding and doping distribution of silicon nanoparticles is solved, and the problems of high thermal conductivity and poor thermal conductivity in the prior art are achieved. The combination of rate and high conductivity improves thermoelectric performance and is suitable for thermoelectric conversion devices with block size.
Patent Information
- Application Number
- CN202380024870.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-21
- Filing Date
- 2023-02-24
- Publication Date
- 2024-11-15
AI Technical Summary
It is difficult for existing thermoelectric conversion materials to improve thermoelectric properties while reducing thermal conductivity, and most of the materials used are high toxicity, poor environmental adaptability and high cost, resulting in the lack of popularity and practicality of thermoelectric conversion devices.
By preparing a silicon bulk thermoelectric conversion material with multiple silicon nanoparticles, the combination of nanoporous structure and nanocrystal structure is used to control the bonding and dopant distribution of silicon nanoparticles, reduce thermal conductivity and improve electrical conductivity, and form electrical conductivity by using the combination of nanoporous structure and nanocrystal structure. path to increase the ZT value.
The combination of low thermal conductivity and high electrical conductivity under the block size is achieved, and the thermoelectric performance is improved. Specifically, the ZT value reaches more than 0.10 and the thermal conductivity is within the range of 2.0W/m·K to 9.0W/m·K , the conductivity and Seebeck coefficient have been significantly improved, and are suitable for energy harvesting equipment such as IoT power supplies.
Smart Images

Figure CN118975435A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to silicon bulk thermoelectric conversion materials. Background Art
[0002] In recent years, there has been an increasing number of studies aimed at improving the performance of thermoelectric conversion materials. Thermoelectric conversion is a technology that can directly convert heat and electricity. Since it can generate electricity from low-temperature heat sources such as waste heat that have been difficult to use until now, it has attracted much attention as a power source for energy harvesting devices such as IoT sensor devices. The performance of thermoelectric conversion materials is expressed by the dimensionless performance index ZT.
[0003] [Mathematical formula 1] Where S is the Seebeck coefficient, σ is the electrical conductivity, T is the absolute temperature, and κ is the thermal conductivity. From this formula, it can be seen that the performance of thermoelectric conversion materials can be improved by any of the following: (1) increasing the Seebeck coefficient S or the electrical conductivity σ, or (2) reducing the thermal conductivity κ.
[0004] In recent years, many research groups have reported research results in which ZT significantly exceeds 1. On the other hand, when considering the use as an energy collection device, a significant increase in the ZT value is not essential, and a higher ZT is not necessarily required as long as the preparation cost can be suppressed to a low level. However, most of the research reported so far has used materials with high toxicity and poor environmental adaptability or high-priced materials. Therefore, the above-mentioned cost-effectiveness problem cannot be solved, and the popularization and practical application of thermoelectric conversion devices have not yet been achieved. Among them, from the perspective of preparation cost, silicon is a material with high buried volume, non-toxicity, and high stability, and the currently popular silicon processing technology can be applied, so it is an effective material as a thermoelectric conversion material. However, the thermal conductivity of silicon is more than 100 W / m·K, and even if it is simply converted into a thermoelectric conversion material, the ZT value is about 0.005, which is currently completely unsuitable for practical application. Therefore, Patent Document 1 achieves a reduction in thermal conductivity by making nanowires with an "aspect ratio of more than 10" (Claim 1, paragraph
[0009] , etc.). In addition, Patent Document 2 provides "a thermoelectric material characterized in that it is composed of a porous body having a plurality of micropores and having any one of magnesium-silicon alloy, magnesium-silicon-tin alloy, silicon, or silicon-germanium alloy as a main component" as a solution. However, this means that a practical ZT value cannot be obtained in single silicon or trace-doped silicon, so thermoelectric materials are explored based on alloy materials (germanium, etc.). Prior art literature Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2016-504756 Patent Document 2: Japanese Patent Application Publication No. 2015-053466 Patent Document 3: International Publication No. 2019 / 131795 Summary of the invention Problem that the invention aims to solve
[0006] Patent document 1 achieves a reduction in thermal conductivity by making nanowires. However, in the case of practical use as a device, since nanowires are not of a practical size, a bulk thermoelectric conversion material needs to be used. On the other hand, it is not easy to prepare a bulk thermoelectric conversion material using nanowires. In addition, it can be seen from Patent document 2 that the reduction in thermal conductivity is achieved by using alloys, and that the material in elemental silicon or in which dopants are doped in silicon has not achieved the production of practical thermoelectric conversion materials. Therefore, one of the purposes of one embodiment of the present invention is to provide a silicon bulk thermoelectric conversion material that has reduced thermal conductivity and improved thermoelectric performance compared to previous materials. Alternatively, one of the purposes of one embodiment of the present invention is to provide a method for preparing a silicon bulk thermoelectric conversion material that has reduced thermal conductivity and improved thermoelectric performance compared to previous methods. Means of solving the problem
[0007] According to one embodiment of the present invention, there is provided a method for preparing a silicon bulk thermoelectric conversion material, which comprises: a receiving step of placing silicon powder containing silicon nanoparticles between a first electrode component and a second electrode component of a heating part, wherein the heating part comprises a first electrode component, a second electrode component and a conductive cylindrical component in which at least one of the first electrode component and the second electrode component is slidably engaged; a heating step of heating the silicon powder by applying a pressure of less than 12 MPa, preferably less than 10 MPa, less than 5 MPa or less than 3 MPa, between the first electrode component and the second electrode component while passing an electric current; and a cooling step of cooling the heated silicon powder.
[0008] The cooling process may include monitoring the displacement of the first electrode member and the second electrode member and stopping the heating when the displacement reaches a specified value.
[0009] The method may further include a preparation step of mixing silicon nanoparticles and dopant particles to prepare silicon powder.
[0010] The average particle size of the silicon nanoparticles may be 100 nm or less.
[0011] The dopant particles are phosphorus particles or boron particles having an average particle diameter of 100 μm or less.
[0012] According to one embodiment of the present invention, a silicon bulk thermoelectric conversion material is provided, which is a silicon bulk thermoelectric conversion material having a plurality of silicon nanoparticles, wherein the plurality of silicon nanoparticles are bonded to each other on a portion of the surface, and the silicon bulk thermoelectric conversion material is provided with holes separating the surfaces of the plurality of silicon nanoparticles from each other, and in the Raman spectrum, the silicon bulk thermoelectric conversion material has a Raman spectrum at 510 cm -1 Over 520cm -1 There is a peak below, and ZT is 0.10 or more in the range of 22°C to 25°C.
[0013] When the weight of the silicon bulk thermoelectric conversion material is set to 100 weight %, phosphorus or boron may be contained in an amount of 1 weight % to 10 weight %.
[0014] The thermal conductivity of the silicon bulk thermoelectric conversion material is within a range of 3.0 W / m·K to 6.0 W / m·K, and longitudinal waves propagate at a sound velocity of 5800 m / s or less and transverse waves at a sound velocity of 4200 m / s or less.
[0015] The thermal conductivity of the silicon bulk thermoelectric conversion material is in the range of 2.0 W / m·K or more and less than 3.0 W / m·K, and the longitudinal wave propagates at a sound velocity of 5300 m / s or less and the transverse wave propagates at a sound velocity of 3400 m / s or less.
[0016] The thermal conductivity of the silicon bulk thermoelectric conversion material is within the range of 3.0 W / m·K or more and less than 4.0 W / m·K, and the longitudinal wave propagates at a sound velocity of 6100 m / s or less and the transverse wave propagates at a sound velocity of 3700 m / s or less.
[0017] The thermal conductivity of the silicon bulk thermoelectric conversion material is within the range of 4.0 W / m·K to 9.0 W / m·K, and the longitudinal wave propagates at a sound velocity of 6400 m / s or less and the transverse wave propagates at a sound velocity of 4200 m / s or less.
[0018] According to one embodiment of the present invention, a silicon bulk thermoelectric conversion material is provided, which is a silicon bulk thermoelectric conversion material including a plurality of silicon nanoparticles; the plurality of silicon nanoparticles are bonded to each other on part of their surfaces; there are holes in the silicon bulk thermoelectric conversion material that separate the surfaces of the plurality of silicon nanoparticles from each other; and the ZT calculated using the conductivity and the Seebeck coefficient measured at any measurement atmosphere temperature within the range of not less than 40°C and not more than 50°C is not less than 0.10.
[0019] According to one embodiment of the present invention, there is provided a thermoelectric conversion element including a component made of any one of the above-mentioned silicon bulk thermoelectric conversion materials, wherein the thickness of the component is 1 mm or more. Effects of the Invention
[0020] According to one embodiment of the present invention, a practical silicon bulk thermoelectric conversion material can be provided. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 FIG. 1 is a schematic diagram showing the structure of a silicon bulk thermoelectric conversion material 100 according to an embodiment of the present invention. Figure 2 1 is a schematic diagram showing a spark plasma sintering apparatus 1 (heating unit) according to one embodiment of the present invention. Figure 3 1 is a diagram for explaining a method for preparing a silicon bulk thermoelectric conversion material 100 according to an embodiment. Figure 4 Schematic diagram showing a thermoelectric conversion element 500 according to an embodiment of the present invention. Figure 5 It is a graph showing the relationship between the displacement amount of the first punch 5a and the second punch 5b and the thermal conductivity. Fig. 6A This is a graph showing the relationship between the Seebeck coefficient and the electrical conductivity of a silicon bulk thermoelectric conversion material. Figure 6B This is a diagram showing the relationship between ZT and temperature of a silicon bulk thermoelectric conversion material. Fig. 7A This is a diagram showing the Raman spectrum of a silicon bulk thermoelectric conversion material. Figure 7B This is a diagram showing the distribution of the acoustic velocity and thermal conductivity of a silicon bulk thermoelectric conversion material. Figure 8 It is a diagram showing the uniformity of the resistivity and Seebeck coefficient of a silicon bulk thermoelectric conversion material. DETAILED DESCRIPTION
[0022] Below, the embodiments of the present invention are described with reference to the accompanying drawings. However, the present invention can be implemented in a plurality of different ways and cannot be interpreted as being limited to the contents of the embodiments illustrated below. In addition, in order to make the description clearer, the width, thickness, shape, etc. of each part compared with the actual method are sometimes schematically shown in the accompanying drawings, but this is only an example and does not limit the interpretation of the present invention. In addition, in this specification and the accompanying drawings, the same elements as those described in the drawings shown are marked with the same figure numerals, and detailed descriptions are sometimes appropriately omitted. In this specification, when a certain component or region is located "above (or below)" another component or region, as long as there is no special limitation, it not only includes the situation that it is located directly above (or directly below) another component or region, but also includes the situation that it is located above (or below) another component or region, that is, it also includes the situation that other structural elements are included between the above (or below) of another component or region.
[0023] In a nanocrystalline structure, when phonons collide with a grain boundary, some phonons are scattered and some phonons are transmitted. On the other hand, in a nanoporous structure, all phonons that collide with the pore surface are scattered. Therefore, it is believed that as long as a nanoporous structure is used, the scattering of phonons can be promoted more than that of a nanocrystalline structure, and thermal conductivity can be reduced without forming an alloy or forming nanowires.
[0024] The inventors of the present invention have shown in Patent Document 3 that thermal conductivity can be reduced to a greater extent than ever before by combining a nanoporous structure and a nanocrystalline structure. In Patent Document 3, a silicon bulk thermoelectric conversion material can be prepared by performing metal-assisted etching on a silicon substrate to form a nanowire array structure, and by plasma sintering while pressurizing, the nanowire array structure is sintered while being crushed into fine particles with a small aspect ratio.
[0025] The inventors of the present invention further discovered that in the preparation method of Patent Document 3, since the nanowire arrangement structure is sintered while being crushed into fine particles with a small aspect ratio, some nanoporous structures disappear due to the melting of the fine particles and the thermal conductivity increases due to the grain growth of the nanocrystalline structure.
[0026] In the present invention, the inventors of the present invention achieved low thermal conductivity by controlling the interface where the silicon fine particles are bonded when sintering the silicon fine particles, thereby reducing the group velocity of phonons.
[0027] [Constitution of the present invention] Figure 1 Schematic diagram showing the structure of a silicon bulk thermoelectric conversion material 100 according to one embodiment of the present invention. Specifically, it was found that the thermal conductivity can be significantly reduced by forming a nanoporous structure with appropriately controlled silicon nanoparticles 110, cavities 120 existing between the silicon nanoparticles 110, and joints 130 mutually joined on a portion of the surface of the silicon nanoparticles 110. It should be noted that in this specification, the so-called "bulk" refers to a size having a length of 1 mm or more in all directions (in mutually orthogonal X-axis directions, Y-axis directions, and Z-axis directions).
[0028] [Silicon Nanoparticles 110] In the present embodiment, the silicon nanoparticles 110 of the silicon bulk thermoelectric conversion material 100 have an average size of 5 nm to 120 nm. The thermal conductivity of the silicon nanoparticles 110 of 34.4 nm to 111.6 nm can be reduced to a range of 1.47 W / mK to 8.95 W / mK, so it is preferred. There are multiple silicon nanoparticles. The so-called silicon nanoparticles 110 of an average of 5 nm to 120 nm means that the size of the silicon nanoparticles 110 (for example, if the cross-sectional shape of the particle is circular, then its diameter; if it is a polygon, then the diameter of its circumscribed circle) has an average value of 5 nm to 120 nm. Among them, the so-called average value of the size of the silicon nanoparticles 110 should not be interpreted as the average value of the entire wide distribution, but should be understood as the particle size with the maximum frequency of the main particle size constituting the peak. In the present invention, the silicon nanoparticles 110 of an average of 5 nm to 120 nm means that the observation area is 0.65 μm using HAADF-STEM (magnification 200,000 times). 2 The average size of the silicon nanoparticles 110 that can be detected in the specified observation area. Any method that includes the observation conditions in the following section and can observe with the same or higher resolution and the same or higher observation area can replace the observation method of the present invention.
[0029] [Crystalline size] In this specification, the size of the silicon nanoparticles 110 of the silicon bulk thermoelectric conversion material 100 can also be evaluated by the crystallite size. The crystallite size is measured by X-ray diffraction (focusing method). The silicon bulk thermoelectric conversion material 100 according to an embodiment of the present invention has a crystallite size of 35 nm or more and 120 nm or less.
[0030] The particle size distribution of the silicon nanoparticles 110 preferably has a sharp peak. With such a particle size distribution, electrical conductivity between the silicon nanoparticles 110 via the junction 130 can be obtained while maintaining the crystal structure of the silicon nanoparticles 110. In addition, phonons are strongly scattered at the interface between the silicon nanoparticles 110 and the cavities 120, so that thermal conductivity can be reduced.
[0031] [Hole 120] There are cavities 120 between the silicon nanoparticles 110. The cavities 120 separate the surfaces of adjacent silicon nanoparticles 110 from each other, so that phonons are strongly scattered at the interface between the silicon nanoparticles 110 and the cavities 120, and thermal conductivity is reduced.
[0032] [Aspect Ratio of Silicon Nanoparticle 110] The aspect ratio of the silicon nanoparticles 110 is less than 2. The aspect ratio literally refers to the ratio of the long side to the short side of a rectangle, but in this specification, it is not limited to rectangles, and circles and polygons can also be considered. The value is calculated by the ratio of the major axis to the minor axis of the rectangle circumscribed to the crystalline silicon nanoparticle. The limitation of the aspect ratio is an important factor in achieving isotropic and good properties in bulk form. As described later, the silicon bulk thermoelectric conversion material 100 is composed of silicon nanoparticles 110 sintered from particles originally having a small aspect ratio. The silicon bulk thermoelectric conversion material of the present invention is very different from the silicon bulk thermoelectric conversion material described in Patent Document 3, which is composed of particles sintered from crushed nanowires originally having a large aspect ratio.
[0033] [Jointing portion 130] In the silicon bulk thermoelectric conversion material 100, the silicon nanoparticles 110 have joints 130 that are joined to each other on a part of the surface. The joints 130 provide conductivity to two adjacent silicon nanoparticles 110 by providing local bonding between the two adjacent silicon nanoparticles 110. In the silicon bulk thermoelectric conversion material 100, a conductive path 140 is formed via the joints 130. The conductive path 140 formed between the silicon nanoparticles 110 constituting the silicon bulk thermoelectric conversion material 100 imparts conductivity to the entire silicon bulk thermoelectric conversion material 100. On the other hand, as described above, the surface of the silicon nanoparticle 110 except the joints 130 maintains the surface structure of the silicon nanoparticle as a raw material, and forms an interface with the cavities 120.
[0034] [Dopant] In one embodiment, the silicon bulk thermoelectric conversion material 100 may include a dopant. In this embodiment, the dopant is dispersed and configured inside the silicon nanoparticle 110, preferably substantially uniformly dispersed and configured. In addition, the dopant may also be configured outside the silicon nanoparticle 110 as a particle containing a dopant within a range that does not damage the conductivity provided by the silicon nanoparticle 110. Phosphorus can be used as an N-type dopant, and boron can be used as a P-type dopant. When the weight of the silicon bulk thermoelectric conversion material 100 is set to 100 weight%, the content of the dopant is 0.01 weight% to 10 weight%, preferably 0.1 weight% to 10 weight%, and more preferably 1 weight% to 3 weight%. It should be noted that the silicon bulk thermoelectric conversion material 100 is doped by heating during sintering in the preparation method described later. Therefore, a portion of the dopant added before sintering is sublimated by heating, and the content of the dopant in the silicon bulk thermoelectric conversion material 100 is lower than the amount of dopant added before sintering.
[0035] [Characteristics of the Silicon Bulk Thermoelectric Conversion Material of the Present Invention] The silicon bulk thermoelectric conversion material 100 having the above-mentioned structure is composed of simple silicon and can achieve a characteristic that ZT exceeds 0.1 in the range of 22°C to 25°C. The so-called simple silicon means that slight impurities are allowed to remain, but it is not an alloy. In addition, as mentioned above, a dopant may be included.
[0036] Among them, in bulk single crystals, the mean free path of each phonon is determined by phonon-phonon scattering. By arranging them on the interface or surface at intervals smaller than the mean free path, thermal conductivity can be effectively reduced from bulk single crystals.
[0037] In the silicon bulk thermoelectric conversion material 100 of this embodiment, by strongly scattering phonons at the interface between the silicon nanoparticles 110 and the holes 120, the conductivity between the silicon nanoparticles 110 in the conductive path 140 provided by the joint 130 can be improved while maintaining the structure with reduced thermal conductivity.
[0038] [Tensile stress] In the silicon bulk thermoelectric conversion material 100, by applying the preparation method described later, tensile stress 150 is generated near the surface of the silicon nanoparticle 110 and inside the silicon nanoparticle 110 near the joint 130. In the silicon bulk thermoelectric conversion material 100, when a P-type dopant is included, the tensile stress of the silicon nanoparticle 110 is, for example, 0.36 GPa or more and 2.43 GPa or less. In addition, when an N-type dopant is included, the tensile stress of the silicon nanoparticle 110 is, for example, 0.36 GPa or more and 0.80 GPa or less. In this specification, tensile stress can be evaluated by Raman spectroscopy. The strain caused by the tensile stress 150 generated near the joint 130 reduces the thermal conductivity in the joint 130. Therefore, in the silicon bulk thermoelectric conversion material 100, two different effects can be achieved at the same time, namely, imparting conductivity through the conductive path in the joint 130 and reducing thermal conductivity through stress.
[0039] [Thermal conductivity] In this specification, the thermal conductivity of the silicon bulk thermoelectric conversion material 100 is calculated by multiplying the thermal diffusivity measured by the laser flash method by the specific heat capacity and the density. The specific heat capacity can be calculated using a measured value or from a literature value of specific heat (e.g., Shanks, HR, Maycock, PD, Sidles, PH & Danielson, GC Thermal conductivity of silicon from 300 to 1400 ° K. Phys. Rev. 130, 1743-1748 (1963)). The silicon bulk thermoelectric conversion material 100 according to an embodiment of the present invention has a thermal conductivity of 1.0 W / m·K or more and 10.0 W / m·K or less, preferably 3.0 W / m·K or more and 6.0 W / m·K or less. As described above, the thermal conductivity of the silicon bulk thermoelectric conversion material 100 which is lower than that of conventional thermoelectric conversion materials can be achieved by configuring the silicon nanoparticles 110 and the cavities 120 and controlling the strain caused by the tensile stress 150 generated near the joint 130 of the silicon bulk thermoelectric conversion material 100.
[0040] [density] In this specification, the density of the silicon bulk thermoelectric conversion material 100 is measured by the Archimedean method. In addition, the relative density is measured by the density of a silicon single crystal (2.33 g / cm 3 ). When the silicon bulk thermoelectric conversion material 100 according to the embodiment of the present invention contains a P-type dopant, it has a value of 1.50 g / cm 3 Above 2.20g / cm 3 Below, preferably 1.90g / cm 3 Above 2.00g / cm 3 When the silicon bulk thermoelectric conversion material 100 according to the embodiment of the present invention contains a P-type dopant, it has a relative density of 67% to 95%, preferably 82% to 86%. In addition, when the silicon bulk thermoelectric conversion material 100 according to the embodiment of the present invention contains an N-type dopant, it has a relative density of 1.60 g / cm 3 Above 2.00g / cm 3 Below, preferably 1.80g / cm 3 Above 1.90g / cm 3 When the silicon bulk thermoelectric conversion material 100 according to the embodiment of the present invention contains an N-type dopant, it has a relative density of 70% to 91%, preferably 78% to 83%.
[0041] [Electrical conductivity] In this specification, the conductivity of the silicon bulk thermoelectric conversion material 100 is measured by a DC four-probe method. In this embodiment, when the conductivity is measured using the same device as the Seebeck coefficient, as described later, when the external atmosphere temperature is in the range of 22°C to 25°C, the temperature of the measurement atmosphere of the sample is set in the range of 40°C to 50°C, or in the range of 43°C to 46°C to measure the conductivity of the silicon bulk thermoelectric conversion material 100. When the silicon bulk thermoelectric conversion material 100 according to an embodiment of the present invention contains a P-type dopant, it has a conductivity of 770S / m to 26000S / m, preferably 10400S / m to 26000S / m. In addition, when containing an N-type dopant, it has a conductivity of 700S / m to 74300S / m, preferably 40500S / m to 74300S / m. When the Seebeck coefficient is constant, the silicon bulk thermoelectric conversion material 100 according to the embodiment of the present invention can achieve a conductivity greater than that of the conventional nanostructured silicon bulk thermoelectric conversion material. This is because, in the silicon bulk thermoelectric conversion material 100, although the thermal conductivity is low, the clean interface of the silicon nanoparticles 110 is maintained, thereby maintaining high conductivity.
[0042] In the silicon bulk thermoelectric conversion material 100, the non-uniform internal strain caused by the silicon nanoparticles 110 and the preparation method described later greatly reduces the transmission speed of phonons. In addition, phonon heat conduction can be suppressed by softening the joint 130 as the heat flux path between the silicon nanoparticles 110, but since the hindrance of the softened joint 130 to electrical conduction is limited, a high electrical conductivity / thermal conductivity ratio is achieved. Therefore, the softening of the joint 130 contributes to the high thermoelectric performance in the silicon bulk thermoelectric conversion material 100.
[0043] [Seebeck coefficient] In this specification, the Seebeck coefficient of the silicon bulk thermoelectric conversion material 100 is measured by the thermoelectric potential method. When the silicon bulk thermoelectric conversion material 100 according to an embodiment of the present invention contains a P-type dopant, it has a Seebeck coefficient of 50 μV / K to 200 μV / K, preferably 100 μV / K to 120 μV / K. When containing an N-type dopant, it has a Seebeck coefficient of 100 μV / K to 350 μV / K, preferably 100 μV / K to 210 μV / K. It should be noted that in the measurement of the Seebeck coefficient, by sandwiching the sample between the upper and lower blocks and heating one of the blocks, a temperature gradient of 30°C to 40°C is generated between the high temperature side end and the low temperature side end of the sample, and the temperature and thermoelectromotive force of the two thermocouples (high temperature side, low temperature side) connected between the two ends are measured. Therefore, in silicon bulk thermoelectric conversion material 100 , even when measured at room temperature of 22° C. to 25° C., the measurement atmosphere temperature of the sample near the thermocouple is, for example, 40° C. to 50° C., or 43° C. to 46° C.
[0044] [ZT] The Seebeck coefficient of the silicon bulk thermoelectric conversion material 100 is not higher than the Seebeck coefficient of the conventional thermoelectric conversion material, but due to the high electrical conductivity of the silicon bulk thermoelectric conversion material 100, a high ZT of 0.10 or more can be achieved within the range of 22°C to 25°C. In addition, when the temperature of the measurement atmosphere when measuring the electrical conductivity is within the range of 40°C to 50°C, or within the range of 43°C to 46°C, the silicon bulk thermoelectric conversion material 100 exhibits a high ZT of 0.10 or more.
[0045] [Speed of sound] In this specification, the sound velocity of the silicon bulk thermoelectric conversion material 100 is measured by an ultrasonic sound velocity measurement method. The thermal conductivity of the silicon bulk thermoelectric conversion material 100 is 1.0 W / m·K to 10.0 W / m·K, preferably the thermal conductivity is in the range of 3.0 W / m·K to 6.0 W / m·K, the longitudinal wave propagates at a sound velocity of 6400 m / s or less, the transverse wave propagates at a sound velocity of 4200 m / s or less, preferably the longitudinal wave propagates at a sound velocity of 5800 m / s or less, and the transverse wave propagates at a sound velocity of 4200 m / s or less. As shown in the embodiments described later, when the silicon bulk thermoelectric conversion material 100 in this embodiment is in the same range of thermal conductivity as the previous silicon bulk thermoelectric conversion material, it has a lower sound velocity of the longitudinal wave and the sound velocity of the transverse wave. Therefore, the lower limits of the sound speed of the longitudinal wave and the sound speed of the transverse wave are not particularly limited. For example, the longitudinal wave propagates at a sound speed of more than 4000 m / s, and the transverse wave propagates at a sound speed of more than 2500 m / s. In one embodiment, the thermal conductivity of the silicon bulk thermoelectric conversion material 100 is in the range of more than 2.0 W / m·K and less than 3.0 W / m·K, the longitudinal wave propagates at a sound speed of less than 5300 m / s, and the transverse wave propagates at a sound speed of less than 3400 m / s. For example, the longitudinal wave propagates at a sound speed of more than 4700 m / s, and the transverse wave propagates at a sound speed of more than 3000 m / s. In addition, in one embodiment, the thermal conductivity of the silicon bulk thermoelectric conversion material 100 is in the range of more than 3.0 W / m·K and less than 4.0 W / m·K, the longitudinal wave propagates at a sound speed of less than 6100 m / s, and the transverse wave propagates at a sound speed of less than 3700 m / s. For example, longitudinal waves propagate at a sound velocity of more than 5000 m / s, and transverse waves propagate at a sound velocity of more than 3200 m / s. Furthermore, in one embodiment, the thermal conductivity of the silicon bulk thermoelectric conversion material 100 is in the range of more than 4.0 W / m·K and less than 9.0 W / m·K, longitudinal waves propagate at a sound velocity of less than 6400 m / s, and transverse waves propagate at a sound velocity of less than 4200 m / s. For example, longitudinal waves propagate at a sound velocity of more than 5200 m / s, and transverse waves propagate at a sound velocity of more than 3300 m / s. A silicon bulk thermoelectric conversion material 100 having such a sound velocity is preferred because the silicon nanoparticles 110 have strain inside.
[0046] [Preparation method] Figure 2Schematic diagram of a spark plasma sintering device 1 (heating unit) according to an embodiment of the present invention. In the present preparation method, the steps of pressurizing and plasma sintering can be implemented by using the spark plasma sintering device 1. The spark plasma sintering device 1 includes, for example, a mold 3 of a cylindrical member, a cylindrical first electrode member (first punch 5a) and a second electrode member (second punch 5b) arranged in contact with the inside of the mold 3 and movable in the up and down direction (L1 direction). The first punch 5a and the second punch 5b are arranged inside the mold 3 to be opposite to each other in the L1 direction. In the spark plasma sintering device 1, at least one of the first punch 5a and the second punch 5b is slidably fitted on the mold 3. In the space surrounded by the mold 3, the first punch 5a and the second punch 5b, a silicon powder 25 containing silicon nanoparticles as a raw material is contained. In addition, although not shown in the drawings, a first electrode is connected to the end of the first punch 5a located outside the mold 3. Similarly, a second electrode is connected to the end of the second punch 5b located outside the mold 3. It should be noted that spacers may be disposed between the first punch 5 a and the first electrode, and between the second punch 5 b and the second electrode.
[0047] In one embodiment, it is preferable to arrange carbon sheets 7 as a protective agent between the die 3 and the first punch 5 a and the second punch 5 b , and between the first punch 5 a and the second punch 5 b and the silicon powder 25 .
[0048] In one embodiment, during the pressurization and plasma sintering process, the sample temperature (the temperature of the silicon powder 25 or the internal temperature of the mold 3) is set to 800°C to 1200°C by electric heating, and the pressure when pressurized along the L1 direction by the first punch 5a and the second punch 5b is 0.3 MPa to 12.0 MPa, preferably to 3.0 MPa or less.
[0049] A general sintered body forms a high-density dense structure by increasing the pressure in the sintering process. In addition, in Patent Document 3, for the purpose of crushing the nanowire arrangement structure, the pressure is applied at a temperature of 50 MPa to 200 MPa. When the powder sample is pressurized with high pressure, the current does not flow through the powder sample, but flows through the mold, thereby increasing the temperature of the heating part. Therefore, the temperature starts to rise from the outside of the powder sample in contact with the mold, and it takes a long time to reach the sintering temperature. In addition, in the case of cooling the silicon bulk thermoelectric conversion material after sintering, the temperature also starts to drop from the heating part, and it also takes a long time to cool the silicon bulk thermoelectric conversion material after sintering. The inventors of the present invention found that during a long period of heating and cooling, grain growth occurs and thermal conductivity increases.
[0050] Figure 31 is a diagram illustrating a method for preparing a silicon bulk thermoelectric conversion material 100 according to an embodiment. Figure 3 In the figure, the solid line represents the preparation method of the silicon bulk thermoelectric conversion material 100 according to the present embodiment, and the dotted line represents the conventional sintering method. In the present embodiment, high-speed sintering and high-speed cooling are applied in the process of pressurization and plasma sintering to suppress the grain growth occurring during heating and cooling. In addition, in the conventional sintering method, the control of turning off the current is implemented after the temperature is raised to a specified temperature and maintained for a specified time, while in the sintering method of the present embodiment, the control of turning off the current is implemented by reaching a specified displacement amount, thereby achieving both control of the thermal conductivity of the sintered body and high-speed sintering / cooling. The specified displacement amount varies depending on the filling amount of silicon nanoparticles as a raw material, the inner diameter of the mold 3 used for sintering, and the initial powder state, but in one embodiment, based on the relationship between the displacement amount and the thermal conductivity (refer to Examples 1, 3 and Figure 5 ), determine the displacement corresponding to a specific thermal conductivity of, for example, 3.0 W / m·K or more and 6.0 W / m·K or less. Alternatively, the specified displacement is determined in the range of 1.5 mm to 2.5 mm or in the range of 0.1 mm to 1.6 mm, respectively, when 0.3 g of silicon nanoparticles with an average particle size of 10 nm or 30 nm is filled in a mold 3 with an inner diameter of 10 mm and heated at a current value of 1000 A while applying a pressure of 0.1 kN. In this embodiment, the displacement of the first punch 5a and the second punch 5b are monitored, and when the displacement reaches a specified value, heating is stopped, thereby cooling. Through such control based on the displacement, the thermal conductivity of the silicon bulk thermoelectric conversion material 100 can be controlled.
[0051] By suppressing the conduction of electricity from the first punch 5a or the second punch 5b to the mold 3 and conducting the conduction of electricity from the first punch 5a or the second punch 5b to the silicon powder 25, the heating of the surfaces of the silicon nanoparticles 110 in contact with each other is promoted to achieve high-speed sintering. Such conduction of electricity can be achieved by pressurizing the silicon powder 25 at a low pressure that has not been previously available as described above. In one embodiment, a current is allowed to flow while a pressure of less than 12 MPa, preferably less than 10 MPa, less than 5 MPa, or less than 3 MPa is applied between the first punch 5a and the second punch 5b. In this embodiment, the silicon powder 25 itself disposed inside the heating portion is heated to promote the heating of the surfaces of the silicon nanoparticles 110 in contact with each other.
[0052] Therefore, if Figure 3 As shown, in the method for preparing the silicon bulk thermoelectric conversion material 100 according to the present embodiment, the current is increased more rapidly than before, and the silicon powder 25 is rapidly heated to the sintering temperature. In addition, since powder is used as the raw material, the first punch 5a or the second punch 5b moves more rapidly than before while sintering is proceeding, and the silicon bulk thermoelectric conversion material 100 is formed.
[0053] In addition, in the present embodiment, since the conduction of electricity from the first punch 5a or the second punch 5b to the mold 3 is suppressed, the temperature rise of the mold 3 is also suppressed. Therefore, after sintering, by cutting off the current flowing to the first punch 5a or the second punch 5b, the heat of the sintered silicon bulk thermoelectric conversion material 100 is released into the mold 3 in a relatively low temperature state, and further released to the outside of the heating unit. Therefore, in the present embodiment, the silicon bulk thermoelectric conversion material 100 can be cooled rapidly, which was not previously possible, and the grain growth can be suppressed. Such rapid cooling generates a large tensile stress near the surface of the silicon nanoparticles 110.
[0054] In the present embodiment, by heating the temperature of the silicon powder 25 to a range of 800°C to 1200°C, the uniformity of the sintering temperature of the silicon powder 25 can be improved, and as a result, a silicon bulk thermoelectric conversion material 100 having a ZT greater than 0.1 can be prepared in a range of 22°C to 25°C. It should be noted that if the heating temperature of the silicon powder 25 is lower than 800°C, the silicon nanoparticles constituting the silicon powder 25 will not be able to bond with each other, and the porosity of the silicon powder 25 will not be reduced, so a sintered body cannot be obtained. On the other hand, if the temperature of the silicon powder 25 exceeds 1200°C, the silicon nanoparticles constituting the silicon powder 25 melt, and the cavities 120 between the silicon nanoparticles 110 are reduced or disappear, and the silicon bulk thermoelectric conversion material 100 according to the present invention having a ZT greater than 0.1 in the range of 22°C to 25°C cannot be obtained. In this specification, the "sintering temperature" is the highest temperature reached during sintering, and is evaluated by the temperature of the mold 3 measured with a radiation thermometer. It should be noted that, although the process of pressurizing and plasma sintering also depends on the filling amount of silicon powder 25, it is preferably carried out for more than 90 seconds and less than 150 seconds. It should be noted that, in this specification, the sintering time when preparing the silicon bulk thermoelectric conversion material 100 refers to the time from the time when sintering starts to the time when the current of the spark plasma sintering device 1 is cut off.
[0055] In this embodiment, the silicon nanoparticles contained in the silicon powder 25 are preferably 10 nm or more and 50 nm or less. In this specification, the particle size of the silicon nanoparticles contained in the silicon powder 25 is measured by the focusing method of X-ray diffraction. In one embodiment, the silicon powder 25 may contain the above-mentioned dopant.
[0056] [Thermoelectric conversion element] Figure 4Schematic diagram of a thermoelectric conversion element 500 according to one embodiment of the present invention. Thermoelectric conversion element 500 includes an N-type thermoelectric conversion material forming component 501; a P-type thermoelectric conversion material forming component 503; a first electrode 511, connecting a first end of the N-type thermoelectric conversion material forming component 501 and a first end of the P-type thermoelectric conversion material forming component 503; a second electrode 513, arranged at a second end opposite to the first end of the N-type thermoelectric conversion material forming component 501; and a third electrode 515, arranged at a second end opposite to the first end of the P-type thermoelectric conversion material forming component 503. The second electrode 513 and the third electrode 515 are connected to wiring 520. Figure 4 , the case where the first electrode 511 is at a high temperature, the second electrode 513 and the third electrode 515 are at a low temperature is shown, and the direction of the current is indicated by an arrow. The N-type thermoelectric conversion material forming part 501 is a part in which the thermoelectric conversion material doped with an N-type dopant described in the above-mentioned embodiment is formed into a shape suitable for the thermoelectric conversion element 500. In addition, the P-type thermoelectric conversion material forming part 503 is a part in which the thermoelectric conversion material doped with a P-type dopant described in the above-mentioned embodiment is formed into a shape suitable for the thermoelectric conversion element 500. In one embodiment, the N-type thermoelectric conversion material forming part 501 and the P-type thermoelectric conversion material forming part 503 have a thickness of 1 mm or more. The above-mentioned silicon bulk thermoelectric conversion material can be applied to such a part having a thickness of 1 mm or more. Example
[0057] In Example 1, a plasma high-speed discharge sintering device (manufactured by Sinterland Co., Ltd., LABOX-300 series) was used to place silicon powder (2% by weight phosphorus) mixed with 0.3 g of silicon nanoparticles (average particle size: 10 nm) and 0.006 g of phosphorus microparticles (average particle size: 45 μm) in a space surrounded by a graphite die 3 with an inner diameter of 10 mm, a first punch 5a, and a second punch 5b, and heated at a current value of 1000 A (current application speed 1000 A / 90 s) while applying a pressure of 1.27 MPa (0.1 kN). When the displacement of the first punch 5a and the second punch 5b reached a value set at 1.5 mm to 2.5 mm, the power supply was immediately stopped (the temperature measured by the radiation thermometer was about 950 to 1250° C.) and cooling was started, thereby obtaining Figure 5 The plurality of silicon bulk thermoelectric conversion materials with different thermal conductivities are indicated by □. The sintering time is about 90 seconds to 150 seconds. It should be noted that the sintering time is the time from the start of sintering to the cutting off of the current of the plasma high-speed discharge sintering device.
[0058] As Example 2, a silicon bulk thermoelectric conversion material of Example 2 was obtained by the same method as Example 1 except that silicon powder (2 wt % boron) mixed with boron particles (average particle size: 45 μm) was used instead of phosphorus particles.
[0059] Figure 3 The lower half of the figure shows the measurement results based on the radiation thermometer. Figure 3 The lower half of the figure shows the heating state of the graphite mold 3 and the silicon powder during sintering. In the sintering of this embodiment, since the pressure in the L1 direction is low when the power is turned on, the current selectively flows in the first punch 5a and the second punch 5b and the silicon powder. Therefore, as shown in FIG. Figure 3 As shown in the start heating in the figure, the center is heated and becomes hot. After that, as during heating, the surrounding graphite mold is also heated, but compared with the prior art, since the adhesion between the first punch 5a and the second punch 5b and the graphite mold 3 is low and the current flowing in the mold 3 is suppressed, it is observed that the temperature is lower than the center and not hot. As shown in the before stop point, the mold 3 is also fully heated before the sintering is about to stop, and at this time, it can be seen from the difference in the luminous intensity of the first punch 5a and the second punch 5b and the mold 3 that the temperature of the center becomes high. After sintering (after the stop point and fast sample cooling), the temperature of the mold 3 around the silicon powder is lower than that of the prior art, which helps to cool the silicon powder at a higher temperature. In addition, since the water-cooled electrode adjacent to the punch is at a low temperature, it helps to cool the sample through the spacer.
[0060] As Example 3, a silicon powder (2 wt% phosphorus) mixed with 0.3 g of silicon nanoparticles (average particle size: 30 nm) and 0.006 g of phosphorus microparticles (average particle size: 45 μm) was used, and heated at a current value of 850 A (current application rate 850 A / 90 s) while applying pressure at 1.27 MPa (0.1 kN). When the displacement of the first punch 5a and the second punch 5b reached a value set at 0.1 mm to 1.6 mm, the power supply was immediately stopped and cooling was started, thereby preparing Figure 5 A plurality of silicon bulk thermoelectric conversion materials having different thermal conductivities are shown in triangles.
[0061] [Relationship between the displacement of the punch and thermal conductivity] For the silicon bulk thermoelectric conversion materials of Example 1 and Example 3, the thermal conductivity was measured by the laser flash method. Specifically, by uniformly irradiating a pulsed laser on one surface of the silicon bulk thermoelectric conversion material, instantaneous heating is performed, and the temperature change of the other surface is measured to observe the state of thermal diffusion, thereby calculating the thermal diffusivity. Before the measurement, both sides of the silicon bulk thermoelectric conversion material were blackened using graphite spraying to improve the absorptivity of the pulsed laser. The measurement was carried out under vacuum conditions and while changing the temperature conditions (room temperature to 500°C). The thermal diffusivity was calculated by fitting the measured data using an analytical model. The specific heat capacity was calculated from the literature value of the specific heat, and the thermal conductivity was calculated from the product of the thermal diffusivity, the specific heat capacity and the density.
[0062] Figure 5 The relationship between the displacement of the first punch 5a and the second punch 5b and the thermal conductivity of the obtained silicon bulk thermoelectric conversion material is shown. Figure 5 The results show that the thermal conductivity of the silicon bulk thermoelectric conversion material is reduced when the displacement of the first punch 5a and the second punch 5b is small. This result can be inferred because the porosity of the cavities 120 between the silicon nanoparticles 110 is controlled by the displacement, which affects the structure of the joint 130 between the silicon nanoparticles 110, and the strain caused by the tensile stress 150 generated near the joint 130 helps control the thermal conductivity at the joint 130. That is, in the method for preparing the silicon bulk thermoelectric conversion material of this embodiment, the thermal conductivity can be controlled by the displacement.
[0063] [Measurement of electrical conductivity and Seebeck coefficient] The conductivity (resistivity) and Seebeck coefficient were measured using a thermoelectric evaluation device ZEM-3 manufactured by ULVAC Corporation. When the thermoelectric evaluation device was used for measurement, the silicon bulk thermoelectric conversion material was processed into a strip shape, and the electrodes were arranged in a manner opposite to the ends of the silicon bulk thermoelectric conversion material in the long axis direction for measurement. In the thermoelectric evaluation device, the conductivity (resistivity) and Seebeck coefficient were measured using a four-terminal lead method and a thermoelectric potential method, respectively. The resistance values of the silicon bulk thermoelectric conversion materials of Examples 1 and 2 are relatively low. When measured using the two-terminal method, the values of the contact resistance and the wiring resistance of the leads are also included in the measurement results. Since they have a large influence on the silicon bulk thermoelectric conversion material, the resistance value of the silicon bulk thermoelectric conversion material cannot be accurately measured. On the other hand, in the four-terminal lead method, by separating the leads through which the current flows and the leads through which the voltage is measured, the contact resistance or the wiring resistance of the leads can be separated from the resistance value of the silicon bulk thermoelectric conversion material, thereby enabling accurate measurement. The thermoelectric potential method for measuring the Seebeck coefficient generates a steady heat flow for the silicon bulk thermoelectric conversion material, generates a thermoelectric potential by forming a temperature gradient at both ends of the silicon bulk thermoelectric conversion material, and measures the temperature difference and potential difference with a probe, and calculates it using the following formula. S=ΔV / ΔT
[0064] In this measurement, the silicon bulk thermoelectric conversion material of Example 1 was processed into 1-3mm×1-3mm×6-8mm, and the side was ground and then set in the device. During the measurement, the chamber was replaced with He gas, and the measurement was carried out in the temperature range from room temperature to about 500°C. At this time, at each temperature for measurement, the temperature difference between the upper and lower electrodes was set to 30°C, 35°C and 40°C, and the average value of the Seebeck coefficient and resistivity obtained at each temperature difference was used. It should be noted that the measurement atmosphere temperature at this time is below 50°C.
[0065] Fig. 6A is a graph showing the relationship between the Seebeck coefficient and conductivity. Figure 6B This is a graph showing the relationship between ZT and temperature. Compared with the known nanostructured silicon bulk, if the Seebeck coefficient is the same, the silicon bulk thermoelectric conversion materials of Examples 1 and 2 show higher conductivity. In addition, the silicon bulk thermoelectric conversion materials of Examples 1 and 2 show excellent performance of ZT of 0.10 or more in the range of 22°C to 25°C.
[0066] [X-ray diffraction (XRD)] The crystallite size was calculated from the half-peak width measured by the silicon bulk thermoelectric conversion material using the Scherrer formula by the focusing method of X-ray diffraction. Among the silicon bulk thermoelectric conversion materials showing the best characteristics, the crystallite size was 35nm in the silicon bulk thermoelectric conversion material doped with an N-type dopant, and the crystallite size was 48nm in the silicon bulk thermoelectric conversion material doped with a P-type dopant, indicating that grain growth was suppressed by high-speed sintering.
[0067] [Raman spectroscopy] The Raman spectrum of the silicon bulk thermoelectric conversion material was obtained by using Raman spectroscopy (InVia (registered trademark) micro Raman system manufactured by Renishaw) with the laser wavelength set to 532 nm and the grating set to 3000. Fig. 7A Raman spectra are shown. Fig. 7A The Raman spectra of silicon bulk thermoelectric conversion materials with thermal conductivity ranging from low to high are shown. Fig. 7A It can be confirmed that due to high-speed sintering, a large tensile stress remains after the silicon nanoparticles are joined. On the other hand, in the silicon bulk thermoelectric conversion material with a thermal conductivity below a certain level, the silicon nanoparticles are not fully joined due to sintering, so the residual tensile stress becomes less, and it is confirmed that the tensile stress toward 520 cm -1 Side peak shift (return).
[0068] As Comparative Example 1, a plasma high-speed discharge sintering device (manufactured by Sinterland Co., Ltd., LABOX-300 series) was used to add silicon powder (2% by weight phosphorus) mixed with 0.3g of silicon nanoparticles (average particle size: 10nm) and 0.006g of phosphorus particles (average particle size: 45μm) to a graphite mold 3 with an inner diameter of 10mm, and the temperature was raised at 300℃ / min while being pressurized at 50MPa (4.2kN). The temperature was measured with a thermocouple, and when the temperature set between 980℃ and 1100℃ was reached, the sintering was performed by heating at this temperature for 10 minutes, then stopping the power supply and starting cooling, and various types of silicon bulk thermoelectric conversion materials with different thermal conductivity were obtained. The current was applied for more than 780 seconds.
[0069] [Sound velocity measurement] The sound velocity of the silicon bulk thermoelectric conversion material of Example 1 was measured using an ultrasonic thickness gauge (38DLP-XJ-MT-JA, Evident Co., Ltd.). In addition, the sound velocity of the silicon bulk thermoelectric conversion material of Comparative Example 1 was also measured. The probes used in the measurement were V222-BB (20MHz, transverse wave) and V1091 (5MHz, longitudinal wave). During the measurement, in order to increase the adhesion between the silicon bulk thermoelectric conversion material and the probe, SH-W25 and B2 gels were applied respectively, and the measurement was performed in the sound velocity measurement mode. In the sound velocity measurement mode, the sound velocity is calculated by inputting the measured value of the thickness and measuring the propagation time using the formula described below. Speed of sound = thickness × 2 / propagation time
[0070] It should be noted that the reason why the frequency of the shear wave probe is high is that it is difficult to distinguish the reflection peak from the initial excitation peak when measuring thin samples, so a high-frequency probe is used. In addition, in theory, interfaces and pores only contribute to the attenuation of the sound velocity signal and do not affect the sound velocity itself. However, when considering actual interfaces, sometimes differences in surface properties or amorphous phases are also included, rather than sharp interfaces, so it is presumed that they effectively affect the sound velocity.
[0071] Figure 7B The silicon bulk thermoelectric conversion material of Example 1 has a longitudinal wave (LA) of 6400 m / s or less and a transverse wave (TA) of 4200 m / s or less within the range of thermal conductivity of 1.0 W / m·K to 10.0 W / m·K.
[0072] In addition, according to Figure 7B The results show that there is a significant difference in the sound velocity between the silicon bulk thermoelectric conversion material of Example 1 and the silicon bulk thermoelectric conversion material of Comparative Example 1. Table 1 summarizes Figure 7B result. Table 1
[0073] This difference in sound velocity indicates that strain exists near the grain boundaries of the silicon nanoparticles in the silicon bulk thermoelectric conversion material of Example 1. It can be inferred that in the silicon bulk thermoelectric conversion material of Example 1, there is a lattice softening effect at the grain boundaries of the junctions of the silicon nanoparticles, which reduces the lattice thermal conductivity and contributes to the improvement of ZT.
[0074] [Uniformity of Silicon Bulk Thermoelectric Conversion Materials] The uniformity of the silicon bulk thermoelectric conversion material of Example 2 was evaluated. The disc-shaped silicon bulk thermoelectric conversion material of Example 2 was cut in the vertical direction to produce a measurement sample of 1 to 3 mm × 1 to 3 mm × 6 to 8 mm. The resistance and Seebeck coefficient of the measurement sample at the center and the adjacent measurement sample were measured. At this time, the measurement was performed at 25°C, but in order to give a temperature difference, the temperature of the measurement sample was made close to 50°C. The measurement results are as follows: Figure 8 As shown. Figure 8 The results show that the central part has a smaller resistance deviation than the adjacent parts. In addition, the power factor of the adjacent parts is not reduced by more than 30% compared with the central part. Therefore, the uniformity of the silicon bulk thermoelectric conversion material is shown. [Industrial Applicability]
[0075] In particular, the ability to produce nanostructured silicon with high thermoelectric performance in bulk size is extremely useful in industry. Due to the abundant deposits of silicon and the ability to utilize previous semiconductor processes, silicon is expected to be a cost-effective thermoelectric material. However, due to its low thermoelectric performance, it has not yet been put into practical use. The silicon bulk thermoelectric conversion material according to the present invention has successfully achieved high performance in bulk size, becoming an effective means to solve these problems. As a result, it can be expected that the popularization of thermoelectric power generation as IoT power sources, etc., will be rapidly carried out worldwide.
Claims
1. A method for preparing a bulk silicon thermoelectric conversion material, characterized in that, include: In the containment process, silicon powder containing silicon nanoparticles is placed between a first electrode component and a second electrode component of a heating section. The heating section includes a first electrode component, a second electrode component, and a conductive cylindrical component slidably fitted with at least one of the first electrode component and the second electrode component. The heating process involves heating the silicon powder by applying a pressure of less than 12 MPa between the first electrode component and the second electrode component while simultaneously passing an electric current; and The cooling process involves cooling the heated silicon powder.
2. The method for preparing bulk silicon thermoelectric conversion material according to claim 1, characterized in that, The cooling process includes: monitoring the displacement of the first electrode component and the second electrode component, and stopping heating when the displacement reaches a predetermined value.
3. The method for preparing the bulk silicon thermoelectric conversion material according to claim 1 or 2, characterized in that, It also includes a preparation step of mixing the silicon nanoparticles and dopant particles to prepare the silicon powder.
4. The method for preparing the bulk silicon thermoelectric conversion material according to claim 1 or 2, characterized in that, The average particle size of the silicon nanoparticles is less than 100 nm.
5. The method for preparing the bulk silicon thermoelectric conversion material according to claim 3, characterized in that, The dopant particles are phosphorus or boron particles with an average particle size of less than 100 μm.
6. A bulk silicon thermoelectric conversion material, characterized in that, Contains multiple silicon nanoparticles, The multiple silicon nanoparticles are bonded together on a portion of the surface. The bulk silicon thermoelectric conversion material is configured with cavities that separate the surfaces of the plurality of silicon nanoparticles from each other. In Raman spectroscopy, the bulk silicon thermoelectric conversion material exhibits a light intensity at 510 cm⁻¹. -1 Above 520cm -1 There is a peak below, and, The ZT value is above 0.10 within the range of 22℃ to 25℃.
7. The bulk silicon thermoelectric conversion material according to claim 6, characterized in that, When the weight of the silicon bulk thermoelectric conversion material is set to 100% by weight, it also contains 0.1% to 10% by weight of phosphorus or boron.
8. The bulk silicon thermoelectric conversion material according to claim 6, characterized in that, The thermal conductivity of the bulk silicon thermoelectric conversion material is in the range of 3.0 W / m·K to 6.0 W / m·K, and longitudinal waves propagate at a sound speed of less than 5800 m / s and transverse waves at a sound speed of less than 4200 m / s.
9. The bulk silicon thermoelectric conversion material according to claim 6, characterized in that, The thermal conductivity of the silicon bulk thermoelectric conversion material is in the range of 2.0 W / m·K to less than 3.0 W / m·K, and the longitudinal wave propagates at a sound speed of less than 5300 m / s and the transverse wave propagates at a sound speed of less than 3400 m / s.
10. The bulk silicon thermoelectric conversion material according to claim 6, characterized in that, The thermal conductivity of the bulk silicon thermoelectric conversion material is in the range of 3.0 W / m·K to less than 4.0 W / m·K, and the longitudinal wave propagates at a sound speed of less than 6100 m / s and the transverse wave at a sound speed of less than 3700 m / s.
11. The bulk silicon thermoelectric conversion material according to claim 6, characterized in that, The thermal conductivity of the bulk silicon thermoelectric conversion material is in the range of 4.0 W / m·K to 9.0 W / m·K, and longitudinal waves propagate at a sound speed of less than 6400 m / s and transverse waves at a sound speed of less than 4200 m / s.
12. A thermoelectric conversion element, characterized in that, A component comprising the bulk silicon thermoelectric conversion material as described in any one of claims 6 to 11, The thickness of the component is 1 mm or more.
13. A bulk silicon thermoelectric conversion material, characterized in that, Contains multiple silicon nanoparticles, The multiple silicon nanoparticles are bonded to each other on a portion of the surface; The bulk silicon thermoelectric conversion material contains cavities that separate the surfaces of the plurality of silicon nanoparticles from each other. The ZT calculated using conductivity measured at any ambient temperature within the range of 40°C to 50°C and Seebeck coefficient is greater than 0.
10.
14. The bulk silicon thermoelectric conversion material according to claim 13, characterized in that, When the weight of the silicon bulk thermoelectric conversion material is set to 100% by weight, it also contains 0.01% to 10% by weight of phosphorus or boron.
15. The bulk silicon thermoelectric conversion material according to claim 13, characterized in that, The thermal conductivity of the bulk silicon thermoelectric conversion material is in the range of 3.0 W / m·K to 6.0 W / m·K, and longitudinal waves propagate at a sound speed of less than 5800 m / s and transverse waves at a sound speed of less than 4200 m / s.
16. The bulk silicon thermoelectric conversion material according to claim 13, characterized in that, The thermal conductivity of the silicon bulk thermoelectric conversion material is in the range of 2.0 W / m·K to less than 3.0 W / m·K, and the longitudinal wave propagates at a sound speed of less than 5300 m / s and the transverse wave propagates at a sound speed of less than 3400 m / s.
17. The bulk silicon thermoelectric conversion material according to claim 13, characterized in that, The thermal conductivity of the bulk silicon thermoelectric conversion material is in the range of 3.0 W / m·K to less than 4.0 W / m·K, and the longitudinal wave propagates at a sound speed of less than 6100 m / s and the transverse wave at a sound speed of less than 3700 m / s.
18. The bulk silicon thermoelectric conversion material according to claim 13, characterized in that, The thermal conductivity of the bulk silicon thermoelectric conversion material is in the range of 4.0 W / m·K to 9.0 W / m·K, and longitudinal waves propagate at a sound speed of less than 6400 m / s and transverse waves at a sound speed of less than 4200 m / s.
19. A thermoelectric conversion element, characterized in that, A component comprising a bulk silicon thermoelectric conversion material as described in any one of claims 13 to 18, The thickness of the component is 1 mm or more.